Degradation auxiliary agent for degrading pp and pe
By using mesoporous silica carriers and biodegradable polymers to wrap photosensitizers and decomposition aids in PP and PE plastics, the problem of photosensitizer precipitation in the existing technology is solved, efficient polymer degradation is achieved, and environmental pollution is reduced. .
Patent Information
- Application Number
- PCT/CN2024/076678
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-02-07
- Publication Date
- 2024-10-31
AI Technical Summary
Existing PP and PE plastics are difficult to effectively degrade after being discarded, resulting in environmental pollution. The existing photosensitizer addition method causes the photosensitizer to precipitate, reducing the degradation effect.
Mesoporous silica is used as the photosensitizer carrier, the photosensitizer and organic decomposition aids are wrapped in biodegradable polymers, the polymer degradation is accelerated through photochemical reactions, and microbial decomposition aids are used to promote degradation.
Significantly improves the degradation performance of PP, PE and their blends, achieves dual degradation capabilities (biodegradability and photodegradability), and accelerates the decomposition process of polymers.
Smart Images

Figure CN2024076678_31102024_PF_FP_ABST
Abstract
Description
A degradation aid for degrading PP and PE Technical Field
[0001] The present application relates to the field of polymer materials, and in particular to a degradation aid for degrading PP and PE. Background Art
[0002] Polypropylene (PP) is a semi-crystalline thermoplastic. It is a colorless, odorless, non-toxic, translucent, lightweight, and high-performance general-purpose synthetic plastic produced through the addition polymerization of propylene. Polyethylene (PE) is a crystalline thermoplastic resin produced through the polymerization of ethylene. Both PP and PE are important general-purpose resins. PP offers advantages such as low specific gravity, outstanding stress cracking resistance, wear resistance, heat resistance, and chemical stability, but suffers from poor brittleness and low-temperature impact resistance. PE has excellent electrical insulation, chemical resistance, low-temperature resistance, and good processing fluidity, but also has significant disadvantages such as poor heat resistance, poor atmospheric aging resistance, and susceptibility to stress cracking. Therefore, polymer alloys such as PP / PE blends offer the potential for a wider range of commercial applications and are attracting increasing research interest. However, all PP, PE, and PP / PE blends pose environmental pollution risks associated with their disposal. Therefore, improving the degradation properties of these plastics to reduce environmental pollution has become a current research hotspot. Summary of the Invention
[0003] The present application provides a degradation aid for degrading PP and PE to solve the environmental pollution problem caused by discarded resin materials.
[0004] The present application provides a degradation aid for degrading PP and PE. The degradation aid mainly comprises the following raw materials in parts by weight: 3-9 parts of a photosensitizer, 2-5 parts of mesoporous silica, 50-76 parts of a biodegradable polymer, and 1-5 parts of an organic decomposition aid.
[0005] The above technical solution provided by the embodiment of the present application has at least the following advantages compared with the prior art:
[0006] Most polymers do not absorb light energy with wavelengths above 285 nm. However, adding photosensitizers or chemical additives with photosensitizing effects to polymers can accelerate the photochemical reaction process. These substances absorb light energy and generate free radicals, or transfer excited state energy to the polymer to generate free radicals, which then promote oxidation reactions in the polymer material, causing the polymer to degrade rapidly. Although adding photosensitizers directly to PP, PE, or PP / PE alloys is relatively simple and quick, and the processing cost is also lower, after this simple addition, the photosensitizers easily diffuse and precipitate from the polymer surface and migrate to substances that the polymer contacts, which will reduce the decomposition effect of the polymer after it is discarded. Therefore, the inventors of this application intend to improve the precipitation of photosensitizers while simplifying the processing technology as much as possible, thereby improving the degradation performance of the polymer. Mesoporous silica is a porous microsphere material with a pore size between 2 and 50 nm, which has good strength, thermal stability, and a high specific surface area. The inventors leveraged the porous microspheres of mesoporous silica as a photosensitizer carrier, first introducing the photosensitizer into a biodegradable polymer and then into polymers such as PP, PE, or PP / PE alloys. This improved the release of the photosensitizer from the polymer and, in turn, enhanced the polymer's degradation performance. Simultaneously, both the photosensitizer and the organic decomposition aid are encapsulated within the biodegradable polymer. When the polymer containing this decomposition aid is discarded, the organic decomposition aid utilizes its ability to recruit microorganisms for decomposition, accelerating the biodegradable polymer's decomposition. This increases the exposure of the photosensitizer and significantly accelerates the polymer's decomposition.
[0007] Furthermore, the photosensitizer is selected from one or more of ferric eleostearate, dodecylferrocene, benzophenone, stearic acid, cerium stearate, iron stearate and nickel stearate.
[0008] Furthermore, the biodegradable polymer is selected from one or more of polylactic acid, polyhydroxyalkanoate, polybutylene succinate, polycaprolactone, PBAT (copolymer of butylene adipate and butylene terephthalate), polyvinyl alcohol and poly-L-lactic acid.
[0009] Furthermore, the organic decomposition aid is selected from one or more of lactose, galactose, vitamin E polyethylene glycol succinate and diisostearyl malate.
[0010] Furthermore, the invention further comprises the following raw materials in parts by weight: 0.5-1.6 parts of a dispersant and 0.8-2 parts of tricarboxylic acid, wherein the dispersant is selected from polypropylene wax and / or polyethylene wax.
[0011] Furthermore, the invention comprises the following raw materials in parts by weight: 4-6 parts of photosensitizer, 2.5-3.6 parts of mesoporous silica, 58-66 parts of biodegradable polymer, 2-3 parts of organic decomposition aid, 0.9-1.2 parts of dispersant and 1.3-1.8 parts of tricarboxylic acid.
[0012] Furthermore, the addition ratio of the prodegradant to PP or PE or PP / PE blend is 10wt%-30wt%.
[0013] Furthermore, the prodegradant is processed by the following steps:
[0014] The photosensitizer, the mesoporous silica, the dispersant and the tricarboxylic acid are mixed, and then the organic decomposition aid and the biodegradable polymer are added to obtain the degradation aid.
[0015] Furthermore, the mesoporous silica, the dispersant and the tricarboxylic acid are stirred and mixed at 130-170° C. for 50-70 minutes, the photosensitizer is added, the rotation speed is increased by 50-80 rpm, the mixture is stirred and mixed for 60-90 minutes, and then extruded and granulated to obtain a first auxiliary material, and the first auxiliary material is then mixed with the organic decomposition auxiliary agent and the biodegradable polymer to obtain the degradation auxiliary agent.
[0016] Furthermore, the organic decomposition aid is heated until melted, and then the first auxiliary material is quickly added at a rotation speed of 100-150 rpm. After the addition is completed, the temperature is lowered at a rate of 5-10°C / min until it reaches room temperature, and then the biodegradable polymer is added. The material is discharged into a twin-screw extruder for extrusion and granulation to obtain the degradation aid.
[0017] The above technical solution provided by the embodiment of the present application has at least the following advantages compared with the prior art:
[0018] Most polymers do not absorb light energy with wavelengths above 285 nm. However, adding photosensitizers or chemical additives with photosensitizing effects to polymers can accelerate the photochemical reaction process. These substances absorb light energy and generate free radicals, or transfer excited state energy to the polymer to generate free radicals, which then promote oxidation reactions in the polymer material, causing the polymer to degrade rapidly. Although adding photosensitizers directly to PP, PE, or PP / PE alloys is relatively simple and quick, and the processing cost is also lower, after this simple addition, the photosensitizers easily diffuse and precipitate from the polymer surface and migrate to substances that the polymer contacts, which will reduce the decomposition effect of the polymer after it is discarded. Therefore, the inventors of this application intend to improve the precipitation of photosensitizers while simplifying the processing technology as much as possible, thereby improving the degradation performance of the polymer. Mesoporous silica is a porous microsphere material with a pore size between 2 and 50 nm, which has good strength, thermal stability, and a high specific surface area. The inventors leveraged the porous microspheres of mesoporous silica as a photosensitizer carrier, first introducing the photosensitizer into a biodegradable polymer and then into polymers such as PP, PE, or PP / PE alloys. This improved the release of the photosensitizer from the polymer and, in turn, enhanced the polymer's degradation performance. Simultaneously, both the photosensitizer and the organic decomposition aid are encapsulated within the biodegradable polymer. When the polymer containing this decomposition aid is discarded, the organic decomposition aid utilizes its ability to recruit microorganisms for decomposition, accelerating the biodegradable polymer's decomposition. This increases the exposure of the photosensitizer and significantly accelerates the polymer's decomposition. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0020] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0021] FIG1 is a photograph of the test materials of Test Example 1 provided in an embodiment of the present application.
[0022] FIG2 is a graph showing the cumulative production of carbon dioxide according to an embodiment of the present application.
[0023] FIG3 is a graph showing the biodegradation rate according to an embodiment of the present invention.
[0024] FIG4 is a photograph of the test sample provided in the examples of the present application after mixing with compost, and a photograph after stacking for 140 days.
[0025] FIG5 is a graph showing the time-cumulative carbon dioxide production (g / container) of blank, sample, and reference materials provided in the examples of the present application.
[0026] FIG6 is a time-biodegradation percentage (%) curve of the samples and reference materials provided in the examples of the present application. Modes for Carrying Out the Invention
[0027] To make the purpose, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0028] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0029] The present application provides a degradation aid for degrading PP and PE, which mainly includes the following raw materials in parts by weight:
[0030] 3-9 parts of photosensitizer, 2-5 parts of mesoporous silica, 50-76 parts of biodegradable polymer and 1-5 parts of organic decomposition auxiliary.
[0031] The organic decomposition aid used in the present invention has the effect of attracting microorganisms in the natural environment to approach, thereby promoting the accelerated decomposition of the biodegradable polymer by the microorganisms.
[0032] The biodegradable polymers used in this invention are polymers produced from reproducibly available natural resources, such as microorganisms, animals, and plants. These biodegradable polymers possess the physical properties of traditional plastics and can replace petroleum-based plastics. They are more environmentally friendly than traditional plastics, and their market demand is growing significantly.
[0033] Most polymers do not absorb light energy with wavelengths above 285 nm. However, adding photosensitizers or photosensitizing chemical additives to polymers can accelerate the photochemical reaction process. These substances absorb light energy and generate free radicals, or transfer excited-state energy to the polymer, causing it to generate free radicals. This then promotes oxidation reactions in the polymer material, causing the polymer to rapidly degrade. Although adding photosensitizers directly to PP, PE, or PP / PE alloys is relatively simple and quick, with lower processing costs, this simple addition process easily allows the photosensitizer to diffuse and precipitate from the polymer surface and migrate to substances it comes into contact with, reducing the decomposition efficiency of the polymer after disposal. Therefore, the inventors of this application intend to improve the precipitation of photosensitizers while simplifying the processing technology as much as possible, thereby enhancing the degradation performance of the polymer.
[0034] Mesoporous silica is a porous microsphere material with pore sizes ranging from 2 to 50 nm. It exhibits excellent strength, thermal stability, and a high specific surface area. The inventors propose leveraging the porous microspheres of mesoporous silica as a photosensitizer carrier, first introducing the photosensitizer into a biodegradable polymer and then into polymers such as PP, PE, or PP / PE alloys. This approach improves the release of the photosensitizer from the polymer and, in turn, enhances the polymer's degradation performance. Simultaneously, both the photosensitizer and the organic decomposition aid are encapsulated within the biodegradable polymer. When the polymer containing this decomposition aid is discarded, the organic decomposition aid utilizes its ability to recruit microorganisms for decomposition, accelerating the degradation of the biodegradable polymer. This increases the exposure of the photosensitizer and significantly accelerates the polymer's decomposition. The combined use of the photosensitizer, biodegradable polymer, and organic decomposition aid results in the PP, PE, or PP / PE blend possessing dual degradation capabilities—biodegradability and photodegradability—when the decomposition aid is added to the PP, PE, or PP / PE blend, resulting in a rapid degradation rate.
[0035] Photosensitizer is selected from one or more of ferric eleostearate, dodecylferrocene, benzophenone, stearic acid, cerium stearate, ferric stearate and nickel stearate.By inventor's test discovery, when photosensitizer is selected from one or more of ferric eleostearate, cerium stearate, ferric stearate and nickel stearate, polymer degradation performance is slightly excellent, it is speculated that the combination of polymer segment and metal ion makes the entanglement distribution of photosensitizer in mesoporous silica more intricate and stable, while polymer segment makes photosensitizer and mesoporous silica compatible degree higher in the polymers such as biodegradable polymer, PP, PE or PP / PE alloy, and the migration of photosensitizer, mesoporous silica is further restricted.The preparation raw materials of ferric eleostearate include tung oil, ethanol, sodium hydroxide solution, ferric chloride hexahydrate etc.The absorption peak of eleostearic acid and ferric eleostearate in ultraviolet range is much higher than other conventional reagents. Eleurotic acid contains three conjugated double bonds, giving it a wide absorption range and stronger absorption of ultraviolet light. After eleurotic acid is synthesized into ferric eleuronate, the addition of a photosensitizing group called iron ion further enhances the range and ability of eleurotic acid to absorb ultraviolet light. The absorption range of ferric eleuronate for ultraviolet light essentially covers the entire wavelength range of ultraviolet light and reaches the wavelength range of visible light, further enhancing its ability to obtain energy from light. Iron ions absorb ultraviolet light to form an excited state. These excited iron ions interact with polypropylene and polyethylene to generate a large number of free radicals, thereby accelerating the degradation rate of the resin. After the excited iron ions react with the resin to produce free radicals, they return to their normal state and continue to absorb ultraviolet light in synergistic interaction with eleurotic acid. This cycle continues, continuously promoting the formation of new free radicals in the resin through a cascade reaction, significantly increasing the photodegradation rate of the resin.
[0036] Furthermore, the biodegradable polymer can be selected from one or more of polylactic acid (PLA), polyhydroxyalkanoate (PHA), polybutylene succinate (PBS), polycaprolactone (PCL), PBAT, polyvinyl alcohol (PVA), and poly-L-lactic acid. The biodegradable polymer can be used to more evenly distribute the photosensitizer in the final polymer (PP, PE, or PP / PE alloy) and induce faster and more complete degradation of the final polymer.
[0037] PCL is a semicrystalline thermoplastic resin with a crystallinity of approximately 45%. Its mechanical properties are similar to those of medium-density polyolefins, and its softness and tensile strength are comparable to those of nylon. PCL has a glass transition temperature of approximately -60°C to 65°C, a melting point of 59°C to 64°C, and a decomposition temperature of approximately 250°C. Due to its low melting point, PCL softens at approximately 40°C, limiting its application. However, the presence of lactone groups in the PCL molecule gives it excellent biodegradability and physiological compatibility, supporting fungal growth and serving as a carbon source for microorganisms. It degrades slowly in soil, with an average degradation time of 12-18 months, making it an excellent biodegradable polymer.
[0038] PBAT is a thermoplastic biodegradable plastic, a copolymer of butylene adipate and butylene terephthalate. It has the characteristics of both PBA and PBT, with good ductility and elongation at break, as well as good heat resistance and impact resistance. In addition, it has excellent biodegradability and is one of the most popular and best-used biodegradable materials in biodegradable plastic research.
[0039] Polybutylene succinate (PBS) is a high molecular weight compound, a white, semi-crystalline polymer. Depending on its molecular structure and molecular weight, its crystallinity ranges from 30% to 60%, with a crystallization temperature of 75°C. High-molecular-weight PBS exhibits superior mechanical properties to PE, with a melting point of approximately 115°C, meeting the requirements for general-purpose plastics. It is stable in dry environments, maintaining its performance over extended storage and trial periods. Because its structural units contain readily hydrolyzed ester groups, it is readily decomposed and metabolized by various naturally occurring microorganisms and enzymes in plants and animals when exposed to specific microorganisms, such as in composting, ultimately forming CO2 and H2O, thereby avoiding environmental contamination. It is important to note that PBS is completely biodegradable in soil, seawater, and compost, and therefore rapidly degrades after use.
[0040] Poly (L-lactic acid) (PLLC) is a polymer material synthesized chemically from L-lactic acid fermented from bioresources such as starch and molasses. PLLC is a thermoplastic material with similar plasticity to polystyrene and polyester. It exhibits high crystallinity, rigidity, and excellent tensile strength.
[0041] Polyvinyl alcohol (PVA) is the only vinyl polymer that can be used by bacteria as a carbon and energy source. Under the action of bacteria and enzymes, it can degrade by 75% in 46 days. It is a biodegradable polymer material that can be mass-produced by non-petroleum-based routes at a low cost. Its outstanding oil and solvent resistance and gas barrier properties offer unique advantages in food and pharmaceutical packaging. Starch-based PVA plastics are fully biodegradable (meaning they can be completely broken down into low-molecular compounds by microorganisms (such as bacteria, fungi, and algae) under appropriate and predictable natural environmental conditions).
[0042] Polylactic acid (PLA) is polymerized from lactide monomers extracted from plant sugars and can be completely degraded into water and carbon dioxide in industrial composting. Polyhydroxyalkanoates (PHA) are aliphatic copolyesters of varying structures synthesized by microorganisms through fermentation of various carbon sources. They are used not only in packaging materials and agricultural films, but also in a wide range of applications such as pharmaceuticals, cosmetics, and animal feed.
[0043] Furthermore, the organic decomposition aid is selected from one or more of lactose, galactose, vitamin E polyethylene glycol succinate and diisostearyl malate.
[0044] To further improve the dispersion uniformity of the photosensitizer, the inventors also proposed adding 0.5-1.6 parts by weight of a dispersant and 0.8-2 parts by weight of tricarboxylic acid to the prodegradant raw material. Furthermore, the dispersant is selected from polypropylene wax and / or polyethylene wax.
[0045] Using polypropylene wax and / or polyethylene wax as dispersants not only improves the uniformity of the photosensitizer's dispersion within the mesoporous silica but also enhances its uniformity in the final polymer after mixing with the prodegradant and PP, PE, or PP / PE alloy. The dispersant significantly enhances the uniformity of the prodegradant's dispersion by attracting and entangled with similar segments of the polypropylene or polyethylene, thereby enabling more uniform and rapid degradation of the PP, PE, or PP / PE alloy. Furthermore, the addition of tricarboxylic acid as a compatibilizer allows the biodegradable polymer encapsulated with the photosensitizer to more stably and rapidly mix with the PP, PE, or PP / PE alloy. The tricarboxylic acid can be one or more of citric acid, aconitic acid, and tricarboxylic acid.
[0046] Furthermore, the degradation aid for degrading PP and PE provided by the present invention can be selected from the following raw materials in parts by weight: 4-6 parts of photosensitizer, 2.5-3.6 parts of mesoporous silica, 58-66 parts of biodegradable polymer, 2-3 parts of organic decomposition aid, 0.9-1.2 parts of dispersant and 1.3-1.8 parts of tricarboxylic acid.
[0047] After repeated experiments by the inventors, it was found that when the degradation pro-agent for degrading PP and PE provided by the present invention is added to PP or PE or a PP / PE blend for use, when the addition ratio of the degradation pro-agent is 10wt%-30wt%, the degradation performance and other mechanical properties of the PP or PE or the PP / PE blend are comprehensively excellent.
[0048] In order to improve the performance of the prodegradant for degrading PP and PE provided by the present invention, the inventors propose to prepare the prodegradant using the following processing steps:
[0049] The mesoporous silica, the dispersant and the tricarboxylic acid are stirred and mixed at 130-170° C. for 50-70 minutes to disperse the mesoporous silica sufficiently evenly, reduce agglomeration, and disperse the tricarboxylic acid sufficiently evenly. Then, the photosensitizer is added, the rotation speed is increased by 50-80 rpm, and the mixture is stirred and mixed for 60-90 minutes. After the rotation speed is increased, the mesoporous silica, the dispersant and the tricarboxylic acid are further dispersed, and the photosensitizer is continuously inserted into the pores of the mesoporous silica. The photosensitizer is gradually sunk deep into the pores of the mesoporous silica. In addition, the presence of the tricarboxylic acid further strengthens the binding of the photosensitizer to the mesoporous silica. In the continuous stirring, the binding of the photosensitizer to the mesoporous silica is further disordered, making it more difficult for the photosensitizer to migrate, thereby ensuring the degradation ability of the polymer. The stirring and mixing is completed for 60-90 minutes, and then extruded and granulated to obtain the first auxiliary material.
[0050] The organic decomposition aid is heated until melted, and then the first auxiliary material is quickly added at a rotation speed of 100-150 rpm. After the addition is completed, the mixture is stirred at a constant speed of 100-150 rpm, and the temperature is simultaneously lowered at a rate of 5-10°C / min to gradually fix the organic decomposition aid on the surface of the first auxiliary material until it reaches room temperature. The biodegradable polymer is then added, and the mixture is discharged into a twin-screw extruder for extrusion and granulation, so that an ordered three-layer structure of biodegradable polymer, organic decomposition aid, and first auxiliary material is formed as much as possible. This allows the PP, PE, or PP / PE alloy to have better stability in use after being added thereto, and its degradation performance can also be guaranteed after being discarded. Finally, the degradation aid is obtained.
[0051] The present application also provides a PP, PE or PP / PE alloy, to which the above-mentioned degradation aid is added.
[0052] The present application will be further described below in conjunction with specific examples. It should be understood that these examples are intended to illustrate the present application only and are not intended to limit the scope of the present application. The experimental methods in the following examples where specific conditions are not specified are usually measured in accordance with national standards. If there are no corresponding national standards, then the methods are carried out in accordance with general international standards, conventional conditions, or according to the conditions recommended by the manufacturer.
[0053] Example 1
[0054] This embodiment provides a PP composite material, which contains 90 wt% PP and 10 wt% prodegradant. The PP and prodegradant are blended to obtain the PP composite material. The PP was purchased from Dongguan Fuzhong Plastic Raw Materials Co., Ltd.
[0055] The raw materials and preparation methods of the degradation aid are as follows:
[0056] 5 g of mesoporous silica, a dispersant (1.6 g of polypropylene wax) and tricarboxylic acid (2 g of aconitic acid) were stirred and mixed at 170° C. for 50 minutes, and then a photosensitizer (9 g of dodecylferrocene) was added. The rotation speed was increased to 80 rpm, and the mixture was stirred and mixed for 60 minutes. The mixture was then extruded and granulated to obtain the first auxiliary material.
[0057] The organic decomposition aid (5 g of lactose) was heated until melted, and then the first auxiliary material was quickly added at a speed of 150 rpm. After the addition, the mixture was stirred at a constant speed of 150 rpm and cooled at a rate of 10°C / min until it reached room temperature. Then, the biodegradable polymer (76 g of polylactic acid) was added and the mixture was discharged into a twin-screw extruder for extrusion and granulation to obtain the degradable aid.
[0058] Example 2
[0059] This example provides a PP composite material containing 70 wt% PP and 30 wt% prodegradant. The PP and prodegradant are blended to form the PP composite material. The PP was purchased from Dongguan Fuzhong Plastic Raw Materials Co., Ltd. ....
[0060] The raw materials and preparation methods of the degradation aid are as follows:
[0061] 2 g of mesoporous silica, a dispersant (0.5 g of polypropylene wax) and tricarboxylic acid (0.8 g of citric acid) were stirred and mixed at 130° C. for 70 minutes, and then a photosensitizer (3 g of stearic acid) was added. The rotation speed was increased by 50 rpm, and the mixture was stirred and mixed for 90 minutes. The mixture was then extruded and granulated to obtain the first auxiliary material.
[0062] The organic decomposition aid (1 g of galactose) was heated until melted, and then the first aid was quickly added at a speed of 100 rpm. After the addition, the mixture was stirred at a constant speed of 100 rpm and cooled at a rate of 5°C / min until it reached room temperature. Then, the biodegradable polymer (50 g of polyhydroxyalkanoate) was added and the mixture was discharged into a twin-screw extruder for extrusion and granulation to obtain the degradable aid.
[0063] Example 3
[0064] This embodiment provides a PP composite material, which contains 80 wt% PP and 20 wt% prodegradant. The PP and prodegradant are blended to obtain the PP composite material. The PP was purchased from Dongguan Fuzhong Plastic Raw Materials Co., Ltd.
[0065] The raw materials and preparation methods of the degradation aid are as follows:
[0066] 4 g of mesoporous silica, a dispersant (1.2 g of polypropylene wax) and tricarboxylic acid (1.2 g of triformic acid) were stirred and mixed at 150° C. for 60 minutes, and then a photosensitizer (6 g of ferric eleostearate) was added. The rotation speed was increased to 70 rpm, and the mixture was stirred and mixed for 80 minutes. The mixture was then extruded and granulated to obtain the first auxiliary material.
[0067] The organic decomposition aid (3 g of vitamin E polyethylene glycol succinate) was heated until melted, and then the first auxiliary material was quickly added at a speed of 130 rpm. After the addition, the mixture was stirred uniformly at a speed of 130 rpm, and the temperature was lowered at a rate of 8°C / min until it reached room temperature. Then, the biodegradable polymer (61 g of polybutylene succinate) was added, and the material was discharged into a twin-screw extruder for extrusion and granulation to obtain the degradation aid.
[0068] Example 4
[0069] This embodiment provides a PE composite material, which contains 90 wt% PE and 10 wt% prodegradant. The PE composite material is obtained by blending the PE and the prodegradant. PE was purchased from Dongguan Yongmao Plastic Materials Co., Ltd.
[0070] The raw materials and preparation methods of the degradation aid are as follows:
[0071] 3 g of mesoporous silica, a dispersant (0.5 g of polyethylene wax) and tricarboxylic acid (0.8 g of citric acid) were stirred and mixed at 130° C. for 70 minutes, and then a photosensitizer (4 g of benzophenone) was added. The rotation speed was increased to 60 rpm, and the mixture was stirred and mixed for 65 minutes. The mixture was then extruded and granulated to obtain the first auxiliary material.
[0072] The organic decomposition aid (2 g of diisostearyl malate) was heated until melted, and then the first auxiliary material was quickly added at a speed of 110 rpm. After the addition, the mixture was stirred uniformly at a speed of 110 rpm, and the temperature was lowered at a rate of 6°C / min until it reached room temperature. Then, the biodegradable polymer (55 g of polycaprolactone) was added, and the material was discharged into a twin-screw extruder for extrusion and granulation to obtain the degradation aid.
[0073] Example 5
[0074] This embodiment provides a PE composite material, which contains 70 wt% PE and 30 wt% prodegradant. The PE composite material is obtained by blending the PE and the prodegradant. PE was purchased from Dongguan Yongmao Plastic Materials Co., Ltd.
[0075] The raw materials and preparation methods of the degradation aid are as follows:
[0076] 4 g of mesoporous silica, a dispersant (0.9 g of polyethylene wax) and tricarboxylic acids (0.8 g of citric acid and 0.5 g of aconitic acid) were stirred and mixed at 140° C. for 65 minutes, and then a photosensitizer (4 g of nickel stearate) was added. The rotation speed was increased to 56 rpm, and the mixture was stirred and mixed for 75 minutes. The mixture was then extruded and granulated to obtain the first auxiliary material.
[0077] The organic decomposition aid (2 g of diisostearyl malate and 1 g of galactose) was heated until melted, and then the first auxiliary material was quickly added at a speed of 110 rpm. After the addition, the mixture was stirred uniformly at a speed of 110 rpm while cooling at a rate of 6°C / min until it reached room temperature. Then, the biodegradable polymer (45 g of polycaprolactone and 13 g of PBAT) was added, and the material was discharged into a twin-screw extruder for extrusion and granulation to obtain the decomposition aid.
[0078] Example 6
[0079] This embodiment provides a PE composite material, which contains 85 wt% PE and 15 wt% prodegradant. The PE composite material is obtained by blending the PE and the prodegradant. The PE was purchased from Dongguan Yongmao Plastic Materials Co., Ltd.
[0080] The raw materials and preparation methods of the degradation aid are as follows:
[0081] 3.6 g of mesoporous silica, a dispersant (1.2 g of polyethylene wax) and tricarboxylic acids (1 g of tricarboxylic acid and 0.8 g of aconitic acid) were stirred and mixed at 140° C. for 65 minutes, and then a photosensitizer (6 g of iron stearate) was added. The rotation speed was increased to 75 rpm, and the mixture was stirred and mixed for 70 minutes. The mixture was then extruded and granulated to obtain the first auxiliary material.
[0082] The organic decomposition aid (2 g of diisostearyl malate) was heated until melted, and then the first auxiliary material was quickly added at a speed of 130 rpm. After the addition, the mixture was stirred uniformly at a speed of 130 rpm, and the temperature was lowered at a rate of 7°C / min until it reached room temperature. Then, the biodegradable polymer (33 g of polyvinyl alcohol and 33 g of poly (L-lactic acid)) was added, and the material was discharged into a twin-screw extruder for extrusion and granulation to obtain the degradable aid.
[0083] Example 7
[0084] This embodiment provides a PP / PE blend material, which contains 45% PP, 45% PE, and 10% prodegradant. The blend material is obtained by melt-blending the three materials according to a conventional blending process.
[0085] The raw materials and preparation methods of the degradation aid are as follows:
[0086] 2.5 g of mesoporous silica, a dispersant (0.5 g of polyethylene wax and 0.5 g of polypropylene wax) and tricarboxylic acid (1 g of tricarboxylic acid and 0.8 g of aconitic acid) were stirred and mixed at 140° C. for 65 minutes, and then a photosensitizer (4 g of cerium stearate) was added. The rotation speed was increased to 65 rpm, and the mixture was stirred and mixed for 70 minutes. The mixture was then extruded and granulated to obtain the first auxiliary material.
[0087] The organic decomposition aid (2 g of diisostearyl malate and 2 g of vitamin E polyethylene glycol succinate) was heated until melted, and then the first auxiliary material was quickly added at a speed of 130 rpm. After the addition, the mixture was stirred uniformly at a speed of 130 rpm, and the temperature was lowered at a rate of 7°C / min until it reached room temperature. Then, a biodegradable polymer (33 g of polyvinyl alcohol, 33 g of poly-L-lactic acid and 4 g of polybutylene succinate) was added, and the material was discharged into a twin-screw extruder for extrusion and granulation to obtain the degradation aid.
[0088] Example 8
[0089] This embodiment provides a PP / PE blend material containing 35% PP, 35% PE, and 30% prodegradant by weight. The blend material is obtained by melt blending the three materials according to a conventional blending process.
[0090] The raw materials and preparation methods of the degradation aid are as follows:
[0091] 4.5 g of mesoporous silica, a dispersant (0.25 g of polyethylene wax and 0.25 g of polypropylene wax) and tricarboxylic acid (1.3 g of tricarboxylic acid) were stirred and mixed at 140° C. for 65 minutes, and then a photosensitizer (4 g of cerium stearate and 3 parts of iron eleostearate) was added. The rotation speed was increased to 65 rpm, and the mixture was stirred and mixed for 70 minutes. The mixture was then extruded and granulated to obtain the first auxiliary material.
[0092] The organic decomposition aid (1 g of lactose and 1.5 g of vitamin E polyethylene glycol succinate) was heated until melted, and then the first auxiliary material was quickly added at a speed of 130 rpm. After the addition, the mixture was stirred uniformly at a speed of 130 rpm, and the temperature was lowered at a rate of 7°C / min until it reached room temperature. Then, a biodegradable polymer (30 g of polyvinyl alcohol and 32 g of polylactic acid) was added, and the material was discharged into a twin-screw extruder for extrusion and granulation to obtain the degradation aid.
[0093] Example 9
[0094] This embodiment provides a PP / PE blend material, which contains 30% PP, 45% PE, and 25% by weight of a prodegradant. The blend material is obtained by melt-blending the three materials according to a conventional blending process.
[0095] The raw materials and preparation methods of the degradation aid are as follows:
[0096] 3.1 g of mesoporous silica, a dispersant (0.8 g of polyethylene wax and 0.8 g of polypropylene wax) and tricarboxylic acid (0.9 g of citric acid) were stirred and mixed at 140°C for 65 minutes, and then a photosensitizer (4 g of cerium stearate and 3 parts of iron eleostearate) was added. The rotation speed was increased to 65 rpm, and the mixture was stirred and mixed for 70 minutes. The mixture was then extruded and granulated to obtain the first auxiliary material.
[0097] The organic decomposition aid (1 g of lactose and 1.5 g of vitamin E polyethylene glycol succinate) was heated until melted, and then the first auxiliary material was quickly added at a speed of 130 rpm. After the addition, the mixture was stirred uniformly at a speed of 130 rpm, and the temperature was lowered at a rate of 7°C / min until it reached room temperature. Then, a biodegradable polymer (30 g of polycaprolactone and 30 g of polylactic acid) was added, and the material was discharged into a twin-screw extruder for extrusion and granulation to obtain the degradation aid.
[0098] Comparative Example 1
[0099] The only difference from Example 3 is the lack of mesoporous silica.
[0100] Comparative Example 2
[0101] The only difference from Example 6 is that the photosensitizer nickel stearate is replaced with an equal mass of benzophenone.
[0102] Test Example 1
[0103] Determination of the final aerobic biodegradability of the PP composite material provided in Example 3
[0104] 1. Test basis and method: Determination of the ultimate aerobic biodegradability of materials under controlled composting conditions, using the method of measuring released carbon dioxide, general method GB / T19277.1-2011.
[0105] 2. The characteristics of the test materials, reference materials and inoculum are shown in Table 1. Photos of the test materials are shown in Figure 1.
[0106] Table 1
[0107]
[0108] 3. Test conditions
[0109] During the test, the dry weight ratio of inoculum to test material / reference material in each 2L test bottle was approximately 6:1; the test system was aerated with decarbonated air so that the oxygen concentration discharged from each test bottle was not less than 6%, and the test was carried out at 58℃±2℃ in the dark; the amount of carbon dioxide produced during the test was determined by titration.
[0110] 4. Cumulative carbon dioxide production during the test period, g / bottle, is shown in Table 2. A graph of cumulative carbon dioxide production is shown in Figure 2.
[0111] Table 2
[0112]
[0113]
[0114] 5. The cumulative decomposition rate during the test period is shown in Table 3 below. The biodegradation rate curve is shown in Figure 3.
[0115] Table 3
[0116]
[0117]
[0118] 6. Test results: The biodegradability of the test material was 81.3% at the end of the 95th day (three parallel values were 78.3%, 81.9%, 83.8%, with an average of 81.3%), and the relative biodegradability was 94.4%.
[0119] 7. Test Conclusion: After testing, the relative biodegradability test results of the sample meet the requirement of "relative biodegradation rate should be ≥90%" in the "Degradation Performance and Labeling Requirements for Biodegradable Plastics and Products" (GB / T 41010-2021), and meet the requirement of "relative biodegradation rate should be ≥90%" for mixtures in the Hainan Provincial Local Standard "General Technical Requirements for Fully Biodegradable Plastic Products" (DB46 / T 505-2020).
[0120] Test Example 2
[0121] Biodegradation Test of PE Composite Materials Provided in Example 6 (Determination of Final Aerobic Biodegradability under Controlled Composting Conditions)
[0122] 1. Test basis: GB / T 19277.1-2011
[0123] 2. The test results are summarized in Table 4 below.
[0124] Table 4
[0125]
[0126] 3. Test Principle
[0127] This method determines the ultimate aerobic biodegradability and degree of disintegration of the test material under simulated conditions of intense aerobic composting. The inoculum used is obtained from a stable, mature compost, if possible, from the compost of organic matter from municipal solid waste. The test material is mixed with the inoculum and introduced into a static composting container. In this container, the mixture is subjected to intense aerobic composting at a specified temperature, oxygen concentration and humidity. The test period does not exceed 6 months.
[0128] During the aerobic biodegradation of the test material, carbon dioxide, water, mineralized inorganic salts, and new biomass are the final products of biodegradation. The carbon dioxide produced is continuously monitored and regularly measured during the test, and the amount of carbon dioxide produced is calculated using an instrument. The ratio of the actual amount of carbon dioxide produced by the test material during the test to the theoretical amount of carbon dioxide that the material can produce is the biodegradation percentage.
[0129] The theoretical release of carbon dioxide can be calculated based on the actual measured total organic carbon (TOC) content. The percentage of biodegradation does not include the amount of carbon converted into new cell biomass, as it is not metabolized into carbon dioxide during the test period.
[0130] 4. Test Materials
[0131] 4.1 Sample
[0132] Name: PE composite material provided in Example 6, made into a plastic bag (film)
[0133] Appearance: solid
[0134] Storage conditions: room temperature
[0135] 4.2 Reference substances
[0136] Reference materials
[0137] Name: Microcrystalline cellulose (column chromatography FCC)
[0138] Reference Material Number: 68005761
[0139] Batch number: 20210720
[0140] Source: Sinopharm Chemical Reagent Co., Ltd.
[0141] Molecular formula: (C6H 10 O5)n
[0142] Molecular weight: (162.14)n
[0143] CAS No.: 9004-34-6
[0144] Appearance: White or off-white powder
[0145] Storage conditions: Store in a dry place at room temperature
[0146] 4.3 Inoculum
[0147] Name: Aerobic Composting
[0148] Source: Homemade
[0149] Fat age: 3 months
[0150] Preliminary treatment: Screen through a 0.5 cm sieve to remove impurities and inert substances.
[0151] 4.4 Test conditions
[0152] The test was carried out at a constant temperature of 58℃±2℃, low light, and in the absence of any steam that may affect the growth of microorganisms.
[0153] 5. Test methods
[0154] (1) Aerate the test system with water-saturated air without CO2 at a flow rate of 0.05 L / min and conduct the test at 58℃±2℃.
[0155] (2) Measure the O2 concentration in the reaction vessel twice a day for the first week, and the number of measurements can be reduced thereafter. If necessary, adjust
[0156] Air flow. CO2 absorption was measured daily for the first 45 days and then twice a week.
[0157] (3) Determination of CO2:
[0158] Sodium hydroxide absorption method: When measuring CO2, remove the sodium hydroxide absorption bottle and connect it directly to the measurement. Move the remaining two absorption bottles forward in sequence and connect them to the anti-backflow device. Connect a fresh sodium hydroxide absorption bottle at the end. Titrate with HCl standard solution.
[0159] (4) Check the air tightness of the test device every day.
[0160] (5) The test container mixture was shaken and inverted every week to mix thoroughly. The pH of the mixture was measured and the following properties were observed: the odor of the exhaust gas from the test container, the moisture, color, and mold formation of the compost, and the structural changes and degree of disintegration of the test material.
[0161] (6) Calculate the theoretical release of carbon dioxide
[0162] The theoretical amount of carbon dioxide released (ThCO2) produced by the test material in each compost container is calculated according to formula (1) and expressed in grams (g).
[0163] ThCO2=M ToT ×C ToT×44 / 12 (1)
[0164] Where:
[0165] M ToT : total dry solids in the test material added to the compost container at the beginning of the test, in grams (g);
[0166] C ToT : the ratio of total organic carbon to total dry solids in the test material, in grams per gram (g / g);
[0167] 44 and 12: represent the molecular weight of carbon dioxide and the atomic weight of carbon respectively.
[0168] (7) Calculation of biodegradation percentage
[0169] During each measurement period, the biodegradation percentage Dt of the test material was calculated based on the cumulative amount of carbon dioxide released using formula (2)
[0170] (%):
[0171] Dt=[(CO2) T -(CO2) B ] / ThCO2×100 (2)
[0172] Where:
[0173] (CO2) T : The cumulative amount of carbon dioxide released from each compost container containing the test mixture, in grams per container (g / container);
[0174] (CO2) B : The average amount of carbon dioxide released by the blank containers, in grams per container (g / container);
[0175] ThCO2: The theoretical release of carbon dioxide produced by the test material, expressed in grams per container (g / container).
[0176] If the relative deviation of each result was less than 20%, the average biodegradation percentage was calculated; otherwise, the value for each compost container was used separately.
[0177] The biodegradation rate of the reference material was calculated using the same method.
[0178] 6. Test results
[0179] The test results are shown in Figures 4, 5, and 6. Figure 4A shows a photograph of the test sample after mixing with compost, and Figure 4B shows a photograph 140 days later. Figure 5 plots the cumulative carbon dioxide production (g / container) versus time for the blank, sample, and reference materials. Figure 6 plots the biodegradation percentage (%) versus time for the sample and reference materials.
[0180] (1) The biodegradation percentages of the three reaction bottles of the reference material at the end of the test (140 days) were 82.63%, 82.75% and 82.55%, respectively, with an average of 82.6%. The relative deviations of the biodegradation percentages of the three reaction bottles were 0.04%, 0.18% and 0.06%, respectively, and all were no more than 20%.
[0181] (2) The biodegradation percentages of the three reaction bottles of the test sample at the end of the test (140 days) were 75.40%, 75.27%, and 75.54%, respectively; the average biodegradation percentage was 75.4%. The relative deviations of the biodegradation percentages of the three reaction bottles were 0.01%, 0.17%, and 0.18%, respectively; all less than 20%. The relative decomposition rate was 91.2%. The volatile solids content of the sample was 56.2%.
[0182] (3) The average decomposition rate is: 75.4%, ≥60%, which is qualified; the relative decomposition rate is: 91.2%, ≥90%, which is qualified; the organic component (volatile solid content) is: 56.2%, ≥51%, which is qualified.
[0183] Test Example 3
[0184] Analysis of degradation behavior of samples provided in the examples under simulated natural environment
[0185] 1. Test Method
[0186] A UV aging chamber (Tianjin Yonglida Material Testing Machine Co., Ltd.) was used to simulate exposure to light and rain in the natural environment to study the degradation behavior of the samples provided in Examples 1, 3, 4, 6, 9, Comparative Example 1, and 2. The seven samples provided in the above Examples and Comparative Examples were made into films according to the national standard GB / T 1040.2, cut into standard strips, and placed in a UV aging chamber for degradation. The films were sprayed for 10 minutes every 12 hours. Samples were removed at 5, 10, 15, 20, 25, and 30 days and dried at 65°C for 4 hours. Five replicates were made for each sample.
[0187] 2. Mechanical properties analysis
[0188] Standard tensile specimens prepared according to GB / T 1040.2 were tested for tensile properties before and after degradation using a QJ210A-1000N universal testing machine manufactured by Shanghai Qingji Instrument Technology Co., Ltd. at a tensile rate of 2 mm / min. Five specimens were tested in each group, and the average value was calculated. The decrease in maximum tensile force of the samples is shown in Table 5. This indicates that the mechanical properties of the sample provided in Example 3 have significantly decreased, and degradation is particularly prominent.
[0189] Table 5
[0190]
[0191] 3. Gel chromatography (GPC)
[0192] The molecular weight distribution and molecular weight of the samples were determined using an Agilent 1200 Series gel permeation chromatography system. Sample preparation: Dissolve the sample in chloroform, filter it through an ultra-microporous filter membrane using a syringe, and inject 2 ml for testing. Chloroform was used as the solvent, and polystyrene was used as the standard.
[0193] After testing, after 30 days of degradation in the aging box, the molecular weight of the samples was significantly reduced. The number average molecular weight of the sample provided in Example 3 was reduced by 86.39%, and the number average molecular weight of the sample provided in Example 6 was reduced by 83.61%. The molecular weight reduction of these two groups of samples was better than that of other groups of samples.
[0194] In summary, the degradation aid for degrading PP and PE provided in this application can effectively ensure the degradation ability of resins such as PP, PE, and PP / PE blends, and has a simple production process, low cost, and is suitable for industrial production.
[0195] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a hard limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numbers within the range. For example, the description of a range from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0196] The foregoing is merely a list of specific embodiments of the present application, intended to enable those skilled in the art to understand or implement the present application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application is not limited to the embodiments shown herein, but is intended to conform to the broadest scope consistent with the principles and novel features of the present application.
Claims
1. A degradation aid for degrading PP and PE, characterized in that: The invention comprises the following raw materials in parts by weight: 3-9 parts of photosensitizer, 2-5 parts of mesoporous silica, 50-76 parts of biodegradable polymer and 1-5 parts of organic decomposition aid.
2. The degradation aid for degrading PP and PE according to claim 1, characterized in that: The photosensitizer is selected from one or more of ferric eleostearate, dodecylferrocene, benzophenone, stearic acid, cerium stearate, iron stearate and nickel stearate.
3. The degradation aid for degrading PP and PE according to claim 1, characterized in that: The biodegradable polymer is selected from one or more of polylactic acid, polyhydroxyalkanoate, polybutylene succinate, polycaprolactone, PBAT, polyvinyl alcohol and poly-L-lactic acid.
4. The degradation aid for degrading PP and PE according to claim 1, characterized in that: The organic decomposition aid is selected from one or more of lactose, galactose, vitamin E polyethylene glycol succinate and diisostearyl malate.
5. The degradation aid for degrading PP and PE according to claim 1, characterized in that: The invention also comprises the following raw materials in parts by weight: 0.5-1.6 parts of a dispersant and 0.8-2 parts of tricarboxylic acid, wherein the dispersant is selected from polypropylene wax and / or polyethylene wax.
6. The degradation aid for degrading PP and PE according to claim 5, characterized in that: The invention comprises the following raw materials in parts by weight: 4-6 parts of photosensitizer, 2.5-3.6 parts of mesoporous silica, 58-66 parts of biodegradable polymer, 2-3 parts of organic decomposition assistant, 0.9-1.2 parts of dispersant and 1.3-1.8 parts of tricarboxylic acid.
7. The degradation aid for degrading PP and PE according to any one of claims 1 to 6, characterized in that: The addition ratio of the prodegradant in PP or PE or PP / PE blend is 10wt%-30wt%.
8. The degradation aid for degrading PP and PE according to claim 5, characterized in that: The prodegradant is processed by the following steps: The photosensitizer, the mesoporous silica, the dispersant and the tricarboxylic acid are mixed, and then the organic decomposition aid and the biodegradable polymer are added to obtain the degradation aid.
9. The degradation aid for degrading PP and PE according to claim 8, characterized in that: The mesoporous silica, the dispersant and the tricarboxylic acid are stirred and mixed at 130-170° C. for 50-70 minutes, and then the photosensitizer is added, the rotation speed is increased by 50-80 rpm, and the mixture is stirred and mixed for 60-90 minutes, and then extruded and granulated to obtain a first auxiliary material, and then the first auxiliary material is mixed with the organic decomposition auxiliary agent and the biodegradable polymer to obtain the degradation auxiliary agent.
10. The degradation aid for degrading PP and PE according to claim 9, characterized in that: The organic decomposition aid is heated until it is melted, and then the first auxiliary material is quickly added at a rotation speed of 100-150 rpm. After the addition is completed, the temperature is lowered at a speed of 5-10°C / min until it reaches room temperature, and then the biodegradable polymer is added. The material is discharged into a twin-screw extruder for extrusion and granulation to obtain the degradation aid.
Citation Information
Patent Citations
Modified polyglycolic acid biodegradable mulch film and preparation method thereof
CN109575536A
Photodegradable polypropylene material and preparation method thereof
CN114395190A
Degradation auxiliary agent for degrading PP (polypropylene) and PE (polyethylene)
CN116178921A
Degradable resin composition and method for producing thereof
KR100639106B1
Degradable resin composition using dditives for plastics and method for producing thereof
KR1020130140347A
Cited By
High-strength material prepared from recycled PP
CN120699357A