Positive electrode sheet, battery, and electric device

By optimizing the proportions of Ni, Fe, Mn and Al elements in the positive electrode film layer of secondary batteries, and combining the use of specific compounds, the problem of insufficient battery energy density and safety performance is solved, and higher energy density and safety performance are achieved. Security.

WO2024221340A1PCT designated stage expired Publication Date: 2024-10-31CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/091187
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing secondary batteries have deficiencies in energy density and safety performance, especially the negative impact of Ni element on battery safety performance, and their high thermal stability and oxygen release, making it difficult to meet the needs for high energy density and high safety.

Method used

By controlling the mass proportions of Ni, Fe, Mn and Al elements in the cathode film layer, combined with the use of compounds such as LiNibCodMneMfO2 and LiaAxMn1-yByP1-zCzO4-nDn, the composition of the cathode active material is optimized to improve the thermal stability and safety of the battery. performance, and improve battery safety through electrolyte salt selection.

Benefits of technology

It achieves higher energy density and higher safety of the battery, reduces the amount of oxygen released, improves the overall performance of the battery, and meets the demand for high energy density and safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023091187_31102024_PF_FP_ABST
    Figure CN2023091187_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides a positive electrode sheet, a battery, and an electric device. The positive electrode sheet of the present application comprises a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector; the positive electrode film layer comprises a positive electrode active material; the positive electrode active material comprises an element Ni, an element Fe, an element Mn, and an optional element Al; and the positive electrode sheet satisfies the following: 0<CNi / (CNi+CFe+CMn+CAl)≤90.10%.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode sheet, battery and power-using device Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a positive electrode sheet, a battery, and an electrical device. Background Art

[0002] In recent years, the application of secondary batteries has become increasingly widespread. They are widely used in energy storage power systems such as hydropower, thermal power, wind power, and solar power stations, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. As secondary batteries have achieved great development, higher requirements have been placed on their energy density and safety performance.

[0003] Summary of the Invention

[0004] This application is made in view of the above-mentioned problems, and its purpose is to provide a positive electrode plate, a battery and an electrical device. The positive electrode plate of this application can improve the safety performance of the battery.

[0005] To achieve the above-mentioned object, the first aspect of the present application provides a positive electrode sheet, comprising a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer comprises a positive electrode active material, wherein the positive electrode active material comprises Ni, Fe, Mn, and optionally Al;

[0006] Furthermore, the positive electrode plate satisfies: 0<C Ni / (C Ni +C Fe +C Mn +C Al )≤90.10%;

[0007] Among them, the C Ni is the mass content of Ni element in the positive electrode film layer, the C Fe is the mass content of Fe element in the positive electrode film layer, the C Mn is the mass content of Mn element in the positive electrode film layer, the C Al is the mass content of Al element in the positive electrode film layer.

[0008] The Ni element is a factor that negatively affects the safety performance of the battery. In addition, the Fe, Mn and Al elements have the function of improving thermal stability. The present application can improve the safety performance of the battery by controlling the mass proportion of the Ni element in the positive electrode film layer among the Ni, Fe, Mn and Al elements within the above range.

[0009] In any embodiment, the positive electrode sheet satisfies: 2.88%≤C Ni / (CNi +C Fe +C Mn +C Al )≤86.10%.

[0010] Therefore, the present application can make the battery have higher energy density and higher safety by controlling the mass ratio of Ni element in Ni, Fe, Mn and Al elements in the positive electrode film layer within the above range.

[0011] In any embodiment, the positive electrode active material includes a first positive electrode active material; the first positive electrode active material includes a compound LiNi b Co d Mn e M f O2; wherein, the M includes one or more elements selected from the group consisting of Mn, Al, Mg, Ca, Na, Ti, W, Zr, Sr, Cr, Zn, Ba, B, S, and Y, and may optionally include Mg and / or Al elements; the b value is 0.314-0.970; the d value is 0-0.320, and may optionally be 0.047-0.320; and the e value is 0.006-0.390; and the sum of b, d, e, and f is 1, and f is greater than or equal to 0.

[0012] In any embodiment, the first positive electrode active material satisfies: 1.65%≤m×b≤79.10%, optionally 1.65%≤m×b≤73.87%, wherein m is the mass content of the first positive electrode active material in the positive electrode active material.

[0013] Therefore, the positive electrode plate of the present application has higher thermal stability and lower oxygen release.

[0014] In any embodiment, in the first positive electrode active material, the molar ratio of Al element in the elements other than Li element and O element is 0-5%, optionally 0.5%-4%; and / or,

[0015] The molar ratio of the Mg element in the elements other than the Li element and the O element is 0-3%, and can be optionally 0.5% to 2.0%.

[0016] The appropriate amount of doping with Al and / or Mg elements is beneficial to improving the thermal stability of the positive electrode plate of the present application.

[0017] In any embodiment, the positive electrode active material further includes a second positive electrode active material; the second positive electrode active material comprises a compound Li a A x Mn 1-y B y P 1-z C z O4-n D n ; wherein, A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; C includes one or more elements selected from B (boron), S, Si and N; D includes one or more elements selected from S, F, Cl and Br; a is 0.9-1.1; x is 0-0.1; y is 0.001-0.5; z is 0.001-0.1; and n is 0-0.1.

[0018] In any embodiment, the second positive electrode active material includes a core and a shell covering the core; the core contains the compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n , the shell comprises carbon element.

[0019] In any embodiment, the second positive electrode active material includes a core and a shell covering the core, the shell including a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer; the core contains the compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n , the first coating layer comprises crystalline pyrophosphate Li g EP2O7 and / or E h (P2O7) i The second coating layer comprises crystalline phosphate X j PO4, the third coating layer contains carbon element;

[0020] Wherein, the crystalline pyrophosphate Li g EP2O7 and E h (P2O7) iwherein E independently includes one or more elements selected from the group consisting of Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al; X includes one or more elements selected from the group consisting of Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al; g is greater than 0 and less than or equal to 2; h is greater than 0 and less than or equal to 4; i is greater than 0 and less than or equal to 3; and j is greater than 0 and less than or equal to 3.

[0021] In any embodiment, the positive electrode active material consists of the first positive electrode active material and the second positive electrode active material.

[0022] Therefore, the present application improves the safety performance of the battery by using the first positive electrode active material and the second positive electrode active material in combination.

[0023] The second aspect of the present application further provides a battery, comprising the positive electrode sheet of the first aspect of the present application.

[0024] Therefore, the present application can improve the safety performance of the battery by controlling the mass ratio of the Ni element in the positive electrode film layer among the Ni, Fe, Mn and Al elements.

[0025] In any embodiment, the battery further includes an electrolyte containing an electrolyte salt; and the battery satisfies: 0<ρ×m×b≤79.1%, wherein ρ is the molar concentration of the electrolyte salt in the electrolyte, in mol / L; m is the mass content of the first positive electrode active material in the positive electrode active material.

[0026] Therefore, commonly used electrolyte salts are easily decomposed, and the safety of the battery can be further improved by controlling the range of the product of ρ, m and b.

[0027] In any embodiment, the electrolyte salt includes one or more of LiPF6, LiBF4, LiN(SO2F)2, LiN(CF3SO2)2, LiClO4, LiAsF6, LiB(C2O4)2 and LiBF2C2O4, and optionally includes one or more of LiPF6, LiN(SO2F)2 and LiN(CF3SO2)2.

[0028] A third aspect of the present application provides an electrical device comprising the battery according to the second aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] FIG1 is a schematic diagram of a secondary battery according to an embodiment of the present application.

[0030] FIG. 2 is an exploded view of the secondary battery according to the embodiment of the present application shown in FIG. 1 .

[0031] FIG3 is a schematic diagram of a battery module according to an embodiment of the present application.

[0032] FIG4 is a schematic diagram of a battery pack according to an embodiment of the present application.

[0033] FIG. 5 is an exploded view of the battery pack shown in FIG. 4 according to an embodiment of the present application.

[0034] FIG6 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.

[0035] Explanation of reference numerals: 1 battery pack; 2 upper case; 3 lower case; 4 battery module; 5 secondary battery; 51 housing; 52 electrode assembly; 53 top cover assembly. DETAILED DESCRIPTION

[0036] Below, the embodiments of the positive electrode sheet, secondary battery, battery module, battery pack and electric device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0037] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0038] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0039] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0040] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, a method includes steps (a) and (b), which indicates that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, a method may further include step (c), which indicates that step (c) may be added to the method in any order, for example, the method may include steps (a), (b), and (c), or may include steps (a), (c), and (b), or may include steps (c), (a), and (b), etc.

[0041] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may indicate that other components not listed may also be included or that only the listed components are included.

[0042] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0043] [Secondary battery]

[0044] Secondary batteries, also known as rechargeable batteries or storage batteries, are batteries that can be recharged to activate the active materials after discharge and continue to be used.

[0045] Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte. During the battery's charge and discharge process, active ions (such as lithium ions) are embedded and released back and forth between the positive and negative electrode sheets. The separator is set between the positive and negative electrode sheets, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The electrolyte between the positive and negative electrode sheets mainly plays the role of conducting active ions.

[0046] [Positive electrode]

[0047] One embodiment of the present application provides a positive electrode sheet, comprising a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer comprises a positive electrode active material, wherein the positive electrode active material comprises Ni, Fe, Mn, and optionally Al.

[0048] Furthermore, the positive electrode plate satisfies: 0<C Ni / (C Ni +C Fe +C Mn +C Al )≤90.10%;

[0049] Among them, the C Ni is the mass content of Ni element in the positive electrode film layer, the C Fe is the mass content of Fe element in the positive electrode film layer, the C Mn is the mass content of Mn element in the positive electrode film layer, the C Al is the mass content of Al element in the positive electrode film layer.

[0050] Although the mechanism is not yet clear, the applicant unexpectedly discovered that the Ni element is a factor that negatively affects the safety performance of the battery. In addition, the Fe, Mn and Al elements have the effect of improving thermal stability. The present application can improve the safety performance of the battery by controlling the mass proportion of the Ni element in the positive electrode film layer among the Ni, Fe, Mn and Al elements within the above range.

[0051] In some embodiments, the positive electrode sheet satisfies: 2.88%≤C Ni / (C Ni +C Fe +C Mn +C Al )≤86.10%, for example, C Ni / (C Ni +C Fe +C Mn +C Al ), 3%, 4%, 7%, 10%, 12%, 15%, 17%, 20%, 21%, 23%, 25%, 27%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 77%, 80%, 82%, 85%, 87%, 88%, 90%, or any range consisting of the above values.

[0052] Therefore, the present application can make the battery have higher energy density and higher safety by controlling the mass ratio of Ni element in Ni, Fe, Mn and Al elements in the positive electrode film layer within the above range.

[0053] In some embodiments, the positive electrode active material includes a first positive electrode active material; the first positive electrode active material includes a compound LiNi b Co d Mn e M f O2; wherein, the M includes one or more elements selected from the group consisting of Mn, Al, Mg, Ca, Na, Ti, W, Zr, Sr, Cr, Zn, Ba, B, S, and Y, and may optionally include Mg and / or Al; the b is 0.314-0.970, such as 0.400, 0.500, 0.600, 0.700, 0.800, 0.900, 0.950, and any of the above values; the d is 0-0.320, and may optionally be 0.047-0.320, such as 0.0 70, 0.090, 0.100, 0.150, 0.200, 0.250, 0.300, 0.310, 0.320, and the range consisting of any of the above values; the e is 0.006-0.390, for example, 0.008, 0.010, 0.050, 0.100, 0.150, 0.200, 0.250, 0.300, 0.320, 0.350, 0.370, and the range consisting of any of the above values; and the sum of b, d, e and f is 1 and f is greater than or equal to 0.

[0054] In some embodiments, the first positive electrode active material satisfies: 1.65%≤m×b≤79.10%, which can be optionally 1.65%≤m×b≤73.87%, for example, m×b is 2%, 3%, 5%, 7%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 50%, 60%, 65%, 70%, 71%, 72%, 73%, 75%, 76%, 78% and the range consisting of any of the above values, wherein m is the mass content of the first positive electrode active material in the positive electrode active material.

[0055] Therefore, the positive electrode plate of the present application has higher thermal stability and lower oxygen release.

[0056] In some embodiments, in the first positive electrode active material, the molar ratio of Al element in the elements other than Li element and O element is 0-5%, optionally 0.5%-4%, for example, 0.2%, 0.7%, 1%, 2%, 3%, 4%, 5% and the range of any of the above values; and / or,

[0057] The molar ratio of Mg in the elements other than Li and O is 0-3%, and can be selected from 0.5% to 2.0%, for example, 0.2%, 0.4%, 0.7%, 0.9%, 1%, 1.5%, 2%, 2.5%, 2.7%, 3% and the range consisting of any of the above values.

[0058] Appropriate doping of Al and / or Mg elements is beneficial to improving the thermal stability of the positive electrode plate of the present application.

[0059] In some embodiments, the positive electrode active material further comprises a second positive electrode active material; the second positive electrode active material comprises a compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n ; wherein, A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; C includes one or more elements selected from B (boron), S, Si and N; D includes one or more elements selected from S, F, Cl and Br; a is 0.9-1.1; x is 0-0.1, for example, 0, 0.02, 0.04, 0.05, 0.07, 0.08, 0.09, 0.1 and any of the above the range consisting of any numerical values; the y is 0.001-0.5, for example, 0.005, 0.01, 0.05, 0.07, 0.1, 0.2, 0.3, 0.4, 0.5 and the range consisting of the above arbitrary numerical values; the z is 0.001-0.1, for example, 0.001, 0.005, 0.008, 0.01, 0.03, 0.05, 0.07, 0.1 and the range consisting of the above arbitrary numerical values; the n is 0-0.1, for example, 0, 0.01, 0.02, 0.05, 0.07, 0.09, 0.1 and the range consisting of the above arbitrary numerical values.

[0060] In some embodiments, the second positive electrode active material includes a core and a shell covering the core; the core comprises a compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n , the shell comprises carbon element.

[0061] In some embodiments, the second positive electrode active material includes a core and a shell covering the core, the shell including a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer; the core includes a compound Li a A x Mn 1-yB y P 1-z C z O 4-n D n , the first coating layer comprises crystalline pyrophosphate Li g EP2O7 and / or E h (P2O7) i The second coating layer comprises crystalline phosphate X j PO4, the third coating layer contains carbon element;

[0062] Wherein, the crystalline pyrophosphate Li g EP2O7 and E h (P2O7) i wherein E independently comprises one or more elements selected from the group consisting of Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; wherein X comprises one or more elements selected from the group consisting of Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; wherein g is greater than 0 and less than or equal to 2, for example, 0.1, 0.5, 0.7, 1, 1.3, 1.5, 1.7, 1.9 and any range thereof; wherein h is greater than 0 and less than or equal to 4, for example, 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4 and any range thereof; wherein i is greater than 0 and less than or equal to 3, for example, 0.1, 0.5, 1, 1.5, 2, 2.5, 3 and any range thereof; wherein j is greater than 0 and less than or equal to 3, for example, 0.1, 0.5, 1, 1.5, 2, 2.5, 3 and any range thereof.

[0063] In some embodiments, LiNi b Co d Mn e M f O2、Li a A x Mn 1-y B y P 1-z C z O 4-n D n 、Li g EP2O7、E h (P2O7) i and X j PO4 is electrically neutral.

[0064] In some embodiments, the positive electrode active material consists of the first positive electrode active material and the second positive electrode active material.

[0065] Therefore, the present application improves the safety performance of the battery by using the first positive electrode active material and the second positive electrode active material in combination.

[0066] In some embodiments, the method for preparing the second positive electrode active material of the present application comprises the following steps:

[0067] Steps for providing core material: The core material contains Li a A x Mn 1-y B y P 1-z C z O 4-n D n , wherein A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo, and W; B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb, and Ge; C includes one or more elements selected from B (boron), S, Si, and N; D includes one or more elements selected from S, F, Cl, and Br; a is 0.9-1.1; x is 0-0.1; y is 0.001-0.5; z is 0.001-0.1; and n is 0-0.1;

[0068] The first coating step: providing a coating containing Li g EP2O7 and / or E h (P2O7) i The first mixture is prepared by mixing the core material with the first mixture, drying, and sintering to obtain a material coated with a first coating layer; wherein the crystalline pyrophosphate Li g EP2O7 and E h (P2O7) i Each of the E's independently comprises one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al; g is greater than 0 and less than or equal to 2; h is greater than 0 and less than or equal to 4; and i is greater than 0 and less than or equal to 3;

[0069] The second coating step: providing a crystalline phosphate X j A second mixture of PO4, mixing the material coated with the first coating layer with the second mixture, drying, and sintering to obtain a material coated with two layers of coating layers; wherein X includes one or more elements selected from the group consisting of Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al; and j is greater than 0 and less than or equal to 3;

[0070] The third coating step is to provide a third mixture containing a carbon source, mix the material coated with the two coating layers with the third mixture, dry, and sinter to obtain a second positive electrode active material.

[0071] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0072] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0073] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0074] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0075] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0076] [Negative electrode]

[0077] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0078] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0079] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0080] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0081] In some embodiments, the negative electrode film layer may further include a binder. For example, the binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0082] In some embodiments, the negative electrode film layer may further include a conductive agent. For example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0083] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0084] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0085] [Electrolytes]

[0086] The electrolyte conducts ions between the positive and negative electrodes. The electrolyte can be liquid, gel, or solid.

[0087] In some embodiments, the electrolyte is liquid and includes an electrolyte salt and a solvent.

[0088] In some embodiments, the secondary battery satisfies: 0<ρ×m×b≤79.1%, wherein ρ is the molar concentration of the electrolyte salt in the electrolyte, in mol / L; m is the mass content of the first positive electrode active material in the positive electrode active material.

[0089] Therefore, commonly used electrolyte salts are easily decomposed, and the safety of the battery can be further improved by controlling the range of the product of ρ, m and b.

[0090] In some embodiments, the electrolyte salt includes one or more of LiPF6, LiBF4, LiN(SO2F)2, LiN(CF3SO2)2, LiClO4, LiAsF6, LiB(C2O4)2 and LiBF2C2O4, and optionally includes one or more of LiPF6, LiN(SO2F)2 and LiN(CF3SO2)2, and more optionally LiPF6.

[0091] In some embodiments, the molar concentration p of the electrolyte salt in the electrolyte is 0.5-1.5 mol / L, such as 0.7 mol / L, 0.9 mol / L, 1.0 mol / L, 1.2 mol / L, or 1.4 mol / L.

[0092] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0093] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0094] [Isolation film]

[0095] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0096] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0097] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0098] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0099] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0100] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG1 shows a secondary battery 5 with a square structure as an example.

[0101] In some embodiments, referring to FIG2 , the outer package may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0102] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0103] Figure 3 shows an example battery module 4. Referring to Figure 3 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0104] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0105] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0106] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 4 and 5 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0107] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0108] As an electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0109] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.

[0110] [Example]

[0111] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0112] Example 1

[0113] (1) Preparation of positive electrode sheet:

[0114] (1) First positive electrode active material:

[0115] LiNi 0.55 Co 0.14 1Mn 0.249 Al 0.04 Mg 0.02 O2 was purchased from Defang Nano.

[0116] (2) Preparation of the second positive electrode active material:

[0117] Step S1: Preparation of Fe, Co, V and S co-doped manganese oxalate

[0118] 574.7g of manganese carbonate, 571.2g of ferrous carbonate, 3.6g of nickel carbonate, and 4.9g of vanadium dichloride were added to a mixer and thoroughly mixed for 6 hours. The resulting mixture was then transferred to a reactor, and 5L of deionized water and 1260.6g of oxalic acid dihydrate were added. The mixture was heated to 80°C and stirred at 500 rpm for 6 hours, mixing until the reaction terminated and no bubbles were generated, to obtain a manganese oxalate suspension co-doped with Fe, Co, and V. The suspension was then filtered, dried at 120°C, and sand-milled to obtain manganese oxalate iron, vanadium, and nickel dihydrate particles with a particle size of 100nm.

[0119] Step S2: Preparation of Li core 0.997 Mn 0.60 Fe 0.393 V 0.004 Co 0.003 P 0.997 S 0.003 O4

[0120] 1794.0 g of the prepared manganese iron vanadium nickel oxalate dihydrate, 369.8 g of lithium carbonate, 1148.9 g of ammonium dihydrogen phosphate, and 0.8 g of silicic acid were added to 20 L of deionized water, stirred thoroughly, and uniformly mixed and reacted at 80°C for 10 hours to obtain a slurry. The slurry was transferred to a spray drying device for spray drying and granulation, and dried at 250°C to obtain a powder. The powder was sintered in a roller kiln at 700°C for 4 hours in a protective atmosphere (90% nitrogen and 10% hydrogen) to obtain a core material. The element content of the core material was detected using inductively coupled plasma emission spectroscopy (ICP) to obtain the core.

[0121] Step S3: Preparation of the first coating layer suspension

[0122] Preparation of Li2FeP2O7 solution: 7.4 g of lithium carbonate, 11.6 g of ferrous carbonate, 23.0 g of ammonium dihydrogen phosphate and 12.6 g of oxalic acid dihydrate were dissolved in 500 mL of deionized water, the pH was controlled to 5, and then stirred and reacted at room temperature for 2 h to obtain a solution. The solution was then heated to 80°C and maintained at this temperature for 4 h to obtain a first coating layer suspension.

[0123] Step S4: coating of the first coating layer

[0124] The doped 1573.0 g core material obtained in step S2 was added to the first coating layer suspension (coating material content of 15.7 g) obtained in step S3, and the mixture was stirred and mixed for 6 h. After mixing evenly, the mixture was transferred to a 120 ° C oven and dried for 6 h, and then sintered at 650 ° C for 6 h to obtain the pyrophosphate-coated material.

[0125] Step S5: Preparation of the second coating layer suspension

[0126] 3.7 g of lithium carbonate, 11.6 g of ferrous carbonate, 11.5 g of ammonium dihydrogen phosphate and 12.6 g of oxalic acid dihydrate were dissolved in 1500 mL of deionized water, and then stirred and reacted for 6 hours to obtain a solution. The solution was then heated to 120° C. and maintained at this temperature for 6 hours to obtain a second coating layer suspension.

[0127] Step S6: Coating with the second coating layer

[0128] 1588.7 g of the pyrophosphate-coated material obtained in step S4 was added to the second coating layer suspension (coating material content of 47.2 g) obtained in step S5, and the mixture was stirred and mixed for 6 h. After mixing evenly, it was transferred to a 120°C oven and dried for 6 h, and then sintered at 700°C for 8 h to obtain a two-layer coated material.

[0129] Step S7: Preparation of the third coating layer aqueous solution

[0130] 37.4 g of sucrose was dissolved in 500 g of deionized water, and then stirred and fully dissolved to obtain a sucrose aqueous solution.

[0131] Step S8: coating with the third coating layer

[0132] 1635.9 g of the two-layer coated material obtained in step S6 was added to the sucrose solution obtained in step S7, stirred and mixed for 6 h, and after mixing evenly, transferred to a 150 ° C oven to dry for 6 h, and then sintered at 630 ° C for 8 h to obtain a three-layer coated material with a core of Li 1.001 Mn 0.50 Fe 0.493 V 0.004 Ni 0.003 P 0.999 Si 0.001 O4, the first coating layer is 1% Li2FeP2O7 (based on the mass of the core), the second coating layer is 3% LiFePO4 (based on the mass of the core), and the third coating layer is 1% carbon (based on the mass of the core).

[0133] (3) Preparation of positive electrode sheet:

[0134] The first positive electrode active material, the second positive electrode active material, the binder polyvinylidene fluoride (PVDF), and the conductive agent acetylene black are dissolved in the solvent N-methylpyrrolidone (NMP) in a mass ratio of 43.2:52.8:2:2, and are fully stirred and mixed to prepare a positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, and then dried, cold pressed, and cut to obtain a positive electrode sheet.

[0135] (2) Preparation of negative electrode sheet:

[0136] The negative electrode active material artificial graphite, the conductive agent acetylene black, the binder styrene-butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC-Na) were dissolved in deionized water in a mass ratio of 96:2:1:1, and the mixture was thoroughly stirred and mixed to prepare a negative electrode slurry; the negative electrode slurry was coated on the negative electrode current collector copper foil, and then dried, cold pressed, and cut to obtain the negative electrode sheet.

[0137] (3) Isolation membrane: A polyethylene microporous film is used as the porous isolation membrane substrate, and inorganic alumina powder, polyvinylpyrrolidone, and acetone solvent are evenly mixed in a weight ratio of 3:1.5:5.5 to form a slurry, which is then coated on both sides of the substrate and dried to obtain an isolation membrane.

[0138] (IV) Preparation of electrolyte:

[0139] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1, and then LiPF6 was uniformly dissolved in the above solution to obtain an electrolyte solution. The concentration of LiPF6 in the electrolyte solution was 1 mol / L.

[0140] (5) Preparation of secondary batteries:

[0141] The positive electrode sheet, separator, and negative electrode sheet are stacked and wound in order to obtain an electrode assembly; the electrode assembly is placed in an outer package, and the above-prepared electrolyte is added. After packaging, standing, formation, aging and other processes, a secondary battery is obtained.

[0142] The secondary battery preparation methods of Examples 2-21 and Comparative Examples 1-2 are similar to those of Example 1, and the different product parameters are detailed in Table 1.

[0143] The first positive electrode active material of Examples 2-3, 6-9, and 11 is the same as the first positive electrode active material in Example 1.

[0144] Preparation Method of the First Positive Electrode Active Material of Examples 4-5, 10, 16-18, 21 and Comparative Example 2

[0145] (1) NiSO4, CoSO4, and MnSO4 were added to water in a molar ratio of 0.869:0.048:0.033 to prepare a mixed solution, wherein the concentration of NiSO4 in the mixed solution was 2 mol / L; and a 6 mol / L NaOH solution was prepared;

[0146] (2) 50 L of the mixed solution was introduced into the reactor, and then 50 L of NaOH solution and an appropriate amount of 0.5 mol / L ammonia solution were introduced into the reactor to adjust the pH value in the reactor to 9.0-12.0, the reaction temperature to 40°C-80°C, and the reaction was carried out under stirring for 60 h at a stirring speed of 300-1000 r / min. After completion, the precipitate was filtered out and washed, and the washed precipitate was vacuum dried at 120°C for 24 h to obtain a precursor;

[0147] (3) LiOH, precursor, Al2O3 and MgO were mixed, wherein the molar ratio of LiOH (calculated as the molar amount of Li element), precursor (calculated as the total molar amount of Ni, Co and Mn elements in the mixed solution), Al2O3 (calculated as the molar amount of Al element) to MgO was 1.05:0.95:0.04:0.01. After mixing, the mixture was placed in a ball mill and ball milled at a speed of 300 r / s for 2 h. The mixture was then placed in a box furnace and heated to 950°C and kept warm for 12 h in an air atmosphere of 0.2 MPa for pre-sintering at a heating rate of 1°C / min. The mixture was then cooled to 600°C at a rate of 1°C / min and kept warm for 8 h for sintering. After sintering, the mixture was cooled to 300°C at a rate of 1°C / min and continued to cool naturally to room temperature. The mixture was then pulverized in a jet mill at a speed of 3000 r / min and 500 m 3 / h of air volume for crushing, crushing for 0.5h, and then sieving through a 500-mesh filter to obtain the first positive electrode active material LiNi 0.869 Co 0.048 Mn 0.033 Al 0.04 Mg 0.01 O2.

[0148] Preparation method of the first positive electrode active material of Example 12

[0149] (1) NiSO4, CoSO4, and MnSO4 were added to water in a molar ratio of 0.573:0.118:0.2893 to prepare a mixed solution, wherein the concentration of NiSO4 in the mixed solution was 2 mol / L; and a 5 mol / L NaOH solution was prepared;

[0150] (2) 50 L of the mixed solution was introduced into the reactor, and then 50 L of NaOH solution and an appropriate amount of 0.5 mol / L ammonia solution were introduced into the reactor to adjust the pH value in the reactor to 9.0-12.0, the reaction temperature to 40°C-80°C, and the reaction was carried out under stirring for 60 h at a stirring speed of 300-1000 r / min. After completion, the precipitate was filtered out and washed, and the washed precipitate was vacuum dried at 120°C for 24 h to obtain a precursor;

[0151] (3) Li2CO3, a precursor and MgO are mixed, wherein the molar ratio of Li2CO3 (calculated as the molar amount of the Li element), the precursor (calculated as the total molar amount of the three elements Ni, Co and Mn in the mixed solution) and MgO is 1.05:0.98:0.02. After mixing, the mixture is placed in a ball mill and ball milled at a speed of 300 r / s for 2 h. The mixture is then placed in a box furnace and heated to 950°C and kept warm for 12 h in an air atmosphere of 0.2 MPa for pre-sintering at a heating rate of 1°C / min. The mixture is then cooled to 600°C at a rate of 1°C / min and kept warm for 8 h for sintering. After sintering, the mixture is cooled to 300°C at a rate of 1°C / min and cooled naturally to room temperature. The mixture is then pulverized in a jet mill at a speed of 3000 r / min and 500 m 3 / h of air volume for crushing, crushing for 0.5h, and then sieving through a 500-mesh filter to obtain the first positive electrode active material LiNi 0.573 Co 0.118 Mn 0.289 Mg 0.02 O2.

[0152] Preparation method of the first positive electrode active material of Example 13

[0153] In step (1), NiSO4, CoSO4 and MnSO4 are added with water in a molar ratio of 0.588:0.118:0.289 to form a mixed solution, wherein the concentration of NiSO4 in the mixed solution is 2 mol / L; and a 5 mol / L NaOH solution is prepared;

[0154] In step (3), the molar ratio of Li2CO3 (based on the molar amount of Li element), precursor (based on the total molar amount of Ni, Co and Mn elements in the mixed solution) and MgO is 1.05:0.98:0.05;

[0155] The rest is the same as the preparation method of the first positive electrode active material of Example 12, and the first positive electrode active material LiNi 0.588 Co 0.118 Mn 0.289 Mg 0.005 O2.

[0156] Preparation method of the first positive electrode active material of Example 15

[0157] (1) NiSO4, CoSO4, and MnSO4 were added to water in a molar ratio of 0.562:0.115:0.283 to prepare a mixed solution, wherein the concentration of NiSO4 in the mixed solution was 2 mol / L; and a 5 mol / L NaOH solution was prepared;

[0158] (2) 50 L of the mixed solution was introduced into the reactor, and then 50 L of NaOH solution and an appropriate amount of 0.5 mol / L ammonia solution were introduced into the reactor to adjust the pH value in the reactor to 9.0-12.0, the reaction temperature to 40°C-80°C, and the reaction was carried out under stirring for 60 h at a stirring speed of 300-1000 r / min. After completion, the precipitate was filtered out and washed, and the washed precipitate was vacuum dried at 120°C for 24 h to obtain a precursor;

[0159] (3) Li2CO3, a precursor and Al2O3 were mixed, wherein the molar ratio of Li2CO3 (calculated as the molar amount of Li element), the precursor (calculated as the total molar amount of the three elements Ni, Co and Mn in the mixed solution) and Al2O3 (calculated as the molar amount of Al element) was 1.05:0.96:0.04. After mixing, the mixture was placed in a ball mill and ball milled at a speed of 300 r / s for 2 h. The mixture was then placed in a box furnace and heated to 950°C and kept warm for 12 h in an air atmosphere of 0.2 MPa for pre-sintering at a heating rate of 1°C / min. The mixture was then cooled to 600°C at a rate of 1°C / min and kept warm for 8 h for sintering. After sintering, the mixture was cooled to 300°C at a rate of 1°C / min and continued to cool naturally to room temperature. The mixture was then pulverized in a jet mill at a speed of 3000 r / min and 500 m 3 / h of air volume for crushing, crushing for 0.5h, and then sieving through a 500-mesh filter to obtain the first positive electrode active material LiNi 0.562 Co 0.115 Mn 0.283 Al 0.04 O2.

[0160] Preparation method of the first positive electrode active material of Example 14

[0161] In step (1), NiSO4, CoSO4 and MnSO4 are added with water in a molar ratio of 0.597:0.115:0.283 to form a mixed solution;

[0162] In step (3), the molar ratio of Li2CO3 (based on the molar amount of Li element), precursor (based on the total molar amount of Ni, Co and Mn elements in the mixed solution) and Al2O3 is 1.05:0.98:0.05;

[0163] The rest is the same as the preparation method of the first positive electrode active material of Example 15, and the first positive electrode active material LiNi 0.597 Co 0.115 Mn 0.283 Al 0.005 O2.

[0164] Preparation Method of the First Positive Electrode Active Material of Example 19

[0165] (1) NiSO4, CoSO4, and MnSO4 were added to water in a molar ratio of 0.585:0.12:0.295 to prepare a mixed solution, wherein the concentration of NiSO4 in the mixed solution was 2 mol / L; and a 5 mol / L NaOH solution was prepared;

[0166] (2) 50 L of the mixed solution was introduced into the reactor, and then 50 L of NaOH solution and an appropriate amount of 0.5 mol / L ammonia solution were introduced into the reactor to adjust the pH value in the reactor to 9.0-12.0, the reaction temperature to 40°C-80°C, and the reaction was carried out under stirring for 60 h at a stirring speed of 300-1000 r / min. After completion, the precipitate was filtered out and washed, and the washed precipitate was vacuum dried at 120°C for 24 h to obtain a precursor;

[0167] (3) Li2CO3, precursor, Al2O3 and MgO were mixed, wherein the molar ratio of Li2CO3 (calculated as the molar amount of Li element), precursor (calculated as the total molar amount of Ni, Co and Mn elements in the mixed solution), Al2O3 (calculated as the molar amount of Al element) to MgO was 1.05:1:0.04:0.02. After mixing, the mixture was placed in a ball mill and ball milled at a speed of 300 r / s for 2 h. The mixture was then placed in a box furnace and heated to 950°C and kept warm for 12 h in an air atmosphere of 0.2 MPa for pre-sintering at a heating rate of 1°C / min. The mixture was then cooled to 600°C at a rate of 1°C / min and kept warm for 8 h for sintering. After sintering, the mixture was cooled to 300°C at a rate of 1°C / min and continued to cool naturally to room temperature. The mixture was then pulverized in a jet mill at a speed of 3000 r / min and 500 m 3 / h of air volume for crushing, crushing for 0.5h, and then sieving through a 500-mesh filter to obtain the first positive electrode active material LiNi 0.585 Co 0.12 Mn 0.295 O2.

[0168] Preparation Method of the First Positive Electrode Active Material of Example 20

[0169] In step (1), NiSO4, CoSO4 and MnSO4 are added with water in a molar ratio of 0.522:0.115:0.283 to form a mixed solution;

[0170] In step (3), the molar ratio of LiOH (based on the molar amount of the Li element), the precursor (based on the total molar amount of the three elements Ni, Co and Mn in the mixed solution), Al2O3 (based on the molar amount of the Al element) and MgO is 1.05:0.92:0.05:0.03;

[0171] The rest of the preparation process is the same as that of the first positive electrode active material in Example 4.

[0172] Battery Test

[0173] (1) Energy density test

[0174] In a constant temperature environment of 25°C, the battery was allowed to stand for 10 minutes and then discharged at a constant current of 0.33C to a cut-off voltage of 2.8V. After standing for 10 minutes, it was charged at a constant current of 0.33C to a target voltage of 4.3V. Constant voltage charging was continued until the current was ≤0.05C. After standing for 10 minutes, it was discharged at a constant current of 0.33C to a cut-off voltage of 2.8V. The discharge capacity was recorded and the discharge capacity was divided by the total mass of the positive electrode active material to obtain the gram capacity of the positive electrode active material in mAh / g.

[0175] (2) Hot box safety test:

[0176] The test refers to the "Heating" section of the safety test in GB 38031-2020, and explores the upper limit. The optimized test conditions are as follows:

[0177] ①Preparation:

[0178] Test conditions: Prepare an explosion-proof oven that can heat the circuit connection port; the test cell is a fresh bare cell (cycle number ≤ 10 times), and attach temperature-sensing wires around the cell and on the poles for temperature monitoring, and also configure a temperature recording device;

[0179] Cell treatment before testing: constant current charging is performed using a 0.33C rate current, and the cell is fully charged to the nominal voltage (such as 4.3V in the present invention).

[0180] ②Test process: Place the sample in a high temperature box, raise the temperature from room temperature to 100℃ at a rate of 5℃ / min, and maintain it for 2h; then increase the temperature at 5℃ / min, and maintain it for 30min every 5℃, until the battery cell loses control (out of control standard: the voltage drops by ≥50% within 1min, and the battery cell temperature rises by ≥50% within 1min) or is heated to 200℃, then stop heating.

[0181] ③Data processing: Find the failure point according to the above conditions and obtain the corresponding holding temperature and holding time, which are recorded as: time@temperature, such as 21min@150℃.

[0182] ④ Benchmarking results:

[0183] Samples that are tested for a longer period of time during the test are safer; samples that are tested for a longer period of time may include: samples with the same failure point temperature but a longer time, samples with the same failure point time but a higher temperature, and samples with different failure point temperatures and times but a higher temperature.

[0184] Table 2: Performance test results of Examples 1-21 and Comparative Examples 1-2

[0185] According to the above results, we can know that:

[0186] Compared with comparative examples 1-2, the battery of Example 1-21 of the present application has higher energy density and higher safety.

[0187] Compared with Examples 18, 19, and 21, the batteries of Examples 1-17 of the present application are safer.

[0188] Compared with Example 20, the batteries of Examples 1, 3-5, 7, and 9-17 of the present application have higher gram capacity and higher energy density.

[0189] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer comprises a positive electrode active material, wherein the positive electrode active material comprises Ni, Fe, Mn and optionally Al; Furthermore, the positive electrode sheet satisfies: 0<C Ni / (C Ni +C Fe +C Mn +C Al )≤90.10%; in, The C Ni is the mass content of Ni element in the positive electrode film layer, and the C Fe is the mass content of Fe element in the positive electrode film layer, and the C Mn is the mass content of Mn element in the positive electrode film layer, and the C Al is the mass content of Al element in the positive electrode film layer.

2. The positive electrode sheet according to claim 1, wherein: The positive electrode sheet meets the following requirements: 2.88%≤C Ni / (C Ni +C Fe +C Mn +C Al )≤86.10%.

3. The positive electrode sheet according to claim 1 or 2, wherein: The positive electrode active material includes a first positive electrode active material; the first positive electrode active material includes a compound LiNi b Co d Mn e M f O2; wherein, M includes one or more elements of Mn, Al, Mg, Ca, Na, Ti, W, Zr, Sr, Cr, Zn, Ba, B, S and Y, and can be optionally Mg element and / or Al element; b is 0.314-0.970; d is 0-0.320, and can be optionally 0.047-0.320; e is 0.006-0.390; and the sum of b, d, e and f is 1 and f is greater than or equal to 0.

4. The positive electrode sheet according to claim 3, wherein: The first positive electrode active material satisfies: 1.65%≤m×b≤79.10%, optionally 1.65%≤m×b≤73.87%, wherein m is the mass content of the first positive electrode active material in the positive electrode active material.

5. The positive electrode sheet according to claim 3 or 4, wherein: In the first positive electrode active material, the molar ratio of Al element in the elements other than Li element and O element is 0-5%, and can be optionally 0.5%-4%; and / or, The molar ratio of Mg in the elements other than Li and O is 0-3%. It can be selected from 0.5% to 2.0%.

6. The positive electrode sheet according to any one of claims 3 to 5, wherein: The positive electrode active material also includes a second positive electrode active material; the second positive electrode active material includes a compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n ; wherein, A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W; B includes one or more elements selected from the group consisting of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; C includes one or more elements selected from the group consisting of B (boron), S, Si and N; D includes one or more elements selected from the group consisting of S, F, Cl and Br; a is 0.9-1.1; x is 0-0.1; y is 0.001-0.5; z is 0.001-0.1; and n is 0-0.

1.

7. The positive electrode sheet according to claim 6, wherein: The second positive electrode active material comprises a core and a shell covering the core; the core comprises the compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n , the shell comprises carbon element.

8. The positive electrode sheet according to claim 6, wherein: The second positive electrode active material comprises a core and a shell covering the core, wherein the shell comprises a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer; the core comprises the compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n , the first coating layer comprises crystalline pyrophosphate Li g EP2O7 and / or E h (P2O7) i The second coating layer comprises crystalline phosphate X j PO4, the third coating layer comprises carbon element; Wherein, the crystalline pyrophosphate Li g EP2O7 and E h (P2O7) i wherein E independently includes one or more elements selected from the group consisting of Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; X includes one or more elements selected from the group consisting of Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; g is greater than 0 and less than or equal to 2; h is greater than 0 and less than or equal to 4; i is greater than 0 and less than or equal to 3; and j is greater than 0 and less than or equal to 3.

9. The positive electrode sheet according to any one of claims 6 to 8, wherein: The positive electrode active material consists of the first positive electrode active material and the second positive electrode active material.

10. A battery comprising the positive electrode sheet according to claim 1 or 2.

11. A battery comprising the positive electrode sheet according to any one of claims 3 to 9.

12. The battery according to claim 11, further comprising an electrolyte, wherein the electrolyte comprises an electrolyte salt; and the battery satisfies: 0<ρ×m×b≤79.1%, wherein, ρ is the molar concentration of the electrolyte salt in the electrolyte, in mol / L; m is the mass content of the first positive electrode active material in the positive electrode active material.

13. The battery according to claim 12, wherein: The electrolyte salt includes one or more of LiPF6, LiBF4, LiN(SO2F)2, LiN(CF3SO2)2, LiClO4, LiAsF6, LiB(C2O4)2 and LiBF2C2O4, and optionally includes one or more of LiPF6, LiN(SO2F)2 and LiN(CF3SO2)2.

14. An electrical device comprising the battery according to any one of claims 10 to 13.

Citation Information

Patent Citations

  • Phosphorus-containing lithium ion battery anode material and preparation method thereof

    CN104600273A

  • Composite material containing lithium manganese ferric phosphate with core-shell structure and preparation method thereof

    CN110416525A

  • Multi-element doped nickel-cobalt-manganese ternary positive electrode material capable of improving safety performance and voltage platform and preparation method of multi-element doped nickel-cobalt-manganese ternary positive electrode material

    CN115632127A

  • High-capacity non-aqueous secondary battery

    JP2002042816A

  • GB380312020TA