Positive electrode active material, and positive electrode and lithium secondary battery comprising same

By controlling sulfur content in the synthesis of Mn-rich perlithium manganese oxide cathode materials, the challenges of high resistance and particle growth are addressed, resulting in improved energy density and stability for lithium secondary batteries.

WO2024219841A1PCT designated stage expired Publication Date: 2024-10-24LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005202
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-17
Filing Date
2024-04-18
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Mn-rich perlithium manganese oxide cathode materials exhibit high resistance and low rate characteristics due to slow oxidation/reduction reactions, limiting the commercialization of lithium secondary batteries, and existing methods to improve structural stability through increased firing temperature lead to excessive primary particle growth.

Method used

A positive electrode active material with a sulfur content of 4,000 ppm or more is synthesized by controlling sulfur-based impurities on the surface during manufacturing, using a method involving a transition metal-containing solution, ammonium cation complex former, and basic compound coprecipitation reaction, followed by water washing and calcination at 800°C to 950°C, which prevents excessive primary particle growth while enhancing structural completeness and lithium ion diffusion.

Benefits of technology

The approach results in improved resistance and capacity characteristics by maintaining a short lithium migration distance and low diffusion resistance, achieving higher energy density and reduced manufacturing costs while minimizing the use of expensive cobalt, with enhanced structural stability and prolonged battery lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005202_24102024_PF_FP_ABST
    Figure KR2024005202_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a positive electrode active material comprising an overlithiated manganese oxide represented by chemical formula 1, with a sulfur content of 4,000 ppm or more on the basis of the total weight of the positive electrode active material as measured at the surface, a method for manufacturing same, and a positive electrode and lithium secondary battery, each containing same.
Need to check novelty before this filing date? Find Prior Art

Description

Cathode active material, cathode containing same, and lithium secondary battery

[0001] Cross-citation with related application(s)

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0050981, filed April 18, 2023; and Korean Patent Application No. 10-2024-0051382, filed April 17, 2024, the entire contents of which are incorporated herein by reference.

[0003] The present invention relates to a manganese-rich cathode active material and a method for producing the same, which improves the lifespan by controlling the content of S-based impurities present on the surface, and to a cathode and a lithium secondary battery including the cathode active material.

[0004]

[0005] Lithium secondary batteries have been used as an energy storage medium in a variety of fields since their commercialization in 1991. As the market for products equipped with lithium secondary batteries expands, research is actively underway to increase their energy density. One of the most notable approaches is the development of cathode active materials with a composition that allows for greater lithium availability than previously possible.

[0006] As positive electrode active materials that can utilize more lithium, perlithium-based transition metal oxides with a layered structure and a molar ratio of lithium to transition metal exceeding 1 are being developed. These perlithium-based transition metal oxides can realize high capacities because they utilize not only the cation redox of the transition metal but also the anion redox using oxygen within the positive electrode structure to realize capacity. A representative perlithium-based transition metal oxide that is currently being actively researched is perlithium manganese-based oxides (hereinafter referred to as Mn-rich perlithium manganese-based oxides) in which the molar ratio of lithium to transition metal exceeds 1 and the manganese content among the total transition metals exceeds 50 mol%.

[0007] However, since Mn-rich lithium manganese oxides have low rate characteristics, i.e. high resistance, they are mainly manufactured in the form of secondary particles in which primary particles are aggregated to reduce the lithium movement distance and lower the diffusion resistance. However, if the sintering temperature is raised to improve the structural stability, the size of the primary particles increases and the resistance cannot be improved. Therefore, a technology is needed that can increase the sintering temperature to increase the structural completeness while not increasing the size of the primary particles beyond a certain level.

[0008]

[0009] Prior art literature

[0010] Patent documents

[0011] KR 2019-0052103 A

[0012]

[0013] The present invention aims to provide a cathode active material and a method for manufacturing the same, which increases structural perfection while not excessively increasing the size of primary particles by controlling the amount of S-based impurities to remain on the surface at a certain level during the synthesis of the cathode active material.

[0014]

[0015] According to one embodiment, the present invention,

[0016] Contains a lithium manganese oxide represented by the following chemical formula 1,

[0017] A cathode active material is provided, the sulfur content of which is 4,000 ppm or more based on the total weight of the cathode active material.

[0018] [Chemical Formula 1]

[0019] Li 1+a [Mn 1-(b+c) Ni b M c ]O2

[0020] In the above chemical formula 1,

[0021] M is at least one selected from the group consisting of Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg, B, W, Ga, In, Ru, Nb, Sn, Sr, and Zr,

[0022] 0.1≤a≤0.5, 0≤b<0.5, 0≤c≤0.1, 0≤a+b+c≤0.5.

[0023]

[0024] According to another embodiment, the present invention,

[0025] A step of forming precursor particles for a cathode active material by supplying a transition metal-containing solution containing nickel and manganese sulfate or sulfide, an ammonium cation complex forming agent, and a basic compound to a reactor and performing a co-precipitation reaction;

[0026] A step of manufacturing a precursor for a positive electrode active material by washing the precursor particles for the positive electrode active material with water; and

[0027] A method for producing the above-described positive electrode active material is provided, comprising a step of mixing a precursor for the positive electrode active material and a lithium raw material and calcining at 800°C to 950°C.

[0028]

[0029] According to another embodiment, the present invention provides a positive electrode for a lithium secondary battery comprising the positive electrode active material described above.

[0030]

[0031] According to another embodiment, the present invention provides a lithium secondary battery comprising the above-described positive electrode; a negative electrode including a negative electrode active material; a separator interposed between the positive electrode and the negative electrode; and an electrolyte.

[0032]

[0033] The present invention provides a method for manufacturing a cathode active material including a Mn-rich lithium manganese oxide having low rate characteristics, wherein the structural stability can be increased while the excessive growth of primary particles can be suppressed by controlling the content of sulfur-based impurities without a separate additional process.

[0034] The cathode active material manufactured in this way has the advantage of excellent resistance and capacity characteristics because the lithium movement distance is short and the diffusion resistance is low.

[0035]

[0036] Figure 1 is a photograph of the positive electrode active material particles manufactured in Example 1 and Comparative Example 1 observed at a magnification of 50k using a scanning electron microscope (SEM).

[0037] Figure 2 is a photograph of the positive electrode active material particles manufactured in Example 1 and Comparative Example 1 observed at a magnification of 20k using a scanning electron microscope (SEM).

[0038] Figure 3 is a photograph of the positive electrode active material particles manufactured in Example 1 and Comparative Example 1 observed at a magnification of 5k using a scanning electron microscope (SEM).

[0039] Figure 4 is a photograph of the positive electrode active material particles manufactured in Comparative Example 2 observed at magnifications of 5k, 20k, and 50k using a scanning electron microscope (SEM).

[0040]

[0041] Hereinafter, the present invention will be described in more detail.

[0042]

[0043] A cathode active material comprising a Mn-rich lithium manganese oxide having a manganese content exceeding 50 mol% among all metals excluding lithium not only has a higher energy density than the currently commercialized lithium nickel cobalt manganese (NCM) active material, but also has the advantage of reducing the manufacturing cost by reducing the amount of expensive cobalt used.

[0044] However, Mn-rich cathode materials have the disadvantage of high resistance and low rate characteristics because the oxidation / reduction reaction of oxygen ions and Mn ions proceeds relatively slowly. Therefore, improvement of these is essential for commercialization of lithium secondary batteries using Mn-rich cathode materials.

[0045] Accordingly, the inventors of the present invention, when manufacturing a cathode active material including Mn-rich lithium manganese oxide, performed washing only with water that did not contain a separate flux material during the precursor cleaning process, thereby controlling the content of residual sulfur to 4,000 ppm or more with respect to the total weight of the cathode active material, and confirmed that through this, the structural completeness of the cathode active material could be increased while the resistance characteristics could be lowered.

[0046] Specifically, when the heat treatment temperature is increased during the mixing and heat treatment of the precursor for the positive electrode active material and the lithium raw material during the manufacturing of the positive electrode active material, the crystallinity of the particles can be improved and the degree of sintering can be improved. However, in the case of lithium manganese oxide, the problem of increased resistance occurs as the size of the primary particles increases due to the high heat treatment temperature. In this case, when the sulfur content in the positive electrode active material is 4,000 ppm or more, the process of growing the primary particles is hindered, so excessive growth of the primary particles can be prevented by heat treatment at a high temperature.

[0047] That is, by increasing the sintering temperature, the crystal size can be secured to a certain level while preventing the growth of primary particles, so that the shape of secondary particles in which primary particles are aggregated is maintained while the movement distance of lithium ions is shortened, thereby reducing the diffusion resistance.

[0048] In the present invention, the sulfur may exist in the form of, for example, metal sulfate (MeSO4), and the content of sulfur refers only to the content of the S element.

[0049]

[0050] In the present invention, the “sulfur content” means the content of elemental sulfur in a positive electrode active material obtained through ICP analysis, and specifically means the result of mixing 0.1 g of the positive electrode active material to be analyzed with 2 mL of distilled water and 1 mL of concentrated nitric acid, diluting it with 50 mL of ultrapure water, and then analyzing it using an ICP-OES (PERKIN-ELMER, Optima 7300DV) device.

[0051] In the present invention, “primary particle” means a particle unit that has no apparent grain boundary when observed at a magnification of 5,000 to 20,000 times using a scanning electron microscope, and “secondary particle” means a particle formed by agglomeration of multiple primary particles.

[0052] In the present invention, the "average particle diameter of primary particles" refers to the arithmetic mean value calculated by measuring the particle diameters of at least 20 primary particles observed in scanning electron microscope images. Here, the particle diameter refers to the longest axis diameter of the primary particles.

[0053] In the present invention, "D 50" refers to the particle size corresponding to 50% of the volume accumulation in the volume accumulation particle size distribution of the corresponding particle powder, and can be measured using a laser diffraction method. For example, after dispersing the positive electrode active material powder in a dispersion medium, it can be measured by introducing it into a commercially available laser diffraction particle size measuring device (e.g., S-3500 from Microtrac) and irradiating it with ultrasonic waves of about 28 kHz at an output of 60 W, obtaining a volume accumulation particle size distribution graph, and finding the particle size at the point where the volume accumulation amount is 50% in the obtained volume accumulation particle size distribution graph.

[0054] In the present invention, "crystallite" refers to a particle unit having substantially the same crystal orientation, which can be confirmed through EBSD (Electron Backscatter Diffraction) analysis. Specifically, it refers to the smallest particle unit displayed in the same color in an IPF map obtained by EBSD analysis of a cross-section of a positive active material cut through ion milling.

[0055] Meanwhile, in the present invention, the "average crystallite size" can be quantitatively analyzed using X-ray diffraction analysis (XRD) using Cu Kα X-rays. Specifically, the average crystallite size of the crystal grains can be quantitatively analyzed by putting the particles to be measured into a holder, irradiating the particles with X-rays, and analyzing the diffraction grating that is generated. Sampling was prepared by putting the powder sample of the particles to be measured into the groove in the center of a general powder holder, smoothing the surface using a slide glass, and ensuring that the sample height is the same as the edge of the holder. Then, X-ray diffraction analysis was performed using a Bruker D8 Endeavor (light source: Cu Kα, λ=1.54Å) equipped with a LynxEye XE-T position sensitive detector, under the conditions of a FDS of 0.5°, a step size of 0.02°, and a total scan time of approximately 20 minutes in the range of 2θ=15° to 90°. For the measured data, Rietveld refinement was performed considering the charge (+3 for metal ions at transition metal sites, +2 for Ni ions at Li sites) and cation mixing at each site. When analyzing the grain size, instrumental brodadening was considered using the Fundamental Parameter Approach (FPA) implemented in the Bruker TOPAS program, and the entire peaks of the measurement range were used for fitting. The peak shape was fitted using only the Lorenzian contribution as the First Principle (FP) among the peak types available in TOPAS, and strain was not considered at this time.

[0056] In the present invention, the "BET specific surface area" is calculated using the BET (Brunauer-Emmett-Teller) multi-point method from a nitrogen adsorption isotherm under a 77K liquid nitrogen atmosphere obtained using BELSORP-MAX (MicrotracBEL corp.).

[0057]

[0058] positive electrode active material

[0059] The positive electrode active material according to the present invention includes a lithium manganese oxide represented by the following chemical formula 1, and the sulfur content may be 4,000 ppm or more, preferably 4,000 ppm to 8,000 ppm, and more preferably 5,000 ppm to 7,000 ppm based on the total weight of the positive electrode active material.

[0060] [Chemical Formula 1]

[0061] Li 1+a [Mn 1-(a+b+c) Ni b M c ]O2

[0062] In the above chemical formula 1,

[0063] M is at least one selected from the group consisting of Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg, B, W, Ga, In, Ru, Nb, Sn, Sr, and Zr,

[0064] 0.1≤a≤0.5, 0≤b<0.5, 0≤c≤0.1, 0≤a+b+c≤0.5.

[0065]

[0066] As described above, however, when the sulfur content in the positive electrode active material is 4,000 ppm or more, excessive growth of primary particles can be prevented even during high-temperature heat treatment. However, when the sulfur content becomes excessively high, the problem of capacity reduction due to an increase in the impurity ratio can be aggravated. Therefore, it is necessary to control the sulfur content taking this into consideration.

[0067] Meanwhile, in the above chemical formula 1, a is the molar ratio of Li in the lithium manganese oxide, and may be 0.1≤a≤0.5, 0.1≤a≤0.4, or 0.12≤a≤1.17. When a satisfies the above range, high capacity can be achieved.

[0068] The above b is the molar ratio of Ni in the lithium manganese oxide, and may be 0≤b<0.5, 0.1≤b≤0.4, or 0.25≤b≤0.35.

[0069] The above c is a molar ratio of the doping element M in the lithium manganese oxide, and may be 0≤c≤0.1, 0≤c≤0.05, or 0≤c≤0.01. The above doping element M may preferably be Co, and if the content of the doping element is too high, it may not only have a negative effect on the capacity of the active material, but also increase the oxygen-redox reaction, which may aggravate gas generation and deterioration of the positive electrode active material, and may deteriorate the life characteristics.

[0070] The above 1-(a+b+c) is the molar ratio of Mn in the lithium manganese oxide, and may be 0≤a+b+c≤0.5, 0≤a+b+c<0.5, or 0.35≤a+b+c≤0.45. When a+b+c exceeds 0.5, that is, when 1-(a+b+c) is less than 0.5, the proportion of the rock salt phase becomes too small, so the effect of improving structural stability is minimal.

[0071] Preferably, in the above chemical formula 1, 0.1≤a≤0.4, 0.1≤b≤0.4, 0≤c≤0.05, 0≤a+b+c<0.5 may be satisfied, and more preferably, 0.12≤a≤0.17, 0.25≤b≤0.35, 0≤c≤0.01, 0.35≤a+b+c≤0.45 may be satisfied.

[0072]

[0073] Meanwhile, in the lithium manganese oxide represented by the above chemical formula 1, the molar ratio of Li to the molar ratio of all metal elements excluding Li (Li / Me) may be 1.1 to 1.5, preferably 1.1 to 1.4, and more preferably 1.12 to 1.17. When the Li / Me ratio satisfies the above range, the rate characteristics and capacity characteristics are excellent. If the Li / Me ratio is too high, the electrical conductivity may decrease and the rock salt phase (Li2MnO3) may increase, which may accelerate the degradation rate, and if it is too low, the effect of improving the energy density is minimal.

[0074] Meanwhile, in the case of lithium manganese oxide containing an excess of lithium, it has a structure in which a layered phase (LiM'O2) and a rock salt phase (Li2MnO3) are mixed, and the composition of the lithium manganese oxide can be represented by the following chemical formula 2.

[0075] [Chemical Formula 2]

[0076] X Li2MnO3·(1-X)Li[Ni 1-y-z Mn y M z ]O2

[0077] In the above chemical formula 2,

[0078] M is at least one selected from the group consisting of Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg, B, W, Ga, In, Ru, Nb, Sn, Sr, and Zr,

[0079] 0.1≤X≤0.5, 0.4≤y<1, 0≤z≤0.2.

[0080] The above X represents the ratio of Li2MnO3 phase in the lithium manganese oxide, and the above y and z represent the molar ratio of Mn and doping element M in the LiM'O2 layer, respectively.

[0081] Meanwhile, the cathode active material according to the present invention may further include a coating layer on the surface of the lithium manganese oxide, if necessary. When the cathode active material includes a coating layer, the contact between the lithium manganese oxide and the electrolyte is suppressed by the coating layer, thereby reducing electrolyte side reactions, thereby improving the life characteristics.

[0082] The above coating layer comprises a coating element M 1 may include the coating element M 1 For example, the coating element M may be at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr and Zr, preferably Al, Co, Nb, W and combinations thereof, and more preferably Al, Co and combinations thereof. 1 It may contain two or more kinds, for example, it may contain Al and Co.

[0083] The above coating element is in the form of oxide within the coating layer, i.e., M 1 It can exist as Oz(1≤z≤4).

[0084] The above coating layer can be formed through methods such as dry coating, wet coating, chemical vapor deposition (CVD), physical vapor deposition (PVD), and atomic layer deposition (ALD). Among these, formation through atomic layer deposition is preferable because it can form a large coating layer area.

[0085] The formation area of ​​the above coating layer may be 10% to 100%, preferably 30% to 100%, and more preferably 50% to 100%, based on the total surface area of ​​the lithium manganese oxide particles. When the formation area of ​​the coating layer satisfies the above range, the effect of improving the life characteristics is excellent.

[0086]

[0087] Meanwhile, the positive electrode active material according to the present invention may be in the form of secondary particles in which a plurality of primary particles are aggregated, and the average particle diameter of the primary particles may be 0.01 μm to 5 μm, preferably 0.01 μm to 2 μm, and more preferably 0.01 μm to 0.1 μm. In order to improve structural stability, the average particle diameter of the primary particles increases as sintering is performed above a certain temperature, but when the average particle diameter of the primary particles exceeds 5 μm, the lithium movement distance increases, which is not preferable because the diffusion resistance increases.

[0088] In addition, D of the above positive electrode active material 50 , i.e. D of the secondary particle 50 It may be 2㎛ to 15㎛, preferably 2㎛ to 13㎛, more preferably 5㎛ to 12㎛. D of the positive electrode active material 50 When this above range is satisfied, the electrode density can be implemented excellently, and the deterioration of capacity and rate characteristics can be minimized.

[0089] In addition, the average crystallite size of the positive electrode active material may be 20 nm to 150 nm, preferably 20 nm to 100 nm, and more preferably 60 nm to 100 nm. In terms of enhancing crystallinity, a larger average crystallite size is desirable, but considering the resulting increase in resistance, it is desirable that it does not exceed 150 nm.

[0090] In addition, the BET specific surface area of ​​the above positive electrode active material is 0.1 m 2 / g to 10m 2 / g, specifically 1m 2 / g to 6m 2 / g, more specifically 1.2m 2 / g to 3m 2 / g. If the BET specific surface area of ​​the positive electrode active material is too low, the reaction area with the electrolyte is insufficient, making it difficult to realize sufficient capacity. If the specific surface area is too high, moisture absorption is rapid, and side reactions with the electrolyte are accelerated, making it difficult to secure life characteristics.

[0091]

[0092] Method for manufacturing positive electrode active material

[0093] The method for producing a positive electrode active material according to the present invention comprises the steps of: supplying a transition metal-containing solution containing sulfate or sulfide of nickel and manganese, an ammonium cation complex forming agent, and a basic compound to a reactor while performing a co-precipitation reaction to form precursor particles for a positive electrode active material; washing the precursor particles for a positive electrode active material with water to produce a precursor for a positive electrode active material; and mixing the precursor for a positive electrode active material with a lithium raw material and calcining the mixture at 800°C to 950°C.

[0094] The step of forming the precursor particles for the above-mentioned positive electrode active material may be prepared by, for example, dissolving each transition metal-containing raw material in a solvent to prepare a transition metal-containing solution, then mixing the transition metal-containing solution, an ammonium cation complex forming agent, and a basic compound, and then performing a coprecipitation reaction. In addition, an oxidizing agent or oxygen gas may be additionally added during the coprecipitation reaction, if necessary.

[0095] Meanwhile, the transition metal-containing raw material may be an acetate, carbonate, nitrate, sulfate, halide, sulfide, etc. of each transition metal. However, the transition metal-containing solution of the present invention contains a sulfate or sulfide of nickel and manganese. Specifically, the transition metal-containing raw material may be NiO, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, nickel sulfide, Mn2O3, MnO2, Mn3O4, MnCO3, Mn(NO3)2, MnSO4·H2O, manganese acetate, manganese halide, manganese sulfide, etc., and the transition metal-containing solution contains at least one selected from the group consisting of NiSO4, NiSO4·6H2O, nickel sulfide, MnSO4·H2O, and manganese sulfide.

[0096] The above ammonium cation complex forming agent may be at least one selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and NH4CO3.

[0097] The basic compound may be at least one selected from the group consisting of NaOH, Na2CO3, KOH, and Ca(OH)2. The form of the precursor may vary depending on the type of basic compound used. For example, when NaOH is used as the basic compound, a precursor in the form of a hydroxide may be obtained, and when Na2CO3 is used as the basic compound, a precursor in the form of a carbonate may be obtained. In addition, when a basic compound and an oxidizing agent are used together, a precursor in the form of an oxide may be obtained.

[0098] Meanwhile, the precursor for the positive electrode active material may be in the form of a hydroxide, oxide or carbonate.

[0099]

[0100] In one embodiment of the present invention, the step of washing the precursor particles for the positive electrode active material with water can be performed using deionized water, and it is preferable that no other substances other than water be added during the washing process. In a typical precursor washing step, a flux material such as NaOH is used, but in this case, it is difficult for the sulfur content to remain above 4,000 ppm.

[0101] Specifically, the washing is preferably performed by stirring the precursor particles at a temperature of 20°C to 30°C, adjusting the weight ratio of the precursor and water to 2:1 to 10:1, and at 1,000 rpm to 3,000 rpm for 10 minutes. After the washing, the particles are filtered and dried by exposing them to a temperature of 100°C to 150°C for 5 to 15 hours.

[0102]

[0103] Meanwhile, examples of the lithium raw material include lithium-containing carbonates (e.g., lithium carbonate, etc.), hydrates (e.g., lithium hydroxide hydrate (LiOH·H2O)), hydroxides (e.g., lithium hydroxide, etc.), nitrates (e.g., lithium nitrate (LiNO3)), chlorides (e.g., lithium chloride (LiCl)), etc., and one of these may be used alone or a mixture of two or more may be used.

[0104] Meanwhile, the precursor for the positive electrode active material and the lithium raw material can be mixed in an amount such that the molar ratio of the total transition metal (Ni+Co+Mn):Li is 1:1.1 to 1:1.5, preferably 1:1.1 to 1:1.4, and more preferably 1:1.12 to 1:1.17.

[0105] Meanwhile, the firing may be performed at a temperature of 800°C to 950°C, preferably 850°C to 950°C, and more preferably 870°C to 920°C. When the firing temperature is 800°C or higher, the structural completeness can be improved, but it is preferable not to exceed 950°C in order to prevent excessive growth of primary particles. The firing time may be 5 to 20 hours, and preferably 10 to 15 hours. In addition, the firing atmosphere may be an air atmosphere or an oxygen atmosphere, and for example, may be an atmosphere containing 20 to 100 volume% of oxygen.

[0106] In general, when manufacturing a cathode active material including Mn-rich lithium manganese oxide, if the sintering temperature is increased to 800°C or higher, there is a problem that the primary particle size becomes excessively large and the resistance increases. However, in the case of the present invention, if 4,000 ppm or more of sulfur remains on the surface, this can be prevented.

[0107]

[0108] Cathode and lithium secondary batteries

[0109] The positive electrode according to the present invention includes the positive electrode active material, and the lithium secondary battery according to the present invention includes the positive electrode, the negative electrode including the negative electrode active material; a separator interposed between the positive electrode and the negative electrode; and an electrolyte.

[0110] The positive electrode according to the present invention and the lithium secondary battery including the same can be manufactured through a conventional positive electrode and lithium secondary battery manufacturing method in the art, except that the positive electrode active material described above is used.

[0111] For example, a lithium secondary battery can be manufactured by sequentially stacking and drying electrode assemblies by interposing a separator between a positive electrode including a positive active material and a negative electrode including a negative active material, inserting the electrode assemblies into a case, injecting an electrolyte, and sealing the case. The lithium secondary battery can be a cylindrical, square, coin-shaped, or pouch-shaped battery.

[0112] The above positive and negative electrodes can be manufactured by applying a composition for forming an active material layer including an electrode active material on a current collector and then drying the composition.

[0113] The composition for forming a positive electrode active material layer may optionally further include a binder, a conductive material, a filler, etc. in addition to the positive electrode active material, as needed. The composition for forming a negative electrode active material layer may optionally further include a binder, a conductive material, a filler, etc. in addition to the negative electrode active material, as needed.

[0114] The current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the current collector can typically have a thickness of 3 ㎛ to 500 ㎛, and fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0115] The above positive electrode may further include a conventional positive electrode active material in addition to the positive electrode active material described above, for example, LCO (LiCoO2), LNO (LiNiO2), LFP (LiFePO4) and NCM (Li[Ni p Co q Mn r1]O2, 0<p<1, 0<q<1, 0<r1<1, p+q+r1=1) may further include one or more positive electrode active materials selected from the group consisting of, but preferably, only the positive electrode active material may be used alone.

[0116] The above positive electrode active material may be included in an amount of 80% to 99% by weight based on the total weight of the positive electrode active material layer.

[0117] In one embodiment of the present invention, the negative electrode may include at least one selected from the group consisting of a carbon-based material; a silicon-based material; a metal or an alloy of these metals and lithium; a metal composite oxide; a material capable of doping and dedoping lithium; lithium metal; and a transition metal oxide as a negative electrode active material, and preferably may include a carbon-based material, a silicon-based material, or a mixture thereof.

[0118] As the above carbon-based material, any carbon-based negative electrode active material commonly used in lithium secondary batteries can be used without particular limitation, and representative examples thereof include crystalline carbon, amorphous carbon, or a combination thereof. Examples of the above crystalline carbon include graphite such as natural graphite or artificial graphite in an amorphous, plate-like, flake-like, spherical, or fibrous form, and examples of the above amorphous carbon include soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide, calcined coke, etc.

[0119] The above silicon-based material is Si, SiO x (0 <x<2) 및 Si-Y 합금(상기 Y는 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 전이금속, 희토류 원소 및 이들의 조합 중 선택되는 원소이며, Si는 될 수 없음.) 중 선택된 1종 이상이고, 바람직하게는 SiO이다. 실리콘계 음극 활물질은 용량이 그라파이트 대비 약 10배 가까이 높아 질량 로딩(mg·cm -2) can be lowered to improve the rapid charging performance of the battery.

[0120] As the above metal or an alloy of these metals with lithium, a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn or an alloy of these metals with lithium may be used.

[0121] The above metal composite oxides include PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3(0≤x≤1), Li x WO2(0≤x≤1) and Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of group 1, 2, and 3 of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8)로 이루어진 군에서 선택된 1종 이상이 사용될 수 있다.

[0122] Materials capable of doping and dedoping the lithium include Sn, SnO2, Sn-Y (wherein Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), and at least one of these may be mixed with SiO2 for use.

[0123] In the above Si-Y and Sn-Y, the element Y may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db(dubnium), Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.

[0124] Examples of the above transition metal oxides include lithium-containing titanium composite oxide (LTO), vanadium oxide, and lithium vanadium oxide.

[0125] The above negative electrode active material may be included in an amount of 80 wt% to 99 wt% based on the total weight of the solid content in the negative electrode slurry.

[0126] The above binder is a component that assists in bonding between the conductive material, the active material, and the current collector, and is typically added in an amount of 0.1 wt% to 10 wt% based on the total weight of the active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0127] The conductive agent is a component for further improving the conductivity of the active material, and may be added in an amount of 10 wt% or less, specifically 5 wt% or less, based on the total weight of the active material layer. The conductive agent is not particularly limited as long as it has conductivity and does not cause a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber or metal fiber; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0128] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in lithium secondary batteries can be used without special restrictions, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. can also be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength can be used, and can optionally be used in a single-layer or multi-layer structure.

[0129] In addition, examples of the electrolyte include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.

[0130] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0131] The organic solvent may be used without any particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R represents a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a linear carbonate compound having low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.

[0132] The above lithium salt can be used without any special limitation as long as it is a compound that can provide lithium ions used in a lithium secondary battery. Specifically, the anion of the above lithium salt is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - At least one selected from the group consisting of, and the lithium salt is LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2) 2. LiCl, LiI, or LiB(C2O4)2 can be used. It is recommended that the concentration of the lithium salt be within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.

[0133] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 wt% based on the total weight of the electrolyte.

[0134]

[0135]

[0136] Hereinafter, the present invention will be described in more detail through specific examples.

[0137]

[0138] [Example: Preparation of positive electrode active material]

[0139] Example 1.

[0140] After adding 4 liters of distilled water to a co-precipitation reactor (capacity 20 L), the temperature was maintained at 50°C, and 100 mL of an ammonia aqueous solution having a concentration of 28 wt% was added. Then, a transition metal solution in which NiSO4 and MnSO4 were mixed so that the molar ratio of nickel:manganese = 35:65, an ammonia aqueous solution, and a sodium hydroxide solution were added to the co-precipitation reactor, and a co-precipitation reaction was performed to form a precursor. The precursor particles were separated, washed by stirring at 2,000 rpm for 10 minutes at a weight ratio of the precursor to ultrapure water of 5:1 at a temperature of 25°C, and then dried in an oven at 130°C to prepare a precursor.

[0141] The precursor synthesized by the coprecipitation reaction and LiOH were mixed so that the molar ratio of transition metal:Li was 1:1.3, and heat-treated at 900°C for 15 hours under an oxygen atmosphere to obtain Li 1.13 Ni 0.31 Mn 0.56 A cathode active material having a composition of O2 was manufactured. The manufactured cathode active material had an average particle diameter of primary particles of 0.05 ㎛ and a D of secondary particles of 50 This 10㎛, average crystallite size 80nm, BET specific surface area 1.5m 2 / g was.

[0142]

[0143] Comparative Example 1.

[0144] A positive electrode active material was prepared in the same manner as in Example 1, except that a 1 M NaOH aqueous solution was used instead of ultrapure water when washing the precursor particles in Example 1. The positive electrode active material prepared in Comparative Example 1 had an average particle size of primary particles of 0.2 μm and a D of secondary particles of 50 This 10㎛, average crystallite size 80nm, BET specific surface area 1.0m 2 / g was.

[0145]

[0146] Comparative Example 2.

[0147] A positive electrode active material was prepared in the same manner as in Example 1, except that a 0.5 M NaOH aqueous solution was used instead of ultrapure water when washing the precursor particles in Example 1. The positive electrode active material prepared in Comparative Example 2 had an average particle size of primary particles of 0.1 μm and a D of secondary particles of 50 This 10㎛, average crystallite size is 80nm, BET specific surface area is 1.2m 2 / g was.

[0148]

[0149] Example 2.

[0150] In the above Example 1, the precursor co-precipitation reaction time was controlled to a level where the D50 value of the precipitated precursor was 3 ㎛, and the weight ratio of the precursor and ultrapure water was changed from 5:1 to 2:1 when washing the precursor particles. A positive electrode active material was manufactured in the same manner as in Example 1, except that the positive electrode active material manufactured in Example 2 had an average particle size of primary particles of 0.05 ㎛ and a D50 value of secondary particles of 0.05 ㎛. 50 This 3㎛, average crystallite size is 80nm, BET specific surface area is 2.5m 2 / g was.

[0151]

[0152] Comparative Example 3.

[0153] A positive electrode active material was prepared in the same manner as in Example 2, except that a 0.5 M NaOH aqueous solution was used instead of ultrapure water when washing the precursor particles in Example 2. The positive electrode active material prepared in Comparative Example 3 had an average particle size of primary particles of 0.1 μm and a D of secondary particles of 50 This 3㎛, average crystallite size is 80nm, BET specific surface area is 1.7m 2 / g was.

[0154]

[0155] Comparative Example 4.

[0156] A positive electrode active material was prepared in the same manner as in Example 2, except that a 1 M NaOH aqueous solution was used instead of ultrapure water when washing the precursor particles in Example 2. The positive electrode active material prepared in Comparative Example 4 had an average particle size of primary particles of 0.2 μm and a D of secondary particles of 50 This 3㎛, average crystallite size is 80nm, BET specific surface area is 1.4m 2 / g was.

[0157]

[0158] [Experimental Example]

[0159] Experimental Example 1. Measurement of S content in positive electrode active material

[0160] 0.1 g of the positive electrode active material powder manufactured in the above Example 1-2 and Comparative Example 1-4 was mixed with 2 mL of distilled water and 1 mL of concentrated nitric acid, then diluted with 50 mL of ultrapure water. The content of elemental sulfur was measured using an ICP-OES (PERKIN-ELMER, Optima 7300DV) device. The results are shown in Table 1 below.

[0161] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 46,000ppm 6500ppm 1,500ppm 3,000ppm 3000ppm 2000ppm

[0162] Experimental Example 2. SEM Analysis

[0163] The photographs of the positive electrode active materials manufactured in Example 1 and Comparative Examples 1-2 observed at magnifications of 50k, 20k, and 5k using a scanning electron microscope (SEM) are shown in FIGS. 1 to 3.

[0164] It can be confirmed through the photograph that the positive electrode active material of Comparative Example 1-2 is composed of larger primary particles compared to the positive electrode active material of Example 1.

[0165]

[0166] Experimental Example 3. Coin Cell Performance Evaluation

[0167] 1) Manufacturing of the anode

[0168] The positive electrode active material of Example 1, conductive agent (carbon black), and binder (polyvinylidene fluoride) were added to N-methyl-2-pyrrolidone (NMP) in a weight ratio of 94:3:3 to prepare a positive electrode slurry having a solid content of 60 wt%. The positive electrode slurry was applied to a 15 μm thick aluminum (Al) film as a positive electrode current collector to a thickness of 45 μm, dried, and then roll pressed to obtain a loading of 2.8 mAh / cm. 2 A positive electrode was manufactured. In the same manner, positive electrodes using the positive electrode active materials of Example 2 and Comparative Examples 1-4 were also manufactured.

[0169] 2) Coin cell manufacturing

[0170] A negative electrode slurry having a solid content of 60 wt% was prepared by adding a negative electrode active material (Graphite), a binder (SBR-CMC), and a conductive agent (carbon black) to a solvent, water, in a weight ratio of 95:3.5:1.5. The negative electrode slurry was applied to a 10 μm thick copper (Cu) thin film as a negative electrode collector to a thickness of 67 μm, dried, and then roll pressed to obtain a loading of 3.0 mAh / cm. 2 A human negative electrode was manufactured.

[0171] For each of the positive electrode of Example 1-2 and the positive electrode of Comparative Example 1-4 manufactured in 1) above, a 15㎛ thick polyethylene separator was interposed between the positive electrode and the negative electrode to manufacture an electrode assembly, which was then placed inside a coin-shaped (2032 type) secondary battery case, and an electrolyte was injected into the case to manufacture a lithium secondary battery. At this time, an electrolyte in which 1M LiPF6 was dissolved in a mixed organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (EMC) was mixed in a volume ratio of 1:2 was injected to manufacture a lithium secondary battery.

[0172] 3) Life evaluation

[0173] Coin cells to which the positive electrode active materials of Examples 1-2 and Comparative Examples 1-4 were applied were formed at 45°C, and then charged at a rate of 0.5C in CCCV mode at 25°C until the voltage reached 4.4V. Thereafter, discharge was performed at a constant current of 0.5C until the voltage reached 2.5V, and the initial discharge capacity and initial resistance were measured. After performing 50 such charge and discharge cycles, the discharge capacity retention rate and resistance increase rate were measured, and the results are shown in Table 2 below.

[0174]

[0175] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 4 Comparative Example 5 Room temperature 1 cycle charge / discharge Initial discharge capacity [mAh / g] 200 205 198 198 200 195 Initial resistance [Ohm @SOC 100%] 28 25 30 29 2830 Room temperature 50 cycle charge / discharge Discharge capacity retention rate [%] 9 5 9 0 8 9 9 18 7 8 6 Resistance increase rate [%] 20 30 55 40 45 60

[0176] Through the results in Table 2 above, it can be confirmed that the coin cell using the positive electrode active material of Example 1-2, in which the content of elemental sulfur in the positive electrode active material is 4,000 ppm or more, shows improved values ​​in terms of initial capacity and initial resistance compared to the coin cell using the positive electrode active material of Comparative Example 1-4, in which the content of elemental sulfur is less than 4,000 ppm. This is a result that proves that even when the same firing temperature is applied, when the content of sulfur in the positive electrode active material is controlled, there is an effect of improving crystallinity and suppressing the growth of primary particles, thereby preventing an increase in resistance. In addition, in terms of capacity retention rate and resistance increase rate after 50 cycles, the coin cell using the positive electrode active material of Example 1-2 shows superior performance compared to the coin cell using the positive electrode active material of Comparative Example 1-4. This is because the stress during repeated charge and discharge processes is reduced as the primary particle size is controlled, resulting in improved capacity and resistance changes as the cycle progresses.

Claims

1. Contains a lithium manganese oxide represented by the following chemical formula 1, A cathode active material having a sulfur content of 4,000 ppm or more based on the total weight of the cathode active material: [Chemical Formula 1] Li 1+a [Mr 1-(a+b+c) Ni b M c ]O2 In the above chemical formula 1, M is at least one selected from the group consisting of Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg, B, W, Ga, In, Ru, Nb, Sn, Sr, and Zr, 0.1≤a≤0.5, 0≤b<0.5, 0≤c≤0.1, 0≤a+b+c≤0.

5.

2. In claim 1, A positive electrode active material having an average primary particle diameter of 0.01 ㎛ to 5 ㎛.

3. In claim 2, A positive electrode active material having an average primary particle diameter of 0.01 ㎛ to 0.1 ㎛.

4. In claim 1, D 50 A positive electrode active material having a size of 2㎛ to 15㎛.

5. In claim 1, A cathode active material having an average crystallite size of 20 nm to 150 nm.

6. In claim 1, A positive electrode active material in the above chemical formula 1, wherein 0.1≤a≤0.4, 0.1≤b≤0.4, 0≤c≤0.05, and 0≤a+b+c<0.

5.

7. In claim 1, A cathode active material having a sulfur content of 4,000 ppm to 8,000 ppm based on the total weight of the cathode active material.

8. A step of forming precursor particles for a cathode active material by supplying a transition metal-containing solution containing nickel and manganese sulfate or sulfide, an ammonium cation complex forming agent, and a basic compound to a reactor and performing a co-precipitation reaction; A step of manufacturing a precursor for a positive electrode active material by washing the precursor particles for the positive electrode active material with water; and A method for producing a positive electrode active material according to claim 1, comprising the step of mixing a precursor for the positive electrode active material and a lithium raw material and calcining at 800°C to 950°C.

9. In claim 8, A method for manufacturing a positive electrode active material, wherein no other substance is added other than water during the washing process.

10. A positive electrode comprising a positive electrode active material according to any one of claims 1 to 7.

11. The anode according to claim 9; A negative electrode comprising a negative active material; A separator interposed between the positive and negative electrodes; and A lithium secondary battery containing an electrolyte.

Citation Information

Patent Citations

  • Spray type bonding device for stability of liquid hard capsule and method thereof

    KR102122015B1

  • Positive electrode active material for lithium secondary battery, and secondary battery using same

    JP1998162830A

  • Positive electrode active material, positive electrode for lithium ion secondary battery, and lithium ion secondary battery

    JP2018163892A

  • Manufacturing method for Ni-Co-Mn composite precursor with high specific surface area

    KR1020180098735A

  • Coolant pump with defoaming function

    KR102338013B1