Preparation method for phosphorus-doped silicon-based composite negative electrode material, and product and use thereof
By performing vapor deposition reaction of phosphine, carbon source gas and silicon source gas and carbon coating treatment at room temperature, a low energy consumption, high performance phosphorus-doped silicon-based composite anode material is prepared, which solves the cycle problem in the existing technology. The problems of poor stability and high temperature energy consumption have resulted in the excellent cycle performance and high first Coulombic efficiency of lithium-ion batteries.
Patent Information
- Application Number
- PCT/CN2023/111898
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2023-08-09
- Publication Date
- 2024-10-31
AI Technical Summary
In the existing technology, the volume change of silicon-based anode materials during the lithium insertion/extraction process leads to poor cycle stability, and the high-temperature energy-consuming gas-phase mixing reaction is not suitable for industrial production, and it is impossible to achieve high first Coulombic efficiency and excellent cycle performance at the same time.
By performing a vapor deposition reaction of phosphine, carbon source gas and silicon source gas at room temperature, a phosphorus-doped silicon-based composite negative electrode material is formed, and the uniformity and performance of the material are improved through carbon coating treatment.
The preparation of phosphorus-doped silicon-based composite anode materials with low energy consumption and high uniformity has been achieved. The cycle stability and first-time Coulombic efficiency of lithium-ion batteries have been significantly improved. The capacity retention rate after 100 cycles is as high as 80%, and the first-time Coulombic efficiency is no more than 80%. Below 90%.
Smart Images

Figure CN2023111898_31102024_PF_FP_ABST
Abstract
Description
Preparation method of phosphorus-doped silicon-based composite negative electrode material and its product and application Technical Field
[0001] The present invention relates to the technical field of lithium battery negative electrode materials, and in particular to a preparation method of a phosphorus-doped silicon-based composite negative electrode material, and its product and application. Background Art
[0002] Silicon is considered to be the most promising candidate to replace graphite. It is the second most abundant element in the earth's crust, is environmentally friendly, and has an ultra-high theoretical capacity (4200mAh / g). However, the drastic change in volume during the lithium insertion / extraction process has caused serious adverse consequences, resulting in very poor cycle stability. Although the volume expansion of silicon oxide materials during the lithium insertion process is greatly reduced compared to silicon alone, and it also has a high theoretical specific capacity (>2000mAh / g), the first coulombic efficiency of silicon oxide is too low (less than 76%), which limits its wider application; and compared to silicon oxide, silicon carbon products on the market have the characteristics of high first efficiency and high capacity, but their cycle performance is far inferior to silicon oxide; therefore, the preparation of a silicon-based negative electrode material with high capacity, high first efficiency and excellent cycle performance is currently an urgent issue to be solved.
[0003] A Chinese patent document with application publication number CN 107623118 A discloses a method for preparing a phosphorus-doped porous carbon negative electrode material with improved first coulombic efficiency. Using elemental red phosphorus as a phosphorus source, an organic carbon source is dispersed in water to form a slurry, which is then evenly mixed with red phosphorus. After drying, the slurry is placed in a sealed can filled with a protective atmosphere and calcined. It is then further calcined in an inert atmosphere tube furnace to prepare a phosphorus-doped porous carbon negative electrode material. This technical solution uses phosphorus as a doping element, claiming to increase the reversible specific capacity of the carbon material and significantly improve the first coulombic efficiency of the material. The preparation method disclosed in this technical solution is simple, but the liquid-solid phase mixing method cannot guarantee the uniformity of the doping, which affects the consistency of the preparation method. Moreover, the first coulombic efficiency of the material obtained by this method is only 71% at most, which is insufficient to meet market demand.
[0004] A Chinese patent application, publication number CN 113809311 A, discloses a phosphorus-doped soft carbon-coated silicon-based lithium-ion anode material, its preparation method, and application. Using a phosphorus-containing gas source or a high-boiling-point phosphorus-containing compound as the doping material, the doping material vapor is mixed with preheated silicon source vapor at 1200-1700°C for 1-24 hours to produce a phosphorus-doped silicon oxide material. The silicon source vapor is a mixture of silicon vapor and silicon dioxide vapor. The phosphorus-doped silicon oxide material is cooled to room temperature and crushed and sieved. The sieved material is analyzed and tested, and the material with doping uniformity that meets preset requirements is carbon-coated to produce a phosphorus-doped silicon-based lithium-ion anode material. This technical solution involves mixing a phosphorus-containing substance with silicon vapor and silicon oxide vapor in a gas phase reaction, ensuring full contact between the reactants to produce a uniformly doped lithium-ion battery anode material. The resulting material exhibits enhanced cycling stability and superior material consistency. However, the phosphorus-doped silicon anode material obtained by this method has a maximum initial efficiency of only 80.6%, which does not have a significant product advantage. More importantly, the energy consumption of this technical solution is very high. The temperature required to preheat silicon and silicon dioxide to form vapor must reach at least 1350°C, and the gas-phase mixing reaction is also carried out at a high temperature of 1200-1700°C. In addition, the subsequent carbon coating also needs to be carried out at a high temperature of 800-1000°C. Therefore, this technical solution is not suitable for large-scale industrial production.
[0005] Summary of the Invention
[0006] In response to the above-mentioned problems existing in the prior art, the present invention discloses a method for preparing a phosphorus-doped silicon-based composite negative electrode material, which has low production energy consumption and high product uniformity. More importantly, the lithium-ion battery assembled from the prepared negative electrode material has excellent cycle stability, high reversible specific capacity and first coulombic efficiency.
[0007] The specific technical solutions are as follows:
[0008] A method for preparing a phosphorus-doped silicon-based composite negative electrode material comprises the following steps:
[0009] (1) Under an inert atmosphere, a phosphorus source gas, a carbon source gas, and a silicon source gas are fully mixed at room temperature to obtain a mixed gas;
[0010] In the mixed gas, based on the total volume of 100%, the volume proportion of the phosphorus source gas is 0.1-3.0%, the volume proportion of the carbon source gas is 15-28%, and the balance is the silicon source gas;
[0011] (2) passing the mixed gas into a deposition furnace containing a substrate material to obtain an intermediate product after thermal deposition;
[0012] (3) The intermediate product is subjected to carbon coating treatment, and then subjected to post-processing to obtain the phosphorus-doped silicon-based composite negative electrode material.
[0013] The present invention discloses a method for preparing a phosphorus-doped silicon-based composite negative electrode material. The method comprises the following steps: using gaseous phosphine at room temperature as a silicon source, and additionally introducing a gaseous carbon source. The gaseous carbon source is mixed with the gaseous silicon source at room temperature to obtain a mixed gas. During a vapor deposition reaction, carbon and phosphorus are respectively bonded with the silicon source material, and then dehydrogenated by pyrolysis. Finally, the phosphorus-doped silicon-based composite negative electrode material is prepared by a carbon coating treatment.
[0014] Experiments have found that the doping of phosphorus atoms in this preparation method can significantly reduce the average particle size of silicon primary grains; and the introduction of gaseous carbon source can produce mutual synergy with the doped phosphorus atoms, which helps to decompose the phosphorus source gas and promote the doping of the phosphorus source. When the two are mixed with the silicon source gas at the same time, the phosphorus-doped silicon-based composite negative electrode material finally prepared through the above series of processes has excellent cycle stability, reversible specific capacity and first coulombic efficiency.
[0015] Experiments have shown that the aforementioned synergistic effect cannot be achieved by using only a combination of phosphorus source gas and silicon source gas, or only a combination of carbon source gas and silicon source gas.
[0016] Further experiments found that even if a combination of phosphorus source gas, carbon source gas and silicon source gas is used, if the volume ratio of the three is not within the above-mentioned range, it is impossible to prepare a lithium-ion battery with excellent cycle stability, high reversible specific capacity and first coulombic efficiency.
[0017] In step (1):
[0018] The phosphorus source gas is selected from phosphine;
[0019] The carbon source gas is selected from alkane gases that can be cracked at 400-800° C., preferably ethylene, propylene, acetylene, etc.
[0020] The silicon source gas is selected from one or more of silane, dichlorosilane, trichlorosilane, and silicon tetrachloride.
[0021] In step (2):
[0022] The total flow rate of the mixed gas is 0.1 to 50 L / min, preferably 20 to 50 L / min, and more preferably 25 to 30 L / min.
[0023] The base material is selected from one or more of hard carbon, conductive carbon black, carbon nanotubes, and graphene; the mass of the added base material accounts for 0.1 to 20.0 wt% of the total mass of the final product.
[0024] Preferably, the D50 of the base material is less than 200 nm.
[0025] The temperature of the thermal deposition is 400-800°C.
[0026] In step (3):
[0027] The intermediate product is pulverized, classified and demagnetized before being subjected to carbon coating treatment;
[0028] Preferably, the particle size concentration (SPAN value) of the intermediate product after pulverization, classification and demagnetization treatment is ≤1.5, and the average particle size is ≤10 μm; more preferably, the SPAN value is ≤1.2.
[0029] In step (3):
[0030] The carbon coating treatment is selected from one or more of gas phase carbon coating, liquid phase carbon coating, and solid phase carbon coating;
[0031] The carbon source used in the gas-phase carbon coating is hydrocarbon gas, such as ethylene, propylene, acetylene, etc. The specific carbon coating process adopts conventional technical means in this field.
[0032] The carbon source used in the liquid phase carbon coating is a carbon-containing high molecular polymer, such as liquid epoxy resin, petroleum residue, liquid asphalt, etc. The specific carbon coating process adopts conventional technical means in this field.
[0033] The carbon source used in the solid-phase carbon coating is asphalt, and the specific carbon coating process adopts conventional technical means in this field.
[0034] The temperature of the carbon coating treatment is selected from 600 to 1000° C. and is adaptively adjusted according to the type of carbon source used.
[0035] In step (3):
[0036] The post-processing includes breaking up and screening, and the specific operations are conventional technical means in this field. For example, the breaking up method adopts spiral breaking up.
[0037] Preferably, the mesh size used for the screening is 100 to 800 meshes.
[0038] Based on the above process and raw materials, preferred:
[0039] In step (1), in the mixed gas, the volume proportion of the phosphorus source gas is 0.5-3.0%, the volume proportion of the carbon source gas is 15-25%, and the balance is the silicon source gas;
[0040] Further preferred:
[0041] In the mixed gas, the volume proportion of the phosphorus source gas is 0.5-1.5%, the volume proportion of the carbon source gas is 15-25%, and the balance is the silicon source gas;
[0042] More preferably, in the mixed gas, the phosphorus source gas, the carbon source gas, and the silicon source gas are fully mixed at room temperature in a volume ratio of 1.5:25:73.5.
[0043] Most preferably, the silicon source is selected from trichlorosilane. Experiments have found that the lithium-ion battery assembled with the phosphorus-doped silicon-based composite negative electrode material finally prepared using trichlorosilane as the silicon source under the above-mentioned further preferred volume ratio has the best cycle stability, reversible specific capacity and first coulombic efficiency.
[0044] The present invention also discloses a phosphorus-doped silicon-based composite negative electrode material prepared according to the above method.
[0045] The present invention also discloses the application of the phosphorus-doped silicon-based composite negative electrode material prepared according to the above method in lithium-ion batteries. Experiments have found that the lithium-ion battery assembled using the negative electrode material has excellent cycle stability, high reversible specific capacity and first coulombic efficiency.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] The invention discloses a method for preparing a phosphorus-doped silicon-based composite negative electrode material. The method uses phosphorus source gas, carbon source gas and silicon source gas as raw materials. The preparation process is simple and controllable, with low energy consumption, and is suitable for industrial production.
[0048] The lithium-ion battery assembled with the phosphorus-doped silicon-based composite negative electrode material prepared by the present invention has excellent cycle stability. The capacity retention rate after 100 cycles is as high as over 80%, and can reach up to 88%; the capacity retention rate after 500 cycles is as high as over 70%, and can reach up to 75.5%; and it has both high reversible specific capacity (higher than 1800mAh / g) and first coulombic efficiency (not less than 90%). BRIEF DESCRIPTION OF THE DRAWINGS
[0049] FIG1 is a SEM image of the intermediate product prepared in Example 1;
[0050] Figures 2 to 4 are distribution diagrams of Si, C, and P elements within the image range of Figure 1, respectively;
[0051] FIG5 is a SEM image of the phosphorus-doped silicon-based composite negative electrode material prepared in Example 1;
[0052] FIG6 is a TEM image of the phosphorus-doped silicon-based composite negative electrode material prepared in Example 1. DETAILED DESCRIPTION
[0053] The specific implementation method of the present invention is further described below with reference to examples. It should be noted that the specific implementation method described here is only for the purpose of illustrating and explaining the present invention, and is not intended to limit the present invention.
[0054] Example 1
[0055] (1) Under an argon atmosphere, phosphine, ethylene, and monosilane were fully mixed at room temperature in a volume ratio of 1.5:25:73.5 to obtain a mixed gas.
[0056] (2) The mixed gas is introduced into a deposition furnace at a total gas volume of 25 L / min at a temperature of 500°C, where 100 g of hard carbon microspheres with a D50 of about 100 nm are placed. The gas is continuously ventilated until the surface of the hard carbon microsphere particles continuously nucleates and grows, and a phosphorus-doped silicon-carbon deposition layer is deposited. The ventilation time is maintained for 10 h.
[0057] (3) The deposition furnace is cooled, and the material is crushed and classified after being discharged from the furnace to obtain uniform particles with a D50 of less than 5 μm and a SPAN value of less than 1.2, and then subjected to magnetic treatment to obtain an intermediate product.
[0058] (4) Under an argon atmosphere, the intermediate product was placed in a chemical vapor deposition furnace, the temperature was raised to 800°C at a rate of 5°C / min, and acetylene gas was introduced at a flow rate of 1 L / min for gas phase cracking and carbon coating deposition. The amount of carbon coating was controlled to account for 4wt% of the total mass of the final product. After the deposition was completed, the temperature was cooled to room temperature, the material was taken out, and it was broken up and sieved to finally obtain a phosphorus-doped silicon-based composite negative electrode material.
[0059] Figure 1 is a mapping image of the intermediate product prepared in step (3) of this embodiment, as well as a distribution diagram of the Si element (Figure 2), the C element (Figure 3) and the P element (Figure 4) within the image range. By observing Figures 2 to 4, it can be found that the intermediate product prepared in this embodiment has been successfully doped with the two elements C and P, and the two elements are evenly dispersed in the intermediate product.
[0060] FIG5 is a SEM image of the final product prepared in this example. From the image, it can be found that the final product prepared in this example is in a regular spherical shape and has a relatively uniform particle size distribution.
[0061] FIG6 is a TEM image of the final product prepared in this example. From the image, it can be found that the surface of the negative electrode material prepared in this example is covered with a uniform carbon layer.
[0062] Example 2
[0063] The preparation process is basically the same as that in Example 1, except that in step (1), the volume ratio of phosphine, ethylene and monosilane is replaced with 3:15:82.
[0064] Example 3
[0065] The preparation process is basically the same as that in Example 1, except that in step (1), the volume ratio of phosphine, ethylene and monosilane is replaced with 0.5:25:74.5.
[0066] Comparative Example 1
[0067] The preparation process is basically the same as that in Example 1, except that in step (1), the volume ratio of phosphine, ethylene and monosilane is replaced with 5:25:70.
[0068] Comparative Example 2
[0069] The preparation process is basically the same as that in Example 1, except that in step (1), only ethylene and monosilane are added in a volume ratio of 25:75 to obtain a mixed gas.
[0070] Comparative Example 3
[0071] The preparation process is basically the same as that in Example 1, except that in step (1), the volume ratio of phosphine, ethylene and monosilane is replaced with 2:30:68.
[0072] Comparative Example 4
[0073] The preparation process is basically the same as that in Example 1, except that in step (1), the volume ratio of phosphine, ethylene and monosilane is replaced with 2:13:85.
[0074] Comparative Example 5
[0075] The preparation process is basically the same as that in Example 1, except that in step (1), only phosphine and monosilane are added in a volume ratio of 2:98 to obtain a mixed gas.
[0076] Example 4
[0077] (1) Under an argon atmosphere, phosphine, propylene, and dichlorosilane were fully mixed at a volume ratio of 1.5:25:73.5 at room temperature to obtain a mixed gas.
[0078] (2) The mixed gas is introduced into a deposition furnace at a total gas volume of 30 L / min at a temperature of 400°C, where 100 g of graphene microspheres with a D50 of about 100 nm are placed. The gas is continuously ventilated until the surface of the graphene microsphere particles continuously nucleates and grows, and a phosphorus-doped silicon-carbon deposition layer is deposited. The ventilation time is maintained for 13 h.
[0079] Steps (3) to (4) are exactly the same as those in Example 1.
[0080] Example 5
[0081] (1) Under an argon atmosphere, phosphine, acetylene, and trichlorosilane were fully mixed at room temperature in a volume ratio of 1.5:25:73.5 to obtain a mixed gas.
[0082] (2) The mixed gas is introduced into a deposition furnace at a total gas volume of 30 L / min at a flow rate of 800°C, where 100 g of conductive carbon black microspheres with a D50 of about 100 nm are placed. The gas is continuously ventilated until the surface of the conductive carbon black microsphere particles continuously nucleates and grows, and a phosphorus-doped silicon-carbon deposition layer is deposited. The ventilation time is maintained for 5 h.
[0083] Steps (3) to (4) are exactly the same as those in Example 1.
[0084] Application Examples
[0085] Batteries were assembled using the negative electrode materials prepared in each embodiment and each comparative example.
[0086] Under a nitrogen atmosphere, the conductive agent SuperP and sodium carboxymethyl cellulose (CMC) were thoroughly mixed and dispersed with deionized water. The negative electrode material was then added and stirred at 2000 rpm for 10 minutes. The aqueous binder AONE (purchased from Shenzhen Yanyi New Materials Co., Ltd.) was then added and stirred at 2000 rpm for 10 minutes to obtain a negative electrode slurry. The mass ratio of the negative electrode material, conductive agent SuperP, sodium carboxymethyl cellulose (CMC), and binder AONE (by dry weight) was 70:15:5:10, and the solid content of the slurry was 15 wt%.
[0087] The negative electrode slurry was coated on the current collector copper foil, dried at 80 ° C for 30 min under a relative vacuum of -0.1 MPa, and then roller pressed at room temperature. The surface density was 9.1 mg / cm 2 , then punched and cut into discs with a diameter of 14 mm to make electrode plates.
[0088] The counter electrode was a lithium sheet CR2016 (purchased from Shenzhen Yongxingye Equipment Technology Co., Ltd.) with a diameter of 16 mm.
[0089] The button cells were assembled in a glove box under an argon atmosphere, with moisture and oxygen levels below 0.01 ppm. The battery was assembled in the following order: negative electrode shell - gasket - lithium sheet - electrolyte - separator - electrolyte - electrode sheet - positive electrode shell. The electrolyte consisted of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) (EC:EMC:DEC volume ratio = 1:1:1), containing 1.0 M LiPF6.
[0090] The diameter of the electrode plate is 14mm, the diameter of the lithium plate is 16mm, the diameter of the diaphragm is 19mm, and the size of the battery shell (positive and negative shells) is 20mm. The diaphragm is a 12μm thick ceramic coated isolation membrane (purchased from Shanghai Enjie New Materials Technology Co., Ltd.). The assembled button battery is placed in the mold groove of a hydraulic sealing machine (purchased from Shenzhen Kejing Zhida Technology Co., Ltd.), locked, and pressurized >500kg / cm 2 , then unlock it and take out the sealed button battery.
[0091] When assembling the battery, five button batteries were prepared for each test, and a total of five sets of data were tested. The final performance was taken as the average value of the five sets of data.
[0092] Performance testing:
[0093] The XRD-D2PHASER of Bruker was used for phase analysis and the Scherrer formula was used for calculation to test the particle size of silicon primary grains.
[0094] The morphology test was performed using the Thermo Fisher Phenom Generation 5.
[0095] The carbon content was tested using a German EL ultra-high frequency infrared carbon-sulfur analyzer.
[0096] The phosphorus content was tested using a German Elimont organic element analyzer.
[0097] The battery cycle performance is tested on the Blue Power Battery Test System CT2001A equipment, specifically:
[0098] At 25°C, the charge and discharge cycle characteristics of the button cell were tested using the above-mentioned blue electric test cabinet. First, discharge at 0.1C to 0.005V, then discharge at 0.08C to 0.001V, discharge at 0.05C to 0.001V, and discharge at 0.02C to 0.001V, and let it stand for 10 minutes; then charge at 0.1C to 1.5V, let it stand for 10 minutes, record the charge and discharge capacity after the first cycle, and calculate the first coulombic efficiency; cycle 100 times in the above manner, record the charge and discharge capacity after 100 cycles, and calculate the capacity retention rate after 100 cycles. The test and calculation process of the capacity retention rate after 500 cycles adopt the same method. The test results are shown in Table 1 below.
[0099] Table 1 1. The mass content of phosphorus in the intermediate product prepared in each embodiment or each comparative example; 2. The mass content of carbon in the intermediate product prepared in each embodiment or each comparative example; 3. The average particle size of silicon primary crystals in the intermediate product prepared in each embodiment or each comparative example.
[0100] Comparing the changes in phosphorus content and carbon content in Table 1 shows that the method disclosed in the present invention can control the phosphorus content and carbon content of the product. Comparing the average particle size of the silicon primary grains in Example 1 with Comparative Examples 2 and 3 shows that the introduction of phosphorus can effectively reduce the average particle size of the silicon primary grains.
[0101] It is worth noting that, based on the above-mentioned design, in order to solve the same technical problem, even if some insubstantial changes or modifications are made to the present invention, the essence of the technical solution adopted is still the same as that of the present invention, and therefore it should also fall within the scope of protection of the present invention.
Claims
1. A method for preparing a phosphorus-doped silicon-based composite negative electrode material, characterized in that: The steps include: (1) Under an inert atmosphere, a phosphorus source gas, a carbon source gas, and a silicon source gas are fully mixed at room temperature to obtain a mixed gas; In the mixed gas, the total volume is 100%, the volume proportion of the phosphorus source gas is 0.1-3.0%, the volume proportion of the carbon source gas is 15-28%, and the balance is the silicon source gas; (2) passing the mixed gas into a deposition furnace containing a substrate material to obtain an intermediate product after thermal deposition; (3) The intermediate product is subjected to carbon coating treatment, and then subjected to post-treatment to obtain the phosphorus-doped silicon-based composite negative electrode material.
2. The method for preparing a phosphorus-doped silicon-based composite negative electrode material according to claim 1, characterized in that: In step (1): The phosphorus source gas is selected from phosphine; The carbon source gas is selected from alkane gases that can be cracked at 400-800°C; The silicon source gas is selected from one or more of silane, dichlorosilane, trichlorosilane, and silicon tetrachloride.
3. The method for preparing the phosphorus-doped silicon-based composite negative electrode material according to claim 1, characterized in that: In step (2): The total flow rate of the mixed gas is 0.1 to 50 L / min; The substrate material is selected from one or more of hard carbon, conductive carbon black, carbon nanotubes, and graphene; The temperature of the thermal deposition is 400-800°C.
4. The method for preparing a phosphorus-doped silicon-based composite negative electrode material according to claim 1, characterized in that: In step (3): The intermediate product is subjected to a carbon coating treatment after being crushed, classified and demagnetized; The particle size concentration of the intermediate product after crushing, classification and demagnetization treatment is ≤1.5 and the average particle size is ≤10μm.
5. The method for preparing the phosphorus-doped silicon-based composite negative electrode material according to claim 1, characterized in that: In step (3): The carbon coating treatment is selected from one or more of gas phase carbon coating, liquid phase carbon coating, and solid phase carbon coating; The temperature of the carbon coating treatment is selected from 600 to 1000°C.
6. The method for preparing a phosphorus-doped silicon-based composite negative electrode material according to claim 1, characterized in that: In step (3): The post-processing includes breaking up and screening.
7. The method for preparing a phosphorus-doped silicon-based composite negative electrode material according to any one of claims 1 to 6, characterized in that: In step (1), in the mixed gas, the volume proportion of the phosphorus source gas is 0.5-3.0%, the volume proportion of the carbon source gas is 15-25%, and the balance is the silicon source gas; In step (2), the total flow rate of the mixed gas is 20 to 50 L / min.
8. The method for preparing the phosphorus-doped silicon-based composite negative electrode material according to claim 7, characterized in that: In the mixed gas, the phosphorus source gas, the carbon source gas and the silicon source gas are fully mixed at a volume ratio of 1.5:25:73.5 at room temperature; The silicon source gas is selected from trichlorosilane.
9. A phosphorus-doped silicon-based composite negative electrode material prepared by the method according to any one of claims 1 to 8.
10. Use of the phosphorus-doped silicon-based composite negative electrode material according to claim 9 in a lithium-ion battery.
Citation Information
Patent Citations
Preparation method of phosphorus-doped porous carbon negative electrode material with improved first coulomb efficiency
CN107623118A
Phosphate-doping silicon carbon negative electrode material for lithium ion battery and preparation method of phosphate-doping silicon carbon negative electrode material
CN108172775A
Phosphorus-doped soft carbon-coated silicon-based lithium ion negative electrode material as well as preparation method and application thereof
CN113809311A
Silicon-phosphorus co-doped hard carbon composite material and preparation method and application thereof
CN114843480A
Preparation method of phosphorus-doped silicon-based composite negative electrode material as well as product and application of phosphorus-doped silicon-based composite negative electrode material
CN116544413A
Cited By
Biomass-based hard carbon negative electrode material, preparation method thereof and sodium ion battery
CN119591083A
Nano lithium phosphide modified silicon-carbon negative electrode material, preparation method thereof and secondary battery
CN122051202A
Phosphorus oxide coated silicon-containing material, preparation method thereof and application of phosphorus oxide coated silicon-containing material in sulfide solid-state battery negative electrode material
CN122348196A