Negative electrode sheet of battery cell, battery cell, battery, and electric device
By increasing the thickness and dispersion concentration of the active material layer in the thinned area of the negative electrode sheet of the battery, the lithium precipitation phenomenon is solved, the service life of the battery is extended and the cost is reduced.
Patent Information
- Application Number
- PCT/CN2023/142731
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2023-12-28
- Publication Date
- 2024-10-31
AI Technical Summary
Existing batteries are prone to lithium precipitation on the edge of the negative electrode during use, which affects the service life and reliability of the battery.
By increasing the thickness and dispersion concentration of the negative active material layer in the thinned area of the negative electrode piece, the problem of insufficient CB value of the negative electrode piece is improved, the phenomenon of lithium deposition is reduced, and the service life and reliability of the battery are extended.
It effectively improves the problem of battery capacity diving and pole piece tearing, prolongs the service life of the battery and reduces the cost.
Smart Images

Figure CN2023142731_31102024_PF_FP_ABST
Abstract
Description
Negative electrode sheet of battery cell, battery cell, battery and electrical device
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application is based on the Chinese patent application with application number 202310483428.5 and application date 2023-04-28, and claims the priority of the above-mentioned Chinese patent application. The entire content of the above-mentioned Chinese patent application is hereby introduced into this application as a reference. Technical Field
[0003] The present application relates to the field of battery technology, and in particular to a negative electrode sheet of a battery cell, a battery cell, a battery, and an electrical device. Background Art
[0004] New energy vehicles have experienced rapid growth in recent years. Batteries, as the power source for electric vehicles, play an irreplaceable and important role. As core components of new energy vehicles, batteries are subject to high demands in terms of both reliability and cycle life. However, some batteries in related technologies suffer from lithium deposition at the edges of the negative electrode, impacting battery life and reliability.
[0005] Summary of the Invention
[0006] The embodiments of the present application provide a negative electrode plate of a battery cell, a battery cell, a battery, and an electrical device, which can extend the service life and reliability of the battery cell.
[0007] In a first aspect, an embodiment of the present application provides a negative electrode plate of a battery cell, comprising: a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the two side surfaces of the negative electrode active material layer being respectively a first surface away from the negative electrode current collector and a second surface close to the negative electrode current collector, the negative electrode active material layer comprising a first portion and a second portion, the second portion being located on a side of the first portion close to an edge of the negative electrode plate in a first direction of the negative electrode plate, the first surface being offset toward the negative electrode current collector at the second portion relative to the first portion; wherein the negative electrode plate is constructed such that: at least a portion of the second surface at the second portion protrudes toward the negative electrode current collector relative to the first portion, and / or the dispersion concentration of the negative electrode active material in the negative electrode active material layer in the second portion is greater than the dispersion concentration in the first portion.
[0008] In the above technical solution, by improving the negative electrode thinning area, the negative electrode active material layer is thickened in the direction toward the negative electrode current collector in the negative electrode thinning area, and / or the dispersion concentration of the negative electrode active material in the negative electrode active material layer is increased in the negative electrode thinning area, thereby increasing the negative electrode active material in the negative electrode thinning area, improving the problem of insufficient CB value in the negative electrode thinning area of the negative electrode sheet, and improving the phenomenon of lithium deposition in the negative electrode thinning area of the negative electrode sheet after long cycles, thereby improving the problem of battery capacity drop and electrode sheet cracking caused by lithium deposition, thereby extending the service life and reliability of the battery cell. Moreover, since only the local improvement of the negative electrode sheet is carried out, the cost of the negative electrode sheet will basically not increase.
[0009] In some embodiments, the negative electrode current collector includes a third portion corresponding to the first portion and a fourth portion corresponding to the second portion, wherein the thickness of the fourth portion is less than the thickness of the third portion to accommodate at least a portion of the negative electrode active material layer protruding toward the negative electrode current collector at the second portion.
[0010] In the above technical solution, the thickness of the fourth portion of the negative electrode current collector can be reduced relative to the third portion to achieve thickening of the negative electrode active material layer in the negative electrode thinning area toward the negative electrode current collector, thereby reducing the difficulty of processing the negative electrode sheet.
[0011] In some embodiments, a functional layer not containing negative electrode active material is provided between the negative electrode collector and the negative electrode active material layer, and the functional layer includes a fifth part corresponding to the first part and a sixth part corresponding to the second part, and the thickness of the sixth part is less than the thickness of the fifth part, so as to accommodate at least a portion of the negative electrode active material layer protruding toward the negative electrode collector at the second part.
[0012] In the above technical solution, the reduced thickness of the sixth portion of the functional layer relative to the fifth portion can be utilized to achieve a thicker negative electrode active material layer in the direction toward the negative electrode current collector in the thinned-out region of the negative electrode, thereby reducing the difficulty of processing the negative electrode sheet. Furthermore, the functional layer, which does not contain negative electrode active material, can be used to improve other properties of the negative electrode sheet.
[0013] In some embodiments, a functional layer containing no negative electrode active material is provided between the negative electrode current collector and the negative electrode active material layer, and the functional layer includes a fifth portion corresponding to the first portion and does not include a portion corresponding to the second portion.
[0014] In the above technical solution, the absence of the portion corresponding to the second portion in the functional layer can be exploited to achieve a thickening of the negative electrode active material layer in the direction toward the negative electrode current collector in the negative electrode thinning area, thereby reducing the difficulty of processing the negative electrode sheet. Furthermore, the functional layer without negative electrode active material can be used to improve other properties of the negative electrode sheet.
[0015] In some embodiments, the functional layer includes a conductive agent and an adhesive, the conductive agent includes at least one of SP and CNT, and the adhesive includes at least one of PVDF and SBR.
[0016] In the above technical solution, a functional layer including a conductive agent and an adhesive is provided between the negative electrode current collector and the negative electrode active material layer, thereby improving the bonding force of the electrode and preventing the decarbonization and powdering problem.
[0017] In some embodiments, the portion of the second surface that protrudes at the second portion is a protrusion, there is only one protrusion, and the length direction of the protrusion extends along the second direction of the negative electrode sheet.
[0018] In the above technical solution, the protrusion extends continuously along the second direction of the negative electrode sheet, thereby facilitating the processing of the negative electrode sheet and effectively improving the lithium deposition phenomenon in the negative electrode thinning area of the negative electrode sheet.
[0019] In some embodiments, the portion of the second surface that protrudes at the second portion is a protrusion, and there are multiple protrusions that are spaced apart along the second direction of the negative electrode sheet.
[0020] In the above technical solution, the protrusion extends discontinuously along the second direction of the negative electrode sheet, thereby saving the material of the negative electrode active material layer and reducing the cost of the negative electrode sheet while improving the lithium deposition phenomenon in the negative electrode thinning area of the negative electrode sheet to a certain extent.
[0021] In some embodiments, the negative electrode active material layer includes a first active material layer and a second active material layer, the dispersion concentration of the negative electrode active material in the first active material layer is greater than the dispersion concentration of the negative electrode active material in the second active material layer, the first active material layer is arranged on the side of the second active material layer away from the negative electrode current collector, and the second active material layer is eliminated at the second part to retain only the first active material layer.
[0022] In the above technical solution, the negative electrode active material layer is easy to process, and it can be easily achieved that the dispersion concentration of the negative electrode active material in the negative electrode active material layer in the second part is greater than the dispersion concentration in the first part, so as to increase the negative electrode active material in the negative electrode thinning area, improve the problem of insufficient CB value in the negative electrode thinning area of the negative electrode plate, and improve the phenomenon of lithium deposition in the negative electrode thinning area of the negative electrode plate after long cycles, thereby improving the problem of battery capacity diving and plate cracking caused by the lithium deposition phenomenon, thereby extending the service life and reliability of the battery cell.
[0023] In the second aspect, an embodiment of the present application also provides a battery cell, including a positive electrode plate, an isolation membrane and the negative electrode plate of the above-mentioned battery cell, the isolation membrane is arranged between the positive electrode plate and the negative electrode plate, the area corresponding to the first part of the negative electrode plate is the negative electrode non-thinning area, and the area corresponding to the second part of the negative electrode plate is the negative electrode thinning area, the positive electrode plate includes a positive electrode collector and a positive electrode active material layer arranged on the positive electrode collector, the positive electrode plate includes a positive electrode non-thinning area and a positive electrode thinning area arranged along a first direction, the positive electrode thinning area is arranged corresponding to the negative electrode non-thinning area, and the negative electrode thinning area is arranged corresponding to the positive electrode non-thinning area.
[0024] In some embodiments, the battery cells are wound cylinders.
[0025] In a third aspect, an embodiment of the present application further provides a battery comprising a plurality of the above-mentioned battery cells.
[0026] In a fourth aspect, an embodiment of the present application further provides an electrical device comprising the above-mentioned battery cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.
[0028] FIG1 is a schematic structural diagram of a vehicle provided in some embodiments of the present application;
[0029] FIG2 is an exploded view of the structure of a battery provided in some embodiments of the present application;
[0030] FIG3 is a schematic diagram of the structure of a negative electrode sheet provided in some embodiments of the present application;
[0031] FIG4 is a partial enlarged view of FIG3;
[0032] FIG5 is a schematic structural diagram of an electrode assembly provided in some embodiments of the present application;
[0033] FIG6 is a schematic structural diagram of a negative electrode sheet provided in some embodiments of the present application;
[0034] FIG7 is a schematic diagram of the structure of a negative electrode sheet provided in some embodiments of the present application;
[0035] FIG8 is a schematic structural diagram of a negative electrode sheet provided in some embodiments of the present application;
[0036] FIG9 is a schematic diagram of the structure of a negative electrode sheet provided in some embodiments of the present application;
[0037] FIG10 is a schematic structural diagram of the negative electrode sheet provided in Example 1 of the present application;
[0038] FIG11 is a schematic structural diagram of a negative electrode sheet provided in Example 2 of the present application;
[0039] FIG12 is a schematic structural diagram of the negative electrode sheet provided in Example 3 of the present application;
[0040] FIG13 is a schematic structural diagram of the negative electrode sheet provided in Comparative Example 1 of the present application;
[0041] FIG14 is a schematic structural diagram of a wound electrode assembly provided in some embodiments of the present application.
[0042] Figures and Symbols: Vehicle 1000; Battery 100; Battery Cell 10; Case 20; First Case Body 201; Second Case Body 202; Electrode Assembly 101; First Direction X; Second Direction Y; Thickness Center Plane S; Shaded Area Z; Negative Electrode Sheet 1; Negative Electrode Skived Area 1a; Negative Electrode Non-Skimmed Area 1b; Negative Electrode Current Collector 11; Third Part 111; Fourth Part 112; Negative Electrode Active Material Layer 12; First Surface 12a; Second Surface 12b ; First part 121; Second part 122; Protrusion 123; First active material layer 1201; Second active material layer 1202; First face 12b1; Second face 12b2; Functional layer 13; Fifth part 131; Sixth part 132; Negative electrode tab area 14; Positive electrode sheet 2; Positive electrode thinning area 2a; Positive electrode non-thinning area 2b; Positive electrode current collector 21; Positive electrode active material layer 22; Positive electrode tab area 23; Isolation membrane 3. DETAILED DESCRIPTION
[0043] To make the purpose, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application will be clearly described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0044] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as commonly understood by those skilled in the art to which this application belongs. The terms used in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first" and "second" in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order or a primary-secondary relationship.
[0045] References to "embodiments" in this application mean that a particular feature, structure, or characteristic described in connection with the embodiment may be included in at least one embodiment of the application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments.
[0046] In the description of this application, it should be noted that, unless otherwise expressly specified or limited, the terms "mounted," "connected," "connected," and "attached" should be understood in a broad sense. For example, they may refer to fixed connections, detachable connections, or integral connections; they may refer to direct connections, indirect connections through an intermediate medium, or internal connections between two components. Those skilled in the art will understand the specific meanings of the above terms in this application based on specific circumstances.
[0047] The term "and / or" in this application simply describes an association between related objects, indicating that three possible relationships exist. For example, A and / or B can represent: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this application generally indicates that the related objects are in an "or" relationship.
[0048] In the embodiments of this application, the same reference numerals represent the same components, and for the sake of brevity, detailed descriptions of the same components in different embodiments are omitted. It should be understood that the thickness, length, width, and other dimensions of the various components in the embodiments of this application, as well as the overall thickness, length, width, and other dimensions of the integrated device shown in the drawings are merely illustrative and should not constitute any limitation on this application.
[0049] The term "plurality" used in this application refers to two or more (including two).
[0050] In this application, battery cells may include lithium-ion secondary batteries, lithium-ion primary batteries, lithium-sulfur batteries, sodium-lithium-ion batteries, sodium-ion batteries, or magnesium-ion batteries, etc., and the embodiments of this application do not limit this. Battery cells may be cylindrical, flat, rectangular, or other shapes, etc., and the embodiments of this application do not limit this. Battery cells are generally divided into three types based on the packaging method: cylindrical battery cells, prismatic battery cells, and soft-pack battery cells, and the embodiments of this application do not limit this.
[0051] The battery referred to in the embodiments of this application refers to a single physical module that includes one or more battery cells to provide higher voltage and capacity. For example, the battery referred to in this application may include a battery module or a battery pack. A battery module generally includes multiple battery cells. A battery pack generally includes a casing for enclosing one or more battery cells or one or more battery modules. The casing can alleviate the problem of liquids or other foreign matter affecting the charging or discharging of battery cells.
[0052] A battery cell typically consists of a casing, an electrode assembly, and an electrolyte. The casing houses the electrode assembly and electrolyte. The electrode assembly consists of a positive electrode sheet, a negative electrode sheet, and a separator. A battery cell primarily operates by the movement of metal ions between the positive and negative electrode sheets.
[0053] A positive electrode sheet generally includes a positive current collector and a positive active material layer. The positive active material layer is directly or indirectly coated on the positive current collector. The uncoated positive current collector protrudes from the coated positive current collector and serves as the positive tab. For lithium-ion batteries, for example, the positive current collector can be made of aluminum, and the positive active material layer can be made of lithium cobalt oxide, lithium iron phosphate, ternary lithium, or lithium manganese oxide.
[0054] A negative electrode sheet generally includes a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer is directly or indirectly coated on the negative electrode current collector. The negative electrode current collector not coated with the negative electrode active material layer protrudes from the negative electrode current collector coated with the negative electrode active material layer. The negative electrode current collector not coated with the negative electrode active material layer serves as the negative electrode tab. For lithium-ion batteries, for example, the negative electrode current collector can be made of copper, and the negative electrode active material layer can be made of carbon, silicon, or other materials.
[0055] In order to allow high current to pass without melting, the number of positive electrode tabs is multiple and stacked together, and the number of negative electrode tabs is multiple and stacked together. In addition, the material of the separator is not limited, for example, it can be polypropylene or polyethylene.
[0056] New energy vehicles have experienced rapid growth in recent years. Batteries, as the power source for electric vehicles, play an irreplaceable and important role. As core components of new energy vehicles, batteries are subject to high demands in terms of both reliability and cycle life. However, some batteries in related technologies suffer from lithium deposition at the edges of the negative electrode, impacting battery life and reliability.
[0057] In general batteries, after the positive and negative pole pieces of the battery cell are coated with the active material layer, the edges on both sides of the width are thinned to form thinned areas. The thickness of the thinned area of the pole piece is reduced by about 1μ-15μ relative to the non-thinned area within a width range of 10mm. The thinned area of the positive pole piece in the electrode assembly faces the non-thinned area of the negative pole piece, and the thinned area of the negative pole piece faces the non-thinned area of the positive pole piece, thereby improving the bulging edge problem at the edge position of the pole piece width, and then improving the local extrusion deformation, wavy edge, rupture and other problems of the electrode assembly caused by the bulging edge problem, thereby improving the reliability of the battery.
[0058] Since the thickness of the negative active material layer in the thinned area of the negative electrode sheet is relatively small, and the thickness of the positive active material layer in the non-thinned area of the opposite positive electrode sheet is relatively large, it is easy to cause the CB value in the thinned area of the negative electrode sheet to be insufficient, causing lithium deposition in the thinned area of the negative electrode sheet. Lithium deposition can cause problems such as battery capacity drop and electrode sheet cracking, thereby affecting the battery life and reliability. It can be understood that "CB value" refers to: cell balance, that is, the margin of the negative electrode capacity exceeding the positive electrode capacity at the same stage and under the same conditions.
[0059] Based on the above considerations, in order to improve the phenomenon of lithium deposition in the thinned area of the negative electrode plate, the present application proposes a negative electrode plate, in which the portion of the negative electrode active material layer corresponding to the thinned area is thickened toward the negative electrode current collector, and / or the dispersion concentration of the negative electrode active material in the negative electrode active material layer in the thinned area is set to be greater than the dispersion concentration in the non-thinned area, thereby facilitating the improvement of the CB value of the thinned area of the negative electrode plate, so as to improve the lithium deposition phenomenon in the thinned area of the negative electrode plate after long-term cycling, thereby improving the battery capacity diving problem and the plate cracking problem caused by the lithium deposition phenomenon, thereby extending the service life and reliability of the battery cell, and since only the local improvement of the negative electrode plate is made, it basically does not cause the cost of the negative electrode plate to increase.
[0060] The battery cells disclosed in the embodiments of the present application can be used, but are not limited to, in electrical devices such as vehicles, ships, or aircraft. Therefore, the embodiments of the present application provide an electrical device that uses a battery cell as a power source. The electrical device can be, but is not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, an electric vehicle, an electric car, a ship, a spacecraft, and the like. Among them, electric toys can include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, and spacecraft can include airplanes, rockets, space shuttles, and spacecraft, and the like.
[0061] For the convenience of description, the following embodiments are described by taking a vehicle as an example of an electrical device according to an embodiment of the present application.
[0062] Please refer to Figure 1, which is a schematic structural diagram of a vehicle 1000 provided in some embodiments of the present application. The vehicle 1000 can be a fuel vehicle, a gas vehicle or a new energy vehicle. The new energy vehicle can be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. The vehicle 1000 is provided with a battery 100, and the battery 100 can be arranged at the bottom, head or tail of the vehicle 1000. The battery 100 can be used to power the vehicle 1000. For example, the battery 100 can serve as an operating power source for the vehicle 1000. The vehicle 1000 may also include a controller and a motor. The controller is used to control the battery 100 to power the motor, for example, for starting, navigating and driving the vehicle 1000.
[0063] In some embodiments of the present application, the battery 100 can serve not only as an operating power source for the vehicle 1000, but also as a driving power source for the vehicle 1000, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 1000.
[0064] Please refer to FIG. 2 , which is an exploded view of the structure of the battery 100 provided in some embodiments of the present application.
[0065] In some embodiments of the present application, a battery 100 includes a housing 20 and a plurality of battery cells 10, with the battery cells 10 housed within the housing 20. The housing 20 provides assembly space for the battery cells 10. In other embodiments of the present application, the battery 100 may not include the housing 20 but may include only a plurality of battery cells 10, which will not be described in detail here.
[0066] In the battery 100, multiple battery cells 10 can be connected in series, in parallel, or in a hybrid connection. A hybrid connection refers to a combination of series and parallel connections among the multiple battery cells 10. Multiple battery cells 10 can be directly connected in series, in parallel, or in a hybrid connection, and then the entire battery 10 can be housed within the housing 20. Of course, the battery 100 can also be in the form of a battery module 100, where multiple battery cells 10 are first connected in series, in parallel, or in a hybrid connection. The multiple battery modules 100 are then connected in series, in parallel, or in a hybrid connection to form a complete battery 100, and then housed within the housing 20. The battery 100 may also include other structures. For example, the battery 100 may also include a busbar component for electrically connecting the multiple battery cells 10.
[0067] The housing 20 can have a variety of structures. For example, in some embodiments, as shown in FIG2 , the housing 20 can include a first housing body 201 and a second housing body 202 . The first housing body 201 and the second housing body 202 overlap each other, and the first housing body 201 and the second housing body 202 together define an assembly space for accommodating the battery cells 10 . For example, the second housing body 202 can be a hollow structure with one end open, and the first housing body 201 can be a plate-like structure. The first housing body 201 overlaps the open side of the second housing body 202 , so that the first housing body 201 and the second housing body 202 together define an assembly space. Alternatively, the first housing body 201 and the second housing body 202 can both be hollow structures with one end open, and the open side of the first housing body 201 overlaps the open side of the second housing body 202 . Of course, the housing 20 formed by the first housing body 201 and the second housing body 202 can have a variety of shapes, such as a cylinder, a rectangular parallelepiped, etc.
[0068] Please refer to FIG3 , which introduces the negative electrode sheet 1 provided in some embodiments of the present application.
[0069] The negative electrode sheet 1 includes a negative electrode current collector 11 and a negative electrode active material layer 12 disposed on the negative electrode current collector 11. It is understood that the negative electrode active material layer 12 can be provided on both sides of the thickness of the negative electrode current collector 11. The negative electrode active material layer 12 can be directly or indirectly coated on the negative electrode current collector 11. That is, there may or may not be a functional layer between the negative electrode current collector 11 and the negative electrode active material layer 12. The portion of the negative electrode current collector 11 not coated with the negative electrode active material layer 12 is the negative electrode tab region 14. The materials of the negative electrode current collector 11 and the negative electrode active material layer 12 can be specifically set according to design requirements and are not described in detail here.
[0070] As shown in Figure 3, the two side surfaces of the negative electrode active material layer 12 are respectively a first surface 12a away from the negative electrode current collector 11 and a second surface 12b close to the negative electrode current collector 11. The negative electrode active material layer 12 includes a first portion 121 and a second portion 122. In the first direction X of the negative electrode plate 1, the second portion 122 is located on the side of the first portion 121 close to the edge of the negative electrode plate 1, and the first surface 12a is offset toward the negative electrode current collector 11 at the second portion 122 relative to the first portion 121.
[0071] In some embodiments of the present application, the first direction X may be the width direction of the negative electrode sheet 1, and the second direction Y may be the length direction of the negative electrode sheet 1. In other embodiments of the present application, the first direction X may also be the length direction of the negative electrode sheet 1, and the second direction Y may be the width direction of the negative electrode sheet 1. To simplify the description, the following description will only use "the first direction X is the width direction of the negative electrode sheet 1, and the second direction Y is the length direction of the negative electrode sheet 1" as an example.
[0072] The manner in which “the first surface 12a is offset toward the negative electrode current collector 11 at the second portion 122 relative to its first portion 121” is not limited. For example, the first surface 12a may be gradually inclined and extended along a straight line or a curve in the second portion 122 in the first direction X along a direction away from the first portion 121 toward the negative electrode current collector 11. For another example, the first surface 12a may be translated toward the negative electrode current collector 11 as a whole at the second portion 122 relative to its first portion 121, so that this area of the first surface 12a presents a stepped shape, and so on.
[0073] For example, as shown in Figures 3 and 4, the distance from the first surface 12a at the first portion 121 to the center plane S of the thickness of the negative electrode current collector 11 is a first distance h1, and the distance from the first surface 12a at the second portion 122 to the center plane S of the thickness of the negative electrode current collector 11 is a second distance h2. The first distance h1 remains substantially constant along the direction from the first portion 121 to the second portion 122, and the second distance h2 gradually decreases along the direction from the first portion 121 to the second portion 122. Thus, the area of the negative electrode sheet 1 corresponding to the first portion 121 can be defined as the negative electrode non-thinned area 1b, and the area of the negative electrode sheet 1 corresponding to the second portion 122 can be defined as the negative electrode thinned area 1a.
[0074] As shown in Figure 3, in some optional embodiments, at least a portion of the second surface 12b at the second portion 122 protrudes toward the negative electrode current collector 11 relative to the first portion 121, thereby equivalent to thickening the negative electrode active material layer 12 at the second portion 122 toward the negative electrode current collector 11, so as to increase the negative electrode active material in the negative electrode thinning area 1a, thereby improving the problem of insufficient CB value at the negative electrode thinning area 1a.
[0075] For example, as shown in Figures 3 and 4, at least a portion of the second surface 12b at the second portion 122 is a protrusion 123, the distance from the second surface 12b at the first portion 121 to the thickness center plane S of the negative electrode current collector 11 is a third distance h3, and the distance from the protrusion 123 of the second surface 12b to the thickness center plane S of the negative electrode current collector 11 is a fourth distance h4, wherein the fourth distance h4 is smaller than the third distance h3, thereby achieving that the second surface 12b protrudes at the protrusion 123 relative to the first portion 121 toward the direction close to the negative electrode current collector 11.
[0076] In some optional embodiments, the dispersion concentration of the negative electrode active material in the negative electrode active material layer 12 in the second portion 122 is greater than the dispersion concentration in the first portion 121. The dispersion concentration may be a mass concentration or a volume concentration. Thus, by increasing the dispersion concentration of the negative electrode active material in the negative electrode active material layer 12 in the second portion 122, the amount of negative electrode active material in the negative electrode skived region 1a can be increased, thereby improving the problem of insufficient CB value in the negative electrode skived region 1a.
[0077] In some optional embodiments, at least a portion of the second surface 12b in the second portion 122 protrudes relative to the first portion 121 toward the negative electrode current collector 11, and the dispersion concentration of the negative electrode active material in the negative electrode active material layer 12 in the second portion 122 is greater than that in the first portion 121. As a result, the amount of negative electrode active material in the negative electrode skived area 1a can be significantly increased, thereby better improving the problem of insufficient CB value in the negative electrode skived area 1a.
[0078] Generally, after the negative electrode current collector 11 of the unslit negative electrode sheet 1 is coated with the negative electrode active material layer 12, the negative electrode active material layer 12 is thinned at the edges on both sides of the width to form a negative electrode thinning area 1a. The portion between the negative electrode thinning areas 1a on both sides is the negative electrode non-thinning area 1b. The unslit negative electrode sheet 1 is then cut along the length centerline to obtain two negative electrode sheets 1 located on both sides of the cutting line. The width edge of each cut negative electrode sheet 1 is the negative electrode thinning area 1a. Similarly, the positive electrode sheet 2 can be made, and then the positive electrode sheet 2, the negative electrode sheet 1 and the separator 3 are combined to form an electrode assembly 101. At this time, the positive electrode non-thinning area 2b of the positive electrode sheet 2 faces the negative electrode thinning area 1a of the negative electrode sheet 1 (for example, as shown in Figure 5). It can be understood that in some other embodiments, after the unslit electrode is coated with the active material layer, the active material layer will be thinned at the edges on both sides of the length to form a thinning area, and then the electrode will be cut along the center line of the width of the electrode, and the edge on one side of the length of the cut electrode will be the thinning area.
[0079] According to the negative electrode sheet 1 of the embodiment of the present application, by improving the negative electrode thinning area 1a, the negative electrode active material layer 12 is thickened in the direction of the negative electrode thinning area 1a toward the negative electrode current collector 11, and / or the dispersion concentration of the negative electrode active material in the negative electrode active material layer 12 is increased in the negative electrode thinning area 1a, thereby increasing the negative electrode active material in the negative electrode thinning area 1a, improving the problem of insufficient CB value in the negative electrode thinning area 1a of the negative electrode sheet 1, and improving the phenomenon of lithium deposition in the negative electrode thinning area 1a of the negative electrode sheet 1 after long cycles, thereby improving the problem of capacity drop of the battery 100 and electrode sheet cracking caused by lithium deposition, thereby extending the service life and reliability of the battery cell 10. Moreover, since only a part of the negative electrode sheet 1 is improved, the cost of the negative electrode sheet 1 is basically not increased.
[0080] In some embodiments, as shown in FIG6 , the negative electrode current collector 11 includes a third portion 111 corresponding to the first portion 121 and a fourth portion 112 corresponding to the second portion 122. The thickness d1 of the fourth portion 112 is less than the thickness d2 of the third portion 111, thereby accommodating at least a portion of the negative electrode active material layer 12 that protrudes toward the negative electrode current collector 11 at the second portion 122. Thus, when the negative electrode active material layer 12 is directly coated on the negative electrode current collector 11, because the thickness d1 of the fourth portion 112 is less than the thickness d2 of the third portion 111, the negative electrode active material layer 12 at the second portion 122 needs to fill the reduced thickness of the fourth portion 112 relative to the third portion 111, thereby easily achieving a second surface 12b that protrudes toward the negative electrode current collector 11 at the second portion 122 relative to the first portion 121.
[0081] In the above technical solution, the thickness of the fourth portion 112 of the negative electrode current collector 11 can be reduced relative to the third portion 111 to achieve thickening of the negative electrode active material layer 12 in the direction from the negative electrode thinned area 1a toward the negative electrode current collector 11, thereby reducing the difficulty of processing the negative electrode sheet 1.
[0082] There are various ways to configure the negative electrode current collector 11 so that the thickness d1 of the fourth portion 112 is less than the thickness d2 of the third portion 111. For example, the thickness of the fourth portion 112 of the negative electrode current collector 11 can be thinned on both sides, or only on one side. For example, when the thickness of the fourth portion 112 of the negative electrode current collector 11 is symmetrically thinned, the distance between the two sides of the thickness of the negative electrode current collector 11 at the fourth portion 112 and the center plane of the thickness of the negative electrode current collector 11 can be d1 / 2. In this case, the negative active material layer 12 on both sides of the thickness of the negative electrode current collector 11 can protrude toward the negative electrode current collector 11 at the second portion 122.
[0083] Furthermore, in some optional examples, when the thickness d1 of the fourth portion 112 is less than the thickness d2 of the third portion 111, the locally thinned functional layer between the negative electrode current collector 11 and the negative electrode active material layer 12 can be omitted, thereby reducing the difficulty in processing the negative electrode sheet 1, reducing the production cost of the negative electrode sheet 1, and improving the production efficiency of the negative electrode sheet 1. However, the present application is not limited thereto. In some embodiments of the present application, when the thickness d1 of the fourth portion 112 is less than the thickness d2 of the third portion 111, a functional layer 13 containing no negative electrode active material can be provided between the negative electrode current collector 11 and the negative electrode active material layer 12. The functional layer 13 includes a fifth portion 131 corresponding to the first portion 121 and a sixth portion 132 corresponding to the second portion 122. The thickness d3 of the sixth portion 132 is less than the thickness d4 of the fifth portion 131. This further increases the amount of negative electrode active material in the negative electrode thinned region 1a, thereby further improving the problem of insufficient CB value in the negative electrode thinned region 1a of the negative electrode sheet 1.
[0084] In some embodiments, as shown in FIG7 , a functional layer 13 not containing a negative electrode active material is provided between the negative electrode current collector 11 and the negative electrode active material layer 12 . The functional layer 13 includes a fifth portion 131 corresponding to the first portion 121 and a sixth portion 132 corresponding to the second portion 122 . The thickness d3 of the sixth portion 132 is less than the thickness d4 of the fifth portion 131 , so as to accommodate at least a portion of the negative electrode active material layer 12 that protrudes toward the negative electrode current collector 11 at the second portion 122 .
[0085] In this way, when the functional layer 13 is coated on the negative electrode current collector 11 and then the negative electrode active material layer 12 is coated on the functional layer 13, since the thickness d3 of the sixth portion 132 is less than the thickness d4 of the fifth portion 131, the negative electrode active material layer 12 needs to fill the thickness of the sixth portion 132 relative to the fifth portion 131 at the second portion 122. This makes it easy to achieve that the second surface 12b protrudes at the second portion 122 relative to the first portion 121 toward the negative electrode current collector 11.
[0086] In the above technical solution, the reduced thickness of the sixth portion 132 of the functional layer 13 relative to the fifth portion 131 can be utilized to achieve an increase in thickness of the negative electrode active material layer 12 in the direction from the negative electrode thinned region 1a toward the negative electrode current collector 11, thereby reducing the difficulty in processing the negative electrode sheet 1. Furthermore, the functional layer 13, which does not contain negative electrode active material, can be utilized to improve other properties of the negative electrode sheet 1.
[0087] Furthermore, in some optional examples, when the thickness d3 of the sixth portion 132 is less than the thickness d4 of the fifth portion 131, there is no need to perform local thinning on the negative electrode current collector 11, which can eliminate the need for special processing of the negative electrode current collector 11, thereby reducing the difficulty and cost of producing the negative electrode sheet 1. However, the present application is not limited thereto. As described above, when the thickness d3 of the sixth portion 132 is less than the thickness d4 of the fifth portion 131, the thickness d1 of the fourth portion 112 of the negative electrode current collector 11 can also be set to be less than the thickness d2 of the third portion 111. This can further increase the amount of negative active material in the negative electrode thinned region 1a, thereby further improving the problem of insufficient CB value in the negative electrode thinned region 1a of the negative electrode sheet 1.
[0088] Specifically, the function of the functional layer 13 is related to the materials it contains, and the corresponding materials can be selected based on the required functions. For example, the functional layer 13 includes a conductive agent and an adhesive, the conductive agent including at least one of SP (conductive carbon black) and CNT (carbon nanotubes), and the adhesive including at least one of PVDF (polyvinylidene fluoride) and SBR (styrene-butadiene latex binder). For example, the functional layer 13 can be a combination of SP and PVDF, a combination of SP and SBR, a combination of CNT and PVDF, a combination of CNT and SBR, and so on, thereby improving the bonding strength of the electrode and preventing decarbonization and powdering. Decarbonization and powdering refers to the problem of negative electrode active material falling off due to weak bonding strength of the electrode during the cycle of the battery cell 10. For another example, the functional layer 13 can be a polymer compound containing a catechol structure. The polymer compound containing a catechol structure is used to prevent oxidation of the negative electrode current collector 11, or to prevent dissolution or precipitation of the negative electrode current collector 11 when charging the lithium-ion battery cell 10 in an over-discharge state. Of course, the present application is not limited to this. For example, the functional layer 13 can also be selected through material selection to serve as a functional layer for alleviating the volume expansion of the negative electrode plate 1 during the charge and discharge cycle, as a functional layer for inhibiting the formation of lithium dendrites, as a functional layer for improving fast charging efficiency, etc., which will not be elaborated here.
[0089] In some embodiments, as shown in FIG3 , a functional layer 13 containing no negative electrode active material is provided between the negative electrode current collector 11 and the negative electrode active material layer 12. The functional layer 13 includes a fifth portion 131 corresponding to the first portion 121 and does not include a portion corresponding to the second portion 122 (e.g., does not include the sixth portion 132 in the embodiment shown in FIG7 ). The functions and optional materials of the functional layer 13 in this embodiment can be found in the previous description and are not further elaborated here.
[0090] In this way, when the functional layer 13 is coated on the negative electrode current collector 11 and then the negative electrode active material layer 12 is coated on the functional layer 13, since it only includes the fifth portion 131 corresponding to the first portion 121 and does not include the portion corresponding to the second portion 122, the negative electrode active material layer 12 needs to fill the missing thickness of the functional layer 13 at the second portion 122, so that the second surface 12b can be easily achieved at the second portion 122 protruding relative to the first portion 121 toward the direction close to the negative electrode current collector 11.
[0091] In the above technical solution, the functional layer 13 can include the fifth portion 131 corresponding to the first portion 121 but not the portion corresponding to the second portion 122, thereby achieving a thickening of the negative electrode active material layer 12 in the direction from the negative electrode thinned region 1a toward the negative electrode current collector 11, thereby reducing the processing difficulty of the negative electrode sheet 1. Furthermore, the functional layer 13, which does not contain negative electrode active material, can be used to improve other properties of the negative electrode sheet 1. In this embodiment, the functions and optional materials of the functional layer 13 can be referred to above and are not further elaborated here.
[0092] Moreover, in some optional examples, when the functional layer 13 includes a fifth part 131 corresponding to the first part 121 and does not include a part corresponding to the second part 122, there is no need to perform local thinning on the negative electrode current collector 11, so that the negative electrode current collector 11 does not require special processing, thereby reducing the production difficulty and production cost of the negative electrode sheet 1.
[0093] Alternatively, in some embodiments of the present application, when the functional layer 13 includes a fifth portion 131 corresponding to the first portion 121 and does not include a portion corresponding to the second portion 122, the negative electrode current collector 11 also includes a third portion 111 corresponding to the first portion 121 and a fourth portion 112 corresponding to the second portion 122, and the thickness d1 of the fourth portion 112 is less than the thickness d2 of the third portion 111. In this way, when the functional layer 13 is coated on the negative electrode current collector 11 and the negative electrode active material layer 12 is then coated on the functional layer 13, the negative electrode active material layer 12 needs to fill the missing thickness of both the functional layer 13 and the negative electrode current collector 11 at the second portion 122, thereby more effectively achieving an increase in thickness of the negative electrode active material layer 12 in the direction from the negative electrode skived region 1a toward the negative electrode current collector 11.
[0094] Alternatively, in some embodiments of the present application, when the functional layer 13 includes a fifth portion 131 corresponding to the first portion 121 and a sixth portion 132 corresponding to the second portion 122, and the thickness d3 of the sixth portion 132 is less than the thickness d4 of the fifth portion 131, and the negative electrode current collector 11 includes a third portion 111 corresponding to the first portion 121 and a fourth portion 112 corresponding to the second portion 122, and the thickness d1 of the fourth portion 112 is less than the thickness d2 of the third portion 111, when the functional layer 13 is coated on the negative electrode current collector 11 and then the negative electrode active material layer 12 is coated on the functional layer 13, the negative electrode active material layer 12 needs to fill the missing thickness of both the functional layer 13 and the negative electrode current collector 11 at the second portion 122, thereby more effectively achieving an increase in thickness of the negative electrode active material layer 12 in the direction from the negative electrode skived region 1a toward the negative electrode current collector 11.
[0095] In the embodiment of the present application, as shown in Figure 3, the portion of the second surface 12b that protrudes at the second portion 122 is the protrusion 123, that is, at least a portion of the second surface 12b at the second portion 122 is the protrusion 123, and the protrusion 123 protrudes relative to the first portion 121 toward the direction close to the negative electrode current collector 11. The protruding thickness of the protrusion 123 is not limited and can be specifically set according to different models of the battery cell 10 to meet different design requirements.
[0096] In some embodiments, as shown in conjunction with FIG3 and FIG8 , the shaded area Z indicates the area where the protrusion 123 is located. There may be only one protrusion 123, and the length direction of the protrusion 123 extends along the second direction Y of the negative electrode sheet 1. In the above technical solution, since the protrusion 123 extends continuously along the second direction Y of the negative electrode sheet 1, the processing of the negative electrode sheet 1 can be facilitated, and the lithium deposition phenomenon in the negative electrode thinned area 1a of the negative electrode sheet 1 can be more effectively improved.
[0097] For example, when the protrusion 123 extends continuously along the second direction Y of the negative electrode sheet 1, with reference to FIG8 , in the second direction Y of the negative electrode sheet 1, the distance L1 between the farthest ends of the protrusion 123 is greater than 90% of the dimension L of the negative electrode sheet 1. In the above technical solution, the protrusion 123 can occupy a larger area in the second direction Y of the negative electrode sheet 1, thereby effectively improving the lithium deposition phenomenon in the negative electrode thinned area 1a of the negative electrode sheet 1.
[0098] Alternatively, in some embodiments, as shown in FIG3 and FIG8 , the shaded area Z indicates the area where the protrusion 123 is located. The protrusion 123 may be multiple and spaced apart along the second direction Y of the negative electrode plate 1. In the above technical solution, since the protrusion 123 extends discontinuously along the second direction Y of the negative electrode plate 1, the lithium deposition phenomenon in the negative electrode thinned area 1a of the negative electrode plate 1 is improved to a certain extent, the material of the negative electrode active material layer 12 is saved, and the cost of the negative electrode plate 1 is reduced.
[0099] For example, when the protrusions 123 extend discontinuously along the second direction Y of the negative electrode sheet 1, with reference to FIG9 , in the second direction Y of the negative electrode sheet 1, the distance L2 between the farthest ends of the two protrusions 123 furthest apart is greater than 70% of the dimension L of the negative electrode sheet 1. In the above technical solution, the protrusions 123 can occupy a larger area in the second direction Y of the negative electrode sheet 1, thereby effectively improving lithium deposition in the negative electrode thinned region 1a of the negative electrode sheet 1.
[0100] In the embodiments of the present application, the negative electrode active material layer 12 can be a single-layer structure or a multi-layer structure. When the negative electrode active material layer 12 is a multi-layer structure, it can be two layers, three layers or more. For example, the following only takes the negative electrode active material layer 12 as a two-layer structure as examples of some embodiments.
[0101] In some embodiments of the present application, as shown in FIG10 , the negative electrode active material layer 12 includes a first active material layer 1201 and a second active material layer 1202. The dispersion concentration of the negative electrode active material in the first active material layer 1201 is greater than the dispersion concentration of the negative electrode active material in the second active material layer 1202. The first active material layer 1201 is disposed on a side of the second active material layer 1202 away from the negative electrode current collector 11. The second active material layer 1202 is eliminated at the second portion 122, i.e., the second active material layer 1202 is eliminated at the second portion 122 to retain only the first active material layer 1201. In other words, the thickness of the second active material layer 1202 at the second portion 122 is zero micrometers, so that the second portion 122 only includes the first active material layer 1201 having a relatively high dispersion concentration of the negative electrode active material.
[0102] In this way, only two layers of slurry with different dispersion concentrations of negative electrode active materials need to be coated, wherein the dispersion concentration of the negative electrode active material of the bottom slurry is relatively low and is eliminated in the negative electrode thinning area 1a, while the dispersion concentration of the negative electrode active material of the top slurry is relatively high and fills the part of the negative electrode thinning area 1a that is eliminated by the bottom slurry. In this way, it is easy to achieve that the dispersion concentration of the negative electrode active material in the negative electrode active material layer 12 in the second part 122 is greater than the dispersion concentration in the first part 121, thereby increasing the negative electrode active material in the negative electrode thinning area 1a and improving the problem of insufficient CB value in the negative electrode thinning area 1a.
[0103] For example, when preparing the slurry, the binder content of the first active material layer 1201 can be set to a relatively low proportion, but the proportion of the negative electrode active material can be relatively large, while the binder content of the second active material layer 1202 can be set to a relatively high proportion, but the proportion of the negative electrode active material can be relatively small. Compared with the second active material layer 1202, the first active material layer 1201 has a lower resistivity and better kinetics. By canceling the second active material layer 1202 in the negative electrode thinning area 1a, the negative electrode thinning area 1a is entirely filled with the first active material layer 1201 with a relatively large proportion of negative electrode active material and relatively low resistivity, which is beneficial to improving the problem of insufficient CB value in the negative electrode thinning area 1a.
[0104] In addition, the negative electrode active materials in the first active material layer 1201 and the second active material layer 1202 are not limited. For example, at least one of artificial graphite, natural graphite, hard carbon, and silicon carbon can be selected, which will not be described in detail here.
[0105] In some embodiments of the present application, when the second active material layer 1202 is eliminated from the second portion 122 to retain only the first active material layer 1201, it is not necessary to provide: at least a portion of the second surface 12b at the second portion 122 is protruded toward the negative electrode current collector 11 relative to the first portion 121. In this way, the problem of insufficient CB value at the negative electrode skived area 1a can be alleviated to a certain extent, while reducing the difficulty of processing the negative electrode sheet 1 and improving the processing efficiency of the negative electrode sheet 1.
[0106] However, in other embodiments of the present application, when the second active material layer 1202 is eliminated from the second portion 122 to retain only the first active material layer 1201, it is also possible to simultaneously configure: at least a portion of the second surface 12b in the second portion 122 protrudes toward the negative electrode current collector 11 relative to the first portion 121. That is, in this case, only the first active material layer 1201 in the second portion 122 protrudes toward the negative electrode current collector 11. This not only increases the active material dispersion concentration in the second portion 122 but also increases the thickness of the second portion 122, which can more effectively improve the problem of insufficient CB value in the negative electrode skived region 1a.
[0107] In an embodiment of the present application, the second surface 12b includes a first face 12b1 and a second face 12b2, that is, the second surface 12b of the negative electrode active material layer 12 (that is, the side surface close to the negative electrode current collector 11) includes the first face 12b1 defined by the first active material layer 1201 in the second part 122, and the second face 12b2 defined by the second active material layer 1202 in the first part 121. More specifically, the first face 12b1 is the side surface of the first active material layer 1201 in the second part 122 close to the negative electrode current collector 11, and the second face 12b2 is the side surface of the second active material layer 1202 in the first part 121 close to the negative electrode current collector 11.
[0108] In some examples, as shown in FIG10 , the first surface 12b1 defined by the first active material layer 1201 is flush with the second surface 12b2 defined by the second active material layer 1202 . In this case, the second surface 12b of the negative electrode active material layer 12 is entirely planar, thereby facilitating processing.
[0109] In other examples, as shown in FIG11 , the first surface 12b1 defined by the first active material layer 1201 protrudes toward the negative electrode current collector 11 relative to the second surface 12b2 defined by the second active material layer 1202. For example, this can be achieved by eliminating the functional layer 13 in the negative electrode skived region 1a or thinning the negative electrode current collector 11 in the negative electrode skived region 1a. In this case, not only does the second surface 12b protrude toward the negative electrode current collector 11 relative to the first surface 121 at the second portion 122, but the dispersion concentration of the negative active material in the negative electrode active material layer 12 in the second portion 122 is greater than that in the first portion 121. This allows for a greater increase in the amount of negative active material in the negative electrode skived region 1a, more effectively addressing the issue of insufficient CB value in the negative electrode skived region 1a.
[0110] In some embodiments of the present application, as shown in FIG3 , the second surface 12b at the second portion 122 is formed as a plane parallel to the thickness center plane S of the negative electrode current collector 11. That is, the second surface 12b at the second portion 122 protrudes as a whole toward the negative electrode current collector 11 and has a uniform protruding thickness. This facilitates processing and allows the negative electrode active material layer 12 to be fully and comprehensively thickened in the negative electrode thinning region 1a toward the negative electrode current collector 11, thereby increasing the amount of negative electrode active material in the negative electrode thinning region 1a, improving the problem of insufficient CB value in the negative electrode thinning region 1a of the negative electrode sheet 1, and improving the phenomenon of lithium deposition in the negative electrode thinning region 1a of the negative electrode sheet 1 after long cycles. This can further improve the problem of capacity drop of the battery 100 and electrode sheet cracking caused by lithium deposition, thereby extending the service life and reliability of the battery cell 10.
[0111] In some embodiments of the present application, as shown in FIG3 , the second surface 12 b and the first surface 12 a are both formed as planes parallel to the thickness center plane S of the negative electrode current collector 11 at the first portion 121. Thus, the first portion 121 can have a uniform thickness, thereby facilitating the processing of the negative electrode active material layer 12 and significantly improving the performance of the negative electrode sheet 1.
[0112] It is understood that, as shown in FIG3 , along the first direction X of the negative electrode sheet 1 , the width W1 of the first portion 121 is greater than the width W2 of the second portion 122 . For example, the width W2 of the second portion 122 may be 10 mm to 15 mm, for example, W2 is 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, etc. Thus, on the one hand, the performance of the negative electrode sheet 1 can be more effectively improved, and on the other hand, the lithium deposition phenomenon in the negative electrode thinned area 1 a of the negative electrode sheet 1 can be more effectively improved.
[0113] In some embodiments of the present application, as shown in FIG3 , the negative electrode sheet 1 is formed into a bilaterally symmetrical structure. That is, the negative electrode sheet 1 is symmetrical about the thickness center plane S of the negative electrode current collector 11, and thus the negative electrode current collector 11 itself is symmetrical about the thickness center plane S of the negative electrode current collector 11. The functional layers 13 on both sides of the negative electrode current collector 11 are symmetrical about the thickness center plane S of the negative electrode current collector 11, and the negative active material layers 12 on both sides of the negative electrode current collector 11 are symmetrical about the thickness center plane S of the negative electrode current collector 11. In the above technical solution, the processing of the negative electrode sheet 1 is facilitated, and it is conducive to uniformly improving the problem of insufficient CB value of each negative electrode thinned area 1a. The improvement effect is consistent, which can better improve the service life and reliability of the battery cell 10.
[0114] In some embodiments, the present application further provides a battery cell 10, which includes at least one electrode assembly 101. As shown in Figures 3 and 5, the electrode assembly 101 includes a positive electrode sheet 2, a separator 3, and a negative electrode sheet 1 of any of the above embodiments. The separator 3 is disposed between the positive electrode sheet 2 and the negative electrode sheet 1. The area of the negative electrode sheet 1 corresponding to the first portion 121 is the negative electrode non-thinned area 1b, and the area of the negative electrode sheet 1 corresponding to the second portion 122 is the negative electrode thinned area 1a. The positive electrode sheet 2 includes a positive electrode current collector 21 and a positive electrode active material layer 22 disposed on the positive electrode current collector 21. The positive electrode sheet 2 includes a positive electrode non-thinned area 2b and a positive electrode thinned area 2a arranged along a first direction X. The positive electrode thinned area 2a is disposed corresponding to the negative electrode non-thinned area 1b, and the negative electrode thinned area 1a is disposed corresponding to the positive electrode non-thinned area 2b.
[0115] During the manufacture of the electrode assembly 101, since the negative electrode skived region 1a of the negative electrode sheet 1 faces the positive electrode non-skived region 2b of the positive electrode sheet 2, the negative electrode sheet 1 of the present embodiment is modified in the skived region 1a to thicken the negative electrode active material layer 12 in the direction toward the negative electrode current collector 11, and / or to increase the concentration of the negative electrode active material in the negative electrode active material layer 12 in the skived region 1a. This increases the amount of negative electrode active material in the skived region 1a, improves the problem of insufficient CB value in the skived region 1a of the negative electrode sheet 1, and improves the phenomenon of lithium deposition in the skived region 1a of the negative electrode sheet 1 after long cycles. This further improves the problem of capacity drop of the battery 100 and electrode sheet cracking caused by lithium deposition, thereby extending the service life and reliability of the battery cell 10. Furthermore, since only a portion of the negative electrode sheet 1 is modified, the cost of the negative electrode sheet 1 is substantially not increased.
[0116] In addition, as described above, the present application also proposes a battery 100 including the above-mentioned battery cell 10. The battery 100 may include a box body 20 or may not include a box body 20. There may be multiple battery cells 10, so that the battery 100 has a higher power capacity and the service life and reliability of the battery 100 can be improved.
[0117] In addition, as described above, the present application also proposes an electrical device including the above-mentioned battery cell 10. The type of the electrical device is not limited. By setting the above-mentioned battery cell 10, the electrical device can improve the battery life and working reliability of the electrical device.
[0118] Next, a battery cell 10 according to a specific embodiment of the present application is described.
[0119] The battery cell 10 includes a housing, an electrode assembly 101 and an electrolyte. The housing is used to contain the electrode assembly 101 and the electrolyte. The electrode assembly 101 is composed of a positive electrode sheet 2, a negative electrode sheet 1 and a separator 3.
[0120] The negative electrode sheet 1 includes a negative electrode current collector 11 and a negative electrode active material layer 12 disposed on the negative electrode current collector 11. The negative electrode sheet 1 includes a negative electrode non-thinned area 1b and a negative electrode thinned area 1a. Along the first direction X of the negative electrode sheet 1, the negative electrode thinned area 1a is located on the side of the negative electrode non-thinned area 1b near the negative electrode tab area 14. The positive electrode sheet 2 includes a positive electrode current collector 21 and a positive electrode active material layer 22 disposed on the positive electrode current collector 21. The positive electrode sheet 2 includes a positive electrode non-thinned area 2b and a positive electrode thinned area 2a. Along the first direction X, the positive electrode thinned area 2a is located on the side of the positive electrode non-thinned area 2b near the positive electrode tab area 23. When the electrode assembly 101 is assembled, the positive electrode thinned area 2a corresponds to the negative electrode non-thinned area 1b, and the negative electrode thinned area 1a corresponds to the positive electrode non-thinned area 2b.
[0121] 3 , a functional layer 13 is provided between the negative electrode current collector 11 and the negative electrode active material layer 12 in the negative electrode non-thinning area 1b, and the outer surface of the negative electrode active material layer 12 is gradually inclined toward the direction close to the negative electrode current collector 11 in the negative electrode thinning area 1a, and the inner surface of the negative electrode active material layer 12 is convex as a whole toward the direction close to the negative electrode current collector 11 in the negative electrode thinning area 1a, so that the negative electrode active material layer 12 is thinned on the outside but thickened on the inside in the negative electrode thinning area 1a, thereby increasing the negative electrode active material in the negative electrode thinning area 1a, improving the problem of insufficient CB value in the negative electrode thinning area 1a of the negative electrode sheet 1, and improving the phenomenon of lithium deposition in the negative electrode thinning area 1a of the negative electrode sheet 1 after long cycles, thereby improving the problem of capacity diving of the battery 100 and electrode sheet cracking caused by the lithium deposition phenomenon, thereby extending the service life and reliability of the battery cell 10. Moreover, since only a part of the negative electrode plate 1 is improved, the cost of the negative electrode plate 1 will basically not be increased.
[0122] Specifically, the size and width of the functional layer 13 can be controlled so that it is 10mm-15mm narrower than the width of the negative active material layer 12. During processing, the functional layer 13 is primed on the negative current collector 11 according to the above size, and then the negative active material layer 12 is normally coated on it to obtain a negative electrode sheet 1 with more negative active material in the negative electrode thinning area 1a. The above-mentioned negative electrode sheet 1 is cold pressed according to a certain compression to obtain a cold-pressed negative electrode sheet 1. The above-mentioned negative electrode sheet 1 and positive electrode sheet 2 are striped, wound, and flattened to obtain an electrode assembly 101 with a through hole in the safety margin area (for example, as shown in Figure 14). The above-mentioned electrode assembly 101 is subjected to processes such as current collecting plate welding and end cover welding to finally obtain a battery cell 10.
[0123] Below, three embodiments and three comparative examples of the present application are introduced.
[0124] Example 1
[0125] Preparation of positive electrode sheets: The positive electrode active material lithium iron phosphate with a Dv50 of 1.05μm, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are dissolved in the solvent N-methylpyrrolidone (NMP) in a mass ratio of 97:0.8:2.2, and the mixture is fully stirred to obtain a slurry of the positive electrode active material layer. The slurry of the positive electrode active material layer is passed through a sieve and coated on the positive electrode current collector, dried at 110℃-120℃, and rolled and cut to obtain the positive electrode sheets.
[0126] Preparation of the negative electrode sheet: Referring to Figure 10 , a slurry for the functional layer 13 was prepared by mixing the conductive agent acetylene black, the binder styrene butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC) in a ratio of 65%, 30%, and 5% by mass. This slurry was then applied to the copper foil of the negative current collector 11. Artificial graphite (a negative electrode active material with a Dv50 of 12.3 μm), the conductive agent acetylene black, the binder styrene butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC) in a mass ratio of 96.5:0.7:1.8:1 were dissolved in deionized water and mixed thoroughly to obtain a slurry for the second active material layer 1202. Artificial graphite (a negative electrode active material with a Dv50 of 12.3 μm), the conductive agent acetylene black, the binder styrene butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose in a mass ratio of 96.9:0.7:1.4:1 were dissolved in deionized water and mixed thoroughly to obtain a slurry for the first active material layer 1201. The slurry of the first active material layer 1201 and the slurry of the second active material layer 1202 are simultaneously passed through a screen and coated on the negative electrode current collector 11 coated with the functional layer 13, wherein the slurry of the second active material layer 1202 is on the lower layer and the slurry of the first active material layer 1201 is on the upper layer. The thickness t1 of the first active material layer 1201 in the negative electrode non-thinning area 1b and the thickness t2 of the second active material layer 1202 in the negative electrode non-thinning area 1b are both 36 μm, the width W1 of the negative electrode thinning area 1a is 10 mm, the thickness of the second active material layer 1202 in the negative electrode thinning area 1a is zero micron, the thickness of the first active material layer 1201 in the negative electrode thinning area 1a gradually decreases in the direction away from the negative electrode non-thinning area 1b, and the thickness t3 of the first active material layer 1201 at the center of the width of the negative electrode thinning area 1a (that is, 5 mm away from the width W3 of the negative electrode non-thinning area 1b) is 68 μm.
[0127] Assembly of battery cells: stack the positive electrode sheet, separator, and negative electrode sheet in order, so that the separator is between the positive electrode sheet and the negative electrode sheet and can isolate the positive electrode sheet from the negative electrode sheet. Then wind the stacked components to obtain an electrode assembly, place the electrode assembly in the outer shell of the battery cell, inject the electrolyte after drying, and obtain the battery cell after processes such as formation and standing.
[0128] Example 2
[0129] As shown in FIG11 , the difference between Example 2 and Example 1 is that the functional layer 13 of the negative electrode thinned area 1 a is removed.
[0130] Example 3
[0131] As shown in Figure 12, the difference between Example 3 and Example 1 is that the functional layer 13 of the negative electrode thinning area 1a is cancelled, but the second active material layer 1202 of the negative electrode thinning area 1a is not cancelled. Instead, the thickness of the second active material layer 1202 in the negative electrode thinning area 1a is set to gradually decrease along the direction close to the negative electrode thinning area 1a, and the thickness t4 of the second active material layer 1202 at the center position of the width of the negative electrode thinning area 1a (that is, 5 mm away from the width W3 of the negative electrode non-thinning area 1b) is 34 μm.
[0132] Comparative Example 1:
[0133] As shown in Figure 13, the difference between Comparative Example 1 and Example 1 is that the second active material layer 1202 in the negative electrode thinning area 1a is not cancelled, but the thickness of the second active material layer 1202 in the negative electrode thinning area 1a is set to gradually decrease along the direction close to the negative electrode thinning area 1a, and the thickness t4 of the second active material layer 1202 at the center position of the width of the negative electrode thinning area 1a (that is, 5 mm away from the width W3 of the negative electrode non-thinning area 1b) is 34 μm.
[0134] Comparative Example 2:
[0135] The difference between Comparative Example 2 and Comparative Example 1 is that the slurry of the second active material layer 1202 is the same as the slurry of the first active material layer 1201, both of which are negative electrode active material artificial graphite with a Dv50 of 12.3 μm, conductive agent acetylene black, binder styrene-butadiene rubber, and thickener sodium carboxymethyl cellulose, dissolved in solvent deionized water in a mass ratio of 96.9:0.7:1.4:1 to obtain a slurry.
[0136] Comparative Example 3:
[0137] The difference between Comparative Example 3 and Comparative Example 1 is that the slurry of the second active material layer 1202 is the same as the slurry of the first active material layer 1201, both of which are negative electrode active material artificial graphite with a Dv50 of 12.3 μm, conductive agent acetylene black, binder styrene-butadiene rubber, and thickener sodium carboxymethyl cellulose, dissolved in solvent deionized water in a mass ratio of 96.5:0.7:1.8:1 to obtain a slurry.
[0138] It is understandable that the greater the resistance, the greater the polarization, the worse the kinetics, and the easier it is to precipitate lithium; conversely, the smaller the resistance, the smaller the polarization, the better the kinetics, and the less likely it is to precipitate lithium. Therefore, this application uses a diaphragm resistance test method to judge the lithium precipitation situation in the negative electrode thinning area. Cut a 20cm length of the negative electrode thinning area 1a along the second direction of the negative electrode pole piece 1 as the diaphragm to be tested, and test it with a resistance meter. The test temperature is 25°C. The specific test method is to use two probes of the resistance meter for testing, place the diaphragm to be tested between the two probes of the resistance meter, set the same test pressure to 2MPa, hold the pressure for 5s, measure the resistance of the diaphragm to be tested, and then take the average value of 5 points at the width center of the negative electrode thinning area 1a and evenly distributed along the second direction of the negative electrode pole piece 1 to obtain the average resistance (mΩ) of the diaphragm to be tested.
[0139] Furthermore, it is understood that lithium deposition in the negative electrode skived area 1a can cause cycle degradation. Improving this can improve cycle life, so cycling tests were also conducted. The cycling test conditions were: charging at 0.5C from 2.5C to 3.65V, and discharging at 0.5C to 2.5V at 25°C, where C represents the nominal capacity of the battery. "Cycles @ 80% SOH" indicates the number of full charge and discharge cycles required to achieve 80% of the initial capacity, with one full charge and discharge cycle being considered. "SOH" indicates the battery's ability to store charge. The test results are shown in the table below.
[0140] From the comparison of the test results in the above table, it can be seen that the resistance of the negative electrode thinned area 1a in Examples 1, 2, and 3 is relatively low, which is beneficial for solving the lithium deposition problem in the negative electrode thinned area 1a. Moreover, in Example 2, when the second active material layer 1202 of the functional layer 13 of the negative electrode thinned area 1a is simultaneously removed, the resistance of the negative electrode thinned area 1a is relatively lower, which is more beneficial for solving the lithium deposition problem in the negative electrode thinned area 1a and has a good effect on improving the cycle life. However, the resistance of the negative electrode thinned area 1a in Comparative Examples 1, 2, and 3 is relatively high, which cannot solve the lithium deposition problem in the negative electrode thinned area 1a and has a relatively obvious cycle attenuation problem.
[0141] It should be noted that, unless there is any conflict, the embodiments and features in the embodiments of this application can be combined with each other.
[0142] The above are merely preferred embodiments of the present application and are not intended to limit the present application. Those skilled in the art will readily appreciate that various modifications and variations are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present application shall be included within the scope of protection of the present application.
Claims
1. A negative electrode plate of a battery cell, wherein: include: A negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, wherein two side surfaces of the negative electrode active material layer are respectively a first surface away from the negative electrode current collector and a second surface close to the negative electrode current collector, the negative electrode active material layer comprises a first portion and a second portion, the second portion is located on a side of the first portion close to an edge of the negative electrode electrode sheet in a first direction of the negative electrode sheet, and the first surface is offset toward the negative electrode current collector at the second portion relative to the first portion; Wherein, the negative electrode plate is constructed such that: at least a portion of the second surface at the second portion protrudes toward the negative electrode collector relative to the first portion, and / or the dispersion concentration of the negative electrode active material in the negative electrode active material layer in the second portion is greater than the dispersion concentration in the first portion.
2. The negative electrode sheet of the battery cell according to claim 1, wherein: The negative electrode current collector includes a third portion corresponding to the first portion and a fourth portion corresponding to the second portion, wherein the fourth portion has a thickness smaller than that of the third portion to accommodate at least a portion of the negative active material layer protruding toward the negative electrode current collector at the second portion.
3. The negative electrode sheet of the battery cell according to claim 1 or 2, wherein: A functional layer not containing negative electrode active material is provided between the negative electrode collector and the negative electrode active material layer, and the functional layer includes a fifth part corresponding to the first part and a sixth part corresponding to the second part, and the thickness of the sixth part is less than the thickness of the fifth part, so as to accommodate at least a part of the negative electrode active material layer protruding toward the negative electrode collector at the second part.
4. The negative electrode sheet of the battery cell according to claim 1, wherein: A functional layer containing no negative electrode active material is disposed between the negative electrode current collector and the negative electrode active material layer, and the functional layer includes a fifth portion corresponding to the first portion and does not include a portion corresponding to the second portion.
5. The negative electrode sheet of the battery cell according to claim 3 or 4, wherein: The functional layer includes a conductive agent and an adhesive, wherein the conductive agent includes at least one of SP and CNT, and the adhesive includes at least one of PVDF and SBR.
6. The negative electrode sheet of a battery cell according to any one of claims 1 to 5, wherein: The portion of the second surface protruding at the second portion is a protrusion, there is one protrusion and the length direction of the protrusion extends along the second direction of the negative electrode plate.
7. The negative electrode sheet of a battery cell according to any one of claims 1 to 5, wherein: The portion of the second surface protruding at the second portion is a protrusion, and there are multiple protrusions and they are arranged at intervals along the second direction of the negative electrode plate.
8. The negative electrode sheet of a battery cell according to any one of claims 1 to 7, wherein: The negative electrode active material layer includes a first active material layer and a second active material layer, the dispersion concentration of the negative electrode active material in the first active material layer is greater than the dispersion concentration of the negative electrode active material in the second active material layer, the first active material layer is arranged on a side of the second active material layer away from the negative electrode current collector, and the second active material layer is eliminated at the second part to retain only the first active material layer.
9. A battery cell, wherein: It includes a positive electrode plate, a separator and a negative electrode plate of a battery cell according to any one of claims 1 to 8, the separator is arranged between the positive electrode plate and the negative electrode plate, the area of the negative electrode plate corresponding to the first part is the negative electrode non-thinning area, the area of the negative electrode plate corresponding to the second part is the negative electrode thinning area, the positive electrode plate includes a positive electrode collector and a positive electrode active material layer arranged on the positive electrode collector, the positive electrode plate includes a positive electrode non-thinning area arranged along the first direction, the positive electrode thinning area is arranged corresponding to the negative electrode non-thinning area, and the negative electrode thinning area is arranged corresponding to the positive electrode non-thinning area.
10. The battery cell according to claim 9, wherein: The battery cell is a wound cylinder.
11. A battery, wherein: Comprising the battery cell according to claim 9 or 10.
12. An electrical device, wherein: Comprising the battery cell according to claim 9 or 10.
Citation Information
Patent Citations
Negative pole piece as well as preparation method thereof, and lithium ion battery
CN108258193A
Electrode pole piece and electrochemical device comprising same
CN110010902A
Current collector, preparation method thereof and pole piece
CN113066986A
Electrode assembly, manufacturing method and manufacturing system thereof, battery cell, and battery
CN115606020A
Current collector, negative pole piece and lithium ion battery
CN212461733U