P-type back contact battery and preparation method therefor, and photovoltaic module

By forming a gettering structure and etching treatment on the process chip of the P-type back contact battery, the problem of impurities in the recombination center is solved, the carrier transmission rate and photoelectric conversion efficiency are improved, and the conversion efficiency of the battery is improved.

WO2024221627A1PCT designated stage expired Publication Date: 2024-10-31HENGDIAN GRP DMEGC MAGNETICS CO LTD

Patent Information

Application Number
PCT/CN2023/109020
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-23
Filing Date
2023-07-25
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Due to the lack of annealing treatment of PERC technology in P-type back contact solar cells, there are many impurities in the recombination center, resulting in low carrier transmission efficiency and affecting the cell conversion efficiency.

Method used

A gettering structure is formed on the process chip of the P-type back contact battery. Through the stacked tunnel layer, polysilicon layer and phosphosilicate glass layer, impurities are absorbed and recombination centers are reduced, the carrier transmission rate is improved, and the gettering structure is formed. The final chip is etched and passivated to protect the battery.

Benefits of technology

It effectively reduces the recombination center formed by impurities, improves carrier transmission efficiency and photoelectric conversion efficiency, and improves the overall performance of P-type back contact cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023109020_31102024_PF_FP_ABST
    Figure CN2023109020_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a P-type back contact battery and a preparation method therefor, and a photovoltaic module. The preparation method for the P-type back contact battery comprises: preparing a process piece of the P-type back contact battery; forming a gettering structure on a first surface side and / or a second surface side, the gettering structure comprising a second tunneling layer, a second polysilicon layer, and a second phosphosilicate glass layer which are stacked; etching the process piece on which the gettering structure is formed, so as to remove the gettering structure, and a first phosphosilicate glass layer on the second surface side; and forming a passivation layer on the first surface side and the second surface side of the process piece respectively. According to the technical solution of the present application, a gettering structure is formed on a first surface side and a second surface side of a P-type back contact battery to absorb impurities on the first surface side and the second surface side of the process piece, so that recombination centers formed by the impurities are reduced, the carrier transport rate is improved, and the conversion efficiency of the P-type back contact battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

A P-type back contact cell and its preparation method, and photovoltaic module Technical Field

[0001] The embodiments of the present application relate to the technical field of solar cells, for example, a P-type back-contact cell and a preparation method thereof, and a photovoltaic module. Background Art

[0002] With the gradual depletion of fossil fuels, solar cells are becoming increasingly popular as a new energy alternative. Solar cells are devices that convert sunlight into electricity. They utilize the photovoltaic principle to generate charge carriers, which are then extracted using electrodes, converting solar energy into electrical energy for use.

[0003] The most significant feature of P-type back-contact solar cells is that the emitter and metal contact are both located on the back of the cell. Without the obstruction of the metal electrode on the front, the cell has a higher short-circuit current (Isc). This allows for wider metal grid lines on the back, reducing the series resistance (Rs) and thus increasing the fill factor (FF). Furthermore, this unobstructed front-facing cell not only has high conversion efficiency but also looks more aesthetically pleasing. Furthermore, modules with full back-contact electrodes are easier to assemble. Back-contact cells are currently one of the technological advancements in achieving high-efficiency crystalline silicon cells.

[0004] However, since the laser window area in the P-type back contact cell has not undergone the annealing in the PERC (Passivated Emitter Rear Cell) cell, its recombination centers will still exist in large quantities. Therefore, how to reduce the recombination centers and thus increase the conversion efficiency of the cell has become an urgent problem to be solved.

[0005] Summary of the Invention

[0006] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0007] The embodiments of the present application provide a P-type back-contact cell and its preparation method, and a photovoltaic module to reduce the recombination centers formed by impurities, improve the carrier transmission efficiency, and thereby improve the conversion efficiency of the P-type back-contact cell.

[0008] In a first aspect, an embodiment of the present application provides a method for preparing a P-type back-contact battery, comprising:

[0009] A process wafer for preparing a P-type back-contact battery; the process wafer includes a P-type silicon-based substrate; the P-type silicon-based substrate includes a first surface and a second surface opposite to each other; a first tunneling layer, a first polysilicon layer, a first phosphosilicate glass layer stacked in sequence, and a groove penetrating the first tunneling layer, the first polysilicon layer, and the first phosphosilicate glass layer are provided on the second surface;

[0010] forming a gettering structure on the first surface side and / or the second surface side; the gettering structure comprises a second tunneling layer, a second polysilicon layer, and a second phosphosilicate glass layer which are stacked;

[0011] Etching the process wafer after forming the gettering structure to remove the gettering structure and the first phosphosilicate glass layer on the second surface side;

[0012] Passivation layers are formed on the first surface side and the second surface side of the process wafer, respectively.

[0013] Optionally, a process sheet for preparing a P-type back contact cell includes:

[0014] Providing a P-type silicon-based substrate;

[0015] forming the first tunneling layer, the first polysilicon layer, and the first phosphosilicate glass layer stacked in sequence on the first surface and the second surface side of the P-type silicon-based substrate respectively;

[0016] forming an opening in the first phosphosilicate glass layer on the second surface side to expose a portion of the first polysilicon layer on the second surface side;

[0017] After forming an opening in the first phosphosilicate glass layer on the second surface side, removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate to expose the first polysilicon layer on the first surface side;

[0018] The first surface and the second surface side of the P-type silicon-based substrate are etched to remove the first polysilicon layer and the first tunneling layer located in the opening to form the groove at the opening, and to remove the first tunneling layer and the first polysilicon layer located on the first surface side.

[0019] Optionally, a process sheet for preparing a P-type back contact cell includes:

[0020] Providing a P-type silicon-based substrate;

[0021] Forming a first tunneling layer, a first polysilicon layer, and a first phosphosilicate glass layer stacked in sequence on the first surface and the second surface side of the P-type silicon-based substrate respectively;

[0022] removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate to expose the first polysilicon layer on the first surface side;

[0023] After removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate, forming an opening on the first phosphosilicate glass layer on the second surface side to expose a portion of the first polysilicon layer on the second surface side;

[0024] The first surface and the second surface side of the P-type silicon-based substrate are etched to remove the first polysilicon layer and the first tunneling layer located in the opening to form the groove at the opening, and to remove the first tunneling layer and the first polysilicon layer located on the first surface side.

[0025] Optionally, etching the first surface and the second surface of the P-type silicon-based substrate includes:

[0026] An alkaline etching solution is used to etch the openings on the first surface side and the second surface side of the P-type silicon-based substrate to remove the first polysilicon layer and the first tunneling layer located in the opening to form the groove at the opening, and to remove the first tunneling layer and the first polysilicon layer located on the first surface side.

[0027] Optionally, forming an opening on the first phosphosilicate glass layer on the second surface side to expose a portion of the first polysilicon layer on the second surface side includes:

[0028] The opening is formed in the first phosphosilicate glass layer on the second surface side of the P-type silicon base substrate using a laser.

[0029] Optionally, forming a gettering structure on the first surface side and / or the second surface side includes:

[0030] The first tunneling layer, the first polysilicon layer and the first phosphosilicate glass layer are sequentially prepared on the first surface side and the second surface side by using any one of high-temperature thermal oxidation, nitric acid oxidation, ozone oxidation and chemical vapor deposition.

[0031] Optionally, etching the process wafer after forming the gettering structure to remove the gettering structure and the first phosphosilicate glass layer on the second surface side includes:

[0032] Etching the second phosphosilicate glass layer on the second surface side, and the second polysilicon layer and the second tunneling layer on the second surface side to form a groove having a polished surface on the second surface side;

[0033] etching the second phosphosilicate glass layer and the second polysilicon layer on the first surface side to remove the second polysilicon layer;

[0034] The second tunneling layer and the second tunneling layer on the first surface side are etched to remove the first phosphosilicate glass layer and the second tunneling layer on the first surface side.

[0035] Optionally, forming a passivation layer on the first surface side and the second surface side of the process wafer respectively includes:

[0036] forming aluminum oxide layers on a first surface side and a second surface side of the process sheet;

[0037] A silicon nitride layer is formed on the side of the aluminum oxide layer on the first surface side and the second surface side facing away from the P-type silicon-based substrate.

[0038] In a second aspect, an embodiment of the present application provides a P-type back-contact battery, which is manufactured using the manufacturing method of the back-contact battery described in the first aspect.

[0039] In a third aspect, an embodiment of the present application provides a photovoltaic module comprising the P-type back-contact cell described in the second aspect.

[0040] The technical solution provided by the embodiment of the present application forms a gettering structure on the first and second surface sides of the process wafer of the P-type back contact battery to absorb impurities on the first and second surface sides of the process wafer, thereby reducing the recombination centers formed by the impurities, improving the carrier transmission rate, and thus improving the conversion efficiency of the P-type back contact battery. After the gettering structure completes the absorption of impurities on the first and second surface sides, the process wafer with the gettering structure formed is etched to remove the first phosphosilicate glass layer on the gettering structure and the second surface side, and then a passivation layer is formed on the first and second surface sides of the process wafer to protect the P-type back contact battery and prevent external contaminants from entering the P-type back contact battery, thereby improving the photoelectric conversion efficiency of the P-type back contact battery.

[0041] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.

[0043] FIG1 is a flow chart of a method for preparing a P-type back-contact battery provided in an embodiment of the present application;

[0044] FIG2 is a schematic structural diagram of a process for preparing a P-type back-contact battery provided in an embodiment of the present application;

[0045] FIG3 is a flow chart of a method for preparing a P-type back-contact cell according to an embodiment of the present application;

[0046] FIG4 is a schematic diagram of the process structure of a process sheet for preparing a P-type back contact battery provided in an embodiment of the present application;

[0047] FIG5 is a flow chart of a method for preparing another process sheet of a P-type back contact battery provided in an embodiment of the present application;

[0048] FIG6 is a schematic diagram of the process structure of another process sheet for preparing a P-type back contact battery provided in an embodiment of the present application;

[0049] FIG7 is a flow chart of another method for preparing a P-type back-contact battery provided in an embodiment of the present application;

[0050] FIG8 is a schematic structural diagram of another process for preparing a P-type back-contact battery provided in an embodiment of the present application;

[0051] FIG9 is a flow chart of a method for preparing another P-type back-contact battery provided in an embodiment of the present application;

[0052] FIG10 is a schematic diagram of the structure of another process for preparing a P-type back-contact battery provided in an embodiment of the present application. DETAILED DESCRIPTION

[0053] The present application will be further described in detail below with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are intended only to illustrate the present application and are not intended to limit the present application. It should also be noted that, for ease of description, the accompanying drawings only illustrate portions of the present application, not all of the structures.

[0054] The present application provides a method for preparing a P-type back-contact battery. The method is suitable for preparing the P-type back-contact battery provided in the present application. FIG1 is a flow chart of a method for preparing a P-type back-contact battery provided in the present application. FIG2 is a schematic diagram of a process structure of preparing a P-type back-contact battery provided in the present application. As shown in FIG1 , the method for preparing a P-type back-contact battery includes:

[0055] S101, process sheet for preparing P-type back contact battery.

[0056] Among them, the process wafer includes a P-type silicon-based substrate; the P-type silicon-based substrate includes a first surface and a second surface relative to each other; the second surface side is provided with a first tunneling layer, a first polysilicon layer, a first phosphosilicate glass layer stacked in sequence, and a groove penetrating the first tunneling layer, the first polysilicon layer and the first phosphosilicate glass layer.

[0057] Specifically, the P-type silicon-based substrate can be obtained by doping trivalent elements, such as boron or gallium, in a wafer or silicon slice. Si semiconductor is a tetravalent element. After forming electron-hole pairs with the trivalent elements, a large number of holes will be generated in the wafer or silicon slice, thereby forming a P-type silicon-based substrate.

[0058] Referring to FIG2 , the first tunneling layer 21 and the first polysilicon layer 22 on the second surface side can be formed using low-pressure chemical vapor deposition. After forming the first tunneling layer 21 and the first polysilicon layer 22, the P-type silicon-based substrate on which the first tunneling layer 21 and the first polysilicon layer 22 are formed is placed in a low-pressure diffusion furnace, and a phosphorus source is deposited on the second surface side to form the first phosphosilicate glass layer 23. A trench 31 is formed at a position corresponding to the secondary gate on the second surface side using a laser or etching process. The trench 31 penetrates the first tunneling layer 21, the first polysilicon layer 22, and the first phosphosilicate glass layer 23.

[0059] It is understandable that the material and thickness of the first tunneling layer 21, the first polysilicon layer 22, and the first phosphosilicate glass layer 23 can be set according to actual needs and are not specifically limited here. For example, the material of the first tunneling layer 21 can include but is not limited to one or more materials such as silicon oxide, aluminum oxide, titanium oxide, chromium dioxide, gallium oxide, tantalum pentoxide, niobium pentoxide, silicon nitride, silicon carbonitride, aluminum nitride, titanium nitride, and titanium carbonitride; the thickness of the first tunneling layer 21 can be 1.1nm-1.8nm, and the thickness of the first polysilicon layer 22 can be 70nm-180nm; the first phosphosilicate glass layer 23 includes elements such as silicon oxide and phosphorus oxide, wherein the phosphorus source deposition concentration can be 3e20-4e22 / cm 3 .

[0060] S102 , forming a gettering structure on the first surface side and / or the second surface side.

[0061] The gettering structure includes a second tunneling layer, a second polysilicon layer, and a second phosphosilicate glass layer that are stacked.

[0062] It can be understood that the gettering structure is formed on the first surface side and / or the second surface side. The gettering structure can be formed only on the first surface side, or only on the second surface side. Alternatively, the gettering structure can be formed on the first surface side and the second surface side respectively. For ease of description, the following explanation is given by taking the example of forming the gettering structure on both the first surface side and the second surface side.

[0063] Specifically, with continued reference to FIG2 , the gettering structure formed on the first surface side includes a stacked second tunneling layer 111, a second polysilicon layer 112, and a second phosphosilicate glass layer 113, and the gettering structure formed on the second surface side includes a stacked second tunneling layer 221, a second polysilicon layer 222, and a second phosphosilicate glass layer 223. Low-pressure chemical vapor deposition can be used to form the second tunneling layer 111, the second polysilicon layer 112, the second tunneling layer 221, and the second polysilicon layer 222 on the first and second surfaces of the process wafer, respectively. The process wafer is then placed in a low-pressure diffusion furnace, where phosphorus diffusion is completed within the process wafer. During the phosphorus diffusion, the second phosphosilicate glass layer 113 is formed on the first surface side, and the second phosphosilicate glass layer 223 is formed on the second surface side.

[0064] In an optional embodiment, the method of forming the doping structure on the first surface side and the second surface side may include: using any one of high-temperature thermal oxidation, nitric acid oxidation, ozone oxidation, and chemical vapor deposition to sequentially prepare a first tunneling layer, a first polysilicon layer, and a first phosphosilicate glass layer on the first surface side and the second surface side.

[0065] Specifically, metallic impurities such as Fe, Na, Cu, and Au, and non-metallic impurities such as O, C, and N may exist on the first and second surfaces of the process wafer of the P-type silicon substrate. The presence of these impurities will introduce deep defect levels in the silicon substrate. These deep defect levels will capture majority and minority carriers, becoming carrier recombination centers, reducing the minority carrier diffusion length and lowering the efficiency of the P-type back-contact cell. In this case, by forming a gettering structure on the first and second surface sides, the material of the second tunneling layers 111 and 221 in the gettering structure can include, but is not limited to, one of silicon oxide, aluminum oxide, titanium oxide, chromium dioxide, gallium oxide, tantalum pentoxide, niobium pentoxide, silicon nitride, silicon carbonitride, aluminum nitride, titanium nitride, and titanium carbonitride. By utilizing the difference in material between the first tunneling layers 111 and 221 and the P-type silicon substrate, that is, the solubility of impurities in the second tunneling layers 111 and 221 is greater than that in the P-type silicon substrate, gettering is performed on the first and second surface sides. Exemplarily, the material of the second tunneling layers 111 and 221 is aluminum oxide, and the solubility of metal impurities in aluminum oxide is greater than that in the P-type silicon-based substrate. When forming the second phosphorus-silicate glass layers 113 and 223 in the gettering structure, the phosphorus element in the second phosphorus-silicate glass layers 113 and 223 will diffuse into the second polysilicon layers 112 and 222. The increase in the phosphorus concentration in the second polysilicon layers 112 and 222 will also enhance the ability to accommodate impurities, thereby increasing the solubility of impurities in the polysilicon layer and thereby reducing the impurity concentration in the P-type silicon-based substrate. In this way, by forming a gettering structure on the first side surface and the second side surface, gettering is achieved on the first surface side and the second surface side of the P-type silicon-based substrate, reducing the recombination center formed by the impurities, improving the carrier transmission efficiency, and thereby improving the conversion efficiency of the P-type back contact battery.

[0066] It is understood that the materials of the second tunneling layer, the second polysilicon layer, and the second phosphosilicate glass layer can be the same as or different from the materials of the first tunneling layer, the first polysilicon layer, and the first phosphosilicate glass layer. The thicknesses of the second tunneling layer, the second polysilicon layer, and the second phosphosilicate glass layer can be set according to actual needs and are not specifically limited here. For example, the thickness of the second tunneling layers 111 and 221 can be 1nm-1.5nm; the thickness of the second polysilicon layers 112 and 222 can be 60nm-120nm; the second phosphosilicate glass layers 113 and 223 include elements such as silicon oxide and phosphorus oxide, wherein the phosphorus source deposition concentration can be 1e20-2e22 / cm 3 .

[0067] S103 , etching the process wafer after the gettering structure is formed to remove the gettering structure and the first phosphosilicate glass layer on the second surface side.

[0068] Specifically, the process wafer after the formation of the gettering structure can be placed in a chain etching machine, and the process wafer can be etched using an alkaline etching solution or an acidic etching solution to remove the gettering structure on the first surface side and the second surface side, as well as the first phosphosilicate glass layer on the second surface side.

[0069] S104 , forming a passivation layer on the first surface side and the second surface side of the process wafer respectively.

[0070] Specifically, the passivation layer can cover the first surface side and the second surface side respectively, which can prevent pollutants in the air from corroding the interior of the P-type back contact battery, protect the P-type back contact battery, and at the same time provide hydrogen passivation, reduce the silicon wafer interface recombination center, thereby improving the photoelectric conversion efficiency of the P-type back contact battery.

[0071] It is understood that the material and thickness of the passivation layer can be set according to actual needs and are not specifically limited here. For example, the material of the passivation layer can include but is not limited to one of the passivation materials such as aluminum oxide, silicon carbide, phosphorus oxide, etc.

[0072] A P-type back-contact battery is prepared using the above-mentioned method provided in an embodiment of the present application. By forming an impurity absorption structure on the first surface side and the second surface side of the process sheet of the P-type back-contact battery, impurities on the first surface side and the second surface side of the process sheet are absorbed, the recombination centers formed by the impurities are reduced, the carrier transmission rate is improved, and the conversion efficiency of the P-type back-contact battery is thereby improved. After forming a doping structure on the first surface side and the second surface side of the process wafer of the P-type back contact battery, the process wafer with the doping structure formed is etched to remove the doping structure and the first phosphorus silicon glass layer on the second surface side to form a polishing surface at the groove on the second surface side. The polishing surface can totally reflect light of different wavelengths to reflect at least part of the light reaching the second surface side through the smooth polishing surface into the P-type silicon-based substrate, thereby realizing the reuse of light, improving the utilization rate of light energy, and further improving the photoelectric conversion efficiency of the back contact. Passivation layers are then formed on the first surface side and the second surface side of the process wafer respectively to protect the P-type back contact battery and prevent external pollutants from entering the P-type back contact battery. At the same time, hydrogen passivation is provided to reduce the silicon wafer interface recombination center, thereby improving the photoelectric conversion efficiency of the P-type back contact battery.

[0073] In an optional embodiment, FIG3 is a flow chart of a method for preparing a process sheet of a P-type back contact battery provided in an embodiment of the present application, and FIG4 is a schematic diagram of a process structure of a process sheet for preparing a P-type back contact battery provided in an embodiment of the present application. As shown in FIG3 , the process sheet for preparing a P-type back contact battery specifically includes:

[0074] S111. Provide a P-type silicon-based substrate.

[0075] Specifically, referring to FIG4 , a P-type silicon-based substrate 4 has a first surface 10 and a second surface 20 that are opposite to each other, and the first surface 10 and the second surface 20 are flat, so that a whole layer of other structures can be subsequently formed on the first surface 10 and the second surface 20. The first surface 10 can be the front surface of a P-type back-contact solar cell, i.e., the surface that receives light, and the second surface 20 can be the back surface of the P-type back-contact solar cell, i.e., the surface facing away from the light.

[0076] S112 , forming a first tunneling layer, a first polysilicon layer, and a first phosphosilicate glass layer stacked in sequence on the first surface and the second surface side of the P-type silicon-based substrate, respectively.

[0077] Specifically, referring to Figure 4, a first tunneling layer 11, a first polysilicon layer 12 and a first phosphosilicate glass layer 13 are formed on the first surface side 10 of the P-type silicon-based substrate 4, and a first tunneling layer 21, a first polysilicon layer 22 and a first phosphosilicate glass layer 23 are formed on the second surface side 20. The specific preparation process can be: a low-pressure chemical vapor deposition preparation method can be first used to form a first tunneling layer 11, a first polysilicon layer 12, a first tunneling layer 21 and a first polysilicon layer 22 on the first surface 10 side and the second surface 20 side of the P-type silicon-based substrate 4, respectively, and then the process wafer is placed in a low-pressure diffusion furnace to form first phosphosilicate glass layers 13 and 23 on the first surface 10 and the second surface side, respectively, and complete phosphorus diffusion in the low-pressure diffusion furnace, that is, the phosphorus in the first phosphosilicate glass layers 13 and 23 can diffuse into the first polysilicon layers 12 and 22 to form high and low potentials.

[0078] S113 , forming an opening on the first phosphosilicate glass layer on the second surface side to expose a portion of the first polysilicon layer on the second surface side.

[0079] Specifically, referring to FIG4 , the first phosphosilicate glass layer 23 on the second surface 20 side of the P-type silicon-based substrate 4 includes an opening 30, which can expose the first polysilicon layer 22 on the second surface 20 side. The opening 30 can be obtained by physical grinding, ion beam etching, or laser etching, etc., which is not specifically limited in the embodiments of the present application.

[0080] In an optional embodiment, forming an opening in the first phosphosilicate glass layer on the second surface side to expose a portion of the first polysilicon layer on the second surface side may include: using a laser to form the opening in the first phosphosilicate glass layer on the second surface side of the P-type silicon-based substrate. Laser processing is non-contact and has minimal impact on the material, allowing for precise control of the size of the opening, thereby improving processing efficiency and quality.

[0081] S114 , after forming an opening on the first phosphosilicate glass layer on the second surface side, remove the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate to expose the first polysilicon layer on the first surface side.

[0082] Specifically, referring to Figure 4, after an opening is formed on the first phosphosilicate glass layer 23 on the second surface 20 side, since the materials of the first phosphosilicate glass layer 13 and the first polysilicon layer 12 are different, the removal method or process is also different. Therefore, before removing the first polysilicon layer 12, the first phosphosilicate glass layer 13 needs to be removed first. The removal method can be laser etching or other methods. The embodiment of the present application does not make specific restrictions on this. For example, the process wafer can be placed in a chain etching machine, and the first phosphosilicate glass layer 13 on the first surface 10 side is etched with a hydrogen fluoride solution. The etching time is related to the concentration of the hydrogen fluoride solution and the thickness of the first phosphosilicate glass layer. It is not specifically limited here. The concentration of the hydrogen fluoride solution can be 75%-85%, and the etching time can be 30s-60s.

[0083] S115. Etch the first surface and the second surface side of the P-type silicon-based substrate to remove the first polysilicon layer and the first tunneling layer located in the opening to form a trench at the opening, and remove the first tunneling layer and the first polysilicon layer located on the first surface side.

[0084] Specifically, referring to FIG4 , after removing the first phosphosilicate glass layer 13 on the first surface 10 side of the P-type silicon-based substrate 4, the first polysilicon layer 22 and the first tunneling layer 21 located in the opening 30 can be removed by liquid chemical reagents or plasma etching to form a groove 31 at the opening 30, and the first tunneling layer 11 and the first polysilicon layer 12 located on the first surface 10 side are removed. In this way, a pyramid-shaped velvet surface can be formed on the first surface 10 side of the P-type silicon-based substrate to increase the utilization rate of light and improve the photoelectric conversion efficiency of the P-type back-contact cell. At the same time, a pyramid-shaped velvet surface is also formed in the groove 31 formed at the opening on the second surface 20 side of the P-type silicon-based substrate.

[0085] Optionally, etching the first and second surfaces of the P-type silicon-based substrate may include: etching the openings on the first and second surfaces of the P-type silicon-based substrate with an alkaline etching solution to remove the first polysilicon layer and the first tunneling layer within the openings to form trenches at the openings, and removing the first tunneling layer and the first polysilicon layer on the first surface. The alkaline etching solution may be a sodium hydroxide solution, for example.

[0086] Specifically, referring to Figure 4, an alkaline etching solution is used to etch the first polysilicon layer 12 and the first tunnel layer 11 on the first surface 10 side, as well as the first polysilicon layer 22 and the first tunnel layer 21 located in the opening 30 on the second surface 20 side. The etching time is related to the concentration of the alkaline etching solution, the thickness of the first polysilicon layer and the first tunnel layer, and the temperature during etching, which is not specifically limited here. When the alkaline etching solution is a sodium hydroxide solution, the concentration of sodium hydroxide can be 1.3%-5%, the temperature during etching can be 74°-82°, and the etching time can be 350s-600s.

[0087] It can be understood that the above-mentioned method for preparing the P-type back-contact battery process wafer is only an exemplary method of the present application, and the method for preparing the P-type back-contact battery process wafer in the embodiment of the present application is not limited to this. For example, after forming the first tunneling layer, the first polysilicon layer and the first phosphosilicate glass layer, the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate can be removed first, and then an opening can be formed on the first phosphosilicate glass layer on the second surface side.

[0088] Optionally, FIG5 is a flow chart of a method for preparing another process sheet of a P-type back contact battery provided in an embodiment of the present application, and FIG6 is a schematic diagram of a process structure of another process sheet for preparing a P-type back contact battery provided in an embodiment of the present application. As shown in FIG5 , the process sheet for preparing a P-type back contact battery may further include:

[0089] S111 ′, providing a P-type silicon-based substrate.

[0090] S112 ′, forming a first tunneling layer, a first polysilicon layer, and a first phosphosilicate glass layer stacked in sequence on the first surface and the second surface side of the P-type silicon-based substrate respectively.

[0091] S113 ′, removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate to expose the first polysilicon layer on the first surface side.

[0092] Specifically, referring to Figure 6, since the materials of the first phosphosilicate glass layer 13 and the first polysilicon layer 12 are different, the removal method or process is also different. Therefore, before removing the first polysilicon layer 12, the first phosphosilicate glass layer 13 needs to be removed first. The removal method can be laser etching or other methods. The embodiment of the present application does not make specific limitations on this. For example, the process wafer can be placed in a chain etching machine, and the first phosphosilicate glass layer 13 on the first surface 10 side can be etched with a hydrogen fluoride solution. The concentration of the hydrogen fluoride solution can be 75%-85%, and the etching time can be 30s-60s.

[0093] S114′, after removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate, forming an opening on the first phosphosilicate glass layer on the second surface side to expose a portion of the first polysilicon layer on the second surface side.

[0094] Specifically, referring to FIG. 6 , the opening 30 may be obtained by physical grinding, ion beam etching, laser etching, or the like, which is not specifically limited in the embodiment of the present application.

[0095] Optionally, an opening is formed in the first phosphosilicate glass layer on the second surface side to expose a portion of the first polysilicon layer on the second surface side. Specifically, a laser can be used to form the opening in the first phosphosilicate glass layer on the second side of the P-type silicon-based substrate. Due to the non-contact nature of laser processing, it has minimal impact on the material, and the size of the opening can be precisely controlled, thereby improving processing efficiency and quality.

[0096] S115', etching the first surface and the second surface side of the P-type silicon-based substrate to remove the first polysilicon layer and the first tunneling layer located in the opening to form a trench at the opening, and remove the first tunneling layer and the first polysilicon layer located on the first surface side.

[0097] The technical solution provided in the embodiment of the present application forms a first tunneling layer, a first polysilicon layer and a first phosphosilicate glass layer stacked in sequence on the first surface and the second surface side of the P-type silicon-based substrate respectively. The first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate can be removed first, and then an opening can be formed on the first phosphosilicate glass layer on the second surface side; or an opening can be formed on the first phosphosilicate glass layer on the second surface side, and then the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate can be removed; then the first surface and the second surface side of the P-type silicon-based substrate are etched to remove the first polysilicon layer and the first tunneling layer located in the opening to form a groove at the opening, and the first tunneling layer and the first polysilicon layer located on the first surface side are removed to form a pyramid-shaped velvet surface on the first surface side to increase the utilization rate of light and improve the photoelectric conversion efficiency of the P-type back-contact battery.

[0098] In an optional embodiment, FIG7 is a flow chart of another method for preparing a P-type back contact cell provided in an embodiment of the present application, and FIG8 is a schematic diagram of the process structure of another method for preparing a P-type back contact cell provided in an embodiment of the present application. As shown in FIG7 , etching is performed on the process wafer after the gettering structure is formed to remove the gettering structure and the first phosphosilicate glass layer on the second surface side, specifically including:

[0099] S131 , etching the second phosphosilicate glass layer on the second surface side to remove the second phosphosilicate glass layer on the second surface side.

[0100] Specifically, referring to FIG8 , due to the material difference between the second phosphosilicate glass layers 113 and 223 and the second polysilicon layers 112 and 222, the second phosphosilicate glass layers 113 and 223 and the second polysilicon layers 112 and 222 cannot be removed simultaneously. An acidic etching solution may be first used to etch the wafer to remove the second phosphosilicate glass layer 223 on the second surface side. The acidic etching solution may include a hydrogen fluoride solution having a concentration range of 75% to 85%, and the reaction time may be 30 seconds to 60 seconds.

[0101] S132 , etching the second phosphosilicate glass layer and the second polysilicon layer on the first surface side, and the second polysilicon layer and the second tunneling layer on the second surface side to form a groove with a polished surface on the second surface side.

[0102] Specifically, referring to FIG8 , after the second phosphosilicate glass layer 223 on the second surface side is removed, an alkaline etching solution can be used to etch the process wafer to remove the second phosphosilicate glass layer 113 and the second polysilicon layer 112 on the first surface side, as well as the second polysilicon layer 222 and the second tunneling layer 221 on the second surface side, and form a polished surface at the groove on the second surface side, wherein the alkaline etching solution can include a sodium hydroxide solution, the concentration of sodium hydroxide can be in the range of 1.5%-5%, the reaction time can be 200s-300s, and the reaction temperature can be 65°-75°. The polished surface can fully reflect light of different wavelengths, so that at least part of the light reaching the second surface side is reflected back into the P-type silicon substrate through the smooth polished surface, thereby achieving light reuse, improving light energy utilization, and further improving the photoelectric conversion efficiency of the back contact.

[0103] S133 , etching the first phosphosilicate glass layer and the second tunneling layer on the first surface side to remove the first phosphosilicate glass layer and the second tunneling layer on the first surface side.

[0104] Specifically, referring to Figure 8, the second tunneling layer 111 and the first phosphosilicate glass layer 23 of the etching process sheet can be etched using an acidic etching solution, wherein the acidic etching solution can include hydrogen fluoride and hydrogen chloride solutions, the concentration range of hydrogen fluoride can be 8%-15%, the concentration range of hydrogen chloride can be 4.5%-10%, and the reaction time can be 150s-300s.

[0105] In an optional embodiment, FIG9 is a flow chart of a method for preparing another P-type back contact cell provided in an embodiment of the present application, and FIG10 is a schematic structural diagram of a process for preparing another P-type back contact cell provided in an embodiment of the present application. As shown in FIG9 , forming a passivation layer on the first surface side and the second surface side of the process wafer respectively specifically includes:

[0106] S141 , preparing an aluminum oxide layer on the first surface side and the second surface side of the process sheet.

[0107] Specifically, referring to FIG10 , an atomic layer deposition apparatus can be used to form a complete layer of aluminum oxide 15 and 25 on the first surface 10 and the second surface 20 of the process wafer. Alternatively, other preparation methods can be used to form the aluminum oxide layers 15 and 25 , which are not specifically limited herein. The thickness of the aluminum oxide layer can be set as needed. For example, the thickness of the aluminum oxide layer can be 2 nm to 10 nm.

[0108] S142 , forming a silicon nitride layer on the side of the aluminum oxide layer on the first surface side and the second surface side facing away from the P-type silicon-based substrate.

[0109] Specifically, referring to FIG10 , after forming an aluminum oxide layer 15 on the first surface 10 and the second surface 20 of the process wafer, a complete layer of silicon nitride can be formed on the sides of the aluminum oxide layers on the first and second surfaces facing away from the P-type silicon substrate using plasma-enhanced chemical vapor deposition. Aluminum oxide layers 15 and 25 can also be formed using other preparation methods, which are not specifically limited herein. The thickness of the silicon nitride layer can be set as needed. For example, the thickness of the silicon nitride layer can be 60 nm to 180 nm.

[0110] Based on the same application concept, an embodiment of the present application provides a P-type back-contact battery. The P-type back-contact battery is manufactured using the manufacturing method of the back-contact battery of any embodiment of the present application, and has the same beneficial effects as the above method. Please refer to the above description and will not repeat it here.

[0111] It can be understood that the back-contact battery provided in the embodiments of the present application can be prepared using the manufacturing method of the back-contact battery provided in any embodiment of the present application. In actual production and application, specific preparation parameters can be adaptively selected according to the parameters mentioned in the embodiments of the present application. The following is a comparative description of the performance of P-type back-contact batteries prepared with different parameters.

[0112] In a first embodiment, a P-type silicon-based substrate is provided, and a first tunneling layer and a first polysilicon layer are formed on the first surface and the second surface side of the P-type silicon-based substrate respectively by low-pressure chemical vapor deposition. The thickness of the first tunneling layer on the first surface side and the second surface side is the same, both being 1.8 nm. The thickness of the first polysilicon layer on the first surface side and the second surface side is the same, both being 180 nm. After the first tunneling layer and the first polysilicon layer are formed on the first surface and the second surface side respectively, the process wafer is placed in a low-pressure diffusion furnace to form a first phosphosilicate glass layer. The phosphorus source deposition concentration in the first phosphosilicate glass layer on the first surface side and the second surface side is the same, both being 4e22 / cm 3. Place the P-type silicon-based substrate into a chain etching machine, and use 85% hydrofluoric acid to etch the first phosphosilicate glass layer on the first surface side. The etching time is 60s to remove the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate; after removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate, use a laser etching method to form an opening on the first phosphosilicate glass layer on the second surface side. The rated power of the laser is 40W, the frequency is 400KHz, and the width of the opening is 250μm; after forming the opening on the first phosphosilicate glass layer on the second surface side, place the P-type silicon-based substrate into a texturing machine, and use 5% sodium hydroxide solution to etch the first polysilicon layer and the first tunneling layer at the opening. The etching time is 600s and the etching temperature is 82° to remove the opening. The first polysilicon layer and the first tunneling layer at the opening are removed to form a pyramid-like groove; after the groove is formed, a second tunneling layer and a second polysilicon layer are formed on the first surface and the second surface side of the P-type silicon-based substrate respectively by low-pressure chemical vapor deposition; the second tunneling layer on the first surface side and the second surface side has the same thickness, both of which are 1.5nm; the second polysilicon layer on the first surface side and the second surface side has the same thickness, both of which are 120nm; after the second tunneling layer and the second polysilicon layer are formed on the first surface and the second surface side of the P-type silicon-based substrate respectively, the process wafer is placed in a low-pressure diffusion furnace to form a second phosphosilicate glass layer; the phosphorus source deposition concentration in the second phosphosilicate glass layer on the first surface side and the second surface side is the same, both of which are 2e22 / cm 3 ; Place the process wafer after the doping structure is formed into a chain etching machine, and use hydrofluoric acid with a concentration of 85% to etch the second phosphosilicate glass layer on the second surface side for 60 seconds to remove the second phosphosilicate glass layer on the second surface side; Place the process wafer with the second phosphosilicate glass layer removed into a polishing machine, and use sodium hydroxide solution with a concentration of 5% to etch the second phosphosilicate glass layer and the second polysilicon layer on the first surface side, as well as the second polysilicon layer and the second tunneling layer on the second surface side, with an etching temperature of 75° and an etching time of 300 seconds to form a polished surface at the groove on the second surface side, and the first surface side still has a pyramid velvet structure. Then, a mixed solution of a 10% hydrogen chloride solution and a 15% hydrogen fluoride solution was used to etch the first phosphosilicate glass layer on the second surface side and the second tunneling layer on the first surface side for 300s. Finally, a plasma-enhanced chemical vapor deposition method was used to form aluminum oxide and silicon nitride layers on the first surface side and the second surface side. The thickness of the aluminum oxide layer was 10nm, and the thickness of the silicon nitride layer was 180nm.

[0113] The P-type back contact battery of the first embodiment prepared by the above preparation method was tested, and the short-circuit current Isc of the P-type back contact battery was found to be 13.643A, the open-circuit voltage Uoc was 0.7049V, the fill factor FF was 81.34, and the photoelectric conversion efficiency was 23.70.

[0114] In a second embodiment, a P-type silicon-based substrate is provided, and a first tunneling layer and a first polysilicon layer are formed on the first surface and the second surface side of the P-type silicon-based substrate respectively by low-pressure chemical vapor deposition. The thickness of the first tunneling layer on the first surface side and the second surface side is the same, both of which are 1.1 nm. The thickness of the first polysilicon layer on the first surface side and the second surface side is the same, both of which are 70 nm. After the first tunneling layer and the first polysilicon layer are formed on the first surface and the second surface side of the P-type silicon-based substrate respectively, the process wafer is placed in a low-pressure diffusion furnace to form a first phosphosilicate glass layer. The phosphorus source deposition concentration in the first phosphosilicate glass layer on the first surface side and the second surface side is the same, both of which are 3e21 / cm 3 ; Place the P-type silicon-based substrate in a chain etching machine, and use hydrofluoric acid with a concentration of 75% to etch the first phosphosilicate glass layer on the first surface side. The etching time is 30s to remove the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate; After removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate, a laser etching method is used to form an opening on the first phosphosilicate glass layer on the second surface side. The rated power of the laser is 20W, the frequency is 350KHz, and the width of the opening is 150μm; After the opening is formed on the first phosphosilicate glass layer on the second surface side, place the P-type silicon-based substrate in a texturing machine, and use sodium hydroxide solution with a concentration of 1.3% to etch the first polysilicon layer at the opening. The etching time is 350s and the etching temperature is 74° to remove the first polysilicon at the opening. The first surface side is also a pyramid surface; after the grooves are formed, a second tunneling layer and a second polysilicon layer are formed on the first surface and the second surface side of the P-type silicon substrate respectively by low-pressure chemical vapor deposition; the second tunneling layer on the first surface side and the second surface side has the same thickness, both of which are 1.0 nm; the second polysilicon layer on the first surface side and the second surface side has the same thickness, both of which are 60 nm; after the second tunneling layer and the second polysilicon layer are formed on the first surface and the second surface side of the P-type silicon substrate respectively, the process wafer is placed in a low-pressure diffusion furnace to form a second phosphosilicate glass layer; the phosphorus source deposition concentration in the second phosphosilicate glass layer on the first surface side and the second surface side is the same, both of which are 1e20 / cm 3; Place the process wafer after the doping structure is formed into a chain etching machine, and use hydrofluoric acid with a concentration of 75% to etch the second phosphosilicate glass layer on the second surface side for 30 seconds to remove the second phosphosilicate glass layer on the second surface side; Place the process wafer with the second phosphosilicate glass layer removed into a polishing machine, and use sodium hydroxide solution with a concentration of 1.5% to etch the second phosphosilicate glass layer and the second polysilicon layer on the first surface side, as well as the second polysilicon layer and the second tunneling layer on the second surface side, with an etching temperature of 65° and an etching time of 200 seconds to form a polished surface at the groove on the second surface side, and the first surface side still has a velvet structure. Then, a mixed solution of a 4.5% hydrogen chloride solution and an 8% hydrogen fluoride solution was used to etch the first phosphosilicate glass layer on the second surface side and the second tunneling layer on the first surface side for 150 seconds. Finally, a plasma-enhanced chemical vapor deposition method was used to form aluminum oxide and silicon nitride layers on the first surface side and the second surface side. The thickness of the aluminum oxide layer was 2 nm, and the thickness of the silicon nitride layer was 60 nm.

[0115] The P-type back contact battery of the second embodiment prepared by the above preparation method was tested, and the short-circuit current Isc of the P-type back contact battery was found to be 13.642A, the open-circuit voltage Uoc was 0.7052V, the fill factor FF was 81.33, and the photoelectric conversion efficiency was 23.70.

[0116] In a third embodiment, a P-type silicon-based substrate is provided, and a first tunneling layer and a first polysilicon layer are formed on the first surface and the second surface side of the P-type silicon-based substrate respectively by low-pressure chemical vapor deposition. The thickness of the first tunneling layer on the first surface side and the second surface side is the same, both being 1.5 nm. The thickness of the first polysilicon layer on the first surface side and the second surface side is the same, both being 120 nm. After the first tunneling layer and the first polysilicon layer are formed on the first surface and the second surface side respectively, the process wafer is placed in a low-pressure diffusion furnace to form a first phosphosilicate glass layer. The phosphorus source deposition concentration in the first phosphosilicate glass layer on the first surface side and the second surface side is the same, both being 8e21 / cm 3. Place the P-type silicon-based substrate in a chain etching machine, and use hydrofluoric acid with a concentration of 80% to etch the first phosphosilicate glass layer on the first surface side. The etching time is 45s to remove the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate; after removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate, use a laser etching method to form an opening on the first phosphosilicate glass layer on the second surface side. The rated power of the laser is 30W, the frequency is 600KHz, and the width of the opening is 200μm; after forming the opening on the first phosphosilicate glass layer on the second surface side, place the P-type silicon-based substrate in a texturing machine, and use a sodium hydroxide solution with a concentration of 2.6% to etch the first polysilicon layer and the first tunneling layer at the opening. The etching time is 500s and the etching temperature is 78° to remove the first polysilicon layer at the opening. The crystalline silicon layer and the first tunneling layer are removed to form a pyramid-like groove, and the first surface side is also a pyramid-like groove. After the groove is formed, a second tunneling layer and a second polysilicon layer are formed on the first surface and the second surface side of the P-type silicon-based substrate respectively by low-pressure chemical vapor deposition. The second tunneling layer on the first surface side and the second surface side has the same thickness, both of which are 1.2 nm. The second polysilicon layer on the first surface side and the second surface side has the same thickness, both of which are 90 nm. After the second tunneling layer and the second polysilicon layer are formed on the first surface and the second surface side of the P-type silicon-based substrate respectively, the process wafer is placed in a low-pressure diffusion furnace to form a second phosphosilicate glass layer. The phosphorus source deposition concentration in the second phosphosilicate glass layer on the first surface side and the second surface side is the same, both of which are 1e21 / cm 3 ; Place the process wafer after the doping structure is formed into a chain etching machine, and use 80% hydrofluoric acid to etch the second phosphosilicate glass layer on the second surface side for 45 seconds to remove the second phosphosilicate glass layer on the second surface side; Place the process wafer after the second phosphosilicate glass layer is removed into a polishing machine, and use 2.5% sodium hydroxide solution to etch the second phosphosilicate glass layer and the second polysilicon layer on the first surface side, as well as the second polysilicon layer and the second tunneling layer on the second surface side, with an etching temperature of 70° and an etching time of 2. The first surface side is provided with a first surface polishing layer, the first surface side is provided with a first phosphosilicate glass layer, and the second tunneling layer on the first surface side is etched for 50s to form a polished surface at the groove on the second surface side, and the first surface side still has a pyramid velvet structure; then, a mixed solution of a 7% hydrogen chloride solution and a 12% hydrogen fluoride solution is used to etch the first phosphosilicate glass layer on the second surface side and the second tunneling layer on the first surface side, and the etching time is 200s; finally, a plasma enhanced chemical vapor deposition method is used to form aluminum oxide and silicon nitride layers on the first surface side and the second surface side, and the thickness of the aluminum oxide layer is 6nm, and the thickness of the silicon nitride layer is 120nm.

[0117] The P-type back contact battery of the third embodiment prepared by the above preparation method was tested, and the short-circuit current Isc of the P-type back contact battery was found to be 13.648A, the open-circuit voltage Uoc was 0.7054V, the fill factor FF was 81.43, and the photoelectric conversion efficiency was 23.75.

[0118] In a first comparative example, a P-type silicon-based substrate is provided, and a first tunneling layer and a first polysilicon layer are formed on the first surface and the second surface side of the P-type silicon-based substrate respectively by low-pressure chemical vapor deposition; the thickness of the first tunneling layer on the first surface side and the second surface side is the same, both being 1.8 nm; the thickness of the first polysilicon layer on the first surface side and the second surface side is the same, both being 180 nm; after the first tunneling layer and the first polysilicon layer are formed on the first surface and the second surface side respectively, the process wafer is placed in a low-pressure diffusion furnace to form a first phosphosilicate glass layer; the phosphorus source deposition concentration in the first phosphosilicate glass layer on the first surface side and the second surface side is the same, both being 4e22 / cm 3 . Place the P-type silicon-based substrate in a chain etching machine, and use hydrofluoric acid with a concentration of 85% to etch the first phosphosilicate glass layer on the first surface side. The etching time is 60s to remove the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate; after removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate, use a laser etching method to form an opening on the first phosphosilicate glass layer on the second surface side. The rated power of the laser is 40W, the frequency is 400KHz, and the width of the opening is 250μm; after forming the opening on the first phosphosilicate glass layer on the second surface side, place the P-type silicon-based substrate in a texturing machine, and use a hydrofluoric acid with a concentration of 5% to etch the first phosphosilicate glass layer on the first surface side. The first polysilicon layer and the first tunneling layer at the opening, as well as the first polysilicon layer and the first tunneling layer on the first surface side, are etched with a sodium hydroxide solution for 600 seconds and an etching temperature of 82° to form a pyramid velvet surface at the opening and on the first surface side; the first phosphosilicate glass layer on the second surface side is then etched with a mixed solution of a 10% hydrogen chloride solution and a 15% hydrogen fluoride solution for 300 seconds, and then aluminum oxide and silicon nitride layers are formed on the first surface side and the second surface side by plasma enhanced chemical vapor deposition, with the aluminum oxide layer having a thickness of 10 nm and the silicon nitride layer having a thickness of 180 nm.

[0119] The first comparative example P-type back contact battery prepared by the above preparation method was tested, and the short-circuit current Isc of the P-type back contact battery was 13.543A, the open-circuit voltage Uoc was 0.7051V, the fill factor FF was 81.30, and the photoelectric conversion efficiency was 23.52.

[0120] In a second comparative example, a P-type silicon-based substrate is provided, and a first tunneling layer and a first polysilicon layer are formed on the first surface and the second surface side of the P-type silicon-based substrate respectively by low-pressure chemical vapor deposition; the thickness of the first tunneling layer on the first surface side and the second surface side is the same, both of which are 1.1 nm; the thickness of the first polysilicon layer on the first surface side and the second surface side is the same, both of which are 70 nm; after the first tunneling layer and the first polysilicon layer are formed on the first surface and the second surface side of the P-type silicon-based substrate respectively, the process wafer is placed in a low-pressure diffusion furnace to form a first phosphosilicate glass layer; the phosphorus source deposition concentration in the first phosphosilicate glass layer on the first surface side and the second surface side is the same, both of which are 3e21 / cm 3 ; Place the P-type silicon-based substrate in a chain etching machine, and use hydrofluoric acid with a concentration of 75% to etch the first phosphosilicate glass layer on the first surface side. The etching time is 30s to remove the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate; After removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate, use a laser etching method to form an opening on the first phosphosilicate glass layer on the second surface side. The rated power of the laser is 20W, the frequency is 350KHz, and the width of the opening is 150μm; After forming the opening on the first phosphosilicate glass layer on the second surface side, place the P-type silicon-based substrate in a texturing machine, and use a hydrofluoric acid with a concentration of 1 .3% sodium hydroxide solution is used to etch the first polysilicon layer and the first tunneling layer at the opening, as well as the first polysilicon layer and the first tunneling layer on the first surface side, with an etching time of 350s and an etching temperature of 74°, to form a pyramid velvet surface at the opening and the first surface side; then a mixed solution of a 4.5% hydrogen chloride solution and an 8% hydrogen fluoride solution is used to etch the first phosphosilicate glass layer on the second surface side, with an etching time of 150s; then, a plasma-enhanced chemical vapor deposition method is used to form aluminum oxide and silicon nitride layers on the first surface side and the second surface side, with a thickness of the aluminum oxide layer being 2nm and a thickness of the silicon nitride layer being 60nm.

[0121] The P-type back contact battery of the second comparative example prepared by the above preparation method was tested, and the short-circuit current Isc of the P-type back contact battery was 13.544A, the open-circuit voltage Uoc was 0.7052V, the fill factor FF was 81.28, and the photoelectric conversion efficiency was 23.52.

[0122] Among them, the photoelectric conversion efficiency Eta is related to the open circuit voltage Uoc, the short circuit current Isc and the fill factor FF. By comparing the P-type back contact batteries of the above-mentioned first to third embodiments with the P-type back contact batteries of the first comparative example and the second comparative example, it can be determined that the photoelectric conversion efficiency Eta of the P-type back contact batteries prepared by the preparation method provided in the present application is improved, that is, the preparation method of the P-type back contact battery provided in the present application can effectively improve the photoelectric conversion efficiency of the P-type back contact battery.

[0123] Based on the same application concept, the embodiment of the present application also provides a photovoltaic component, including the P-type back-contact battery provided in the embodiment of the present application, which can achieve the beneficial effects of the P-type back-contact battery provided in the embodiment of the present application. The similarities can be referred to the above description and will not be repeated here.

[0124] Note that the above are only preferred embodiments of the present application and the technical principles employed. Those skilled in the art will understand that the present application is not limited to the specific embodiments described herein, and that various obvious changes, readjustments, combinations, and substitutions can be made by those skilled in the art without departing from the scope of protection of the present application. Therefore, although the present application has been described in more detail through the above embodiments, the present application is not limited to the above embodiments and may include more other equivalent embodiments without departing from the concept of the present application, and the scope of the present application is determined by the scope of the appended claims.

Claims

1. A method for preparing a P-type back contact battery, wherein include: Process sheet for preparing P-type back contact cells; The process wafer includes a P-type silicon-based substrate; The P-type silicon-based substrate comprises a first surface and a second surface opposite to each other; a first tunneling layer, a first polysilicon layer, a first phosphosilicate glass layer stacked in sequence, and a groove penetrating the first tunneling layer, the first polysilicon layer and the first phosphosilicate glass layer are disposed on the second surface side; forming a gettering structure on the first surface side and / or the second surface side; the gettering structure comprises a second tunneling layer, a second polysilicon layer, and a second phosphosilicate glass layer which are stacked; Etching the process wafer after forming the gettering structure to remove the gettering structure and the first phosphosilicate glass layer on the second surface side; Passivation layers are formed on the first surface side and the second surface side of the process sheet, respectively.

2. The method according to claim 1, in, The process of preparing a P-type back contact cell includes: Providing a P-type silicon-based substrate; Forming the first tunneling layer, the first polysilicon layer and the first phosphosilicate glass layer stacked in sequence on the first surface and the second surface side of the P-type silicon-based substrate respectively; forming an opening on the first phosphosilicate glass layer on the second surface side to expose a portion of the first polysilicon layer on the second surface side; After forming an opening on the first phosphosilicate glass layer on the second surface side, removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate to expose the first polysilicon layer on the first surface side; The first surface and the second surface side of the P-type silicon-based substrate are etched to remove the first polysilicon layer and the first tunneling layer located in the opening to form the groove at the opening, and to remove the first tunneling layer and the first polysilicon layer located on the first surface side.

3. The method according to claim 1, in, The process of preparing a P-type back contact cell includes: Providing a P-type silicon-based substrate; Forming a first tunneling layer, a first polysilicon layer and a first phosphosilicate glass layer stacked in sequence on the first surface and the second surface of the P-type silicon-based substrate respectively; Removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate to expose the first polysilicon layer on the first surface side; After removing the first phosphosilicate glass layer on the first surface side of the P-type silicon-based substrate, forming an opening on the first phosphosilicate glass layer on the second surface side to expose a portion of the first polysilicon layer on the second surface side; The first surface and the second surface side of the P-type silicon-based substrate are etched to remove the first polysilicon layer and the first tunneling layer located in the opening to form the groove at the opening, and to remove the first tunneling layer and the first polysilicon layer located on the first surface side.

4. The method according to claim 2 or 3, in, Etching the first surface and the second surface side of the P-type silicon-based substrate comprises: An alkaline etching solution is used to sequentially etch the openings on the first surface side and the second surface side of the P-type silicon-based substrate to remove the first polysilicon layer and the first tunneling layer located in the opening to form the groove at the opening, and to remove the first tunneling layer and the first polysilicon layer located on the first surface side.

5. The method according to claim 2 or 3, in, An opening is formed on the first phosphosilicate glass layer on the second surface side to expose a portion of the first polysilicon layer on the second surface side, comprising: The opening is formed on the first phosphosilicate glass layer on the second surface side of the P-type silicon base substrate using a laser.

6. The method according to claim 1, in, Forming a gettering structure on the first surface side and / or the second surface side includes: The first tunneling layer, the first polysilicon layer and the first phosphosilicate glass layer are sequentially prepared on the first surface side and the second surface side by using any one of high-temperature thermal oxidation, nitric acid oxidation, ozone oxidation and chemical vapor deposition methods.

7. The method according to claim 1, in, Etching the process wafer after forming the gettering structure to remove the gettering structure and the first phosphosilicate glass layer on the second surface side, comprising: Etching the second phosphosilicate glass layer on the second surface side to remove the second phosphosilicate glass layer on the second surface side; Etching the second phosphosilicate glass layer and the second polysilicon layer on the first surface side, and the second polysilicon layer and the second tunneling layer on the second surface side to form a groove having a polished surface on the second surface side; The first phosphosilicate glass layer and the second tunneling layer on the first surface side are etched to remove the The first phosphosilicate glass layer and the second tunneling layer on the first surface side.

8. The method according to claim 1, in, Forming a passivation layer on the first surface side and the second surface side of the process sheet respectively comprises: forming an aluminum oxide layer on a first surface side and a second surface side of the process sheet; A silicon nitride layer is formed on the side of the aluminum oxide layer on the first surface side and the second surface side facing away from the P-type silicon-based substrate.

9. A P-type back contact battery, in, The back contact battery is manufactured by the manufacturing method of any one of claims 1 to 8. 10 . A photovoltaic module comprising the P-type back contact cell according to claim 9 .

Citation Information

Patent Citations

  • N-type TOPCon solar cell and manufacturing method thereof

    CN113851555A

  • Full back contact solar cell and manufacturing method thereof

    CN115020508A

  • Solar battery cell and solar battery module

    JP2014170774A

Cited By

  • Back contact cell and photovoltaic system

    WO2026123888A1