Separator, battery cell, battery and electric device
By designing recessed areas and a porous base membrane structure on the isolation membrane, the problem of insufficient cycle performance of the battery cells is solved, better gas discharge and liquid retention capabilities are achieved, and the service life of the battery is extended.
Patent Information
- Application Number
- PCT/CN2023/133300
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2023-11-22
- Publication Date
- 2024-10-31
AI Technical Summary
The cycle performance of battery cells needs to be improved. The existing isolation membrane has insufficient liquid retention capacity, which leads to volume expansion of the electrode assembly and rapid consumption of electrolyte during charge and discharge, affecting the cycle life of the battery.
An isolation membrane is designed with a recessed area on the surface that runs through the membrane body along the thickness direction. The arrangement and shape of the recessed area are adjusted to quickly guide the gas outflow, improve the liquid retention capacity, and pass through the porous base membrane and appropriate pore structure. Improve mechanical strength and structural stability.
It effectively reduces the risk of volume expansion of electrode components, extends the cycle life of battery cells, improves the liquid retention capacity of the isolation membrane, and improves the cycle performance of the battery.
Smart Images

Figure CN2023133300_31102024_PF_FP_ABST
Abstract
Description
Separator, battery cell, battery and electrical device
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 202310449846.2, filed on April 24, 2023, entitled “Separation membrane, battery cell, battery and electrical device,” the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to the field of battery technology, and more specifically, to a separator, a battery cell, a battery, and an electrical device. Background Art
[0004] Battery cells are widely used due to their reliable performance, pollution-free operation, and zero memory effect. For example, with increasing attention paid to environmental protection and the growing popularity of new energy vehicles, the demand for power battery cells is expected to experience explosive growth.
[0005] As battery applications become increasingly widespread, the requirements for battery performance are becoming increasingly stringent. However, the cycle performance of battery cells still needs to be improved.
[0006] Summary of the Invention
[0007] The present application provides a separator, a battery cell, a battery and an electrical device, which can improve the cycle performance of the battery cell.
[0008] In a first aspect, an embodiment of the present application provides an isolation membrane, which includes two surfaces opposite to each other along its own thickness direction, at least one of the two surfaces includes at least one recessed area, and the recessed area penetrates the isolation membrane along a first direction, wherein the first direction is perpendicular to the thickness direction of the isolation membrane.
[0009] Therefore, in the embodiment of the present application, the recessed area penetrates the isolation membrane, which can guide the gas flow and discharge the isolation membrane, so that a large amount of gas will not remain in the isolation membrane, reducing the risk of volume expansion of the electrode assembly, thereby improving the liquid retention capacity of the isolation membrane and enhancing the cycle performance of the battery cell.
[0010] In some embodiments, the angle between the first direction and the length direction of the separator is between -30° and 30°. The embodiments of the present application adjust the arrangement of the recessed areas so that the recessed areas extend parallel or approximately parallel to the height direction of the battery cell (e.g., the length direction of the separator), thereby quickly guiding the gas out of the electrode assembly.
[0011] In some embodiments, the angle between the first direction and the width direction of the separator is between -30° and 30°. The embodiments of the present application adjust the arrangement of the recessed areas so that the recessed areas extend parallel or approximately parallel to the height direction of the battery cell (e.g., the width direction of the separator), thereby quickly guiding the gas out of the electrode assembly.
[0012] In some embodiments, multiple recessed areas are provided, and the multiple recessed areas are spaced apart. The multiple recessed areas can be spaced apart, which can increase the mechanical strength of the isolation membrane and improve the structural stability of the isolation membrane while increasing the overall volume occupied by the multiple recessed areas.
[0013] In some embodiments, two adjacent recessed areas are disposed continuously along the thickness direction of the isolation membrane. This arrangement of two adjacent recessed areas is beneficial for increasing the overall occupied volume of the multiple recessed areas, improving the gas conduction capacity of the recessed areas, and improving the liquid retention capacity of the isolation membrane.
[0014] In some embodiments, the cross-sectional shape of the recessed area parallel to the second direction is polygonal or arc-shaped, and the second direction, the first direction, and the thickness direction of the isolation film are perpendicular to each other.
[0015] In some embodiments, the polygon is a triangle, a trapezoid, a regular quadrilateral, a pentagon, or a hexagon.
[0016] In some embodiments, the volume percentage of the recessed area relative to the total volume of the isolation film is 2% to 10%.
[0017] In some embodiments, the isolation film satisfies at least one of the following conditions:
[0018] (1) The porosity of the isolation membrane is 40% to 70%;
[0019] (2) The separator includes a pore structure, and the average pore size of the pore structure is 0.03 μm to 1.5 μm;
[0020] (3) The thickness of the isolation film is 7 μm to 150 μm.
[0021] Therefore, the separator according to the embodiment of the present application has a porous structure, which is conducive to liquid absorption and retention inside the separator, thereby improving the cycle performance of the battery cell.
[0022] In some embodiments, the isolation membrane includes a porous base membrane, and the main material of the porous base membrane includes one or more of polyolefin, polyethylene terephthalate PET, polyimide PI, polyetheretherketone PEEK, meta-aramid, polybenzimidazole, polyphenylene sulfide, polybenzimidazole and glass fiber;
[0023] In some embodiments, the polyolefin includes one or more of polyethylene (PE), polypropylene (PP), and polyvinylidene fluoride (PVDF).
[0024] In a second aspect, an embodiment of the present application provides a battery cell, wherein the battery cell includes the isolation membrane of any embodiment of the first aspect of the present application.
[0025] In some embodiments, the battery cell includes a positive electrode sheet, the positive electrode sheet includes a positive electrode active material layer containing a positive electrode active material, and the positive electrode active material includes: Na x M y P m O n , wherein M represents a transition metal element, the transition metal element includes at least one of Mn, Fe, Co, Cu, Al, Ti, and V, 1≤x≤2, 0≤y≤1, 0≤m≤2, 4≤n≤8, and 0<x / m≤1; optionally, 0<y≤1; and / or 0<m≤2.
[0026] In a third aspect, an embodiment of the present application provides a battery, which includes a battery cell according to any embodiment of the second aspect of the present application.
[0027] In a fourth aspect, an embodiment of the present application provides an electrical device, which includes a battery according to any embodiment of the third aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.
[0029] FIG1 is a schematic diagram of an isolation film according to an embodiment of the present application.
[0030] FIG. 2 is a schematic diagram of the isolation film shown in FIG. 1 at another angle.
[0031] FIG3 is a schematic diagram of another embodiment of the isolation film of the present application.
[0032] FIG. 4 is a schematic diagram of a battery cell according to an embodiment of the present application.
[0033] FIG. 5 is an exploded schematic diagram of an embodiment of the battery cell of FIG. 4 .
[0034] FIG6 is a schematic diagram of an embodiment of a battery module of the present application.
[0035] FIG7 is a schematic diagram of an embodiment of a battery pack of the present application.
[0036] FIG8 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG7 .
[0037] FIG9 is a schematic diagram of an embodiment of an electric device including the battery cell of the present application as a power source.
[0038] FIG10 is a schematic diagram of the isolation film of Comparative Example 2. FIG.
[0039] The drawings are not necessarily drawn to scale.
[0040] The following are the descriptions of the reference numerals:
[0041] X, thickness direction; Y, first direction; Z, second direction;
[0042] 1. Battery pack; 2. Upper box; 3. Lower box; 4. Battery module;
[0043] 5. Battery cell; 51. Housing; 52. Electrode assembly;
[0044] 53. Cover plate;
[0045] 6. Electrical devices;
[0046] 7. Isolation film; 71. Recessed area; DETAILED DESCRIPTION
[0047] Below, the embodiments of the separator, battery cell, battery, and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially identical structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided to enable those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0048] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0049] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0050] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0051] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0052] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0053] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0054] A battery cell includes an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator. The separator is located between the positive electrode sheet and the negative electrode sheet to isolate the positive electrode sheet and the negative electrode sheet. Active ions migrate between the positive electrode sheet and the negative electrode sheet through the electrolyte, thereby realizing the charging and discharging of the battery cell.
[0055] During the charge and discharge process of the battery cell, the volume of the electrode assembly may change (such as volume expansion), and since a large number of chemical reactions may produce gas during the charge and discharge process, the liquid retention capacity of the isolation membrane is poor. During the battery cycle charge and discharge process, the electrolyte is continuously consumed and consumed rapidly, which will deteriorate the cycle performance of the battery cell.
[0056] In view of this, the present application improves the isolation membrane by setting a recessed area structure on the surface of the isolation membrane so that the gas can be discharged from the electrode assembly along the recessed area and then discharged from the battery cell, thereby improving the liquid retention capacity of the isolation membrane, reducing capacity loss, and extending the cycle life of the battery cell.
[0057] Isolation film
[0058] In a first aspect, an embodiment of the present application provides an isolation membrane.
[0059] As shown in Figures 1 and 2, the isolation membrane 7 includes two surfaces opposite to each other along its own thickness direction X, at least one of the two surfaces includes at least one recessed area 71, and the recessed area 71 penetrates the isolation membrane 7 along a first direction Y, wherein the first direction Y is perpendicular to the thickness direction X of the isolation membrane 7.
[0060] In the embodiment of the present application, the first direction Y can be understood as the extension direction of the recessed area 71. The recessed area 71 extends along the first direction Y, and its two ends extend to the edges of the isolation membrane 7 respectively, so that the recessed area 71 passes through the isolation membrane 7, which is conducive to the recessed area 71 to guide the gas. The recessed area 71 can extend along a straight line or along a curve, which means that the first direction Y can be a direction parallel to the straight line or a direction parallel to the curve (non-straight line). The first direction Y can be parallel to the length direction of the isolation membrane 7, or parallel to the width direction of the isolation membrane 7, or between the length direction and the width direction of the isolation membrane 7. It should be noted that when the recessed area 71 is set to multiple, each recessed area 71 can extend in different directions. In this case, the first direction Y can include multiple directions. Figures 1 and 2 show that the first direction Y is a single direction and is parallel to the width direction of the isolation membrane 7.
[0061] The separator 7 includes two surfaces, one of which is positioned near the positive electrode tab of the battery cell, and the other is positioned near the negative electrode tab of the battery cell. One of the two surfaces may include a recessed region 71, or both surfaces may include a recessed region 71. For example, the surface near the negative electrode tab includes a recessed region 71, which facilitates the discharge of gas near the negative electrode tab. The surface near the positive electrode tab includes a recessed region 71, which facilitates the discharge of gas near the positive electrode tab.
[0062] The recessed area 71 refers to a cavity formed by a portion of the surface of the isolation membrane 7 being recessed toward the interior of the isolation membrane 7. Since the cavity penetrates the isolation membrane 7, it can guide the gas flow and discharge the isolation membrane 7, so that a large amount of gas will not remain in the isolation membrane 7, reducing the risk of volume expansion of the electrode assembly, thereby improving the liquid retention capacity of the isolation membrane 7 and enhancing the cycle performance of the battery cell.
[0063] To further increase the rate of gas discharge, the embodiments of the present application adjust the arrangement of the recessed regions 71, for example, by extending the recessed regions 71 parallel or approximately parallel to the height direction of the battery cell, thereby quickly guiding the gas out of the electrode assembly. The electrode assembly can be prepared through a winding process or a lamination process. The height direction of the battery cell can be parallel to the length direction of the separator 7, or parallel to the width direction of the separator 7. In other words, the extension direction of the recessed regions 71 can be parallel or approximately parallel to the length direction of the separator 7, or parallel or approximately parallel to the width direction of the separator 7.
[0064] In some embodiments, the angle between the first direction Y and the length direction of the isolation membrane 7 is -30° to 30°. For example, the angle between the first direction Y and the length direction of the isolation membrane 7 can be -30°, -25°, -20°, -15°, -10°, -5°, -2°, -1°, 0°, 1°, 2°, 5°, 10°, 15°, 20°, 25°, 30°, or a range consisting of any two of the above values. Optionally, it can be -20° to 20°, -15° to 15°, -10° to 10°, or -5° to 5°. In the embodiment of the present application, when the angle between the first direction Y and the length direction of the isolation membrane 7 is 0°, it means that the first direction Y is parallel to the length direction of the isolation membrane 7.
[0065] As shown in Figures 2 and 3, in some embodiments, the angle between the first direction Y and the width direction of the isolation membrane 7 is -30° to 30°. For example, the angle between the first direction Y and the width direction of the isolation membrane 7 can be -30°, -25°, -20°, -15°, -10°, -5°, -2°, -1°, 0°, 1°, 2°, 5°, 10°, 15°, 20°, 25°, 30°, or a range consisting of any two of the above values. It can be selected from -20° to 20°, -15° to 15°, -10° to 10°, or -5° to 5°. In the embodiment of the present application, when the angle between the first direction Y and the width direction of the isolation membrane 7 is 0°, it means that the first direction Y is parallel to the width direction of the isolation membrane 7. Figure 3 shows an example in which the first direction Y has a certain angle with the width direction of the isolation membrane 7, for example, an angle of 5°.
[0066] The number of the recessed areas 71 may be one or more, and the extending direction of the recessed areas 71 may be set according to the number of the recessed areas 71 .
[0067] When there is only one recessed region 71 , the extending direction of the recessed region 71 , ie, the first direction Y, is unique. For example, the recessed region 71 extends along the length direction of the isolation film 7 .
[0068] In the case of multiple recessed regions 71, the extending direction of the recessed regions 71, i.e., the first direction Y, can be unique. For example, the recessed regions 71 extend along the length of the isolation membrane 7, with the multiple recessed regions 71 arranged in parallel. The first direction Y can also include multiple directions. For example, the extending direction of one recessed region 71 is parallel to the length of the isolation membrane 7, while the extending direction of another recessed region 71 forms an angle of 5° with the length of the isolation membrane 7. In this arrangement, the two recessed regions 71 may appear to intersect.
[0069] In some embodiments, a plurality of recessed regions 71 may be provided, and the plurality of recessed regions 71 may be spaced apart. This can, on the one hand, increase the mechanical strength of the separator 7 and improve the structural stability of the separator 7 while increasing the overall volume occupied by the plurality of recessed regions 71. For example, the plurality of recessed regions 71 are spaced apart along the second direction Z, and the second direction Z, the first direction Y, and the thickness direction X of the separator 7 are perpendicular to each other. For example, the first direction Y is parallel to the height direction of the battery cell (e.g., the length direction of the separator 7), and the second direction Z is parallel to the width direction of the separator 7. Figure 1 shows a schematic diagram of the plurality of recessed regions 71 being spaced apart.
[0070] In other embodiments, a plurality of recessed regions 71 may be provided, with two adjacent recessed regions 71 being disposed continuously along the projection of the thickness direction X of the isolation membrane 7. In other words, the continuous provision of two adjacent recessed regions 71 is beneficial for increasing the overall occupied volume of the plurality of recessed regions 71, improving the gas conduction capacity of the recessed regions 71, and improving the liquid retention capacity of the isolation membrane 7.
[0071] In some embodiments, the volume percentage of the recessed regions 71 relative to the total volume of the isolation membrane 7 is between 2% and 10%. When the volume percentage of the recessed regions 71 falls within this range, it helps increase the overall occupied volume of the multiple recessed regions 71, improves the air conduction capacity of the recessed regions 71, and helps improve the liquid retention capacity of the isolation membrane 7. It should be noted that the total volume of the isolation membrane 7 includes the volume of the recessed regions 71.
[0072] Illustratively, the volume percentage of the recessed area 71 relative to the total volume of the isolation film 7 may be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range consisting of any two of the above values.
[0073] In some embodiments, the cross-sectional shape of the recessed area 71 parallel to the second direction Z may be polygonal or arc-shaped.
[0074] For example, the polygon may be a regular polygon or an irregular polygon; for example, the polygon may be a triangle, a trapezoid, a regular quadrilateral, a pentagon or a hexagon, etc. FIG1 shows a schematic diagram of a cross-section of the recessed area 71 parallel to the second direction Z being a regular quadrilateral.
[0075] Illustratively, the arc may be a portion of a circle or an ellipse, such as a semicircle, a semi-ellipse, a 1 / 3 circle, and the like.
[0076] When there are multiple recessed areas 71 , the cross-sectional shapes of the recessed areas 71 may be the same or different. For example, the cross-sectional shape of one recessed area 71 may be semicircular, while the cross-sectional shape of another recessed area 71 may be triangular.
[0077] In some embodiments, the separator 7 has a porous structure, which is beneficial for liquid absorption and retention inside the separator 7, thereby improving the cycle performance of the battery cell.
[0078] In some embodiments, the porosity of the separator 7 may be 40% to 70%. The relatively high porosity of the separator 7 is beneficial for further improving the liquid retention capacity of the separator 7, thereby further improving the cycle performance of the battery cell.
[0079] Illustratively, the porosity of the isolation film 7 may be 40%, 45%, 50%, 55%, 60%, 65%, 70%, or a range consisting of any two of the above values.
[0080] In this embodiment, porosity refers to the ratio of the pore volume within the separator 7 to the total volume of the separator 7. Porosity can be measured using the gas displacement method in accordance with GB / T 24586. Porosity (P%) = (L1 - L2) / L1 * 100%, where L1 is the apparent volume of the sample and L2 is the actual volume of the sample.
[0081] In some embodiments, the isolation membrane 7 has a pore structure, and the average pore size of the pore structure can be 0.03 μm to 1.5 μm. When the average pore size of the isolation membrane 7 is within the above range, it is beneficial to further enhance the liquid retention capacity of the isolation membrane 7, thereby further improving the cycle performance of the battery cell.
[0082] Illustratively, the average pore size of the isolation membrane 7 may be 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.08 μm, 0.09 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, or a range consisting of any two of the above values.
[0083] In the embodiment of the present application, the average pore size of the isolation membrane 7 has a well-known meaning in the art and can be tested using equipment and methods known in the art. For example, a BET nitrogen adsorption-desorption test can be used according to GB / T 19587-2017.
[0084] In some embodiments, the thickness of the isolation membrane 7 may be 7 μm to 150 μm. When the thickness of the isolation membrane 7 is within the above range, the mechanical strength of the isolation membrane 7 can be improved, and the structural stability of the isolation membrane 7 can be enhanced.
[0085] Exemplarily, the thickness of the isolation film 7 can be 7μm, 8μm, 10μm, 12μm, 15μm, 18μm, 20μm, 22μm, 24μm, 25μm, 28μm, 29μm, 30μm, 32μm, 34μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, 75μm, 80μm, 85μm, 90μm, 95μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm or a range consisting of any two of the above values.
[0086] The separator 7 according to the embodiments of the present application has various structural forms. For example, the separator 7 may include a porous base membrane, and the recessed region 71 may be formed by applying pressure to the surface of the porous base membrane. Alternatively, the separator 7 may include a porous base membrane and a coating disposed on at least one surface of the porous base membrane, wherein the coating may include heat-resistant particles, etc. The recessed region 71 may be formed by applying pressure to the surface of the coating after disposing the coating on the porous base membrane, or by applying a coating slurry with a different thickness during coating, thereby drying to form the coating having the recessed region 71.
[0087] In some embodiments, the main material of the porous base membrane may include one or more of polyolefin, polyethylene terephthalate (PET), polyimide (PI), polyetheretherketone (PEEK), meta-aramid, polybenzimidazole, polyphenylene sulfide, polybenzimidazole, and glass fiber. The main material of the porous base membrane refers to the main component of the porous base membrane, and the porous base membrane may also include other components. Of course, the porous base membrane can also be composed of the main material. For example, the porous substrate can be a non-woven fabric or glass fiber.
[0088] Optionally, the polyolefin includes one or more of polyethylene (PE), polypropylene (PP) and polyvinylidene fluoride (PVDF).
[0089] In some embodiments, the heat-resistant filler includes at least one of inorganic particles and organic particles.
[0090] In some embodiments, the heat-resistant inorganic particles may include at least one of inorganic particles having a dielectric constant of 5 or more, inorganic particles having the ability to transport active ions, and inorganic particles capable of electrochemical oxidation and reduction.
[0091] In some embodiments, inorganic particles having a dielectric constant of 5 or higher may include boehmite (γ-AlOOH), aluminum oxide (Al2O3), barium sulfate (BaSO4), magnesium oxide (MgO), magnesium hydroxide (Mg(OH)2), silicon oxide SiO x(0<x≤2), tin dioxide (SnO2), titanium oxide (TiO2), calcium oxide (CaO), zinc oxide (ZnO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), nickel oxide (NiO), hafnium dioxide (HfO2), cerium oxide (CeO2), zirconium titanate (ZrTiO3), barium titanate (BaTiO3), magnesium fluoride (MgF2), Pb(Zr,Ti)O3 (abbreviated as PZT), Pb 1-m La m Zr 1-n Ti n O3 (abbreviated as PLZT, 0<m<1, 0<n<1) and Pb(Mg3Nb 2 / 3 ) at least one of O3-PbTiO3 (abbreviated as PMN-PT).
[0092] In some embodiments, the inorganic particles capable of transporting active ions may include lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0<x<2, 0<y<3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0<x<2, 0<y<1, 0<z<3), (LiAlTiP) x O y Glass-like (0<x<4, 0<y<13), lithium lanthanum titanate (Li x La y TiO3, 0<x<2, 0<y<3), lithium germanium thiophosphate (Li x Ge y P z S w , 0<x<4, 0<y<1, 0<z<1, 0<w<5), lithium nitride (Li x N y , 0<x<4, 0<y<2), SiS2 type glass (Li x Si y S z , 0<x<3, 0<y<2, 0<z<4) and P2S5 type glass (Li x P y S z , 0<x<3, 0<y<3, 0<z<7).
[0093] In some embodiments, the inorganic particles capable of electrochemical oxidation and reduction may include at least one of lithium-containing transition metal oxides, lithium-containing phosphates with olivine structures, carbon-based materials, silicon-based materials, tin-based materials, and lithium titanium compounds.
[0094] In some embodiments, the organic particles may include at least one of polystyrene, polyethylene, polyimide, melamine resin, phenolic resin, polypropylene, polyester (e.g., polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate), polyphenylene sulfide, polyaramid, polyamideimide, polyimide, copolymer of butyl acrylate and ethyl methacrylate, and mixtures thereof.
[0095] In some embodiments, the coating comprises a binder; optionally, the binder comprises one or more of polyacrylate, acrylic acid, carboxymethyl cellulose, tetrafluoroethylene, polyethylene, polypropylene, and cyanoethyl pullulan.
[0096] battery cells
[0097] In a second aspect, the present application provides a battery cell, wherein the battery cell includes a separator, and the separator is a separator according to any embodiment of the first aspect of the present application.
[0098] [Positive electrode]
[0099] The battery cell further includes a positive electrode sheet, which includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector.
[0100] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is provided on either or both of the two facing surfaces of the positive electrode current collector.
[0101] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector and containing a positive electrode active material.
[0102] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0103] The embodiment of the present application is applicable to the sodium salt system of polyanion materials, for example, the positive electrode active material includes Na x M y P m O n, wherein M represents a transition metal element, and the transition metal element includes at least one of Mn, Fe, Co, Cu, Al, Ti, and V, 1≤x≤2, 0≤y≤1, 0≤m≤2, 4≤n≤8, and 0<x / m≤1.
[0104] In some embodiments, 0<y≤1.
[0105] In some embodiments, 0<m≤2.
[0106] As some examples, the polyanionic material includes one or more of phosphates, pyrophosphates, and mixed polyanionic compounds.
[0107] For example, the phosphate includes one or more of NaCoPO4, NaFePO4, NaMnPO4 and Na3V2(PO4)3. Na3V2(PO4)3 is converted to NaV2(PO4)3 with a molar amount of sodium being 1. 2 / 3 (PO4).
[0108] Illustratively, the pyrophosphate includes one or more of Na2CoP2O7, Na2FeP2O7, and Na2MnP2O7.
[0109] For example, the mixed polyanionic compound includes one or more of Na4Co3(PO4)2P2O7, Na4Fe3(PO4)2P2O7 and Na4Mn3(PO4)2P2O7. Na4Co3(PO4)2P2O7 is converted to NaCo with a molar amount of sodium being 1. 0.75 (PO4) 0.5 (P2O7) 0.25 (NaCo 0.75 P1O 3.75 ); Na4Fe3(PO4)2P2O7 is converted to NaFe with the molar amount of sodium as 1 0.75 (PO4) 0.5 (P2O7) 0.25 (NaFe 0.75 P1O 3.75 ); Na4Mn3(PO4)2P2O7 is converted to NaMn with the molar amount of sodium as 1 0.75 (PO4) 0.5 (P2O7) 0.25 (NaFe 0.75 P1O 3.75 ).
[0110] In the present application, the polyanionic compound may also be modified, for example, by doping modification and / or surface coating modification.
[0111] In some embodiments, the positive electrode active material layer may further optionally include a positive electrode conductive agent. The present application does not particularly limit the type of the positive electrode conductive agent. By way of example, the positive electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the positive electrode conductive agent is ≤5% based on the total mass of the positive electrode active material layer.
[0112] In some embodiments, the positive electrode active material layer may further optionally include a positive electrode binder. The present application embodiment has no particular restrictions on the type of the positive electrode binder. As an example, the positive electrode binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin. In some embodiments, based on the total mass of the positive electrode active material layer, the mass percentage of the positive electrode binder is ≤5%.
[0113] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0114] [Negative electrode]
[0115] The battery cell also includes a negative electrode plate.
[0116] In some embodiments, the negative electrode plate includes a negative electrode current collector. During charging, sodium ions gain electrons on the surface of the negative electrode current collector to form a sodium metal layer.
[0117] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As examples of metal foil, aluminum foil or copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0118] Furthermore, the negative electrode plate further includes a conductive layer disposed on the negative electrode current collector, the conductive layer including a negative electrode conductive agent. As an example, the negative electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0119] In other embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector and comprising a negative electrode active material. For example, the negative electrode current collector has two opposing surfaces in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposing surfaces of the negative electrode current collector.
[0120] The material of the negative electrode current collector is as described above and will not be repeated here.
[0121] The negative electrode active material can be any negative electrode active material known in the art for use in battery cells. For example, the negative electrode active material may include, but is not limited to, at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may include at least one of elemental silicon, silicon oxide, a silicon-carbon composite, a silicon-nitrogen composite, and a silicon alloy. The tin-based material may include at least one of elemental tin, tin oxide, and a tin alloy.
[0122] In some embodiments, the negative electrode film layer may further optionally include a negative electrode conductive agent. The present application does not particularly limit the type of the negative electrode conductive agent. For example, the negative electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the negative electrode conductive agent is ≤5 wt% based on the total weight of the negative electrode film layer.
[0123] In some embodiments, the negative electrode film layer may further optionally include a negative electrode binder. The present application does not particularly limit the type of the negative electrode binder. As an example, the negative electrode binder may include at least one of styrene-butadiene rubber (SBR), a water-soluble unsaturated resin SR-1B, a water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). In some embodiments, the mass percentage of the negative electrode binder is ≤5 wt% based on the total weight of the negative electrode film layer.
[0124] In some embodiments, the negative electrode film layer may optionally include other additives. For example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC), a PTC thermistor material, or the like. In some embodiments, the other additives may comprise ≤ 2 wt % of the total weight of the negative electrode film layer.
[0125] The negative electrode film layer is typically formed by coating a negative electrode slurry onto a negative electrode current collector, drying, and cold pressing. The negative electrode slurry is typically formed by dispersing a negative electrode active material, an optional conductive agent, an optional binder, and other optional additives in a solvent and stirring uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.
[0126] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate described herein further includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector. In other embodiments, the negative electrode plate described herein further includes a protective layer covering the surface of the negative electrode film layer.
[0127] [Electrolytes]
[0128] Battery cells also include an electrolyte, which conducts ions between the positive and negative electrodes. The present embodiments do not specifically limit the type of electrolyte; the electrolyte can be selected based on needs. For example, the electrolyte can be liquid, gel, or solid.
[0129] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0130] As an example, the electrolyte salt may include, but is not limited to, at least one of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bisfluorosulfonyl imide (NaFSI), sodium bistrifluoromethanesulfonyl imide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalatoborate (NaDFOB), sodium dioxalatoborate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorobisoxalatophosphate (NaDFOP) and sodium tetrafluorooxalatophosphate (NaTFOP).
[0131] As an example, the solvent may include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).
[0132] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0133] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0134] In some embodiments, the battery cell may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0135] In some embodiments, the outer packaging of the battery cell may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the battery cell may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0136] The present application has no particular limitation on the shape of the battery cell, which can be cylindrical, square or any other shape. FIG4 shows a battery cell 5 with a square structure as an example.
[0137] In some embodiments of the present application, as shown in FIG2 , the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and side plates connected to the bottom plate, and the bottom plate and the side plates enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process and / or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, which can be adjusted according to demand.
[0138] The preparation method of the battery cell of the present application is well known. In some embodiments of the present application, a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte can be assembled to form a battery cell. As an example, the positive electrode sheet, separator, and negative electrode sheet can be formed into an electrode assembly through a winding process and / or a lamination process. The electrode assembly is placed in an outer packaging, dried, and then injected with electrolyte. The battery cell is then vacuum packaged, allowed to stand, formed, and shaped.
[0139] In some embodiments of the present application, the battery cells according to the present application can be assembled into a battery module. The battery module can contain multiple battery cells, and the specific number can be adjusted according to the application and capacity of the battery module.
[0140] Figure 3 is a schematic diagram of the structure of an exemplary battery module. As shown in Figure 3 , within a battery module 4, multiple battery cells 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple battery cells 5 may be secured together using fasteners.
[0141] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.
[0142] In some embodiments of the present application, the above-mentioned battery modules may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0143] Figures 4 and 5 are schematic diagrams of an exemplary battery pack. As shown in Figures 4 and 5, a battery pack 1 may include a battery case and multiple battery modules 4 disposed within the battery case. The battery case comprises an upper case 2 and a lower case 3. The upper case 2 covers the lower case 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the battery case.
[0144] In the embodiments of the present application, a battery cell, a battery module or a battery pack can be used as specific examples of batteries.
[0145] Electrical devices
[0146] In a third aspect, the present application provides an electrical device comprising one or more of the battery cells, battery modules, or battery packs of the second aspect of the present application. The battery cells, battery modules, or battery packs can serve as a power source for the electrical device or as an energy storage unit for the electrical device.
[0147] In this application, electrical devices include, but are not limited to, mobile phones, tablets, laptops, electric toys, electric tools, battery-powered vehicles, electric cars, ships, spacecraft, energy storage systems, etc. Electric toys may include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Spacecraft may include airplanes, rockets, space shuttles, and spacecraft, etc.
[0148] In addition, the electrical device can select a battery cell, a battery module or a battery pack according to its usage requirements.
[0149] Figure 6 is a schematic diagram of the structure of an exemplary electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module may be used.
[0150] The following examples further describe the present disclosure. These examples are intended for illustrative purposes only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. All reagents used in the examples are commercially available or synthesized according to conventional methods and used without further processing. All instruments used in the examples are commercially available.
[0151] Example 1 Preparation of sodium ion battery
[0152] 1. Positive electrode
[0153] The positive electrode active material NaFePO4, the conductive agent acetylene black, and the binder carboxymethyl cellulose are fully stirred and mixed in an appropriate amount of N-methylpyrrolidone (NMP) at a mass ratio of 90:5:5 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying, cold pressing, and die-cutting, the positive electrode sheet is obtained.
[0154] 2. Negative electrode
[0155] A copper foil with a thickness of 8 μm was used as a negative electrode current collector, and the negative electrode current collector was used as a negative electrode plate.
[0156] 3. Isolation film
[0157] A 12μm polyethylene film is used as the porous base film. A pressing roller is used to press the polyethylene film, creating a gravure print. This gravure print forms a recessed area that extends along the length of the separator. The shape of the recessed area can be adjusted based on the shape of the pressing roller.
[0158] 4. Electrolyte
[0159] In an argon-filled glove box with a water content of <1 ppm, diethylene glycol dimethyl ether and tetrahydrofuran were mixed in a mass ratio of 1:3, sodium hexafluorophosphate (NaPF6) with a concentration of 1.0 mol / L was added, and the mixture was stirred evenly to obtain an electrolyte.
[0160] 5. Preparation of sodium ion battery monomers
[0161] The positive electrode sheet, separator and negative electrode sheet are formed into an electrode assembly through a lamination process, the electrode assembly is placed in an outer package, and after drying, the electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a sodium ion battery cell is obtained. The sodium ion battery cell is placed vertically with its height direction parallel to the length direction of the separator.
[0162] Example 2
[0163] A sodium ion battery was prepared using a method similar to that of Example 1. The difference from Example 1 was that the angle between the recessed area and the length direction of the isolation membrane was adjusted in Examples 2-1 and 2-3.
[0164] Example 3
[0165] A sodium ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, the volume percentage of the recessed area was adjusted in Examples 3-1 and 3-2.
[0166] Example 4
[0167] A sodium ion battery was prepared using a method similar to that of Example 1. The difference from Example 1 was that the material of the porous base membrane in the isolation membrane was adjusted in Examples 4-1 and 4-2.
[0168] Comparative Example 1
[0169] A sodium ion battery was prepared by a method similar to that of Example 1. The difference from Example 1 was that a 12 μm polyethylene film was used in Comparative Example 1, and the polyethylene film was not rolled.
[0170] Comparative Example 2
[0171] A sodium ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, Comparative Example 2 adjusted the preparation method of the isolation membrane:
[0172] A 12 μm polyethylene film is used, and a pressing roller is used to press the polyethylene film to form a circular gravure. The gravure forms a recessed area, and the recessed areas are distributed at intervals on the surface of the isolation film, and the recessed areas do not penetrate the isolation film.
[0173] Test section
[0174] 1. Cycle performance of sodium ion batteries
[0175] At 25°C, a secondary battery is charged at a constant current of 0.33C to 3.65V, then charged at a constant voltage of 3.65V to a current of 0.05C, and then discharged at a constant current of 1C to 1.5V. This constitutes one charge-discharge cycle. Taking the initial discharge capacity as 100%, calculate the capacity retention after 500 cycles. Capacity retention after 500 cycles (%) = discharge capacity at the 500th cycle / initial discharge capacity × 100%.
[0176] Test results
[0177] The test results are shown in Table 1.
[0178] Table 1
[0179] It can be seen from Table 1 that compared with Comparative Example 1 and Comparative Example 2 (Figure 10 shows a schematic diagram of the distribution of the recessed area in the isolation membrane of Comparative Example 2), the isolation membrane surface of the embodiment of the present application includes a recessed area, which penetrates the isolation membrane and can effectively guide the gas in the electrode assembly to the outside of the electrode assembly, thereby reducing the risk of volume expansion of the electrode assembly and improving the liquid retention capacity of the isolation membrane, thereby improving the cycle performance of the battery cell.
[0180] The embodiments of the present application can adjust the exhaust capacity and liquid retention capacity of the isolation membrane by adjusting at least one of the extension direction of the recessed area, the arrangement of the recessed area (spaced arrangement or continuous setting), the volume percentage, the shape, etc., thereby further adjusting and improving the cycle performance of the battery cell.
[0181] The embodiments of the present application can also improve the isolation membrane and the liquid retention capacity by adjusting the material and pore parameters (porosity and average pore size, etc.) of the porous base membrane, thereby further adjusting and improving the cycle performance of the battery cell.
[0182] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions, and modifications may be made to the embodiments without departing from the spirit, principles, and scope of the present application.
Claims
1. An isolation film, comprising two surfaces opposite to each other along its own thickness direction, at least one of the two surfaces comprising at least one recessed area, the recessed area penetrating the isolation film along a first direction, wherein: The first direction is perpendicular to a thickness direction of the isolation film.
2. The isolation film according to claim 1, wherein: The angle between the first direction and the length direction of the isolation film is -30° to 30°; or The angle between the first direction and the width direction of the isolation film is -30° to 30°.
3. The isolation film according to claim 1 or 2, wherein: The recessed areas are provided in a plurality, A plurality of the recessed areas are arranged at intervals; or The projections of two adjacent recessed areas along the thickness direction of the isolation film are continuously arranged.
4. The separator according to any one of claims 1 to 3, wherein: The cross-sectional shape of the recessed area parallel to the second direction is a polygon or an arc, and the second direction, the first direction and the thickness direction of the isolation film are perpendicular to each other; Optionally, the polygon is a triangle, a trapezoid, a regular quadrilateral, a pentagon or a hexagon.
5. The separator according to any one of claims 1 to 4, wherein: The volume percentage of the recessed area relative to the total volume of the isolation film is 2% to 10%.
6. The isolation film according to any one of claims 1 to 5, wherein: The isolation film satisfies at least one of the following conditions: (1) The porosity of the isolation membrane is 40% to 70%; (2) The isolation membrane includes a pore structure, and the average pore size of the pore structure is 0.03 μm to 1.5 μm; (3) The thickness of the isolation film is 7 μm to 150 μm.
7. The separator according to any one of claims 1 to 6, wherein: The isolation membrane comprises a porous base membrane, and the main material of the porous base membrane comprises one or more of polyolefin, polyethylene terephthalate PET, polyimide PI, polyetheretherketone PEEK, meta-aramid, polybenzimidazole, polyphenylene sulfide, polybenzimidazole and glass fiber; Optionally, the polyolefin includes one or more of polyethylene PE, polypropylene PP and polyvinylidene fluoride PVDF. 8 . A battery cell comprising the separator according to claim 1 .
9. The battery cell according to claim 8, wherein the battery cell comprises a positive electrode plate, wherein the positive electrode plate comprises a positive electrode active material layer containing a positive electrode active material, wherein the positive electrode active material comprises: Na x M y P m O n , wherein M represents a transition metal element, the transition metal element includes at least one of Mn, Fe, Co, Cu, Al, Ti, and V, 1≤x≤2, 0≤y≤1, 0≤m≤2, 4≤n≤8, and 0<x / m≤1; optionally, 0<y≤1; and / or 0<m≤2.
10. A battery comprising the battery cell according to claim 8 or 9.
11. An electrical device comprising the battery as claimed in claim 10.
Citation Information
Patent Citations
Nonaqueous secondary battery and separator
CN103915645A
Separator having fine pattern, wound body, and non-aqueous electrolyte battery
CN112352344A
Isolating membrane, isolating membrane preparation method and electrochemical device
CN114725622A
Diaphragm, secondary battery and electronic device
CN115986321A
Accumulator comprising resin composition with hydrophilic radical polyolefine as main component