Manufacturing method for continuous fiber composite architecture
By pre-joining the connection points before hot pressing of fiber composite materials, the problems of low material yield and high energy consumption of fiber composite materials are solved, efficient and environmentally friendly complex structure molding is achieved, and the mechanical properties and precision of the finished product are improved. .
Patent Information
- Application Number
- PCT/CN2023/091678
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-31
AI Technical Summary
The existing manufacturing methods of fiber composite materials result in low material yield, high energy consumption and poor forming quality, and it is difficult to produce complex and fine structures.
By bending continuous fiber bundles in space to form structural units, and pre-joining the connection points before hot press forming, ultrasonic welding, local heating welding or gluing technology is used to reduce the hot press forming temperature and improve efficiency and accuracy.
Save energy, increase material yield, reduce waste, achieve high-quality complex structure molding, extend mold life, and improve the mechanical properties and environmental protection of finished products.
Smart Images

Figure CN2023091678_31102024_PF_FP_ABST
Abstract
Description
Method for making continuous fiber composite structure Technical Field
[0001] The present invention relates to a skeleton, and in particular to a method for manufacturing a continuous fiber composite material framework. Background Art
[0002] Fiber composites, due to their exceptionally high toughness and strength, excellent material properties, and lightweight advantages, are increasingly being used in a wide range of applications, from sports equipment and construction, wind energy, to transportation, shipbuilding, and aerospace. However, existing fiber composite applications often utilize sheet, flake, or full-surface fiber composites to create surface structures, or by cutting a desired structure from a full-surface fiber composite woven fabric. This results in poor mechanical properties, such as strength and modulus, in the finished product. Furthermore, cutting the desired portion from a full-surface fiber composite woven fabric generates excess waste, reducing yield, wasting resources, polluting the environment, and increasing waste disposal costs.
[0003] In addition, some existing fiber composite parts are manufactured by hot pressing each component unit. This involves placing pre-impregnated fiber materials, such as pre-impregnated fiber cloth or pre-impregnated fiber bundles, as the component units of the part into a hot press mold. The components are then joined and formed by heating the pre-impregnated resin material to a temperature exceeding the melting point of the pre-impregnated fiber cloth or pre-impregnated fiber bundle and applying pressure. However, manufacturing fiber composite parts in this manner requires heating the entire mold to a high temperature, consuming a large amount of energy. Furthermore, each component unit may shift within the mold and deviate from its original position. Furthermore, each component unit may not fit properly within the mold, resulting in poor molding quality, loss of fine structure, and reduced part strength.
[0004] In view of this, developing an energy-saving, high-efficiency and high-quality manufacturing method for fiber composite structures has become an urgent goal in the relevant fields.
[0005] Summary of the Invention
[0006] In order to improve the problems of low material yield, energy consumption and poor forming quality in the existing fiber composite parts manufacturing, the present invention provides a method for manufacturing a continuous fiber composite skeleton, which comprises the following steps:
[0007] Heating at least partially one or more continuous fiber bundles to make them bendable, and bending each of the continuous fiber bundles in three dimensions including its axial direction to produce a plurality of structural units, wherein each of the continuous fiber bundles comprises a plurality of fiber bundles and a thermoplastic resin coating the fiber bundles;
[0008] Connecting the corresponding connection points between the structural units to form a structural prototype;
[0009] Furthermore, the method for manufacturing the continuous fiber composite material skeleton provided by the present invention also includes the following steps: placing the prototype of the structure into a hot pressing mold to form a continuous fiber composite material structure.
[0010] The connection points are joined together by ultrasonic welding.
[0011] The connection points are joined to each other by local heating and welding.
[0012] The connection points are joined to each other by gluing.
[0013] The temperature of the hot pressing mold is not higher than the melting point of the thermoplastic resin.
[0014] The material of the fiber bundle includes carbon fiber, glass fiber, aramid fiber or ceramic fiber.
[0015] The thermoplastic resin includes polyoxymethylene (POM), acrylonitrile-butadiene-styrene (ABS), polyphenylene sulfide (PPS), polysulfone (PSU), polyethersulfone (PES), polyetheretherketone (PEEK), aromatic polyester liquid crystal polymer (LCP), polyetherimide (PEI), polyamideimide (PAI), polyacetal (POM), nylon (PA), polycarbonate (PC), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyphenylene ether (PPE), styrene Acrylic adhesive: one or a combination of acrylonitrile (ASA), polystyrene (PS), polymethyl methacrylate (PMMA), styrene copolymer (MS), cellulose acetate (CA), thermoplastic polyurethane (TPU), thermoplastic polyester elastomer (TPEE), styrene elastomer (TPS), elastomer (PAE), polytetrafluoroethylene (PTFE), vinylon (vinylon), polypropylene (PP), polyethylene (PE), ethylene / vinyl acetate copolymer (EVA) or polyvinyl chloride (PVC).
[0016] Part or all of the structural units are closed ring structures connected head to tail.
[0017] The method for manufacturing the continuous fiber composite material structure further includes the step of coating the continuous fiber composite material structure with a coating material.
[0018] Wherein, the coating material is an elastomer, a foam material, a porous material or a resin material.
[0019] Wherein, the coating material is thermoplastic polyurethane, ethylene / vinyl acetate copolymer, rubber or polyolefin.
[0020] Furthermore, one of the structural units is a rod, and the other structural units are wound around the surface of the rod.
[0021] Furthermore, the bending comprises passing the continuous fiber bundle through a mold after local heating, wherein the mold is a tubular mold cavity with three-dimensional bending.
[0022] Furthermore, the bending includes conveying the continuous fiber bundle to a bending machine and providing a heat source, so as to use the bending machine to bend at least a partially heated and softened portion of the continuous fiber bundle.
[0023] It can be seen from the above description that the present invention has the following characteristics:
[0024] 1. The method for manufacturing the continuous fiber composite material structure provided by the present invention can reduce the heating temperature required for hot pressing by pre-joining the connection points of the structural unit before hot pressing, thereby achieving significant energy savings.
[0025] 2. The method for manufacturing a continuous fiber composite material structure provided by the present invention can reduce the heating temperature required for hot pressing by pre-joining the connection points of the structural unit before hot pressing, avoiding heating the entire structural prototype to a high temperature above the melting point of the thermoplastic resin, which would cause damage to the fiber bundle impregnation structure and surface structure, and can also reduce the time and cost required for secondary processing.
[0026] 3. The method for manufacturing a continuous fiber composite material structure provided by the present invention can reduce the heating temperature required for hot pressing by pre-joining the connection points of the structural unit before hot pressing. This can significantly reduce the time required for heating and cooling, greatly increasing production efficiency. The reduced temperature difference can also reduce the deformation of the hot pressing mold, making the surface of the continuous fiber composite material structure smoother and improving the precision, achieving the effect of producing a complex continuous fiber composite material structure with a fine structure, and significantly increasing the life of the hot pressing mold.
[0027] 4. The method for manufacturing a continuous fiber composite material structure provided by the present invention reduces the heating temperature required for hot pressing by pre-joining the connection points of the structural unit before hot pressing, thereby making the selection of mold materials more diverse and reducing the high mold costs and process improvement costs caused by the high temperature required for the process, which requires the mold material to have a high melting point and low thermal deformation.
[0028] 5. The method for manufacturing a continuous fiber composite material structure provided by the present invention pre-joins the connection points of the structural units before hot pressing. This pre-forming can more accurately control the fine structure of the structure and ensure the quality of the structure forming, achieving a configuration and level of fineness that cannot be achieved by traditional hot pressing of the components.
[0029] 6. The method for manufacturing a continuous fiber composite structure provided by the present invention reduces the heating temperature required for hot pressing because the connection points of the structural unit are pre-joined before hot pressing. Since the structural unit does not need to be heated above the melting point of the thermoplastic resin, which would cause the structural unit to soften excessively and the thermoplastic resin to begin to flow during the hot pressing process of the structural prototype, the hot pressing mold does not need to completely cover the structural prototype as in traditional processes. Instead, the hot pressing mold can be placed more flexibly and elastically, and the structural prototype can be hot pressed locally without affecting other parts of the structural prototype, thereby reducing mold costs and allowing the size of the structural prototype to be unrestricted by the size of the hot pressing mold.
[0030] 7. The method of the present invention for producing a continuous fiber composite material structure using a continuous fiber composite material can save production raw materials, improve material yield, reduce manufacturing costs and reduce waste.
[0031] 8. The present invention uses thermoplastic resin as the base material of the composite material, so that the finished product can be recycled and reused at the end of its life cycle, achieving green and environmental protection.
[0032] 9. The framework of the present invention can form a three-dimensional structure in three dimensions, offering a high degree of freedom and the ability to create complex structural components. It is highly customizable and can be formed into a single piece, avoiding structural weaknesses caused by joints at vulnerable points. This significantly improves the mechanical properties of the object, achieving applications with high structural strength and a high elastic modulus. The present invention also allows for the combination of multiple frameworks or the inclusion of further materials around the framework, making configurations convenient and highly flexible. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] FIG1 is a step diagram of the present invention.
[0034] Explanation of symbols: S10-S40: Steps DETAILED DESCRIPTION
[0035] To more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing each embodiment. Obviously, the drawings described below are merely examples or embodiments of the present invention. Those skilled in the art can apply the present invention to other similar scenarios based on these drawings without inventive effort. Unless otherwise apparent from the context or otherwise noted, the same reference numerals in the figures represent the same structure or operation.
[0036] As used herein and in the claims, unless the context clearly indicates otherwise, the words "a," "an," "an," or "the" do not necessarily refer to one item but may also include multiple items. Generally speaking, the terms "comprises" and "include" only indicate the inclusion of the steps and elements specifically identified, and these steps and elements do not constitute an exclusive list. A method or apparatus may also include additional steps or elements.
[0037] Flowcharts are used in this disclosure to illustrate the operations performed by systems according to embodiments of the present invention. It should be understood that the preceding and following operations do not necessarily need to be performed in exact order. Instead, the steps may be processed in reverse order or simultaneously. Furthermore, other operations may be added to these processes, or one or more operations may be removed from these processes.
[0038] Please refer to FIG1 , which is a diagram of the steps of the present invention. The present invention mainly includes steps S10 to S30, and optionally includes step S40.
[0039] Step S10: At least partially heating one or more continuous fiber bundles to render them bendable, and bending each of the continuous fiber bundles in three dimensions along their axial direction in space to produce a plurality of structural units, wherein each of the continuous fiber bundles comprises a plurality of fiber bundles and a thermoplastic resin coating the fiber bundles. In step S10, at least partially heating the continuous fiber bundles and bending them in three dimensions along their axial direction in space, the continuous fiber bundles that have been solidified and formed are locally heated, causing the locally heated portions of the continuous fiber bundles that have been coated with the thermoplastic resin and solidified to soften. At this point, the locally heated portions are bendable without breaking, and the bundles are bent in three dimensions. After the locally heated portions cool, the structural units having a fixed shape and structure are formed. The so-called coating includes but is not limited to impregnation, co-extrusion, etc. to completely adhere the thermoplastic resin to the fiber bundle. In one embodiment, the continuous fiber bundle is impregnated with a thermoplastic resin, so that the thermoplastic resin adheres to and coats the continuous fiber bundle to form a composite material, and the thermoplastic resin is cooled and solidified.
[0040] The fiber material of the continuous fiber bundle includes carbon fiber, glass fiber, aramid fiber or ceramic fiber or a combination of the above fiber materials. The thermoplastic resin includes polyoxymethylene (POM), acrylonitrile-butadiene-styrene (ABS), polyphenylene sulfide (PPS), polysulfone (PSU), polyethersulfone (PES), polyetheretherketone (PEEK), aromatic polyester liquid crystal polymer (LCP), polyetherimide (PEI), polyamideimide (PAI), polyacetal (POM), nylon (PA), polycarbonate (PC), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyphenylene ether (PPE), styrene acrylic adhesive acrylonitrile Polymer materials or combinations thereof include polyurethane (ASA), polystyrene (PS), polymethyl methacrylate (PMMA), styrene copolymer (MS), cellulose acetate (CA), thermoplastic polyurethane (TPU), thermoplastic polyester elastomer (TPEE), styrene elastomer (TPS), elastomer (PAE), polytetrafluoroethylene (PTFE), vinylon, polypropylene (PP), polyethylene (PE), ethylene / vinyl acetate copolymer (EVA), or polyvinyl chloride (PVC). The so-called continuous fiber bundle refers to a plurality of fiber yarns assembled into a bundle, and the fiber yarns maintain a continuity of at least 2 cm in the longitudinal direction. Preferably, the fiber yarns are continuous fibers of at least 10 cm. More preferably, the continuous fiber bundle is longer than 1 meter; more preferably, most of the continuous fibers are fiber yarns with a length equal to the length of a major axis of the continuous fiber bundle. The fiber bundle can be made of carbon fiber, glass fiber, aramid fiber, or ceramic fiber.
[0041] The so-called bending in three-dimensional space refers to the bending of the continuous fiber bundle in any direction of the extendable axis, and is not limited to one bend being in the same plane as any other two bends. The bending method may include manual bending, using hand tools such as pliers, hammers or nails to bend the continuous fiber bundle into the desired shape, or mechanical bending, using a mechanical device such as a rolling machine, a bending machine or a shearing machine to bend the continuous fiber bundle into the desired shape, or guiding the continuous fiber bundle to advance into a mold so that the continuous fiber bundle is bent according to the shape of the mold. In one embodiment, the continuous fiber bundle is softened by conveying the continuous fiber bundle to a bending machine and providing a heat source, wherein the heat source provides a heat source that exceeds the glass transition temperature of the thermoplastic resin but is lower than the thermal decomposition temperature of the thermoplastic resin to heat the continuous fiber bundle. The continuous fiber bundle is bent using the bending machine at least partially at the heat-softened portion of the continuous fiber bundle. The bending machine is not limited to bending in a single plane and can bend in three dimensions by rotating the bending machine or the continuous fiber bundle. Preferably, by continuously feeding the continuous fiber bundle through the bending machine and rotating and bending it at designated locations, the continuous fiber bundle can be bent in three dimensions in space sequentially from one end to the other.
[0042] In another preferred embodiment, the continuous fiber bundle is locally heated and passed through a mold, wherein the mold is a tubular mold cavity with a three-dimensional bend. The continuous fiber bundle is at least locally heated to above the glass transition temperature of the thermoplastic resin and passed through the three-dimensionally bent tubular mold cavity of the mold to a designated position. The continuous fiber bundle is then cooled and solidified before being removed. Preferably, the continuous fiber bundle is driven by one or more rotating wheels within the tubular mold cavity to pass through the tubular mold cavity to form a bend. In another preferred embodiment, the front end of the continuous fiber bundle is fixed to a yarn guide structure, which moves along the tubular mold cavity to pull and guide the continuous fiber bundle through the tubular mold cavity to form a bend.
[0043] Furthermore, the structural units produced by locally heating and bending the continuous fiber bundles can have the same or different structural shapes. Some or all of the structural units can be connected radially from end to end to form a closed annular structure. The annular structure can be a deformed annular shape and have different winding numbers. In one embodiment, some of the structural units have multiple interleaving points, and some of the structural units have spiral or braided windings within or between the structural units.
[0044] In the case of multiple continuous fiber bundles, the structural units generated by each continuous fiber bundle can have identical shapes and structures, or can have partially identical or completely different shapes and structures. In one embodiment, a portion of the structural units have closed annular structures, while another portion have other three-dimensional configurations. Furthermore, the fiber bundle materials and the thermoplastic resin components coated therein of the different continuous fiber bundles can be identical or different, so that the fiber bundle materials and the thermoplastic resin components coated therein of the structural units formed by each continuous fiber bundle can be identical or different, thereby creating structural units with identical or different material properties.
[0045] Furthermore, the cross-sectional size and shape of each continuous fiber bundle can be completely identical, partially identical, or completely different. In one embodiment, one of the structural units can be a rod with a larger cross-sectional area, and the other structural units with smaller cross-sectional areas are wound around the peripheral surface of the rod. In this embodiment, the rod is a continuous fiber bundle formed by continuous carbon fibers coated with a thermoplastic resin and extending in the axial direction, while the other structural units with smaller cross-sectional areas are glass fibers coated with the thermoplastic resin. This allows the rod with a larger cross-sectional area to serve as a shaft core, and the winding of the other structural units with smaller cross-sectional areas can further enhance the radial and circumferential strength and rebound force of the shaft core.
[0046] Step S20: Joining the multiple connection points of the structural unit to produce a structural prototype. The so-called mutual joining refers to that at least two corresponding connection points among the multiple connection points are fixed together by joining. Among them, the connection point can be a local point in the structural unit that can be fixed to another connection point. The joining of at least two corresponding connection points can be the mutual joining of two or more connection points in the same structural unit, or the mutual joining of different connection points on two or more structural units. The so-called joining refers to the process of fixing two or more connection points together to make each connection point become one. Furthermore, the mutual joining of the multiple connection points also includes a joining method in which a continuous plurality of connection points form a line or even a surface. In one embodiment, the two annular structural units each have a continuous plurality of connection points forming a connecting line, and the connecting lines on each structural unit are joined to each other so that the two structural units have at least a portion of a linear connection. The joining method of step S20 includes but is not limited to welding, welding, dissolving, compression joining, gluing, etc. Preferably, in one embodiment, step S20 utilizes ultrasonic welding, wherein a high-frequency signal is generated by a sound generator of an ultrasonic welding machine, and a welding head transmits the ultrasonic energy to at least two corresponding and contacting connection points, causing their contact surfaces to melt. Upon completion, the connection points are joined together. During ultrasonic welding, the welding head can apply moderate pressure to ensure a tighter and more secure bond between the connection points. In another embodiment, step S20 locally heats the at least two corresponding and contacting connection points at a temperature above the melting point of the thermoplastic resin at each connection point, maintaining contact until the contacting areas cool and the thermoplastic resin coating them solidifies, thereby joining the connection points together. In another preferred embodiment, step S20 glues at least a portion of the connection points with a thermoplastic resin material. The thermoplastic resin material can be the same or different in composition from the thermoplastic resin coating the continuous fiber bundles of each structural unit. In another preferred embodiment, step S20 is to apply a solvent of the thermoplastic resin to at least a portion of the connection points, and then contact the corresponding connection points, and then connect the corresponding connection points to each other after the solvent evaporates.
[0047] In a preferred embodiment, the head and tail ends of the continuous fiber bundle are joined to each other, so that the continuous fiber bundle has no obvious endpoints.
[0048] After joining the structural units at multiple connection points, a prototype is produced after all corresponding joints are fully bonded and fixed. This prototype can be used directly as a continuous fiber composite structure without further processing, or it can be further modified through subsequent processing steps. In one embodiment, after joining multiple structural units with more complex structures to form a prototype, the prototype can be partially cut or perforated to create a more complex configuration while still maintaining the main structural strength and improving manufacturing efficiency.
[0049] Step S30: The structural prototype is placed in a hot press mold to form a continuous fiber composite material structure. In this step S30, the structural prototype joined in step S20 is placed in a mold cavity of the hot press mold, and the hot press mold is closed and pressurized and heated to soften and bend the structural prototype, thermoforming it into the final shape to produce the desired curve and surface morphology. The hot press mold is then cooled to solidify the thermoplastic resin, and the formed continuous fiber composite material structure can be taken out. In one embodiment, the hot press mold only covers a portion of the structural prototype, so that the hot press mold changes the local curve and surface morphology of the structural prototype and strengthens the strength of the connection points. In another embodiment, the structural prototype is completely covered in the hot press mold and shaped.
[0050] Preferably, the temperature of the hot pressing mold does not exceed the melting point of the thermoplastic resin. Heating at a temperature not exceeding the melting point of the thermoplastic resin can avoid the displacement of the fiber bundle coated by the thermoplastic resin in the mold due to the melting of the thermoplastic resin, resulting in poor quality of the finished product, and can also avoid the loss of fine structure and the need for secondary processing. The heat source input to the hot pressing mold causes the heating temperature to exceed the glass transition temperature of the thermoplastic resin. Preferably, the heating temperature exceeds the heat deformation temperature of the thermoplastic resin but does not exceed the melting point of the thermoplastic resin. When the structural prototype is composed of two or more thermoplastic resins with different components, the temperature of the hot pressing mold does not exceed the melting point of the thermoplastic resin with the highest melting point. Since the structural units within and between the structural units in the structural prototype have already been joined, the heat source input to the hot pressing mold can be significantly reduced compared to the heat source required by the traditional high-temperature molding mold. The location of the hot pressing mold can also be planned more flexibly. The hot pressing mold can be used for thermoplastic forming only where the surface morphology of the structural prototype is modified or the bonding strength of each connection point is enhanced.
[0051] Step S40: Coating the continuous fiber composite structure with a coating material. In step S40, the method for manufacturing the continuous fiber composite structure further includes coating the continuous fiber composite structure in the coating material. This step S40 is optional. The coating material can further strengthen and protect the continuous fiber composite structure, making the continuous fiber composite structure more widely applicable. The continuous fiber composite structure can create a skeleton with strong rigidity along the axial direction of the continuous fiber bundle. Combined with the external coating material, it can provide a buffer when the continuous fiber bundle is subjected to radial forces, preventing the continuous fiber composite structure from breaking. The coating material can be an elastomer, a foam material, a porous material, or a resin material. The resin material can be a thermosetting resin or a thermoplastic resin. If the resin material is a thermoplastic resin, the thermoplastic resin can have the same or different composition as the thermoplastic resin coating the continuous fiber composite structure. Furthermore, the resin material can include fibers, and the fibers can be continuous fibers or short fibers. In some embodiments, the continuous fiber composite structure is placed in a mold by overmolding or insert injection molding, and then overmolded with the overmolding material. The method of the present invention can be used for, but is not limited to, frames of electronic devices such as mobile phones, monitors, laptops, and AR / VR hardware. It can also be used in eyeglass frames, golf club heads, specialized functional shoe soles, and various sports product structures.
[0052] Furthermore, the coating material can be a component such as thermoplastic polyurethane, ethylene / vinyl acetate copolymer, rubber or polyolefin, so that the method of the present invention can produce the continuous fiber composite material structure for the sole, and the continuous fiber composite material structure is then coated with the coating material after completion.
[0053] It can be seen from the above description that the present invention achieves the following effects:
[0054] 1. The method for manufacturing the continuous fiber composite material structure provided by the present invention can reduce the heating temperature required for hot pressing by pre-joining the connection points of the structural unit before hot pressing, thereby achieving significant energy savings.
[0055] 2. The method for manufacturing a continuous fiber composite material structure provided by the present invention can reduce the heating temperature required for hot pressing by pre-joining the connection points of the structural unit before hot pressing, avoiding heating the entire structural prototype to a high temperature above the melting point of the thermoplastic resin, which would cause displacement of the continuous fibers and damage to the fiber bundle impregnation structure and surface structure, thereby reducing the strength of the continuous fiber composite material structure, and can also reduce the time and cost required for secondary processing.
[0056] 3. The method for manufacturing a continuous fiber composite material structure provided by the present invention can reduce the heating temperature required for hot pressing by pre-joining the connection points of the structural unit before hot pressing. This can significantly reduce the time required for heating and cooling, greatly increasing production efficiency. The reduced temperature difference can also reduce the deformation of the hot pressing mold, making the surface of the continuous fiber composite material structure smoother and improving the precision, achieving the effect of producing a complex continuous fiber composite material structure with a fine structure, and significantly increasing the life of the hot pressing mold.
[0057] 4. The method for manufacturing a continuous fiber composite material structure provided by the present invention reduces the heating temperature required for hot pressing by pre-joining the connection points of the structural unit before hot pressing, making the selection of mold materials more diverse and flexible, and reducing the high mold costs and process improvement costs caused by the high temperature required for the process, which requires the mold material to have a high melting point and low thermal deformation.
[0058] 5. The method for manufacturing a continuous fiber composite material structure provided by the present invention pre-joins the connection points of the structural units before hot pressing. This pre-forming can more accurately control the fine structure of the structure and ensure the quality of the structure forming, achieving a configuration and level of fineness that cannot be achieved by traditional hot pressing of the components.
[0059] 6. The method for manufacturing a continuous fiber composite structure provided by the present invention reduces the heating temperature required for hot pressing because the connection points of the structural unit are pre-joined before hot pressing. Since the structural unit does not need to be heated above the melting point of the thermoplastic resin, which would cause the structural unit to soften excessively and the thermoplastic resin to flow during the hot pressing process of the structural prototype, the hot pressing mold does not need to completely cover the structural prototype as in traditional processes. Instead, the hot pressing mold can be placed more flexibly and elastically, and the structural prototype can be hot pressed locally without affecting other parts of the structural prototype. This reduces mold costs and allows the size of the structural prototype to be unrestricted by the size of the hot pressing mold, thereby realizing large and complex continuous fiber composite structures.
[0060] 7. The method of the present invention for producing a continuous fiber composite material structure using a continuous fiber composite material can save production raw materials, improve material yield and reduce waste generation, thereby reducing manufacturing costs and reducing waste.
[0061] 8. The present invention uses thermoplastic resin as the base material of the composite material, so that the finished product can be recycled and reused at the end of its life cycle, achieving green and environmental protection.
[0062] 9. The framework of the present invention can be formed into a three-dimensional structure in three dimensions, offering a high degree of freedom and the ability to create complex structural components. It is highly customizable and can be formed into a single piece, avoiding structural weaknesses caused by joints at vulnerable points. This significantly improves the mechanical properties of the object, achieving applications with high structural strength and a high elastic modulus. The present invention also allows for the combination of multiple frameworks or the inclusion of additional materials, making configurations convenient and highly flexible.
[0063] It should be noted that, based on the explanations and elaborations of the above description, those skilled in the art may also make changes and modifications to the above embodiments. Therefore, the present disclosure is not limited to the specific embodiments disclosed and described above, and equivalent modifications and variations of the present disclosure are also within the scope of protection of the claims of the present disclosure. Furthermore, although certain specific terms are used in this description, these terms are for convenience only and do not constitute any limitation on the invention.
Claims
1. A method for manufacturing a continuous fiber composite material structure, characterized in that: It contains the following steps: Heating at least partially one or more continuous fiber bundles to make the continuous fiber bundles bendable, and bending each of the continuous fiber bundles in three dimensions in the axial direction thereof to generate a plurality of structural units, wherein each of the continuous fiber bundles comprises a plurality of fiber bundles and a thermoplastic resin coating the fiber bundles; The corresponding connection points between the structural units are connected to each other to generate a structural prototype.
2. The method for manufacturing a continuous fiber composite material structure according to claim 1, wherein: The method also includes the following steps: placing the prototype of the structure into a hot pressing mold to form a continuous fiber composite material structure.
3. The method for manufacturing a continuous fiber composite material structure according to claim 1, characterized in that: The connection points are joined together by ultrasonic welding.
4. The method for manufacturing a continuous fiber composite material structure according to claim 1, characterized in that: The connection points are joined to each other by local heating and welding.
5. The method for manufacturing a continuous fiber composite material structure according to claim 1, characterized in that: The connection points are joined to each other by gluing.
6. The method for manufacturing a continuous fiber composite material structure according to claim 2, characterized in that: The temperature of the hot press molding is not higher than the melting point of the thermoplastic resin.
7. The method for manufacturing a continuous fiber composite material structure according to claim 1, characterized in that: The fiber bundle is made of carbon fiber, glass fiber, aramid fiber or ceramic fiber.
8. The method for manufacturing a continuous fiber composite material structure according to claim 1, characterized in that: The thermoplastic resin comprises polyoxymethylene (POM), acrylonitrile-butadiene-styrene (ABS), polyphenylene sulfide (PPS), polysulfone (PSU), polyethersulfone (PES), polyetheretherketone (PEEK), aromatic polyester liquid crystal polymer (LCP), polyetherimide (PEI), polyamideimide (PAI), polyacetal (POM), nylon (PA), polycarbonate (PC), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyphenylene ether (PPE), styrene acrylic adhesive acrylonitrile (ASA), polystyrene (PS), polymethyl methacrylate (PMMA), styrene copolymer (MS), cellulose acetate (CA), thermoplastic polyurethane (TPU), thermoplastic polyester elastomer (TPEE), styrene elastomer (TPS), elastomer (PAE), polytetrafluoroethylene (PTFE), vinylon (vinylon), polypropylene (PP), polyethylene (PE), ethylene / vinyl acetate copolymer (EVA) or polyvinyl chloride (PVC) or a combination thereof.
9. The method for manufacturing a continuous fiber composite material structure according to claim 1 or 2, characterized in that: Part or all of the structural units are closed ring structures connected head to tail.
10. The method for manufacturing a continuous fiber composite material structure according to claim 1, characterized in that: The method for manufacturing the continuous fiber composite material structure further comprises the step of coating the continuous fiber composite material structure with a coating material.
11. The method for manufacturing a continuous fiber composite material structure according to claim 10, characterized in that: The coating material is an elastomer, a foaming material, a porous material or a resin material.
12. The method for manufacturing a continuous fiber composite material structure according to claim 10 or 11, characterized in that: The coating material is thermoplastic polyurethane, ethylene / vinyl acetate copolymer, rubber or polyolefin.
13. The method for manufacturing a continuous fiber composite material structure according to claim 1, 2 or 11, characterized in that: One of the structural units is a rod, and the other structural units are wound around the surface of the rod.
14. The method for manufacturing a continuous fiber composite material structure according to claim 1 or 2, characterized in that: The bending comprises passing the continuous fiber bundle through a mold after local heating, wherein the mold is a tubular mold cavity with three-dimensional bending.
15. The method for manufacturing a continuous fiber composite material structure according to claim 1 or 2, characterized in that: The bending comprises conveying the continuous fiber bundle to a bending machine and providing a heat source, so as to use the bending machine to bend at least a part of the continuous fiber bundle that is softened by heat.
Citation Information
Patent Citations
Resin prepreg fiber sheet composite material production method
CN103507280A
Method and system for batch preforming of fiber bundles
CN113891793A
Thermoplastic light composite material and preparation method thereof
CN113968051A
Rapid forming method of continuous fiber reinforced thermoplastic composite material composite component
CN115782245A
Fiber bundle
JP2010156073A
Cited By
Intelligent design method and system for fiber composite anchor rod
CN119623305A