IBC battery and manufacturing method therefor

By setting a protective layer in the preparation of IBC cells and optimizing the texturing and polishing processes of the silicon wafer, the difficulty in preparing the front texturing and back polishing structures is solved, the conversion efficiency and short-circuit current of the solar cell are improved, and more efficient light is achieved. Can be converted.

WO2024221612A1PCT designated stage expired Publication Date: 2024-10-31HENGDIAN GRP DMEGC MAGNETICS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/107435
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2023-07-14
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing IBC battery preparation methods ignore the difficulties in structural preparation of the front-side texturing and back-side polishing of the silicon wafer, resulting in insufficient battery conversion efficiency and short-circuit current.

Method used

A protective layer is set during the preparation process of the IBC battery. Through texturing, polishing and laser windowing technology, an optimized front texture and back polishing structure is formed. The protective layer is used to avoid damage to the front texture and block phosphorus doping of the polysilicon layer. Improve short circuit current and conversion efficiency.

Benefits of technology

It achieves more efficient long-wave light reflection and carrier excitation, improving the conversion efficiency of solar cells. The short-circuit current reaches more than 13.639A, and the efficiency can reach more than 23.69%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023107435_31102024_PF_FP_ABST
    Figure CN2023107435_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed herein are an IBC battery and a manufacturing method therefor. The manufacturing method comprises the following steps: (1) carrying out texturing treatment on an original silicon wafer, coating a protective layer, and etching and modifying the protective layer; (2) polishing the modified silicon wafer, subjecting the polished silicon wafer into LPCVD for growing a TOPCon battery structure, and then using laser to form an opening thereon; and (3) cleaning a polycrystalline silicon layer and the protective layer of the silicon wafer after laser opening formation, preparing a passivation layer, and then carrying out metallization manufacturing to obtain the IBC battery. The present application concerns the neglected problems of front side texturing and back side polishing of silicon wafers in related art, and provides the protective layer during the manufacturing process of the IBC battery, thus satisfying the requirements for a textured surface on the front side and a polished surface on the back side at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

IBC battery and preparation method thereof Technical Field

[0001] The embodiments of the present application relate to the technical field of solar cells, for example, an IBC cell and a method for preparing the same. Background Art

[0002] IBC cells, with no front-side busbar and positive and negative electrodes located on the back, eliminate the need for front-side metal contacts, resulting in maximum cell optimization. N-type silicon wafers, with their advantages of low light-induced degradation and long minority carrier lifetime, have garnered significant attention in the photovoltaic industry. However, they also have a price disadvantage compared to P-type silicon wafers. Furthermore, given that most battery manufacturers still primarily utilize P-type PERC cells, P-type IBCs have also garnered significant attention to extend plant life.

[0003] From the perspective of polished surface and velvet surface, the polished surface has a stronger control ability for interface composite. At the same time, the polished surface has a greater possibility of total reflection of light of different wavelengths, especially long-wavelength light. Therefore, the polished surface becomes the first choice for the back of the battery, and the pyramid velvet surface is the inevitable choice for the front of the battery due to the need to trap light.

[0004] CN108447947A discloses a method for preparing an IBC cell with passivated contacts, comprising growing a back surface oxide layer on the back surface of an N-type crystalline silicon substrate, then growing an intrinsic polysilicon layer or an intrinsic amorphous silicon layer on the back surface oxide layer, then implanting boron ions into the intrinsic polysilicon layer or the intrinsic amorphous silicon layer; then growing a mask, then laser-cutting to form intersecting p+ and n+ regions, and finally annealing the p+ region and doping the n+ region simultaneously using phosphorus diffusion, thereby forming alternating p+ and n+ doped regions on the back surface. The method has the following beneficial effects: the oxide layer provides improved surface passivation for the back surface of the N-type crystalline silicon substrate, while carriers can be freely transmitted through the oxide layer, resulting in a cell with higher open-circuit voltage and conversion efficiency; the back surface n+ doped region and the back surface p+ doped region are formed together in a single high-temperature process, significantly reducing the number of high-temperature processes and saving production costs. However, this method does not address front-side velvet removal and back-side polishing of the silicon wafer, ignoring the difficulties in fabricating the structure.

[0005] Summary of the Invention

[0006] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0007] An embodiment of the present application provides an IBC battery and a method for preparing the same. The present application focuses on the problems of linting on the front side and polishing on the back side of silicon wafers that have been ignored in the related art. A protective layer is provided during the preparation of the IBC battery to simultaneously meet the needs of linting on the front side and polishing on the back side.

[0008] In a first aspect, an embodiment of the present application provides a method for preparing an IBC battery, the method comprising the following steps:

[0009] (1) After the original silicon wafer is textured, a protective layer is coated and the protective layer is etched and modified;

[0010] (2) The modified silicon wafer is polished, and the polished silicon wafer is placed into the LPCVD growth TOPCon cell structure and then laser windowing is performed;

[0011] (3) The polysilicon layer and the protective layer of the silicon wafer after laser windowing are cleaned, and a passivation layer is prepared and then metallized to obtain the IBC battery.

[0012] In this application, after the silicon wafer is textured, a protective material of a certain thickness is used to protect the silicon wafer. The protective layer is used to avoid the destruction of the front texture surface caused by back polishing, providing the best process for front light trapping, and on the other hand, to block the phosphorus doping in the polysilicon layer to form a recombination center.

[0013] This application aims at the formation of the P region, does not require the incorporation of boron, and uses a protective layer to protect the front velvet surface with the lowest possible reflectivity, thereby increasing the short-circuit current. At the same time, the laser window area is formed into a polished state, so that the long-wave light transmitted into the battery cell is maximized. The reflection is helpful to form more carrier excitations, thereby improving the battery conversion efficiency.

[0014] Preferably, the temperature of the texturing treatment in step (1) is 75-82°C, for example, 75°C, 76°C, 78°C, 80°C or 82°C.

[0015] Preferably, the texturing treatment time is 400-600 s, for example, 400 s, 450 s, 500 s, 550 s or 600 s.

[0016] Preferably, alkali washing is performed before the texturing treatment.

[0017] Preferably, the alkali solution for texturing comprises sodium hydroxide and additives.

[0018] Preferably, the mass concentration of sodium hydroxide in the alkali solution is 1.5-5%, for example, 1.5%, 2%, 3%, 4% or 5%.

[0019] Preferably, the mass concentration of the additive in the alkali solution is 0.3-1.5%, for example, 0.3%, 0.5%, 0.8%, 1% or 1.5%.

[0020] Preferably, the texturing treatment is followed by alkali washing, acid washing, slow extraction and drying.

[0021] Preferably, the material of the protective layer in step (1) includes silicon nitride.

[0022] Preferably, the protective layer has a thickness of 60 to 200 nm, for example, 60 nm, 80 nm, 100 nm, 150 nm or 200 nm.

[0023] The thickness of the protective layer will affect the performance of the IBC battery. If it exceeds the above range, stress may be generated, causing the silicon wafer to warp and affecting the automated operation.

[0024] Preferably, the modification treatment in step (1) includes etching treatment.

[0025] Preferably, the etching solution used in the etching process includes hydrofluoric acid.

[0026] Preferably, the concentration of the hydrofluoric acid is 75-85%, for example, 75%, 78%, 80%, 82% or 85%.

[0027] Preferably, the modification treatment time is 30 to 60 seconds, for example, 30 seconds, 35 seconds, 40 seconds, 50 seconds or 60 seconds.

[0028] Preferably, the temperature of the polishing treatment in step (2) is 68-75°C, for example, 68°C, 69°C, 70°C, 72°C or 75°C.

[0029] Preferably, the polishing treatment time is 200 to 300 seconds, for example, 200 seconds, 220 seconds, 250 seconds, 280 seconds or 300 seconds.

[0030] Preferably, the mass concentration of sodium hydroxide in the alkali solution used in the polishing treatment is 1.5-5%, for example: 1.5%, 2%, 3%, 4% or 5%.

[0031] Preferably, the mass concentration of the additive in the alkali solution is 0.9-1.4%, for example, 0.9%, 1%, 1.1%, 1.2% or 1.4%.

[0032] Preferably, the polishing treatment is followed by alkali washing, pickling, slow extraction and drying.

[0033] Preferably, the thickness of the tunneling layer in the TOPCon battery structure grown in step (2) is 1.2 to 1.8 nm, for example, 1.2 nm, 1.4 nm, 1.5 nm, 1.6 nm or 1.8 nm.

[0034] Preferably, the thickness of the polysilicon layer in the grown TOPCon cell structure is 80-180 nm, for example, 80 nm, 100 nm, 120 nm, 150 nm or 180 nm.

[0035] Preferably, the phosphorus concentration in the grown TOPCon cell structure is 1e 20 ~4e 21 / cm 3 , for example: 1e 20 / cm 3 、2e 20 / cm 3 、3e 21 / cm 3 、4e 21 / cm 3 wait.

[0036] Preferably, the power of the laser window opening in step (2) is 20 to 40 W, for example, 20 W, 25 W, 30 W, 35 W or 40 W.

[0037] Preferably, the frequency of the laser windowing is 400-800 kHz, for example, 400 kHz, 500 kHz, 600 kHz, 700 kHz or 800 kHz.

[0038] Preferably, the width of the laser-windowed main gate is 800-1000 μm, for example, 800 μm, 850 μm, 900 μm, 950 μm or 1000 μm.

[0039] Preferably, the interval between the laser-windowed main grids is 15-20 mm, for example, 15 mm, 16 mm, 17 mm, 18 mm, 19 mm or 20 mm.

[0040] Preferably, the width of the secondary grid of the laser window is 180-250 μm, for example, 180 μm, 190 μm, 200 μm, 220 μm or 250 μm.

[0041] Preferably, the sub-grating interval of the laser window is 1.1-1.5 mm, for example, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm or 1.5 mm.

[0042] Preferably, the cleaning temperature of the polysilicon layer in step (3) is 70-85°C, for example, 70°C, 72°C, 75°C, 80°C or 85°C.

[0043] Preferably, the cleaning time of the polysilicon layer is 300-450s, for example, 300s, 320s, 350s, 400s or 450s.

[0044] Preferably, the concentration of NaOH in the cleaning solution for the polysilicon layer is 1.5-5%, for example, 1.5%, 2%, 3%, 4% or 5%.

[0045] Preferably, the concentration of the additive in the cleaning solution for the polysilicon layer is 0.5-2.5%, for example, 0.5%, 1%, 1.5%, 2% or 2.5%.

[0046] Preferably, the concentration of HF in the cleaning solution for the protective layer is 8-20%, for example, 8%, 10%, 12%, 15% or 20%.

[0047] Preferably, the concentration of HCl in the cleaning solution for the protective layer is 4.5-10%, for example, 4.5%, 5%, 6%, 8% or 10%.

[0048] Preferably, the cleaning time of the protective layer is 150 to 300 seconds, for example, 150 seconds, 180 seconds, 200 seconds, 250 seconds or 300 seconds.

[0049] Preferably, the passivation layer in step (3) includes an aluminum oxide layer and a silicon nitride layer.

[0050] Preferably, the thickness of the aluminum oxide layer is 2-10 nm, for example, 2 nm, 4 nm, 6 nm, 8 nm or 10 nm.

[0051] Preferably, the thickness of the silicon nitride layer is 60-180 nm, for example, 60 nm, 80 nm, 100 nm, 150 nm or 180 nm.

[0052] Preferably, the virtual-to-real ratio of the metallized laser is (0.5-0.8):0.3, for example: 0.5:0.3, 0.6:0.3, 0.7:0.3 or 0.8:0.3.

[0053] Preferably, the aspect ratio of the silver grid lines produced by metallization is 1:(3-6), for example, 1:3, 1:4, 1:5 or 1:6.

[0054] Preferably, the aspect ratio of the aluminum grid lines produced by metallization is 1:(5-7), for example, 1:5, 1:5.5, 1:6, 1:6.5 or 1:7.

[0055] Preferably, the total wet weight of the silver paste produced by the metallization is 120-170 g, for example, 120 g, 130 g, 140 g, 150 g, 160 g or 170 g.

[0056] Preferably, the wet weight of the total aluminum paste produced by the metallization is 120-150 g, for example, 120 g, 130 g, 140 g or 150 g.

[0057] In a second aspect, an embodiment of the present application provides an IBC battery, which is manufactured by the method described in the first aspect.

[0058] Compared with the related art, the embodiments of the present application have the following beneficial effects:

[0059] (1) The embodiment of the present application ensures the formation of a structure with a velvet surface on the front and a polished surface in the laser area on the back, thereby more effectively utilizing long-wavelength light, increasing the number of excited carriers, and thus improving the conversion efficiency of the solar cell.

[0060] (2) The efficiency of the IBC battery described in the embodiment of the present application can reach more than 23.69%, and the short-circuit current can reach more than 13.639A.

[0061] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.

[0063] FIG1 is a flow chart of the preparation of the IBC battery described in Example 1 of the present application.

[0064] FIG2 is a schematic diagram of the preparation of the IBC battery described in Example 1 of the present application.

[0065] Figure 3 is a schematic structural diagram of the IBC battery described in Example 1 of the present application, 1-silicon substrate; 2-oxide layer; 3-p-type / n-type polysilicon layer; 4-aluminum oxide; 5-silicon nitride; 6-silver electrode; 7-aluminum electrode.

[0066] FIG4 is a diagram of the IBC battery described in Example 1 of the present application, 3-p-type / n-type polysilicon layer; 6-silver electrode; 7-aluminum electrode. DETAILED DESCRIPTION

[0067] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.

[0068] Example 1

[0069] This embodiment provides an IBC battery. The preparation flow chart of the IBC battery is shown in FIG1 , the preparation schematic diagram of the IBC battery is shown in FIG2 , and the preparation method of the IBC battery is as follows:

[0070] (1) The original silicon wafer is placed in a texturing machine and texturing is performed after pre-alkali washing. The texturing temperature is 82°C, the time is 600s, the NaOH concentration is 5%, and the additive concentration is 0.3%. Then, it is post-alkali washing, acid washing, slow extraction, and drying. The silicon wafer after texturing is coated with a protective layer with a thickness of 200nm. The silicon wafer after protective layer coating is placed in a chain etching machine with an HF concentration of 85% and a reaction time of 60s.

[0071] (2) The etched silicon wafer is put into the polishing machine and polished after pre-alkali washing. The polishing temperature is 75 ° C, the time is 300 s, the NaOH concentration is 5%, the additive concentration is 0.9%, and then it is post-alkali washing, acid washing, slow extraction, and drying. The polished silicon wafer is put into the LPCVD growth TOPCon cell structure. The thickness of the growth tunneling layer is 1.8 nm, the thickness of the polysilicon layer is 180 nm, and the phosphorus concentration is 4e 21 / cm 3 , the silicon wafer after growing the TOPCon cell structure was laser windowed, the laser rated power was 40W, the frequency was 400KHz, the main grid width was 1000μm, the interval was 20mm, the secondary grid width was 250μm, and the secondary grid interval was 1.5mm;

[0072] (3) The polysilicon layer and protective layer of the silicon wafer after laser windowing are cleaned. The front PSG is cleaned in an etching machine, and then the polysilicon layer is cleaned. The reaction temperature is 85°C, the time is 450s, the NaOH concentration is 5%, and the additive concentration is 0.5%. The protective layer is then cleaned after post-alkali washing. The HF concentration is 20%, the HCl concentration is 10%, and the reaction time is 300s. The cleaned silicon wafer is sequentially put into NCD and PECVD to grow aluminum oxide and silicon nitride. The aluminum oxide thickness is 10nm and the silicon nitride thickness is 180nm. Metallization preparation is performed. The laser virtual-real ratio is 0.8:0.3, the silver grid line aspect ratio is 1:6, the aluminum grid line aspect ratio is 1:7, the total silver paste wet weight is 170g, and the total aluminum paste wet weight is 150g. The IBC battery is obtained. The structural schematic diagram of the IBC battery is shown in Figure 3, and the IBC battery diagram is shown in Figure 4.

[0073] Example 2

[0074] This embodiment provides an IBC battery, and the preparation method of the IBC battery is as follows:

[0075] (1) The original silicon wafer is placed in the texturing machine and texturing is performed after pre-alkali washing. The texturing temperature is 75°C, the time is 400 seconds, the NaOH concentration is 1.5%, and the additive concentration is 1.5%. Then, it is post-alkali washing, acid washing, slow extraction, and drying. The silicon wafer after texturing is double-inserted for protective layer coating. The thickness of the protective layer is 60nm. The silicon wafer after protective layer coating is placed in the chain etching machine with an HF concentration of 75% and a reaction time of 30 seconds.

[0076] (2) The etched silicon wafer is put into the polishing machine and polished after the pre-alkali washing. The polishing temperature is 68 ° C, the time is 200 s, the NaOH concentration is 1.5%, and the additive concentration is 1.4%. Then it is post-alkali washing, acid washing, slow extraction, and drying. The polished silicon wafer is put into the LPCVD to grow the TOPCon cell structure. The thickness of the tunneling layer is 1.2 nm, the thickness of the polysilicon layer is 80 nm, and the phosphorus concentration is 1e 20 / cm 3 , the silicon wafer after growing the TOPCon cell structure was laser windowed, the laser rated power was 20W, the frequency was 800KHz, the main grid width was 800μm, the interval was 15mm, the secondary grid width was 180μm, and the secondary grid interval was 1.1mm;

[0077] (3) The polysilicon layer and protective layer of the silicon wafer after laser windowing are cleaned. The front PSG is cleaned in an etching machine, and then the polysilicon layer is cleaned. The reaction temperature is 70°C, the time is 300s, the NaOH concentration is 1.5%, and the additive concentration is 2.5%. The protective layer is then cleaned after post-alkali washing. The HF concentration is 8%, the HCl concentration is 4.5%, and the reaction time is 150s. The cleaned silicon wafer is sequentially grown in NCD and PECVD to grow aluminum oxide and silicon nitride. The aluminum oxide thickness is 2nm and the silicon nitride thickness is 60nm. Metallization preparation is performed. The laser virtual-real ratio is 0.5:0.3, the silver grid line aspect ratio is 1:3, the aluminum grid line aspect ratio is 1:5, the total silver paste wet weight is 120g, and the total aluminum paste wet weight is 120g to obtain the IBC battery.

[0078] Example 3

[0079] This embodiment provides an IBC battery, and the preparation method of the IBC battery is as follows:

[0080] (1) The original silicon wafer is placed in the texturing machine and texturing is performed after pre-alkali washing. The texturing temperature is 78°C, the time is 500s, the NaOH concentration is 3.0%, and the additive concentration is 1.0%. Then, it is post-alkali washing, acid washing, slow extraction, and drying. The silicon wafer after texturing is double-inserted for protective layer coating. The thickness of the protective layer is 120nm. The silicon wafer after protective layer coating is placed in the chain etching machine, the HF concentration is 80%, and the reaction time is 45s.

[0081] (2) The etched silicon wafer is put into the polishing machine and polished after the pre-alkali washing. The polishing temperature is 72 ° C, the time is 250s, the NaOH concentration is 3.5%, the additive concentration is 1.1%, and then the post-alkali washing, acid washing, slow lifting, and drying are carried out. The polished silicon wafer is put into the LPCVD to grow the TOPCon cell structure. The thickness of the tunneling layer is 1.5nm, the thickness of the polysilicon layer is 120nm, and the phosphorus concentration is 6e 20 / cm 3 , the silicon wafer after growing the TOPCon cell structure was laser windowed, the laser rated power was 30W, the frequency was 600KHz, the main grid width was 900μm, the interval was 18mm, the secondary grid width was 220μm, and the secondary grid interval was 1.3mm;

[0082] (3) The polysilicon layer and protective layer of the silicon wafer after laser windowing are cleaned. Enter the etching machine to clean the front PSG, and then clean the polysilicon layer. The reaction temperature is 75°C, the time is 360s, the NaOH concentration is 3.5%, and the additive concentration is 1.5%. Then, the protective layer is cleaned after post-alkali washing. The HF concentration is 15%, the HCl concentration is 7.5%, and the reaction time is 220s. The cleaned silicon wafer is sequentially put into NCD and PECVD to grow aluminum oxide and silicon nitride. The aluminum oxide thickness is 6nm and the silicon nitride thickness is 120nm. Metallization preparation is carried out. The laser virtual-real ratio is 0.6:0.3, the silver grid line aspect ratio is 1:4.5, the aluminum grid line aspect ratio is 1:6, the total silver paste wet weight is 140g, the total aluminum paste wet weight is 135g, and the total aluminum paste wet weight is 120g, thereby obtaining the IBC battery.

[0083] Comparative Example 1

[0084] This comparative example provides an IBC battery, and the preparation method of the IBC battery is as follows:

[0085] (1) The original silicon wafer is put into the texturing machine, and the texturing is carried out after the pre-alkali washing. The texturing temperature is 82 ° C, the time is 600 s, the NaOH concentration is 5%, and the additive concentration is 0.3%. Then it is post-alkali washing, acid washing, slow extraction, and drying;

[0086] (2) The textured silicon wafer is placed into the LPCVD growth TOPCon cell structure, with a tunneling layer thickness of 1.8 nm, a polysilicon layer thickness of 180 nm, and a phosphorus concentration of 4e 21 / cm 3 , the silicon wafer after growing the TOPCon cell structure is laser windowed, the laser rated power is 40W, the frequency is 400KHz, the main grid width is 1000um, the interval is 20mm, the secondary grid width is 250um, and the secondary grid interval is 1.5mm;

[0087] (3) After laser windowing, the polycrystalline layer and protective layer of the silicon wafer are cleaned, and the silicon wafer is put into the etching machine to clean the front PSG, and then the polysilicon layer is cleaned. The reaction temperature is 85°C, the time is 450s, the NaOH concentration is 5%, and the additive concentration is 0.5%; the protective layer is then cleaned after post-alkali washing. The HF concentration is 20%, the HCl concentration is 10%, and the reaction time is 300s. The cleaned silicon wafer is sequentially put into NCD and PECVD to grow aluminum oxide and silicon nitride. The thickness of aluminum oxide is 10nm and the thickness of silicon nitride is 180nm. The metallization preparation has a laser virtual-to-real ratio of 0.8:0.3, a silver grid line aspect ratio of 1:6, an aluminum grid line aspect ratio of 1:7, a total silver paste wet weight of 170g, and a total aluminum paste wet weight of 150g to obtain the IBC battery.

[0088] Comparative Example 2

[0089] This comparative example provides an IBC battery, and the preparation method of the IBC battery is as follows:

[0090] (1) The original silicon wafer is put into the texturing machine, and the texturing is carried out after the pre-alkali washing. The texturing temperature is 75 ° C, the time is 400 s, the NaOH concentration is 1.5%, and the additive concentration is 1.5%. Then it is post-alkali washing, acid washing, slow extraction, and drying;

[0091] (2) The textured silicon wafer is placed into the LPCVD growth TOPCon cell structure, with a tunneling layer thickness of 1.2nm, a polysilicon layer thickness of 80nm, and a phosphorus concentration of 1e 20 / cm 3 , the silicon wafer after growing the TOPCon cell structure was laser windowed, the laser rated power was 20W, the frequency was 800KHz, the main grid width was 800um, the interval was 15mm, the secondary grid width was 180um, and the secondary grid interval was 1.1mm;

[0092] (3) The polycrystalline layer and protective layer of the silicon wafer after laser windowing are cleaned. Enter the etching machine to clean the front PSG, and then clean the polysilicon layer. The reaction temperature is 70°C, the time is 300s, the NaOH concentration is 1.5%, and the additive concentration is 2.5%. Then, the protective layer is cleaned after post-alkali washing. The HF concentration is 8%, the HCl concentration is 4.5%, and the reaction time is 150s. The cleaned silicon wafer is sequentially put into NCD and PECVD to grow aluminum oxide and silicon nitride. The aluminum oxide thickness is 2nm and the silicon nitride thickness is 60nm. Metallization is performed to prepare the laser virtual-real ratio of 0.5:0.3, the silver grid line height-to-width ratio is 1:3, the aluminum grid line height-to-width ratio is 1:5, the total silver paste wet weight is 120g, and the total aluminum paste wet weight is 120g, thereby obtaining the IBC battery.

[0093] Performance testing:

[0094] After three batch experiments, the efficiency (Eta), short-circuit current (Isc), open-circuit voltage (Uoc) and fill factor (FF) of the final silicon wafer product were tracked. The test results are shown in Table 1:

[0095] Table 1

[0096] As can be seen from Table 1, from Examples 1-3, the efficiency of the IBC battery described in the present application can reach more than 23.69%, and the short-circuit current can reach more than 13.639A. Compared with the comparative example, the efficiency Eta is increased by 0.16-0.22%. The main improvements come from Isc, Uoc, and FF, especially in the short-circuit current Isc, which is increased by 96mA-106mA.

[0097] By comparing Example 1 with Comparative Examples 1 and 2, it can be seen that Example 1 achieves a polished surface of the back laser window area by adding a front protective film, while in Comparative Examples 1 and 2, the laser window area is a velvet surface. The two have little difference in Uoc, but Isc, Example 1 is 96mA larger, which directly leads to a difference in Eta of nearly 0.16%.

[0098] The applicant declares that the above is only a specific implementation method of the present application, but the protection scope of the present application is not limited thereto. Technical personnel in the relevant technical field should understand that any changes or substitutions that can be easily thought of by technical personnel in the relevant technical field within the technical scope disclosed in this application fall within the protection scope and disclosure scope of this application.

Claims

1. A method for preparing an IBC battery, comprising the following steps: (1) After the original silicon wafer is textured, a protective layer is coated and the protective layer is etched and modified; (2) polishing the modified silicon wafer, placing the polished silicon wafer into the LPCVD grown TOPCon cell structure and then laser windowing; (3) The polysilicon layer and the protective layer of the silicon wafer after laser windowing are cleaned, and a passivation layer is prepared and then metallized to obtain the IBC battery.

2. The preparation method according to claim 1, wherein The temperature of the texturing treatment in step (1) is 75-82°C.

3. The preparation method according to claim 1 or 2, wherein: The texturing process lasts for 400 to 600 seconds.

4. The preparation method according to any one of claims 1 to 3, wherein The texturing process is preceded by alkali washing.

5. The preparation method according to any one of claims 1 to 4, wherein: The alkali solution for making the texturing comprises sodium hydroxide and additives; Preferably, the mass concentration of sodium hydroxide in the alkali solution is 1.5-5%; Preferably, the mass concentration of the additive in the alkali solution is 0.3-1.5%; Preferably, the texturing treatment is followed by post-alkali washing, acid washing, slow washing and drying.

6. The preparation method according to any one of claims 1 to 5, wherein: The material of the protective layer in step (1) includes silicon nitride; Preferably, the thickness of the protective layer is 60-200 nm.

7. The preparation method according to any one of claims 1 to 6, wherein: The modification treatment in step (1) includes etching treatment; Preferably, the etching solution used in the etching process includes hydrofluoric acid; Preferably, the concentration of the hydrofluoric acid is 75-85%; Preferably, the modification treatment takes 30 to 60 seconds.

8. The preparation method according to any one of claims 1 to 7, wherein: The temperature of the polishing treatment in step (2) is 68-75° C. Preferably, the polishing time is 200 to 300 seconds; Preferably, the mass concentration of sodium hydroxide in the alkali solution used in the polishing process is 1.5-5%; Preferably, the mass concentration of the additive in the alkali solution is 0.9-1.4%; Preferably, the polishing treatment is followed by alkaline washing, acid washing, slow washing and drying.

9. The preparation method according to any one of claims 1 to 8, wherein: The thickness of the tunneling layer in the grown TOPCon battery structure in step (2) is 1.2 to 1.8 nm; Preferably, the thickness of the polysilicon layer in the grown TOPCon cell structure is 80 to 180 nm; Preferably, the phosphorus concentration in the grown TOPCon cell structure is 1e 20 ~4e 21 / cm 3 .

10. The preparation method according to any one of claims 1 to 9, wherein: The power of the laser window opening in step (2) is 20 to 40 W; Preferably, the frequency of the laser windowing is 400 to 800 kHz; Preferably, the width of the laser-opened main grid is 800-1000 μm; Preferably, the main grid spacing of the laser window is 15 to 20 mm; Preferably, the width of the secondary grid of the laser window opening is 180-250 μm; Preferably, the sub-grid interval of the laser window is 1.1-1.5 mm.

11. The preparation method according to any one of claims 1 to 10, wherein: The cleaning temperature of the polysilicon layer in step (3) is 70-85° C. Preferably, the cleaning time of the polysilicon layer is 300 to 450 seconds; Preferably, the NaOH concentration in the cleaning solution of the polysilicon layer is 1.5-5%; Preferably, the concentration of the additive in the cleaning solution for the polysilicon layer is 0.5 to 2.5%; Preferably, the concentration of HF in the cleaning solution of the protective layer is 8-20%; Preferably, the concentration of HCl in the cleaning solution of the protective layer is 4.5-10%; Preferably, the cleaning time of the protective layer is 150 to 300 seconds.

12. The preparation method according to any one of claims 1 to 11, wherein: The passivation layer in step (3) comprises an aluminum oxide layer and a silicon nitride layer; Preferably, the thickness of the aluminum oxide layer is 2 to 10 nm; Preferably, the thickness of the silicon nitride layer is 60 to 180 nm; Preferably, the virtual-real ratio of the laser produced by the metallization is (0.5-0.8):0.3; Preferably, the aspect ratio of the silver grid lines produced by metallization is 1:(3-6); Preferably, the aspect ratio of the aluminum grid line produced by metallization is 1:(5-7); Preferably, the total wet weight of the silver paste produced by the metallization is 120-170 g; Preferably, the wet weight of the total aluminum paste produced by the metallization is 120-150 g.

13. An IBC battery, wherein: The IBC battery is prepared by the method according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Method for preparing passivated contact IBC battery

    CN108447947A

  • Preparation method of IBC battery and IBC battery

    CN114664969A

  • Full back contact solar cell and manufacturing method thereof

    CN115020508A

  • Preparation method of back patterned N region of IBC battery

    CN115020534A

  • Preparation method of back double POLO structure of IBC battery

    CN115020535A