Sodium battery cell, secondary battery and electrical device
By introducing a liquid-retaining pad between the isolation film and the negative electrode sheet in the sodium battery cell, the electrolyte consumption and safety problems caused by volume expansion of the sodium battery are solved, and the battery cycle life is extended and the SOC is uniformed. , improving the overall performance of the battery.
Patent Information
- Application Number
- PCT/CN2024/072049
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-01-12
- Publication Date
- 2024-10-31
AI Technical Summary
In sodium batteries, the electrolyte is continuously consumed due to the volume expansion of the positive and negative electrode materials, which affects the safety performance and life of the battery.
A liquid-retaining pad is introduced into the sodium battery cell, which is located between the isolation film and the negative electrode sheet. It is used to store the electrolyte in advance and release the electrolyte during the charge and discharge process, supplement the insoluble by-product reaction at the positive and negative electrode interface, and reduce adverse interface reactions. occurrence, extending the cycle life of the battery.
The design of the liquid-retaining pad effectively alleviates the safety issues and electrolyte consumption caused by the volume expansion of sodium batteries, improves the cycle life of the battery, reduces the probability of internal SOC non-uniformity, and enhances the overall stability of the battery. performance.
Smart Images

Figure CN2024072049_31102024_PF_FP_ABST
Abstract
Description
Sodium battery cells, secondary batteries and electrical equipment
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 2023104830388, filed on April 28, 2023, entitled “Sodium Battery Cells, Secondary Batteries and Electrical Equipment,” the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to the field of batteries, and in particular to a sodium battery cell, a secondary battery and an electrical device. Background Art
[0004] As the application of lithium-ion battery technology in markets such as consumer electronics, electric vehicles, and energy storage continues to expand, the issue of lithium resource shortages has become increasingly prominent. Sodium batteries, due to their abundant sodium reserves, have gradually attracted attention and hold a strategic position in cost-sensitive applications such as energy storage. Furthermore, sodium batteries offer 20% higher conductivity than lithium batteries at the same electrolyte concentration, further reducing production costs.
[0005] However, due to the higher reduction potential and larger relative molecular mass of metallic sodium compared to metallic lithium, the energy density of sodium batteries with similar working principles is significantly lower than that of lithium batteries. At the same time, sodium ions have a larger ionic radius than lithium ions, which also makes the volume expansion associated with their insertion and extraction in the positive and negative electrode materials larger. The volume expansion affects the safety performance of the sodium battery and causes the electrolyte to be continuously consumed, which in turn degrades the cycle performance of the sodium battery and ultimately affects the battery life.
[0006] Summary of the Invention
[0007] In view of the above problems, the present application provides a sodium battery cell, a secondary battery and an electrical device, which can alleviate the safety issues caused by volume expansion during the use of sodium batteries and the problem of electrolyte consumption affecting battery life.
[0008] In a first aspect, the present application provides a sodium battery cell, the sodium battery cell comprising:
[0009] negative electrode;
[0010] Positive electrode;
[0011] electrolyte;
[0012] A separator; the separator is located between the positive electrode sheet and the negative electrode sheet;
[0013] Wherein, a liquid retaining pad is provided between at least part of the isolation membrane and the negative electrode plate.
[0014] In the technical solution of the embodiment of the present application, the present application chooses to arrange a liquid-retaining pad between the isolation membrane and the negative electrode plate. This is because during the battery cycle, there is always a part of the sodium ions that cannot be completely released from the negative electrode and are deposited on the surface of the negative electrode plate as insoluble by-products. The insoluble by-products need to continuously consume the electrolyte, causing the problem of continuous consumption of the electrolyte.
[0015] Moreover, the liquid retaining pad has the ability to retain liquid, so that when the battery cell is filled with liquid, the liquid retaining pad can store part of the electrolyte in advance. Subsequently, as the battery charge and discharge cycle proceeds, the positive and negative electrode materials expand and continuously consume the electrolyte. The electrolyte stored in the liquid retaining pad is released in a timely and effective manner to replenish the electrolyte. On the one hand, the replenished electrolyte can ensure that the insoluble by-products at the positive and negative electrode interfaces continue to react, but reduce the safety problems caused by adverse reactions on the interface. On the other hand, sufficient electrolyte reduces the probability of forming a "dry area" inside the battery, which is beneficial to ensure the uniformity of the SOC in the battery, thereby improving the cycle life of the battery.
[0016] The above “at least part” includes any one or more liquid-retaining pads, that is, the liquid-retaining and liquid-releasing functions can be achieved by arranging more than one liquid-retaining pad, and each liquid-retaining pad is arranged between the isolation membrane and the negative electrode.
[0017] In some embodiments, the liquid-retaining pad comprises micropores, and the pore size of the micropores is 3 μm to 25 μm.
[0018] The liquid-retaining pad with the above-mentioned micropores in the present application provides a channel for storing electrolyte in advance and releasing electrolyte.
[0019] In some embodiments, the volume percentage of pores with a diameter of 3 μm to 5 μm is 10% to 50%; the volume percentage of pores with a diameter of 5 μm < 9 μm is 30% to 70%, and the rest is other pore sizes.
[0020] This application improves the uniformity of micropore diameter, which is conducive to achieving the technical effect of storing and releasing electrolyte in advance.
[0021] In some embodiments, the porosity of the liquid-retaining pad is 35% to 65%.
[0022] The liquid-retaining pad of the present application having the above-mentioned porosity is conducive to achieving the technical effect of storing electrolyte in advance and releasing electrolyte.
[0023] In some embodiments, the porosity of the liquid-retaining pad is 40% to 65%.
[0024] The liquid-retaining pad of the present application having the above-mentioned porosity is conducive to further achieving the technical effect of storing and releasing the electrolyte in advance.
[0025] In some embodiments, the porosity of the liquid-retaining pad is 55% to 65%.
[0026] The liquid-retaining pad of the present application having the above-mentioned porosity releases electrolyte to improve the wettability of the isolation membrane when the positive and negative electrode materials expand and continuously consume the electrolyte, thereby reducing safety issues caused by adverse interfacial reactions and increasing the cycle life of the battery.
[0027] In some embodiments, the material of the liquid-retaining pad includes at least one of polyolefin, polyester, polyimide, glass fiber, and super absorbent resin.
[0028] In some embodiments, the polyolefin comprises any one of polyethylene, polypropylene, or polypropylene.
[0029] In some embodiments, the polyester comprises a thermoplastic polyester, and the thermoplastic polyester comprises any one of polyethylene terephthalate and polybutylene terephthalate.
[0030] In some embodiments, the polyimide comprises thermoplastic polyimide, and the thermoplastic polyimide comprises any one of pyrophthalic anhydride-type polyimide, ether anhydride-type polyimide, ketone anhydride-type polyimide, or fluoroanhydride-type polyimide.
[0031] The super absorbent resin comprises any one of polyacrylate, sodium polyacrylate, starch sodium acrylate polymer, and polyvinyl alcohol.
[0032] In some embodiments, the glass fiber includes any one of alkali-free fiber and high-alkali fiber.
[0033] In the present application, raw materials containing the above materials are used to prepare a liquid-retaining pad through a film-forming process.
[0034] In some embodiments, the material of the liquid-retaining pad includes any one of thermoplastic polyester, polyimide, and glass fiber.
[0035] The raw materials of the above materials in the present application are advantageous for preparing a liquid-retaining pad through a simple and operable film-forming process.
[0036] The raw materials of the present application having the above-mentioned materials are convenient for preparing the liquid-retaining pad through a simple and operable film-forming process, and are also conducive to achieving the above-mentioned uniform pore size and porosity.
[0037] In some embodiments, the thickness of the liquid-retaining pad is 100 μm to 3000 μm.
[0038] The thickness of the liquid-retaining pad in this application affects the amount of electrolyte it stores and ultimately affects the battery performance. When designing the thickness of the liquid-retaining pad, both battery performance and battery preparation process must be considered. This application selects the above range value based on comprehensive considerations of these two dimensions.
[0039] In some embodiments, the thickness of the liquid-retaining pad is 500 μm to 3000 μm.
[0040] The liquid-retaining pad of the present application with the above-mentioned thickness can conveniently and more effectively improve the battery safety and cycle life, provided that the battery preparation process is operable.
[0041] In some embodiments, the thickness of the liquid-retaining pad is 1000 μm to 3000 μm.
[0042] The liquid-retaining pad of the present application with the above-mentioned thickness can relatively better improve the battery safety problem and cycle life under the premise that the battery preparation process is operable.
[0043] In some embodiments, the elastic modulus of the liquid-retaining pad is 500 MPa to 86,000 MPa.
[0044] The elastic modulus of the liquid-retaining pad designed in the present application has a relatively large range of values, which is designed in combination with the material and pore structure of the liquid-retaining pad.
[0045] In some embodiments, the elastic modulus of the liquid-retaining pad is 3000 MPa to 50000 MPa.
[0046] The liquid-retaining pad of the present application with the above-mentioned elastic modulus can effectively release the electrolyte to improve the wettability of the isolation membrane when the positive and negative electrode materials expand and continuously consume the electrolyte, thereby reducing the safety problems caused by adverse interface reactions and improving the cycle life of the battery.
[0047] In some embodiments, the elastic modulus of the liquid-retaining pad is 15,000 MPa to 50,000 MPa.
[0048] The liquid-retaining pad of the present application having the above elastic modulus can relatively better improve battery safety issues and cycle life.
[0049] In some embodiments, the battery cell includes a laminated battery cell and a wound battery cell, wherein both the laminated battery cell and the wound battery cell can ensure that the liquid retaining pad can achieve the liquid retaining and releasing functions, but from the perspective of process preparation, the liquid retaining pad is easier to arrange in the laminated battery cell, that is, it is more conducive to exerting its excellent liquid retaining and releasing functions.
[0050] In some embodiments, the battery cell is preferably a laminated battery cell.
[0051] In some embodiments, the number of the liquid-retaining pads is m, and m is a positive integer greater than or equal to 1.
[0052] The present application describes here that a liquid retaining pad is designed between the isolation membrane and the negative electrode plate, because designing a liquid retaining pad between the isolation membrane and the negative electrode plate is sufficient to ensure the liquid retaining and liquid release capabilities. If there are more than two liquid retaining pads, the two or more liquid retaining pads can be arranged between adjacent isolation membranes and negative electrode plates, or they can be arranged non-adjacently. The number of liquid retaining pads is affected by battery performance.
[0053] In a second aspect, the present application provides a secondary battery comprising the battery cell according to the first aspect. The safety and cycle life of the secondary battery are improved compared to batteries without a liquid retaining pad.
[0054] In a third aspect, the present application provides an electrical device comprising the secondary battery described in the second aspect or the battery cell described in the first aspect. The electrical device can be used as a power source or as an energy storage unit, and has relatively promising application prospects in the power and / or energy storage fields.
[0055] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to denote the same components. In the drawings:
[0057] FIG1 is a schematic diagram showing the positional relationship between the liquid retaining pad, the electrode, and the isolation membrane in some embodiments of the present application;
[0058] FIG2 is a schematic structural diagram of a liquid-retaining pad in some embodiments of the present application;
[0059] The reference numerals in the specific embodiments are as follows: 1. separator; 2. negative electrode plate; 3. positive electrode plate; 4. liquid retaining pad.
[0060] Wherein, the coordinate axis z direction represents the thickness direction of the liquid retaining pad;
[0061] The y-axis direction represents the length or width direction of the liquid-retaining pad. DETAILED DESCRIPTION
[0062] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.
[0063] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.
[0064] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0065] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists, A and B exist at the same time, and B exists. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.
[0066] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0067] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.
[0068] Lithium accounts for only 0.0065% of the Earth's crust, while sodium accounts for a whopping 2.64%, giving sodium batteries a natural cost advantage over lithium batteries. However, sodium's standard electrode potential is 0.33V higher than lithium's, and its atomic weight and ionic radius are also larger than lithium. During the charge-discharge cycle of sodium batteries, irreversible reactions occur during the intercalation and disintercalation of positive and negative electrode materials. These reaction products, as insoluble byproducts, deposit on the surface of the negative electrode, causing irreversible expansion of the battery. On the one hand, these insoluble byproducts continuously consume electrolyte during the charge-discharge cycle, potentially leading to safety issues caused by poor interfacial properties. On the other hand, the increased expansion coefficient of the negative electrode reduces the electrolyte retention capacity of the sodium battery separator, forming "dry zones" within the cell. These dry zones reduce the amount of active material available for charge-discharge reactions, causing localized SOC unevenness within the battery, accelerating localized aging, degrading the battery's cycling performance, and ultimately affecting its lifespan.
[0069] Currently, improvements are being made to the separator membrane of sodium batteries, such as improving the material or structure of the separator membrane to improve the separator membrane's ability to retain detergent and liquid. However, this approach has limited improvement in the cyclability of sodium batteries and is limited by the preparation process of sodium batteries.
[0070] In order to alleviate the problem of premature depletion of the electrolyte, the study found that if a liquid-retaining pad with a liquid-retaining function is arranged between the isolation membrane and the negative electrode, the excellent liquid-retaining and liquid-releasing performance of the liquid-retaining pad can effectively alleviate the safety problems caused by volume expansion during the use of the sodium battery and the problem of electrolyte consumption affecting the battery life. Specifically, when the battery cell is filled with liquid, the liquid-retaining pad can store part of the electrolyte in advance. Subsequently, as the battery charge and discharge cycle proceeds, the positive and negative electrode materials expand and continuously consume the electrolyte. The electrolyte stored in the liquid-retaining pad is released in a timely and effective manner to replenish the electrolyte. On the one hand, the replenished electrolyte can ensure that the insoluble by-products at the positive and negative electrode interfaces continue to react, but reduces the safety problems caused by poor interface. On the other hand, sufficient electrolyte reduces the probability of forming a "dry area" inside the battery, which is beneficial to ensure the uniformity of SOC in the battery, thereby improving the cycle life of the battery.
[0071] Based on the above considerations, in order to alleviate the safety issues caused by volume expansion during the use of sodium batteries and the problem of electrolyte consumption affecting battery life. The present application designs a sodium battery cell and a preparation method thereof. The sodium battery cell comprises a negative electrode sheet, a positive electrode sheet, an electrolyte and an isolation membrane, and the isolation membrane is located between the positive electrode sheet and the negative electrode sheet, wherein a liquid retaining pad is also provided between at least part of the isolation membrane and the negative electrode sheet. The present application chooses to arrange a liquid retaining pad between the isolation membrane and the negative electrode sheet, because during the battery cycle, there is always a part of the sodium ions that cannot be completely released from the negative electrode and are deposited on the surface of the negative electrode sheet as insoluble by-products, and the insoluble by-products need to continuously consume the electrolyte, causing the problem of the electrolyte being continuously consumed. The present application chooses to arrange a liquid retaining pad between part of the isolation membrane and the negative electrode sheet, which is more conducive to alleviating the above-mentioned problem of the electrolyte being continuously consumed.
[0072] The sodium battery cell manufacturing method includes first preparing a liquid-retaining pad using a film-forming process, and then arranging the liquid-retaining pad between at least a portion of the separator and the negative electrode. Experimental investigations have shown that the placement of one or more liquid-retaining pads can achieve both liquid retention and release functions. This arrangement is simple and flexible, effectively improving the safety and cycle life of sodium batteries without changing existing sodium battery manufacturing processes or production lines. It is highly feasible in actual production and suitable for mass production.
[0073] The sodium battery cell provided in the present application can be formed into a secondary battery through a subsequent conventional sodium battery preparation process assembly production line. The specific assembly process includes but is not limited to any conventional assembly process in the art.
[0074] Among them, the above-mentioned secondary batteries can be used to make electrical equipment, which can be used as a power source or as an energy storage unit. The electrical equipment has good application prospects in the power field, such as two-wheeled electric vehicles, low-speed electric vehicles, electric ships, buses / coaches, etc., and / or energy storage fields, such as home / industrial energy storage, 5G communication base stations, data centers, renewable energy access, etc., but is not limited to the above-mentioned fields.
[0075] According to some embodiments of the present application, the present application provides a sodium battery cell, which includes a negative electrode plate, a positive electrode plate, an electrolyte and a separator; wherein the separator is located between the positive electrode plate and the negative electrode plate; in addition, the sodium battery cell of the present application also includes a liquid retaining pad, specifically, the liquid retaining pad is located between part of the separator and the negative electrode plate.
[0076] At the same time, the negative electrode sheets, separators and positive electrode sheets are overlapped in a cross-arrangement, and the arrangement includes any conventional form in the art. The above-mentioned "at least part" includes the arrangement of liquid-retaining pads between any one or more separators and each negative electrode sheet, that is, the arrangement of more than one liquid-retaining pad can achieve the liquid-retaining and liquid-releasing functions. If two or more liquid-retaining pads are arranged, the two or more liquid-retaining pads can be overlapped together, or they can be arranged separately between each separator and each negative electrode sheet. When separate arrangements are adopted, the liquid-retaining pads can be arranged between adjacent separators and negative electrode sheets, or they can be arranged non-adjacently. Various arrangements do not affect the overall liquid-retaining and liquid-releasing functions, and are all within the scope of protection of this application.
[0077] Specifically, FIG1 schematically shows a liquid-retaining pad 4 arranged between the separator 1 and the negative electrode plate 2. Although the figure does not show other arrangements of liquid-retaining pads, arrangements that meet the above description are all within the scope of protection of this application.
[0078] When the battery cell with the above design is prepared by the liquid injection process, the liquid retaining pad can store part of the electrolyte in advance. Subsequently, as the battery is charged and discharged, the positive and negative electrode materials expand and continuously consume the electrolyte. The electrolyte stored in the liquid retaining pad is released in a timely and effective manner to replenish the electrolyte. For example, the replenished electrolyte can ensure that the insoluble by-products at the positive and negative electrode interfaces continue to react, but reduce the safety problems caused by poor interface. At the same time, sufficient electrolyte reduces the probability of forming a "dry area" inside the battery, which is conducive to ensuring the uniformity of the SOC in the battery, thereby improving the cycle life of the battery.
[0079] According to some embodiments of the present application, the liquid-retaining pad includes micropores, and the pore size of the micropores is 3 μm to 25 μm.
[0080] The micropores in this application refer to pores with a micron size, and the pore diameter includes the diameter of the micropores, which can be any one of 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 15μm, 18μm, 20μm, 22μm, and 25μm, or any one of the values in the above range. The micropores include any pores that are connected or unconnected inside the liquid-retaining pad, and the pore size measurement method includes any conventional form in the art, such as using a scanning electron microscope to obtain an image of the liquid-retaining pad on the surface of a slice, and then measuring it with a measuring instrument. It can also be measured and calculated by using the gas adsorption BET method of GB / T 19587-2017 to determine the specific surface area of a solid substance.
[0081] When the pore diameter is less than 3 μm, it is difficult to precisely control the pore precision, making it difficult to achieve. When the pore diameter is greater than 25 μm, the electrolyte cannot be effectively and stably stored and released, especially the purpose of retaining the electrolyte is not well achieved, thus affecting the battery life. The liquid-retaining pad with the above-mentioned micropores in this application provides a channel for pre-storing and releasing the electrolyte.
[0082] According to some embodiments of the present application, the volume percentage of pores with a diameter of 3 μm to 5 μm is 10% to 50%; the volume percentage of pores with a diameter of 5 μm < ≤ 9 μm is 30% to 70%, and the rest is the proportion of other pore sizes.
[0083] In this application, "the remainder" includes all pore sizes except those between 3μm and 5μm and between 5μm and 9μm. The volume percentage of each pore size is calculated by scanning electron microscopy to obtain an image of the liquid-retaining pad on a specific slice surface. To further improve the uniformity of micropore size and enhance the uniformity of pre-storage and release of electrolyte, this application selects the volume percentage of each pore size to fall within the above range.
[0084] According to some embodiments of the present application, the porosity of the liquid-retaining pad is 35% to 65%. The definition of porosity includes the definition in the field of materials. As shown in Figure 2, the porosity is represented by the number of pores, but the figure is only a schematic diagram and does not represent the actual number. The porosity can be measured and calculated using the following test method, or it can be measured or calculated using other conventional methods in the field.
[0085] For example, the dried liquid-retaining pad sample is cut into a square sample of about 20 mm × 20 mm. The thickness and actual side length are measured by a digital micrometer and a vernier caliper. The volume V is calculated and the weight M0 is weighed. Then the square sample is immersed in the electrolyte and soaked for 2 hours at room temperature and air atmosphere. After that, it is taken out and the electrolyte liquid adsorbed on the surface is absorbed. Then the weight M is weighed. t , then the porosity of the liquid-retaining pad satisfies the following mathematical relationship:
[0086] The ρ in the above mathematical relationship is the density of the electrolyte, in mm 3 / g, V is the volume of the square sample of the liquid-retaining pad, in mm 3 , weight M0 and M t The unit is g, the weight measuring instrument is a thousandth balance, and the models of the thousandth balance, digital display micrometer, and vernier caliper include but are not limited to any conventional models in the art.
[0087] The porosity of the liquid-retaining pad of the present application can be any one of 35%, 36%, 38%, 40%, 45%, 50%, 55%, 58%, 60%, 62%, 65% or any one of the above range values. The liquid-retaining pad with this porosity is conducive to achieving the technical effect of storing electrolyte in advance and releasing electrolyte. The porosity of the isolation membrane in the prior art is about 40-50%. If the porosity of the isolation membrane of the present application is designed to be less than 35%, its liquid-retaining and liquid-releasing capacity may be equivalent to that of the isolation membrane, which is not conducive to achieving the technical purpose of the present application. If the porosity of the isolation membrane is designed to be greater than 65%, even if the liquid-retaining pad is compressed by the positive and negative electrodes, its liquid-retaining capacity is limited. For example, the liquid-retaining pad stores a certain amount of electrolyte and then quickly releases the electrolyte, which cannot match the charge and discharge cycle of the battery, and cannot achieve the technical effect of effectively improving the cycle life of the battery.
[0088] According to some embodiments of the present application, the porosity of the liquid-retaining pad is 40% to 65%. The liquid-retaining pad of the present application with the above porosity is conducive to further achieving the technical effect of pre-storing and releasing the electrolyte.
[0089] According to some embodiments of the present application, the porosity of the liquid-retaining pad is 55% to 65%. When the positive and negative electrode materials expand and continuously consume electrolyte, the liquid-retaining pad with this porosity releases electrolyte to improve the wettability of the separator, thereby reducing safety issues caused by adverse interfacial reactions and increasing the cycle life of the battery.
[0090] According to some embodiments of this application, the material of the liquid-retaining pad includes, but is not limited to, at least one of polyolefin, polyester, polyimide, glass fiber, and superabsorbent resin. In principle, this application utilizes raw materials containing these materials through a film-forming process to produce the liquid-retaining pad. Any of these materials, provided the preparation process and resulting product structure or parameters meet the aforementioned requirements, are protected by this application.
[0091] According to some embodiments of the present application, the polyolefin includes but is not limited to any conventional type in the art, such as any one of polyethylene, polypropylene or polypropylene.
[0092] According to some embodiments of the present application, the polyester comprises a thermoplastic polyester, and the thermoplastic polyester includes, but is not limited to, any conventional type in the art, such as polyethylene terephthalate or polybutylene terephthalate. Polyethylene terephthalate or polybutylene terephthalate includes any conventional type in the art, in terms of molecular weight or other form.
[0093] According to some embodiments of the present application, the super absorbent resin includes any one of polyacrylate, sodium polyacrylate, sodium starch acrylate polymer, and polyvinyl alcohol.
[0094] According to some embodiments of the present application, the polyimide includes a thermoplastic polyimide, and the thermoplastic polyimide includes but is not limited to any conventional type in the art, such as any one of phthalic anhydride-type polyimide, ether anhydride-type polyimide, ketone anhydride-type polyimide or fluoroanhydride-type polyimide. Among them, phthalic anhydride-type polyimide is a polyimide generated by reacting phthalic acid dianhydride with aromatic diamine and then undergoing imidization treatment; the phthalic anhydride-type polyimide of the present application includes any conventional molecular weight or other form type in the art. Ether anhydride-type polyimide is a product obtained by the reaction of diphenyl ether tetracarboxylic anhydride and aromatic diamine. The ether anhydride-type polyimide of the present application includes any conventional molecular weight or other form type in the art. Ketone anhydride-type polyimide is a product obtained by the reaction of dibenzophenone tetracarboxylic dianhydride and aromatic diamine. The ketone anhydride-type polyimide of the present application includes any conventional molecular weight or other form type in the art. Fluoroanhydride polyimides are products obtained by the reaction of hexafluorodianhydride and aromatic diamines. The fluoroanhydride polyimides herein include any conventionally used polyimide having any molecular weight or other form. The aromatic diamines may include any conventionally used polyimide, such as p-phenylenediamine, m-phenylenediamine, or biphenylenediamine. The aromatic diamines and hexafluorodianhydride are not limited by manufacturer or type.
[0095] According to some embodiments of the present application, the glass fiber comprises any one of an alkali-free fiber and a high-alkali fiber. The alkali-free fiber comprises any conventional glass fiber in the art, such as the alkali-free fiber of the present application comprising aluminoborosilicate, while the high-alkali fiber comprises any conventional glass fiber in the art, such as glass fiber obtained by drawing raw materials to a relatively high alkali metal oxide content, wherein the alkali metal oxide content in the alkali-free fiber and the high-alkali fiber comprises any conventional content in the art.
[0096] The present application uses the above materials to form a liquid-retaining pad through a film-forming process. The film-forming process of the present application includes but is not limited to any conventional form in the art. The film-forming process of the liquid-retaining pad will be discussed below in conjunction with specific materials.
[0097] According to some embodiments of the present application, the material of the liquid-retaining pad includes any one of thermoplastic polyester, fluoroanhydride polyimide, and high-alkali glass fiber. The raw materials of the present application having the above materials are conducive to being used to prepare the liquid-retaining pad through a simple and operable film-forming process. The liquid-retaining pad having this material is relatively good for improving the recycling effect of the present application. Among them, the preparation of each liquid-retaining pad includes but is not limited to the use of a template method for film formation, for example: using fluoroanhydride polyamide ester as a reaction precursor to first prepare a fluoroanhydride polyamide composite membrane containing a porogen, and then using chemical corrosion, solvent dissolution or calcination to remove the porogen to obtain a fluoroanhydride polyamide microporous membrane. Commonly used porogens include but are not limited to SiO2, and chemical corrosion, solvent dissolution or calcination methods include but are not limited to any conventional form in the art. The liquid-retaining pad made of glass fiber includes but is not limited to first purchasing the raw materials from the supplier, such as high-alkali glass fiber membranes from General Electric, Tianze Filtration, Whatman and other companies, and then also using the above-mentioned template method to form a pore to prepare a glass fiber microporous membrane. Suppliers of thermoplastic polyester include but are not limited to Toray and Teijin.
[0098] The raw materials of the present application having the above-mentioned materials are convenient for preparing the liquid-retaining pad through a simple and operable film-forming process, and are also conducive to achieving the above-mentioned uniform pore size and porosity.
[0099] According to some embodiments of the present application, the thickness of the liquid-retaining pad is 100μm to 3000μm. In conjunction with Figure 2, it can be seen that the thickness h of the liquid-retaining pad is the distance between the two end surfaces, and the thickness value can be measured using conventional measuring instruments such as a micrometer. The thickness of the liquid-retaining pad of the present application can be any one of 100μm, 200μm, 300μm, 400μm, 500μm, 800μm, 1000μm, 1500μm, 1800μm, 2000μm, 2200μm, 2500μm, 2800μm, 3000μm or any one of the above range values. The thickness of the liquid-retaining pad affects the amount of electrolyte it stores and ultimately affects the battery performance. When designing the thickness of the liquid-retaining pad, both the battery performance and the battery preparation process must be considered. The present application selects the above range value under comprehensive consideration of these two dimensions. The length and width of the liquid-retaining pad are related to the actual size of the battery cell during preparation, and include any conventional size in the art, which will not be described in detail in this application.
[0100] According to some embodiments of the present application, the thickness of the liquid retaining pad is 500 μm to 3000 μm. The liquid retaining pad of the present application with the above thickness can more effectively improve the battery safety and cycle life under the premise that the battery manufacturing process is feasible.
[0101] According to some embodiments of the present application, the thickness of the liquid retaining pad is 1000 μm to 3000 μm. The liquid retaining pad of the present application with the above thickness can better improve the battery safety and cycle life under the premise that the battery manufacturing process is feasible.
[0102] According to some embodiments of the present application, the elastic modulus of the liquid-retaining pad is 500 MPa to 86,000 MPa. The elastic modulus is affected by the material and structure, and is related to the liquid-retaining, release, and deformation capabilities of the liquid-retaining pad. The elastic modulus of the liquid-retaining pad designed in this application has a relatively large range of values, which is designed based on the material and pore structure of the liquid-retaining pad. The elastic modulus can be measured by any method conventional in the art, such as testing and calculation using the GB-T1040-92 Plastic Tensile Properties Test Method.
[0103] The elastic modulus of the liquid-retaining pad of the present application can be any one of 500Mpa, 1000Mpa, 2000Mpa, 3000Mpa, 4000Mpa, 5000Mpa, 8000Mpa, 10000Mpa, 12000Mpa, 15000Mpa, 20000Mpa, 25000Mpa, 30000Mpa, 35000Mpa, 40000Mpa, 45000Mpa, and 50000Mpa, or any one of the values within the above range. A liquid-retaining pad that meets the parameter requirements is beneficial for ensuring the stability of its liquid retention and release, and can also effectively prevent short circuits caused by dendrites and burrs on the surface of the electrode from piercing the gasket, thereby improving the safety of the battery.
[0104] According to some embodiments of the present application, the elastic modulus of the liquid-retaining pad is 3000 MPa to 50000 MPa.
[0105] The liquid-retaining pad of the present application with the above-mentioned elastic modulus can effectively release the electrolyte to improve the wettability of the isolation membrane when the positive and negative electrode materials expand and continuously consume the electrolyte, thereby reducing the safety problems caused by adverse interface reactions and improving the cycle life of the battery.
[0106] According to some embodiments of the present application, the elastic modulus of the liquid-retaining pad is 15,000 MPa to 50,000 MPa.
[0107] The liquid-retaining pad of the present application having the above elastic modulus can relatively better improve battery safety issues and cycle life.
[0108] According to some embodiments of the present application, the battery cell includes a laminated cell and a wound cell. Both laminated and wound cells can ensure that the liquid-retaining pad can achieve the liquid-retaining and liquid-releasing functions. However, from a manufacturing process perspective, the liquid-retaining pad is easier to arrange in a laminated cell, which is more conducive to its excellent liquid-retaining and liquid-releasing functions. Therefore, the present application prefers the laminated cell as the battery cell.
[0109] According to some embodiments of the present application, the number of liquid-retaining pads is m, and m is a positive integer greater than or equal to 1.
[0110] The present application describes here that a liquid retaining pad is designed between the isolation membrane and the negative electrode plate, because designing a liquid retaining pad between the isolation membrane and the negative electrode plate is sufficient to ensure the liquid retaining and liquid release capabilities. If there are more than two liquid retaining pads, the two or more liquid retaining pads can be arranged between adjacent isolation membranes and negative electrode plates, or they can be arranged non-adjacently. The number of liquid retaining pads is affected by battery performance.
[0111] In addition, the positive electrode sheet constituting the sodium battery cell includes a positive electrode active material, which is at least one of a sodium transition metal oxide, a polyanion compound, and a Prussian blue compound. Among them, the transition metal in the sodium transition metal oxide can be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. The sodium transition metal oxide is, for example, Na x MO2, wherein M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1. Polyanionic compounds include one or more of sodium vanadium trifluorophosphate Na3V2(PO4)2F3, sodium vanadium fluorophosphate NaVPO4F, sodium vanadium phosphate Na3V2(PO4)3, Na4Fe3(PO4)2P2O7, NaFePO4, and Na3V2(PO4)3. Prussian blue compounds are Na x M1M2(CN)6, wherein M1 and M2 are one or more of Fe, Mn, Co, Ni, Cu, Zn, Cr, Ti, V, Zr, and Ce, and 0<x≤2.
[0112] A binder and / or a conductive agent may also be added to the positive electrode active material. There is no limitation on the types of the binder and the conductive agent, and those skilled in the art may select them according to actual needs. For example, the binder may be one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid (PAA), polyvinyl alcohol (PVA), and styrene-butadiene rubber (SBR). The conductive agent may be one or more of graphite, superconducting carbon, acetylene black, carbon black, carbon nanotubes, graphene, and carbon nanofibers.
[0113] The negative electrode plates that make up the sodium battery cells are carbon-based negative electrode materials, titanium-based oxide negative electrode materials, metal and alloy negative electrode materials, and non-metallic elements. Among them, carbon-based negative electrode materials include hard carbon and soft carbon, titanium-based oxide negative electrode materials include titanium dioxide and other optimized materials, metal and alloy negative electrode materials can be tin, antimony, germanium and lead, etc., and non-metallic elements include carbon elements, etc.
[0114] The isolation membrane constituting the sodium battery cell includes at least one of a polypropylene microporous membrane, a polyethylene microporous membrane, a polyimide microporous membrane, and a polyethylene terephthalate microporous membrane. The thickness of the isolation membrane is any conventional form in the art.
[0115] The electrolyte that makes up the sodium battery cell includes sodium salt and organic solvent. Specifically, there is no special restriction on the organic solvent in the electrolyte, and the organic solvent can be an organic solvent commonly used in the art for electrolyte. As an example, the organic solvent can be selected from at least one of ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, propylene carbonate, methyl acetate, ethyl propionate, fluoroethylene carbonate, ethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and methyl tert-butyl ether. Ether solvents are preferably used to adjust the sodium ion deposition morphology, thereby inhibiting the massive growth of sodium dendrites. In the electrochemical device of the present application, there is no special restriction on the sodium salt in the electrolyte, and the sodium salt can be a sodium salt commonly used in the art for electrolyte. As an example, the sodium salt may include, but is not limited to, at least one of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoromethanesulfonate, sodium tetrafluoroborate, sodium difluorophosphate, sodium perchlorate, and sodium chloride.
[0116] In addition, the assembly process of the battery cells, the injection of electrolytes, etc. all meet the requirements of existing battery production lines and are all conventional in this field.
[0117] In order to make the purpose, technical solutions and advantages of this application clearer, the sodium battery monomer protected by this application is described in detail below with reference to specific embodiments.
[0118] Example 1 to Example 8
[0119] A method for preparing a sodium battery cell is provided:
[0120] A positive electrode sheet is selected, wherein the positive electrode active material contained in the positive electrode sheet is a Prussian blue compound (Na2Mn[Fe(CN)6]); the preparation method of the positive electrode sheet comprises: taking Na2Mn[Fe(CN)6], a conductive agent acetylene black (Denka, Denka Black), and a binder polyvinylidene fluoride (Arkema, HSV 900) in an N-methylpyrrolidone solvent in a weight ratio of 90:5:5, and stirring and mixing them thoroughly to obtain a positive electrode slurry with a solid content of 30%. The positive electrode slurry is applied to both sides of an aluminum foil with a thickness of 12μm using a scraper to form a wet coating with a thickness of 120μm on each side. The sheet is transferred to an oven and dried at a temperature of 150°C for 60 minutes. The sheet is then cold pressed using a cold press with a pressure of 60 tons to obtain a positive electrode film layer with a thickness of 130μm on both sides of the aluminum foil and a compaction density of 1.3g / cm 3The positive electrode sheet. A negative electrode sheet is selected, the active material of which is hard carbon; the preparation method of the negative electrode sheet comprises: dispersing hard carbon, conductive agent acetylene black, binder styrene-butadiene rubber, and thickener sodium carboxymethyl cellulose in a deionized water solvent in a weight ratio of 95:2:2:1, stirring and mixing them thoroughly to obtain a negative electrode slurry with a solid content of 15%, and using a scraper to apply the negative electrode slurry on both sides of an aluminum foil with a thickness of 12 μm to form a wet coating with a thickness of 120 μm each. Transfer it into an oven, dry it at a temperature of 150°C for 60 minutes, and use a cold press to perform cold pressing at a pressure of 50 tons to obtain a negative electrode film layer with a thickness of 60 μm on both sides of the aluminum foil and a compaction density of 0.95 g / cm 3 The negative electrode.
[0121] Selecting an isolation membrane, which is a polypropylene microporous membrane;
[0122] Preparation of a liquid-retaining pad: Using fluoroanhydride-type polyamide ester as a reaction precursor, a fluoroanhydride-type polyamide composite membrane containing a porogen SiO2 is first prepared, and then the porogen is removed to obtain a fluoroanhydride-type polyamide microporous membrane; the fluoroanhydride-type polyamide ester is a product obtained by the reaction of hexafluorodianhydride and p-phenylenediamine;
[0123] The positive electrode sheet, the negative electrode sheet, the isolation membrane and a liquid retaining pad are assembled together according to the stacking process, the electrolyte sodium hexafluorophosphate + diethylene glycol dimethyl ether is injected and the battery cell is formed through subsequent processes, wherein the concentration of sodium hexafluorophosphate is 1 mol / L.
[0124] Among them, the performance parameters of the liquid-retaining pad are shown in Table 1;
[0125] The sodium battery cell is cyclically charged and discharged at 25°C, and the number of cycles at which the capacity remains at about 80% is shown in Table 2.
[0126] Among them, the fluoroanhydride type polyamide microporous membrane listed is only for illustrating the pore size distribution, porosity, etc. of the liquid-retaining pad of this application. Other fluoroanhydride type polyamide materials not listed are also within the protection scope of this application.
[0127] Example 9 to Example 10
[0128] A method for preparing a sodium battery cell is provided. A liquid-retaining pad in the preparation method is made of glass fiber, and the glass fiber is a high-alkali glass fiber membrane produced by Tianze Filtration Co., Ltd. The high-alkali glass fiber membrane is used as a reaction precursor to first prepare a composite membrane containing a porogen SiO2. The porogen is then removed to obtain a glass fiber microporous membrane. The performance parameters of the liquid-retaining pad are shown in Table 1. The number of cycles during which the sodium battery cell maintains approximately 80% of its capacity under cyclic charge and discharge conditions at 25°C is shown in Table 2.
[0129] The glass fiber microporous membrane listed in this embodiment is only for illustrating the pore size distribution, porosity, etc. of the liquid-retaining pad of this application. Other glass fiber materials not listed are also within the scope of protection of this application.
[0130] Example 11 to Example 12
[0131] Provided is a method for preparing a sodium battery cell. The liquid-retaining pad in the preparation method is made of polyethylene terephthalate, and the supplier of the polyethylene terephthalate is Toray.
[0132] The polyethylene terephthalate listed in this embodiment is only for illustrating the pore size distribution, porosity, etc. of the liquid-retaining pad of this application. Other polyesters not listed are also within the scope of protection of this application.
[0133] Table 1 Performance parameters of liquid retaining pad
[0134] Although the above embodiments only discuss polyimide, glass fiber, and polyethylene terephthalate materials, the present application also includes other materials that meet the design requirements of the present application such as pore size and porosity.
[0135] Comparative Example 1
[0136] The difference from Example 1 is that no liquid-retaining pad is added, and the rest is the same as Example 1.
[0137] Comparative Example 2
[0138] The difference from Example 1 is that the pore size of the liquid-retaining pad is larger than 25 μm, and the pore size is between 25 and 40 μm through the film-forming process, and the proportion of each pore size inside is not concerned.
[0139] Comparative Example 3
[0140] The difference from Example 1 is that the pore size of the liquid retaining pad is between 3 μm and 25 μm, and the size of the porogen in the film forming process is controlled so that the pore size above 9 μm accounts for about 65%.
[0141] The cycle performance tests of the sodium batteries prepared in the above examples and comparative examples are as follows:
[0142] At a test temperature of 25°C, the battery was charged at a constant current of 0.33C to 3.65V, then charged at a constant voltage of 0.01C. After standing for 5 minutes, it was discharged at 0.33C to 1.5V. The capacity obtained in this step was considered the initial capacity. A 0.33C charge / 1C discharge cycle test was then performed. The ratio of the capacity at each step to the initial capacity was calculated as the capacity retention rate. When the capacity retention rate was approximately 80%, the number of cycles for each embodiment and comparative example was calculated, and the specific values are shown in Table 2 below:
[0143] Table 2 Cycle performance list
[0144] From Table 1 and Table 2, it can be seen that the factors affecting the liquid retaining and releasing functions of the liquid retaining pad of the present application include the micropore size distribution, porosity, thickness and elastic modulus, etc. From Comparative Example 1, it can be seen that the liquid retaining pad designed in the present application has better improved the battery cycle life. While the capacity is maintained at about 80%, the life is increased by more than 2 times, and the liquid retaining and releasing function of the liquid retaining pad provided in Example 8 of the present application is limited by its own thickness, and the improvement of the battery cycle life is worse than that of other embodiments; From Comparative Examples 2 and 3, it can be seen that the micropore size of the liquid retaining pad does not meet the protection scope of the present application, and the effect on improving the cycle life of the battery is limited. This may be because the liquid retaining ability of the liquid retaining pad itself is not ideal.
[0145] To summarize, a liquid-retaining pad with liquid-retaining and liquid-releasing functions is arranged between the isolation membrane and the negative electrode sheet. With the help of the excellent liquid-retaining and liquid-releasing performance of the liquid-retaining pad, the safety issues caused by volume expansion during the use of sodium batteries and the problem of electrolyte consumption affecting battery life can be effectively alleviated. Specifically, when the battery cell is prepared in the liquid injection process, the liquid-retaining pad can store part of the electrolyte in advance. Subsequently, as the battery charge and discharge cycle proceeds, the positive and negative electrode materials expand and continuously consume the electrolyte. The electrolyte stored in the liquid-retaining pad is released in a timely and effective manner to replenish the electrolyte. For example, the replenished electrolyte can ensure that the insoluble by-products at the positive and negative electrode interfaces continue to react, but reduce the safety issues caused by poor interfaces. On the other hand, sufficient electrolyte reduces the probability of forming a "dry area" inside the battery, which is beneficial to ensure the uniformity of SOC in the battery, thereby improving the cycle life of the battery.
[0146] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A sodium battery cell, characterized in that: The battery cell comprises: Negative electrode; Positive electrode; Electrolyte; A separator; the separator is located between the positive electrode sheet and the negative electrode sheet; Wherein, a liquid retaining pad is provided between at least part of the isolation membrane and the negative electrode plate.
2. The battery cell according to claim 1, characterized in that: The liquid-retaining pad contains micropores, and the pore diameter of the micropores is 3 μm to 25 μm; Preferably, the volume percentage of pores with a diameter of 3 μm to 5 μm is 10% to 50%; the volume percentage of pores with a diameter of 5 μm < 9 μm is 30% to 70%, and the rest is other pore sizes.
3. The battery cell according to any one of claims 1 to 2, characterized in that: The porosity of the liquid-retaining pad is 35% to 65%, preferably 40% to 65%, and more preferably 55% to 65%.
4. The battery cell according to any one of claims 1 to 3, characterized in that: The material of the liquid-retaining pad includes at least one of polyolefin, polyester, polyimide, glass fiber, and highly absorbent resin.
5. The battery cell according to claim 4, characterized in that: The polyimide includes thermoplastic polyimide, and the thermoplastic polyimide includes any one of phthalic anhydride type polyimide, ether anhydride type polyimide, ketone anhydride type polyimide or fluoroanhydride type polyimide.
6. The battery cell according to any one of claims 4 to 5, characterized in that: The polyester includes a thermoplastic polyester, and the thermoplastic polyester includes any one of polyethylene terephthalate and polybutylene terephthalate.
7. The battery cell according to any one of claims 4 to 6, characterized in that: The glass fiber includes any one of alkali-free fiber and high-alkali fiber.
8. The battery cell according to any one of claims 1 to 7, characterized in that: The thickness of the liquid-retaining pad is 100 μm to 3000 μm, preferably 500 μm to 3000 μm, and more preferably 1000 μm to 3000 μm.
9. The battery cell according to any one of claims 1 to 8, characterized in that: The elastic modulus of the liquid-retaining pad is 500 MPa to 86000 MPa, preferably 3000 MPa to 50000 MPa, and more preferably 15000 MPa to 50000 MPa.
10. The battery cell according to any one of claims 1 to 9, characterized in that: The battery core is a laminated battery core.
11. A secondary battery, characterized in that: The secondary battery comprises the battery cell according to any one of claims 1 to 10.
12. An electrical device, characterized in that: The electrical device comprises the battery cell according to any one of claims 1 to 10 or the secondary battery according to claim 11.
Citation Information
Patent Citations
Cell, battery, liquid-preserving coating, battery pole piece and preparation method thereof
CN110071293A
Laminated battery cell and lithium ion battery
CN112259796A
Lithium-sulfur battery
CN112768746A
Method for improving multiplying power and prolonging cycle life of silicon-based negative electrode battery
CN112993486A
Flat plate type sodium metal battery and electrochemical device
CN114597479A