Battery and electric apparatus

By introducing the positive electrode film layer and lithium replenishing agent into the secondary battery, optimizing the structure of the electrolyte and active materials, the problem of insufficient battery cycle performance and power capacity is solved, and higher battery performance and longer service life are achieved.

WO2024222152A1PCT designated stage expired Publication Date: 2024-10-31CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2024/076845
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-02-08
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing secondary batteries have deficiencies in cycle performance, capacity development and power capabilities, making it difficult to meet increasingly high application demands.

Method used

By introducing a positive electrode film layer and a lithium replenishing agent into the battery, the wettability of the electrolyte and the transmission path of active ions are optimized, the active ion conductivity of the positive electrode sheet is improved, and the positive electrode active material with a multi-layer coating structure is used to enhance the battery. overall power capabilities and cycle performance.

Benefits of technology

It significantly improves the overall power capability and cycle performance of the battery, improves the power capability at low SOC, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024076845_31102024_PF_FP_ABST
    Figure CN2024076845_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides a battery and an electric apparatus. The battery comprises a cell, a cell shell wrapping the cell and an electrolyte. The cell comprises a cathode piece, the cathode piece comprises a cathode current collector and a cathode film layer arranged on at least one surface of the cathode current collector, and the cathode film layer comprises a cathode active material. The battery satisfies the following: α×ρEL / (PD×Ccathode)+V×h / Ccell≤mEL.
Need to check novelty before this filing date? Find Prior Art

Description

Battery and power device

[0001] This application claims priority to Chinese patent application No. 202310477745.6 filed on April 28, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0002] The present application relates to the technical field of secondary batteries, and in particular to a battery and an electrical device. Background Art

[0003] In recent years, the application of secondary batteries has become increasingly widespread. They are widely used in energy storage power systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. As secondary batteries have achieved great development, higher requirements have been placed on their cycle performance, capacity utilization, and power capabilities.

[0004] Summary of the Invention

[0005] This application is made in view of the above-mentioned problems, and its purpose is to provide a battery and an electrical device. The overall power capability of the battery of the application is improved, and the cycle performance and capacity are improved.

[0006] To achieve the above-mentioned object, the present application provides a battery in a first aspect, comprising a battery cell, a battery cell shell covering the battery cell, and an electrolyte, wherein the battery cell comprises a positive electrode sheet, the positive electrode sheet comprises a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, the positive electrode film layer comprising a positive electrode active material;

[0007] Furthermore, the battery satisfies: α×ρ EL / (PD×C cathode )+V×h / C cell ≤m EL

[0008] Wherein, α is the porosity of the positive electrode sheet; ρ EL is the density of the electrolyte, in g / cm 3 PD is the compaction density of the positive electrode sheet under a pressure of 20-80 tons, in g / cm 3 ; C cathode is the gram capacity of the positive electrode active material, in mAh / g; V is the volume of the battery shell, in cm 3 ; h is the ratio of the thickness of the battery cell to the thickness of the battery cell shell; C cell is the capacity of the battery, in Ah; m EL is the minimum filling coefficient of the battery cell.

[0009] Therefore, the battery of the present application meets the above conditions, improves the wettability of the electrolyte to the positive electrode plate, shortens the transmission path of the active ions, improves the overall power capacity of the battery, and at the same time improves the active ion conductivity of the positive electrode plate interface, thereby improving the battery's cycle performance and capacity.

[0010] In any embodiment, the battery has at least two voltage plates;

[0011] Optionally, the battery has at least one voltage platform ≤3.5V;

[0012] Optionally, the battery has at most one voltage plateau ≤ 3.4V.

[0013] As a result, the power capability of the battery at low SOC is improved, and the overall power capability of the battery is improved.

[0014] In any embodiment, the battery's discharge capacity of ≤3.5V accounts for 2%-50% of the entire discharge capacity, and can be optionally 5%-30%.

[0015] As a result, the power capability of the battery at low SOC is improved, the overall power capability of the battery is enhanced, and / or the cycle performance of the battery is improved.

[0016] In any embodiment, the positive electrode film layer further includes a lithium supplement agent;

[0017] Optionally, the lithium supplement includes one or more of Li3N, Li2S / Co composite material, LiF / Co composite material, Li2O / Co composite material, Li2O2, Li2NiO2, Li5FeO4, Li2C2O4, Li2C4O4, Li2C3O5 and Li2C4O6;

[0018] Optionally, the mass content of the lithium supplement in the positive electrode film layer is 1%-40%.

[0019] Therefore, the present application increases the infiltration effect of the electrolyte, shortens the transmission path of active ions, improves the overall power capacity of the battery and / or improves the cycle performance of the battery by using a lithium supplement agent to form in situ pores.

[0020] In any embodiment, the positive electrode active material includes a first positive electrode active material; the first positive electrode active material includes a compound LiNi b Co d Mn e M fO2, wherein the M includes one or more elements of Al, Mg, Ca, Na, Ti, W, Zr, Sr, Cr, Zn, Ba, B, S and Y, and can optionally include Mg element and / or Al element; the b is 0.314-0.970; the d is 0-0.320, and can optionally be 0.047-0.320; the e is 0.006-0.390; and the sum of b, d, e and f is 1 and f is greater than 0.

[0021] In any embodiment, the mass content of the first positive electrode active material in the positive electrode active material is 20%-98%, thereby increasing the overall power capacity of the battery and / or improving the cycle performance of the battery.

[0022] In any embodiment, the positive electrode active material further includes a second positive electrode active material; the second positive electrode active material comprises a compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n , wherein A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; C includes one or more elements selected from B (boron), S, Si and N; D includes one or more elements selected from S, F, Cl and Br; a is 0.9-1.1; x is 0-0.1; y is 0.001-0.6; z is 0.001-0.1; and n is 0-0.1.

[0023] In any embodiment, the second positive electrode active material includes a core and a shell covering the core; the core contains the compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n , the shell comprises carbon element.

[0024] In any embodiment, the second positive electrode active material includes a core and a shell covering the core; the shell includes a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer; wherein the core contains the compound Li a A x Mn 1-y By P 1- z C z O 4-n D n , the first coating layer comprises crystalline pyrophosphate Li g EP2O7 and / or E h (P2O7) i The second coating layer comprises crystalline phosphate X j PO4, the third coating layer contains carbon;

[0025] Wherein, the crystalline pyrophosphate Li g EP2O7 and E h (P2O7) i wherein E independently includes one or more elements selected from the group consisting of Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al; X includes one or more elements selected from the group consisting of Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al; g is greater than 0 and less than or equal to 2; h is greater than 0 and less than or equal to 4; i is greater than 0 and less than or equal to 3; and j is greater than 0 and less than or equal to 3.

[0026] In any embodiment, the positive electrode active material consists of the first positive electrode active material and the second positive electrode active material.

[0027] As a result, the overall power capability of the battery is enhanced, and the power capability of the battery at low SOC is improved.

[0028] In any embodiment, the mass content of the polycrystalline particles in the positive electrode active material is 0%-100%;

[0029] Optionally, the primary particle size of the polycrystalline particles is 20-1000 nm.

[0030] This helps shorten the transmission path of active ions and further improve the power capacity of the battery.

[0031] The second aspect of the present application further provides an electrical device comprising the battery of the first aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] FIG1 is a schematic diagram of a secondary battery according to an embodiment of the present application.

[0033] FIG. 2 is an exploded view of the secondary battery according to the embodiment of the present application shown in FIG. 1 .

[0034] FIG3 is a schematic diagram of a battery module according to an embodiment of the present application.

[0035] FIG4 is a schematic diagram of a battery pack according to an embodiment of the present application.

[0036] FIG. 5 is an exploded view of the battery pack shown in FIG. 4 according to an embodiment of the present application.

[0037] FIG6 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.

[0038] Explanation of reference numerals: 1 battery pack; 2 upper case; 3 lower case; 4 battery module; 5 secondary battery; 51 housing; 52 electrode assembly; 53 top cover assembly. DETAILED DESCRIPTION

[0039] Below, the embodiments of the secondary battery, battery module, battery pack and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0040] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0041] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0042] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0043] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, a method includes steps (a) and (b), which indicates that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, a method may further include step (c), which indicates that step (c) may be added to the method in any order, for example, the method may include steps (a), (b), and (c), or may include steps (a), (c), and (b), or may include steps (c), (a), and (b), etc.

[0044] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may indicate that other components not listed may also be included or that only the listed components are included.

[0045] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0046] Unless otherwise specified, in the present application, the term "single crystal / quasi-single crystal particle" means a single particle (ie, a primary particle).

[0047] If not otherwise specified, in this application, the terms "secondary particles" and "polycrystalline material particles" generally have similar meanings, which refer to particles formed by the agglomeration of more than 100 primary particles with an average particle size in the range of 50-800 nm.

[0048] [Secondary battery]

[0049] Secondary batteries, also known as rechargeable batteries or storage batteries, are batteries that can be recharged to activate the active materials after discharge and continue to be used.

[0050] Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte. During the battery's charge and discharge process, active ions (such as lithium ions) are embedded and released back and forth between the positive and negative electrode sheets. The separator is set between the positive and negative electrode sheets, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The electrolyte between the positive and negative electrode sheets mainly plays the role of conducting active ions.

[0051] One embodiment of the present application provides a battery, comprising a battery cell, a battery cell shell covering the battery cell, and an electrolyte, wherein the battery cell comprises a positive electrode sheet, the positive electrode sheet comprises a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, the positive electrode film layer comprising a positive electrode active material;

[0052] Furthermore, the battery satisfies: α×ρ EL / (PD×C cathode )+V×h / C cell ≤m EL

[0053] Wherein, α is the porosity of the positive electrode sheet; ρ EL is the density of the electrolyte, in g / cm 3 PD is the compaction density of the positive electrode sheet under a pressure of 20-80 tons, in g / cm 3 ; C cathode is the gram capacity of the positive electrode active material, in mAh / g; V is the volume of the battery shell, in cm 3 ; h is the ratio of the thickness of the battery cell to the thickness of the battery cell shell; C cell is the capacity of the battery, in Ah; m EL is the minimum filling coefficient of the battery cell.

[0054] Although the mechanism is still unclear, the applicant unexpectedly discovered that: by making the battery meet the above conditions, the present application improves the wettability of the electrolyte to the positive electrode plate, shortens the transmission path of the active ions, and improves the overall power capacity of the battery. At the same time, it improves the conductivity of the active ions at the interface of the positive electrode plate, thereby improving the battery's cycle performance and capacity.

[0055] In some embodiments, the porosity α of the positive electrode sheet is tested using conventional methods in the art; for example, referring to the method of GB / T 24586-2009, the positive electrode sheet is immersed in ethyl methyl carbonate (EMC) for cleaning, and the true volume V0 and apparent volume V of the positive electrode sheet are measured by a porosimeter using a gas displacement method at room temperature and a relative humidity of ≤2% RH. The porosity α of the positive electrode sheet is calculated according to the following formula; α = 100% × (V-V0) / V.

[0056] In some embodiments, the density of the electrolyte is EL The electrolyte density ρ is tested using conventional methods in the field, for example, according to the "Test Method B—U-type Vibrating Tube Method" in the standard GB / T 2013-2010. EL .

[0057] In some embodiments, the compaction density PD of the positive electrode sheet under a pressure of 20-80 tons is tested using conventional methods in the art; for example, the positive electrode sheet is placed in a special compaction mold, and then the mold is placed on a compaction density instrument, and a pressure of 20-80 tons is applied. After the pressure is released, a high-precision balance is used to measure the surface density of the positive electrode sheet, and a micrometer is used to measure the thickness of the positive electrode sheet. The compaction density PD of the positive electrode sheet is calculated according to the following formula; PD = surface density of the positive electrode sheet / thickness of the positive electrode sheet.

[0058] In some embodiments, the gram capacity C of the positive electrode active material is cathode The test is conducted using conventional methods in the field; for example, a button cell is made of a positive electrode sheet and a counter electrode lithium sheet. In a constant temperature environment of 25°C, the battery is charged to the target voltage using a constant current of 0.1C, and then discharged to the cut-off voltage using a constant current of 0.1C to obtain the discharge capacity of the battery. The gram capacity C of the positive electrode active material is calculated by dividing the discharge capacity of the battery by the mass of the positive electrode active material in the positive electrode sheet. cathode .

[0059] In some embodiments, the volume V of the battery cell casing is measured using conventional methods in the art; for example, the length, width, and height of the battery cell casing are measured using a micrometer, and the product of the length, width, and height is calculated.

[0060] In some embodiments, the ratio h of the thickness of the battery cell to the thickness of the battery cell shell is tested using conventional methods in the art; for example, a micrometer is used to measure the thickness of a single battery cell and the thickness of the battery cell shell, and the ratio h of the battery cell thickness to the battery cell shell thickness is calculated.

[0061] In some embodiments, the capacity of the battery C cell The conventional method in the field is used for testing; for example, in a constant temperature environment of 25°C, the battery is left to stand for 10 minutes, then discharged at 0.33C to the cut-off voltage, left to stand for 10 minutes, charged at a constant current of 0.33C to the target voltage, charged at a constant voltage until the current is ≤0.05C, and left to stand for 10 minutes, discharged at 0.33C to the cut-off voltage. The discharge capacity at this time is C0; left to stand for 10 minutes, charged at a constant current of 0.33C0 to the target voltage, charged at a constant voltage until the current is ≤0.05C0, and left to stand for 10 minutes, discharged at 0.33C0 to the cut-off voltage. The discharge capacity at this time is recorded as the capacity C of the battery. cell .

[0062] In some embodiments, the minimum filling coefficient m of the battery cell is EL Use conventional methods in the field to test. For example, the capacity of the battery cells with a series of gradient injection coefficients is tested in the same way as above. cellIn the test, each cell is measured multiple times in parallel, the highest and lowest values ​​are removed, and the remaining average is taken as the cell capacity; the filling coefficient is used as the X-axis and the cell capacity is used as the Y-axis to make a segmented line graph. The X-axis value corresponding to the inflection point on the graph is the minimum filling coefficient m of the cell. EL .

[0063] In some embodiments, the battery has at least two voltage platforms, such as 2, 3, 4, 5, 6, 7, 8, 9, 10, and ranges consisting of any of the above values;

[0064] Optionally, the battery has at least one voltage platform ≤ 3.5 V, such as 1, 2, 3, 4, 5, 6, or any range thereof;

[0065] Optionally, the battery has at most one voltage platform ≤ 3.4V, for example, 0 or 1.

[0066] As a result, the power capability of the battery at low SOC is improved, and the overall power capability of the battery is improved.

[0067] In some embodiments, the number of voltage plateaus is determined using routine methods in the art. For example, the test method is as follows: in a constant temperature environment of 25°C, the battery is allowed to stand for 10 minutes, then discharged at 0.33C to the cut-off voltage, allowed to stand for 10 minutes, charged at a constant current of 0.33C to the target voltage, charged at a constant voltage to a current ≤0.05C, allowed to stand for 10 minutes, discharged at 0.33C to the cut-off voltage, and the discharge capacity at this time is recorded as C0; allowed to stand for 10 minutes, then charged at a constant current of 0.33C0 to the target voltage, charged at a constant voltage to a current ≤0.05C0, allowed to stand for 10 minutes, discharged at 0.33C0 to the cut-off voltage, and the discharge capacity at this time is recorded as 100% SOC; the discharge capacity is plotted against the voltage to obtain the SOC-OCV curve, and the dQ / dV curve is obtained by taking the derivative once. The number of peaks appearing on the dQ / dV curve is the number of voltage platforms of the battery, the number of peaks appearing in the voltage range ≤3.5V is the number of voltage platforms of the battery ≤3.5V, and the number of peaks appearing in the voltage range ≤3.4V is the number of voltage platforms of the battery ≤3.4V.

[0068] In some embodiments, the battery's ≤3.5V discharge capacity accounts for 2%-50% of the total discharge capacity, optionally 5%-30%, for example, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% and any range consisting of the above values.

[0069] As a result, the power capability of the battery at low SOC is improved, the overall power capability of the battery is enhanced, and / or the cycle performance of the battery is improved.

[0070] In some embodiments, the proportion of the battery's discharge capacity at ≤3.5V to the total discharge capacity is measured using conventional methods in the art. For example, the test method is as follows: On the SOC-OCV curve, the discharge capacity corresponding to a voltage of 3.5V is Q1, and the full discharge voltage corresponds to the total discharge capacity Q2. The proportion of the battery's discharge capacity at ≤3.5V to the total discharge capacity, C, is calculated using the following formula: C (%) = 100 × (Q2 - Q1) / Q2.

[0071] In some embodiments, the positive electrode film layer further includes a lithium supplement agent;

[0072] Optionally, the lithium supplement includes one or more of Li3N, Li2S / Co composite material, LiF / Co composite material, Li2O / Co composite material, Li2O2, Li2NiO2, Li5FeO4, Li2C2O4, Li2C4O4, Li2C3O5 and Li2C4O6;

[0073] Optionally, the mass content of the lithium supplement in the positive electrode film layer is 1%-40%, for example, 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40% and any range thereof.

[0074] Therefore, the present application increases the infiltration effect of the electrolyte, shortens the transmission path of active ions, improves the overall power capacity of the battery and / or improves the cycle performance of the battery by using a lithium supplement agent to form in situ pores.

[0075] Li2S / Co composite materials, LiF / Co composite materials, and Li2O / Co composite materials are all conventional composite materials in the art. Their element ratios, compound ratios, and preparation methods are well known to those skilled in the art. The preparation methods of the above composite materials include but are not limited to melting methods.

[0076] In some embodiments, the positive electrode active material includes a first positive electrode active material; the first positive electrode active material includes a compound LiNi b Co d Mn e M fO2, wherein the M includes one or more elements selected from the group consisting of Al, Mg, Ca, Na, Ti, W, Zr, Sr, Cr, Zn, Ba, B, S, and Y, and may optionally include Mg and / or Al; the b is 0.314-0.970, such as 0.314, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.8, 0.9, 0.97, and any of the above values; the d is 0-0.3 20, which can be selected from 0.047-0.320, for example, 0, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.32, and any range thereof; said e is 0.006-0.390, for example, 0.01, 0.05, 0.1, 0.12, 0.15, 0.18, 0.2, 0.25, 0.3, 0.35, 0.39, and any range thereof; and the sum of b, d, e, and f is 1, and f is greater than 0.

[0077] In some embodiments, the mass content of the first positive electrode active material in the positive electrode active material is 20%-98%, for example, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 60%, 70%, 80%, 85%, 90%, 95%, 98%, and any range thereof. Thus, the overall power capability of the battery is increased and / or the cycle performance of the battery is improved.

[0078] In some embodiments, the positive electrode active material further comprises a second positive electrode active material; the second positive electrode active material comprises a compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n, wherein A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo, and W; B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb, and Ge; C includes one or more elements selected from B (boron), S, Si, and N; D includes one or more elements selected from S, F, Cl, and Br; a is 0.9-1.1, for example, 0.9, 0.95, 1, 1.05, 1.1, and the range of any of the above values; x is 0-0.1, for example, 0, 0.02, 0.05, 0.07, 0.1, and the range of any of the above values. The y range is 0.001-0.6, for example, 0.005, 0.01, 0.015, 0.02, 0.025, 0.03, 0.04, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, and any range thereof; the z range is 0.001-0.1, for example, 0.001, 0.005, 0.01, 0.03, 0.05, 0.07, 0.1, and any range thereof; the n range is 0-0.1, for example, 0, 0.001, 0.003, 0.005, 0.01, 0.03, 0.05, 0.07, 0.1, and any range thereof.

[0079] In some embodiments, the second positive electrode active material includes a core and a shell covering the core; the core comprises a compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n , the shell comprises carbon element.

[0080] In some embodiments, the second positive electrode active material includes a core and a shell covering the core; the shell includes a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer; wherein the core comprises a compound Li a A x Mn 1-y B y P 1- z C z O 4-n D n , the first coating layer comprises crystalline pyrophosphate Li g EP2O7 and / or E h (P2O7) i The second coating layer comprises crystalline phosphate X jPO4, the third coating layer contains carbon;

[0081] Wherein, the crystalline pyrophosphate Li g EP2O7 and E h (P2O7) i wherein E independently comprises one or more elements selected from the group consisting of Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; wherein X comprises one or more elements selected from the group consisting of Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; wherein g is greater than 0 and less than or equal to 2, for example, 0.5, 1, 1.5, 2, and a range consisting of any of the above values; wherein h is greater than 0 and less than or equal to 4, for example, 0.5, 1, 1.4, 2, 2.5, 3, 3.6, 4, and a range consisting of any of the above values; wherein i is greater than 0 and less than or equal to 3, for example, 0.5, 1, 1.4, 2, 2.5, 3, and a range consisting of any of the above values; wherein j is greater than 0 and less than or equal to 3, for example, 0.5, 1, 1.4, 2, 2.5, 3, and a range consisting of any of the above values.

[0082] In some embodiments, the positive electrode active material consists of the first positive electrode active material and the second positive electrode active material.

[0083] As a result, the overall power capability of the battery is enhanced, and the power capability of the battery at low SOC is improved.

[0084] In some embodiments, the mass content of the polycrystalline particles in the positive electrode active material is 0%-100%;

[0085] Optionally, the primary particle size of the polycrystalline particles is 20-1000 nm.

[0086] This helps shorten the transmission path of active ions and further improve the power capacity of the battery.

[0087] In some embodiments, the primary particle size of the polycrystalline particles is tested using conventional methods in the art; for example, the testing method is: using a scanning electron microscope to test the positive electrode active material, adjusting the sample and magnification so that there are more than 10 agglomerated particles in the field of view, measuring the number of primary particles that make up each agglomerated particle, and using a ruler to measure the length direction of the primary particles as the particle size, sorting the particle size of the primary particles in each agglomerated particle from large to small, removing 1 / 10 of the largest particle size data and 1 / 10 of the smallest particle size data, and taking the average of the remaining particle size data as the average particle size of the primary particles in the agglomerated particle. If the number and average particle size of the primary particles in more than 50% (including 50%) of the agglomerated particles meet the definition of "polycrystalline material particles", the positive electrode active material is determined to be a polycrystalline material, and the average particle size of the primary particles of the polycrystalline material is recorded as the particle size of the primary particles.

[0088] In some embodiments, the polycrystalline particle content in the positive electrode active material is tested using conventional methods in the art; for example, the testing method includes: testing the positive electrode active material using SEM and EDS, confirming the elemental species of the polycrystalline material using the EDS elemental testing results, and combining the particle morphology obtained by SEM to determine the elemental differences between the polycrystalline particles and the single crystal particles. The element species and proportions are obtained by ICP testing the positive electrode active material, thereby calculating the polycrystalline particle content in the positive electrode active material.

[0089] In this application, LiNi b Co d Mn e M f O2、Li a A x Mn 1-y B y P 1-z C z O 4-n D n 、Li g EP2O7、E h (P2O7) i and X j PO4 remains electrically neutral.

[0090] Unless otherwise specified, in the above chemical formula, when M is two or more elements, the above-mentioned numerical ranges for f are not only defined for the stoichiometric coefficients of each element serving as M, but also for the sum of the stoichiometric coefficients of each element serving as M. For example, when M is two or more elements M1, M2, ..., Mn, the stoichiometric coefficients f1, f2, ..., fn of each of M1, M2, ..., Mn must each fall within the numerical range defined for f in this application, and the sum of f1, f2, ..., fn must also fall within this numerical range. Similarly, for the case where A, B, C, D, E, and X are two or more elements, the numerical ranges for their stoichiometric coefficients defined in this application also have the above meanings.

[0091] The preparation method of the second positive electrode active material of the present application comprises the following steps:

[0092] Steps for providing core material: The core material contains Li a A x Mn 1-y B y P 1-z C z O 4-n D n , wherein A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo, and W; B includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb, and Ge; C includes one or more elements selected from B (boron), S, Si, and N; D includes one or more elements selected from S, F, Cl, and Br; a is 0.9-1.1; x is 0-0.1; y is 0.001-0.6; z is 0.001-0.1; and n is 0-0.1;

[0093] The first coating step: providing a coating containing Li g EP2O7 and / or E h (P2O7) i The core material and the first mixture are mixed, dried, and sintered to obtain a material coated with a first coating layer; wherein the crystalline pyrophosphate Li g EP2O7 and E h (P2O7) i Each of the E's independently comprises one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al; g is greater than 0 and less than or equal to 2; h is greater than 0 and less than or equal to 4; and i is greater than 0 and less than or equal to 3;

[0094] The second coating step: providing a crystalline phosphate X jA second mixture of PO4, mixing the material coated with the first coating layer with the second mixture, drying, and sintering to obtain a material coated with two layers of coating layers; wherein X includes one or more elements selected from the group consisting of Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al; and j is greater than 0 and less than or equal to 3;

[0095] The third coating step is to provide a third mixture containing a carbon source, mix the material coated with the two coating layers with the third mixture, dry, and sinter to obtain a second positive electrode active material.

[0096] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0097] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0098] In some embodiments, the second positive electrode active material may be replaced by other positive electrode active materials known in the art, including, by way of example, but not limited to, lithium iron phosphate (also referred to as LFP), lithium manganese iron phosphate (also referred to as LMFP), lithium vanadium phosphate (also referred to as LVP), and the like.

[0099] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0100] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0101] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0102] [Negative electrode]

[0103] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0104] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0105] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0106] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0107] In some embodiments, the negative electrode film layer may further include a binder. For example, the binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0108] In some embodiments, the negative electrode film layer may further include a conductive agent. For example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0109] In some embodiments, the negative electrode film layer may optionally further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0110] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0111] [Electrolytes]

[0112] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.

[0113] In some embodiments, the electrolyte is liquid and includes an electrolyte salt and a solvent.

[0114] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0115] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0116] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0117] [Isolation film]

[0118] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0119] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0120] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0121] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0122] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0123] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG1 shows a secondary battery 5 with a square structure as an example.

[0124] In some embodiments, referring to FIG2 , the outer package may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0125] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0126] Figure 3 shows an example battery module 4. Referring to Figure 3 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0127] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0128] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0129] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 4 and 5 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0130] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0131] As an electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0132] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.

[0133] [Example]

[0134] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0135] Example 1

[0136] (1) Preparation of positive electrode sheet:

[0137] (1) Preparation of the first positive electrode active material:

[0138] 1) NiSO4, CoSO4, and MnSO4 were added to water in a molar ratio of 0.55:0.235:0.155 to form a mixed solution, wherein the concentration of NiSO4 in the mixed solution was 2 mol / L; and a 5 mol / L NaOH solution was prepared;

[0139] 2) 50 L of the mixed solution was introduced into a reactor, and then 50 L of NaOH solution and an appropriate amount of 0.5 mol / L ammonia solution were introduced into the reactor to adjust the pH value in the reactor to 9.0-12.0, the reaction temperature was 40°C-80°C, and the reaction was stirred for 60 h at a stirring speed of 300-1000 r / min. After completion, the precipitate was filtered and washed, and the washed precipitate was vacuum dried at 120°C for 24 h to obtain a precursor;

[0140] 3) Li2CO3, a precursor, Al2O3 and MgO are mixed, wherein the molar ratio of Li2CO3 (based on the molar amount of Li element), the precursor (based on the total molar amount of Ni, Co and Mn elements in the mixed solution), Al2O3 (based on the molar amount of Al element) and MgO is 1.05:0.94:0.04:0.02. After mixing, the mixture is placed in a ball mill and ball milled at a speed of 300 r / s for 2 hours, and then placed in a box furnace. Under a 0.2 MPa air atmosphere, the temperature is raised to 950 ° C and kept warm for 12 hours for pre-calcination, and the heating rate is 1 ° C / min. Then, the temperature is lowered to 600 ° C at a rate of 1 ° C / min and kept warm for 8 hours for sintering. After sintering, the temperature is lowered to 300 ° C at a rate of 1 ° C / min, and it is naturally cooled to room temperature. Thereafter, it is passed through a jet mill at a speed of 3000 r / min and 500 m 3 / h of air volume for crushing, crushing for 0.5h, and then sieving through a 500-mesh filter to obtain the first positive electrode active material LiNi 0.55 Co 0.235 Mn 0.155 Al 0.04 Mg 0.02 O2.

[0141] (2) Preparation of positive electrode sheet:

[0142] The first positive electrode active material, binder polyvinylidene fluoride (PVDF), and conductive agent acetylene black are dissolved in solvent N-methylpyrrolidone (NMP) in a mass ratio of 96:2:2, and are fully stirred and mixed to prepare a positive electrode slurry; the positive electrode slurry is evenly coated on the surface of the positive electrode collector, and then dried, cold pressed, and cut to obtain a positive electrode sheet.

[0143] (2) Preparation of negative electrode sheet:

[0144] The negative electrode active material artificial graphite, the conductive agent acetylene black, the binder styrene-butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC-Na) were dissolved in deionized water in a mass ratio of 96:2:1:1, and the mixture was thoroughly stirred and mixed to prepare a negative electrode slurry; the negative electrode slurry was coated on the negative electrode current collector copper foil, and then dried, cold pressed, and cut to obtain the negative electrode sheet.

[0145] (3) Isolation film: polypropylene film.

[0146] (4) Preparation of electrolyte:

[0147] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1, and then LiPF6 was uniformly dissolved in the above solution to obtain an electrolyte solution. The concentration of LiPF6 in the electrolyte solution was 1 mol / L.

[0148] (5) Preparation of secondary batteries:

[0149] The positive electrode sheet, separator, and negative electrode sheet are stacked and wound in order to obtain a battery cell; the battery cell is placed in a battery cell shell, and then placed in an outer package, and the above-prepared electrolyte is added. After packaging, standing, formation, aging and other processes, a secondary battery is obtained.

[0150] The secondary battery preparation methods of Examples 2-17 and the comparative example are similar to those of Example 1. The different product parameters are detailed in Table 1-2.

[0151] The mass contents of the binder and the conductive agent in the positive electrode film layer are the same as those in Example 1.

[0152] Preparation method of the second positive electrode active material of Examples 8-14

[0153] Step S1: Preparation of Fe, Co, V and S co-doped manganese oxalate

[0154] 689.6g of manganese carbonate, 455.3g of ferrous carbonate, 4.7g of cobalt sulfate, and 4.9g of vanadium dichloride were added to a mixer and thoroughly mixed for 6 hours. The resulting mixture was then transferred to a reactor, and 5L of deionized water and 1260.6g of oxalic acid dihydrate were added. The mixture was heated to 80°C and stirred at 500 rpm for 6 hours, mixing until the reaction terminated and no bubbles were generated, resulting in a manganese oxalate suspension co-doped with Fe, Co, and V. The suspension was then filtered, dried at 120°C, and sand-milled to obtain manganese oxalate particles with a particle size of 100nm.

[0155] Step S2: Prepare the core

[0156] Take 1793.1g of the prepared manganese oxalate, 368.3g of lithium carbonate, 1146.6g of ammonium dihydrogen phosphate and 4.9g of dilute sulfuric acid, add them to 20L of deionized water, stir thoroughly, mix evenly and react at 80°C for 10h to obtain a slurry. The slurry is transferred to a spray drying equipment for spray drying and granulation, and dried at a temperature of 250°C to obtain a powder. In a protective atmosphere (90% nitrogen and 10% hydrogen), the powder is sintered in a roller kiln at 700°C for 4h to obtain a core material. The element content of the core material is detected by inductively coupled plasma emission spectroscopy (ICP), and the core Li 0.997 Mn 0.60 Fe 0.393 V 0.004 Co 0.003 P 0.997 S 0.003 O4.

[0157] Step S3: Preparation of the first coating layer suspension

[0158] Preparation of Li2FeP2O7 solution: 7.4 g of lithium carbonate, 11.6 g of ferrous carbonate, 23.0 g of ammonium dihydrogen phosphate and 12.6 g of oxalic acid dihydrate were dissolved in 500 mL of deionized water, the pH was controlled to 5, and then stirred and reacted at room temperature for 2 h to obtain a solution. The solution was then heated to 80°C and maintained at this temperature for 4 h to obtain a first coating layer suspension.

[0159] Step S4: coating of the first coating layer

[0160] 1571.9 g of the doped lithium manganese phosphate core material obtained in step S2 was added to the first coating layer suspension (coating material content of 15.7 g) obtained in step S3, and the mixture was stirred and mixed for 6 h. After mixing evenly, it was transferred to a 120 ° C oven and dried for 6 h, and then sintered at 650 ° C for 6 h to obtain the pyrophosphate-coated material.

[0161] Step S5: Preparation of the second coating layer suspension

[0162] 3.7 g of lithium carbonate, 11.6 g of ferrous carbonate, 11.5 g of ammonium dihydrogen phosphate and 12.6 g of oxalic acid dihydrate were dissolved in 1500 mL of deionized water, and then stirred and reacted for 6 hours to obtain a solution. The solution was then heated to 120° C. and maintained at this temperature for 6 hours to obtain a second coating layer suspension.

[0163] Step S6: Coating with the second coating layer

[0164] 1586.8 g of the pyrophosphate-coated material obtained in step S4 was added to the second coating layer suspension (coating material content of 47.1 g) obtained in step S5, and the mixture was stirred and mixed for 6 h. After mixing evenly, it was transferred to a 120°C oven and dried for 6 h, and then sintered at 700°C for 8 h to obtain a two-layer coated material.

[0165] Step S7: Preparation of the third coating layer aqueous solution

[0166] 37.3 g of sucrose was dissolved in 500 g of deionized water, and then stirred and fully dissolved to obtain a sucrose aqueous solution.

[0167] Step S8: coating with the third coating layer

[0168] 1633.9 g of the two-layer coated material obtained in step S6 was added to the sucrose solution obtained in step S7, and stirred and mixed together for 6 hours. After mixing evenly, it was transferred to a 150°C oven for drying for 6 hours, and then sintered at 700°C for 10 hours to obtain a three-layer coated material.

[0169] Preparation method of the second positive electrode active material of Examples 15-17

[0170] Step S1: Preparation of manganese oxalate particles

[0171] 459.7g of manganese carbonate, 686.9g of ferrous carbonate, 4.8g of vanadium dichloride, and 3.6g of nickel carbonate were added to a mixer and thoroughly mixed for 6 hours. The resulting mixture was then transferred to a reactor, and 5L of deionized water and 1260.6g of oxalic acid dihydrate were added. The mixture was heated to 80°C and stirred at 500 rpm for 6 hours, mixing until the reaction terminated and no bubbles were generated, resulting in a manganese oxalate suspension co-doped with Fe, Co, and V. The suspension was then filtered, dried at 120°C, and sand-milled to obtain manganese oxalate particles with a particle size of 100nm.

[0172] Step S2: Prepare the core

[0173] 1794.9g of the prepared manganese oxalate, along with 369.8g of lithium carbonate, 1148.9g of ammonium dihydrogen phosphate, and 0.8g of silicic acid, were added to 20L of deionized water, stirred thoroughly, and uniformly mixed at 80°C for 10 hours to obtain a slurry. The slurry was transferred to a spray dryer for spray drying and granulation, and then dried at 250°C to obtain a powder. The powder was sintered in a roller kiln at 700°C for 4 hours in a protective atmosphere (90% nitrogen and 10% hydrogen) to obtain the core material. The core material was analyzed for elemental content using inductively coupled plasma emission spectroscopy (ICP).

[0174] Step S3: Preparation of the first coating layer suspension

[0175] Preparation of Li2FeP2O7 solution: 7.4 g of lithium carbonate, 11.6 g of ferrous carbonate, 23.0 g of ammonium dihydrogen phosphate and 12.6 g of oxalic acid dihydrate were dissolved in 500 mL of deionized water, the pH was controlled to 5, and then stirred and reacted at room temperature for 2 h to obtain a solution. The solution was then heated to 80°C and maintained at this temperature for 4 h to obtain a first coating layer suspension.

[0176] Step S4: coating of the first coating layer

[0177] The doped 1573.9 g core material obtained in step S2 was added to the first coating layer suspension (coating material content of 31.4 g) obtained in step S3, and the mixture was stirred and mixed for 6 h. After mixing evenly, the mixture was transferred to a 120 ° C oven and dried for 6 h, and then sintered at 650 ° C for 6 h to obtain the pyrophosphate-coated material.

[0178] Step S5: Preparation of the second coating layer suspension

[0179] 3.7 g of lithium carbonate, 15.5 g of cobalt sulfate, 11.5 g of ammonium dihydrogen phosphate and 12.6 g of oxalic acid dihydrate were dissolved in 1500 mL of deionized water, and then stirred and reacted for 6 hours to obtain a solution. The solution was then heated to 120° C. and maintained at this temperature for 6 hours to obtain a second coating layer suspension.

[0180] Step S6: Coating with the second coating layer

[0181] 1605.4 g of the pyrophosphate-coated material obtained in step S4 was added to the second coating layer suspension (coating material content of 63.0 g) obtained in step S5, and the mixture was stirred and mixed for 6 h. After mixing evenly, it was transferred to a 120°C oven and dried for 6 h, and then sintered at 750°C for 8 h to obtain a two-layer coated material.

[0182] Step S7: Preparation of the third coating layer aqueous solution

[0183] 37.4 g of sucrose was dissolved in 500 g of deionized water, and then stirred and fully dissolved to obtain a sucrose aqueous solution.

[0184] Step S8: coating with the third coating layer

[0185] 1668.3 g of the two-layer coated material obtained in step S6 was added to the sucrose solution obtained in step S7, and stirred and mixed together for 6 hours. After mixing evenly, it was transferred to an 80°C oven for drying for 6 hours, and then sintered at 600°C for 6 hours to obtain a three-layer coated material.

[0186] Test Case

[0187] (1) Porosity test of positive electrode sheet:

[0188] With reference to the method of GB / T 24586-2009, the positive electrode sheet was immersed in ethyl methyl carbonate (EMC) for cleaning. At room temperature and relative humidity ≤2% RH, the true volume V0 and apparent volume V of the positive electrode sheet were measured by a porosimeter (model AccuPycⅡ1340) by gas displacement method. The porosity α of the positive electrode sheet was calculated according to the following formula; α=100%×(V-V0) / V.

[0189] (2) Test of the compaction density of the positive electrode:

[0190] Place the positive electrode sheet in a special compaction mold, then place the mold on a compaction density instrument and apply 30 tons of pressure. After releasing the pressure, use a high-precision balance to measure the surface density of the positive electrode sheet, and use a micrometer to measure the thickness of the positive electrode sheet (the number of collection points is 10, and the average value is taken). Calculate the compaction density PD of the positive electrode sheet according to the following formula; PD = surface density of the positive electrode sheet / thickness of the positive electrode sheet.

[0191] (3) Test of gram capacity of positive electrode active material:

[0192] The positive electrode sheet and the counter electrode lithium sheet were made into a button battery. In a constant temperature environment of 25℃, the battery was charged to 4.3V with a constant current of 0.1C, and then discharged to 2.8V with a constant current of 0.1C. The discharge capacity of the battery was obtained. The gram capacity C of the positive electrode active material was calculated by dividing the discharge capacity of the battery by the mass of the positive electrode active material in the positive electrode sheet. cathode .

[0193] (4) Test of electrolyte density:

[0194] The density of the electrolyte ρ is tested according to the "Test Method B—U-type Vibrating Tube Method" in the standard GB / T 2013-2010 EL Before testing, the electrolyte was kept at room temperature and the density meter was rinsed three times with the electrolyte.

[0195] (5) Volume test of battery cell shell:

[0196] In a constant temperature environment of 25°C, the battery cell shell is a rectangular parallelepiped structure. The length, width and height of the battery cell shell are measured with a micrometer, and the product of the length, width and height is calculated to obtain the volume V of the battery cell shell.

[0197] (6) Test of the ratio of cell thickness to cell shell thickness:

[0198] In a constant temperature environment of 25°C, use a micrometer to measure the thickness of a single battery cell (i.e., the thickness of the battery cell in the stacking direction of the positive electrode sheet, separator and negative electrode sheet) and the thickness of the battery cell shell (i.e., the thickness of the battery cell shell in the stacking direction of the positive electrode sheet, separator and negative electrode sheet), and calculate the ratio h of the battery cell thickness to the battery cell shell thickness.

[0199] (7) Battery capacity test:

[0200] In a constant temperature environment of 25℃, let the battery stand for 10 minutes, then discharge it to 2.8V at 0.33C. Let it stand for 10 minutes, then charge it to 4.3V at 0.33C constant current, charge it to 0.05C at constant voltage, let it stand for 10 minutes, then discharge it to 2.8V at 0.33C. The discharge capacity at this time is C0. Let it stand for 10 minutes, then charge it to 4.3V at 0.33C0 constant current, charge it to 0.05C0 at constant voltage, let it stand for 10 minutes, then discharge it to 2.8V at 0.33C0. The discharge capacity at this time is recorded as the battery capacity C cell .

[0201] (8) Test of the minimum filling coefficient of the battery cell:

[0202] The capacity of the battery cells with filling coefficients of 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, and 5 was tested. The test method was the same as item (7) above. Each battery cell was measured 5 times in parallel. The highest and lowest values ​​were removed, and the average of the remaining 3 values ​​was taken as the battery cell capacity.

[0203] Use the filling coefficient as the X-axis and the cell capacity as the Y-axis to draw a segmented line graph. The X-axis value corresponding to the inflection point on the graph is the minimum filling coefficient m of the cell. EL .

[0204] (9) Testing of the battery voltage platform and its corresponding state of charge (SOC):

[0205] In a constant temperature environment of 25°C, the battery was allowed to stand for 10 minutes, then discharged at 0.33C to 2.8V. After standing for 10 minutes, the battery was charged to 4.3V at a constant current of 0.33C, charged at a constant voltage to a current of ≤0.05C, and discharged to 2.8V at 0.33C after standing for 10 minutes. The discharge capacity at this time was recorded as C0. After standing for 10 minutes, the battery was charged to 4.3V at a constant current of 0.33C0, charged at a constant voltage to a current of ≤0.05C0, and discharged to 2.8V at 0.33C0 after standing for 10 minutes. The discharge capacity at this time was recorded as 100% SOC. The discharge capacity was plotted against the voltage to obtain the SOC-OCV curve, and the dQ / dV curve was obtained by taking the derivative once. The number of peaks appearing on the dQ / dV curve is the number of voltage platforms of the battery. The number of peaks appearing in the voltage range of ≤3.5V is the number of voltage platforms of the battery ≤3.5V, and the number of peaks appearing in the voltage range of ≤3.4V is the number of voltage platforms of the battery ≤3.4V.

[0206] On the SOC-OCV curve, the discharge capacity corresponding to a voltage of 3.5V is Q1, and the full discharge voltage of 2.8V corresponds to the total discharge capacity Q2. The proportion of the battery's discharge capacity ≤ 3.5V in the total discharge capacity, C, is calculated according to the following formula: C (%) = 100 × (Q2 - Q1) / Q2

[0207] (10) Test of the content of polycrystalline particles and primary particle size in the positive electrode active material:

[0208] The positive electrode active material is tested using a scanning electron microscope. The sample and magnification are adjusted so that there are more than 10 agglomerated particles in the field of view. The number of primary particles that make up each agglomerated particle is measured, and the length direction of the primary particle is measured with a ruler and recorded as the particle size. The particle size of the primary particles in each agglomerated particle is sorted from large to small, and 1 / 10 of the largest particle size data and 1 / 10 of the smallest particle size data are removed. The average value of the remaining particle size data is taken as the average particle size of the primary particles in the agglomerated particle. If the number and average particle size of the primary particles in more than 50% (including 50%) of the agglomerated particles meet the definition of "polycrystalline material particles", the positive electrode active material is determined to be a polycrystalline material. Otherwise, it is determined to be a single crystal or quasi-single crystal material. The average particle size of the primary particles of the polycrystalline material is recorded as the particle size of the primary particles.

[0209] Test of the content of polycrystalline particles in positive electrode active materials:

[0210] SEM and EDS testing of positive electrode active materials were used. EDS elemental testing confirmed the elemental composition of polycrystalline materials, and the elemental differences between polycrystalline and single-crystal particles were determined by combining the particle morphology obtained through SEM. ICP testing of the positive electrode active materials revealed the elemental composition and proportions, allowing the polycrystalline content in the positive electrode active material to be calculated.

[0211] (11) Power test:

[0212] In a constant temperature environment of 25°C, after standing the battery for 10 minutes, discharge it at 0.33C to 2.8V, stand for 10 minutes, charge it at a constant current of 0.33C to 4.3V, charge it at a constant voltage until the current ≤ 0.05C, stand for 10 minutes and then discharge it at 0.33C to 2.8V. At this time, the discharge capacity is C0; stand for 10 minutes and then discharge it at 0.33C0 to 2.8V, stand for 10 minutes; charge it at a constant current of 0.33C0 to 4.3V, charge it at a constant voltage until the current ≤ 0.05C0, stand for 10 minutes and then discharge it at 0.33C0 to 80% C0, stand for 120 minutes, discharge it at a current of 2C0 for 30 seconds, and record the voltage at this time as V1; stand for 10 minutes, and cycle the process of 0.33C0 constant current charging, constant voltage charging, standing, 0.33C0 discharging to 80% C0, standing, discharging at a current of Xi (i = 2, 3, 4, 5... n) for 30 seconds and recording the voltage Vi (i = 2, 3, 4, 5... n) until the recorded voltage Vi is within the range of V0 (2.8V) ± 0.05V, record the corresponding Xi, and obtain the power of the battery according to Xi × Vi.

[0213] In the above process, it is set that the previous cycle uses the current Xi-1 to obtain the voltage Vi-1, and the next cycle uses the current Xi to obtain the voltage Vi. If the voltage Vi-1 obtained in the previous cycle < V-0.05V, then the next cycle uses the current Xi < Xi-1. Conversely, the next cycle uses the current Xi > Xi-1, and the difference between Xi and Xi-1 is 0.2C0.

[0214] (12) Cycle life test:

[0215] In a constant temperature environment of 25°C, after standing the battery for 10 minutes, discharge it at 0.33C to 2.8V, stand for 10 minutes, charge it at a constant current of 0.33C to 4.3V, charge it at a constant voltage until the current ≤ 0.05C, stand for 10 minutes and then discharge it at 0.33C to 2.8V, and record the discharge capacity of the first cycle of the battery as D1; repeat the above operations, and record the discharge capacity of each cycle as D n (n = 2, 3...); Calculate the attenuation degree (State of health SOH) of the battery cell according to the following formula, and record the number of cycles n when the attenuation degree reaches 80% SOH. The attenuation degree of the battery cell = 100% × D n / D3.

[0216] The test results of each item are shown in Table 3.

[0217] Table 3: Performance test results of Examples 1-17 and Comparative Examples

[0218] According to Table 3, we can see that:

[0219] Compared with the battery of the comparative example, the battery of the present application has higher power capability, longer cycle life and better capacity performance;

[0220] Compared with the batteries of Examples 1-8, 13-14, and 17 of the present application, the power capability of the batteries of Examples 10-12 of the present application is further improved and the cycle life is further improved; compared with the batteries of Example 9 of the present application, the power capability of the batteries of Examples 10-12 of the present application is further improved; compared with the batteries of Examples 15-16 of the present application, the cycle life of the batteries of Examples 10-12 of the present application is further improved;

[0221] Compared with Examples 1 and 7, the power capabilities of the batteries of Examples 2-6, 8-17 of the present application are further improved and the cycle life is further extended;

[0222] Compared with Examples 1-7 and 14, the power capabilities of the batteries of Examples 8-12 and 15 of the present application are further improved and the cycle life is further extended. The power capabilities of the batteries of Examples 13 and 16 of the present application are further improved.

[0223] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A battery comprising a battery cell, a battery cell shell covering the battery cell, and an electrolyte, wherein: The battery cell comprises a positive electrode sheet, the positive electrode sheet comprises a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, the positive electrode film layer comprises a positive electrode active material; Furthermore, the battery meets the following requirements: α×ρ EL / (PD×C cathode )+V×h / C cell ≤m EL Wherein, α is the porosity of the positive electrode sheet; ρ EL is the density of the electrolyte, in g / cm 3 PD is the compaction density of the positive electrode sheet under a pressure of 20-80 tons, in g / cm 3 ; C cathode is the gram capacity of the positive electrode active material, in mAh / g; V is the volume of the battery shell, in cm 3 ; h is the ratio of the thickness of the battery cell to the thickness of the battery cell shell; C cell is the capacity of the battery, in Ah; m EL is the minimum filling coefficient of the battery cell.

2. The battery according to claim 1, wherein The battery has at least two voltage platforms; Optionally, the battery has at least one voltage platform of ≤3.5V; Optionally, the battery has at most one voltage plateau ≤ 3.4V.

3. The battery according to claim 1 or 2, wherein: The battery's discharge capacity of ≤3.5V accounts for 2%-50% of the entire discharge capacity, and can be optionally 5%-30%.

4. The battery according to any one of claims 1 to 3, wherein The positive electrode film layer also includes a lithium supplement agent; Optionally, the lithium supplement includes one or more of Li3N, Li2S / Co composite material, LiF / Co composite material, Li2O / Co composite material, Li2O2, Li2NiO2, Li5FeO4, Li2C2O4, Li2C4O4, Li2C3O5 and Li2C4O6; Optionally, the mass content of the lithium supplement in the positive electrode film layer is 1%-40%.

5. The battery according to any one of claims 1 to 4, wherein The positive electrode active material includes a first positive electrode active material; the first positive electrode active material includes a compound LiNi b Co d Mn e M f O2, wherein M includes one or more elements of Al, Mg, Ca, Na, Ti, W, Zr, Sr, Cr, Zn, Ba, B, S and Y, and can be optionally Mg element and / or Al element; b is 0.314-0.970; d is 0-0.320, and can be optionally 0.047-0.320; e is 0.006-0.390; and the sum of b, d, e and f is 1 and f is greater than 0.

6. The battery according to claim 5, wherein The mass content of the first positive electrode active material in the positive electrode active material is 20%-98%.

7. The battery according to claim 5 or 6, wherein: The positive electrode active material also includes a second positive electrode active material; the second positive electrode active material includes a compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n , wherein A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W; B includes one or more elements selected from the group consisting of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; C includes one or more elements selected from the group consisting of B (boron), S, Si and N; D includes one or more elements selected from the group consisting of S, F, Cl and Br; a is 0.9-1.1; x is 0-0.1; y is 0.001-0.6; z is 0.001-0.1; and n is 0-0.

1.

8. The battery according to claim 7, wherein The second positive electrode active material comprises a core and a shell covering the core; the core comprises the compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n , the shell comprises carbon element.

9. The battery according to claim 7, wherein: The second positive electrode active material comprises a core and a shell covering the core; the shell comprises a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer; wherein the core comprises the compound Li a A x Mn 1-y B y P 1-z C z O 4-n D n , the first coating layer comprises crystalline pyrophosphate Li g EP2O7 and / or E h (P2O7) i The second coating layer comprises crystalline phosphate X j PO4, the third coating layer comprises carbon element; Wherein, the crystalline pyrophosphate Li g EP2O7 and E h (P2O7) i wherein E independently includes one or more elements selected from the group consisting of Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; X includes one or more elements selected from the group consisting of Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; g is greater than 0 and less than or equal to 2; h is greater than 0 and less than or equal to 4; i is greater than 0 and less than or equal to 3; and j is greater than 0 and less than or equal to 3.

10. The battery according to any one of claims 7 to 9, wherein The positive electrode active material consists of the first positive electrode active material and the second positive electrode active material.

11. The battery according to any one of claims 1 to 10, wherein The mass content of the polycrystalline particles in the positive electrode active material is 0%-100%; Optionally, the primary particle size of the polycrystalline particles is 20-1000 nm.

12. An electrical device comprising the battery according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Battery and electric device

    CN118867402A

  • Method for determining retaining amount and injection amount of electrolyte solution of lithium ion battery

    CN105787140A

  • Lithium ion battery and power vehicle

    CN114430039A

  • Positive pole piece of lithium ion battery as well as preparation method and application of positive pole piece

    CN114864867A

  • Metal lithium battery and preparation method thereof

    CN114899475A

Cited By

  • Secondary battery and electric device

    WO2026103021A1