Preparation method for waste rubber reducing material, and reduction method for waste rubber
By using high-speed dry powder mixer and low-temperature mechanical mixing technology in waste rubber regeneration, the problem of physical property degradation and environmental pollution caused by high-temperature heat treatment is solved, efficient regeneration of waste rubber and effective utilization of resources are achieved, and recycling costs are reduced. And improve the applicability of rubber.
Patent Information
- Application Number
- PCT/CN2024/081718
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-31
AI Technical Summary
In the existing technology, there are problems such as high-temperature heat treatment during the waste rubber regeneration process, which leads to a decrease in physical properties, an increase in costs, and environmental pollution. In particular, the microwave absorption efficiency of non-polar rubber materials is low and toxic gases are produced.
A high-speed dry powder mixer is used to mix accelerator materials, processing oil and filler material particles to form composite particles, and the vulcanized rubber is destroyed through low-temperature mechanical mixing, and its structure is rearranged to return to the state before vulcanization to prepare waste rubber reduction materials.
Under low temperature conditions, the physical properties of rubber are improved, recycling costs are reduced, the generation of toxic gases is avoided, the applicability of rubber is improved, and it has environmental protection advantages.
Smart Images

Figure PCTCN2024081718-FTAPPB-I100001 
Figure PCTCN2024081718-FTAPPB-I100002 
Figure PCTCN2024081718-FTAPPB-I100003
Abstract
Description
Preparation method of waste rubber reduction material and waste rubber reduction method Technical Field
[0001] The present invention relates to a method for preparing a reducing material and a reducing method, and to a method for preparing a reducing material of waste rubber and a reducing method of waste rubber. Background Art
[0002] With the increasing amount of waste rubber and the enormous amount of rubber consumed, recycled rubber has emerged as a necessity in the era of a low-carbon economy. However, waste rubber is considered a hazardous industrial waste, a serious threat to the environment, including deteriorating vegetation, affecting human health, and endangering the Earth's ecosystem.
[0003] Improper rubber formulation and process operation during production will result in waste products and rubber edges, including rubber from the extruder die, burnt rubber that prematurely vulcanizes during mixing, and flash and runner rubber from molding. This waste rubber cannot be reused in rubber product production and can only be processed into recycled rubber. The production process of rubber products inevitably produces some waste, scraps, and test waste from trials, which become one of the main sources of raw materials for recycled rubber.
[0004] Various rubber products gradually lose their value during use. Waste rubber products, which can be recycled and reused, are another source of recycled rubber raw materials. Data shows that raw rubber consumed in the transportation and automotive industries accounts for 75% of global rubber consumption, and waste tires account for approximately 50% of total rubber consumption. Therefore, waste tires, among other waste rubber products, are the primary source of recycled rubber, and the comprehensive utilization of waste tires is a key focus of waste rubber recycling. Waste rubber products from hoses, tapes, and industrial rubber are generally not used as raw materials for recycled rubber due to their diverse variety and difficulty in recycling, resulting in a waste of resources.
[0005] The recycling and restoration of general waste rubber often involves high-temperature heat treatment. By using high temperature (150°C to 250°C) conditions, the SS bonds or CS bonds in the waste rubber structure can be broken, restoring the reprocessability of the recycled rubber. Since the above-mentioned heat treatment method randomly breaks covalent bonds through high-temperature thermal motion, random bond breaking often causes a significant decrease in the physical properties of the recycled rubber under long-term high-temperature conditions, thereby limiting the applicability of the restored product. In addition, heat treatment, such as using microwaves, has too low microwave absorption efficiency for non-polar rubber materials (such as NR, SBR, EPDM), which will not be conducive to improving chain scission efficiency. Although carbon black is often added to general rubber to improve microwave absorption efficiency, the filler content of the recycled material must be screened and graded to facilitate the stability of the properties after heat treatment.
[0006] On the other hand, if the reduction of vulcanized rubber involves heat treatment, bond breakage during the heat reduction process will produce toxic gases such as SO2 and H2S, which in turn raises concerns about environmental pollution. Furthermore, random bond breakage during heat treatment often deactivates the sulfur-containing components of the original scrap rubber. Therefore, during the subsequent re-vulcanization process of the recycled rubber, more sulfur bridging agents must be added to restore the desired physical properties, which increases recycling costs.
[0007] Based on the above, developing a method for preparing a waste rubber reduction material and a method for reducing waste rubber to improve the physical properties of the recycled rubber and reduce the recycling cost is an important research topic currently required.
[0008] Summary of the Invention
[0009] The invention provides a method for preparing a waste rubber reduction material and a method for reducing waste rubber, so as to improve the physical properties of the recycled rubber and reduce the recycling cost.
[0010] The method for preparing a waste rubber reduction material of the present invention comprises the following steps: An accelerator material, processing oil, and filler particles are mixed using a high-speed dry powder mixer, wherein the processing oil adheres to the accelerator material. The filler particles then coat the accelerator material with the processing oil to form composite particles. Subsequently, an unvulcanized rubber-plastic polymer is bonded to the composite particles using a kneading device. The composite particles are then surface-treated with a surface treatment material, and a dispersing material is added and mixed to form the waste rubber reduction material.
[0011] In one embodiment of the present invention, the method for preparing the waste rubber reduction material further comprises extruding the waste rubber reduction material in the form of masterbatch, sheet, film or block.
[0012] In one embodiment of the present invention, the accelerator material includes thiazoles, thioureas, sulfenamides, thiurams, or dithiocarbamates.
[0013] In one embodiment of the present invention, the process oil includes paraffin-based, naphthenic-based or aromatic-based process oil.
[0014] In one embodiment of the present invention, the filler material particles include inorganic filler material particles, and the inorganic filler material particles include calcium carbonate, calcium sulfate, or magnesium carbonate.
[0015] In one embodiment of the present invention, the particle size of the accelerator material is 100 μm to 3000 μm.
[0016] In one embodiment of the present invention, the size of the filler particles is 0.1 μm to 15 μm.
[0017] In one embodiment of the present invention, based on 100wt% of the total amount of the waste rubber recycling material, the content of the filler material particles is 10wt% to 25wt%, the content of the accelerator material is 5wt% to 40wt%, the content of the unvulcanized rubber and plastic polymer is 15wt% to 50wt%, the content of the processing oil is 0.1wt% to 3wt%, the content of the surface treatment material is 2wt% to 5wt%, and the content of the dispersed material is 0.5wt% to 5wt%.
[0018] In one embodiment of the present invention, the unvulcanized rubber or plastic polymer includes natural rubber (NR), isoprene rubber (IR), butyl rubber (IIR), polybutadiene rubber (BR), nitrile rubber (NBR), ethylene propylene rubber (EPDM), chloroprene rubber (CR), styrene butadiene rubber (SBR), or unbridged ethylene vinyl acetate copolymer (EVA).
[0019] In one embodiment of the present invention, the surface treatment material includes a titanate coupling agent, an alkoxysilane coupling agent, a methacryloxy coupling agent, an amino coupling agent, a mercapto coupling agent, or a combination thereof.
[0020] In one embodiment of the present invention, the surface treatment process has a treatment temperature of 40° C. to 90° C. and a treatment time of 5 minutes to 10 minutes.
[0021] In one embodiment of the present invention, the dispersion material includes polyethylene wax, stearic acid or oxidized polyethylene wax.
[0022] The waste rubber reduction method of the present invention comprises the following steps: mixing a waste rubber reduction material with waste rubber under mechanical force to destroy the vulcanized waste rubber and restore the workability of the waste rubber. The waste rubber reduction material is prepared by the above-mentioned waste rubber reduction material preparation method.
[0023] In one embodiment of the present invention, the operating temperature of the waste rubber reduction method is 50° C. to 100° C., and the operating time is 20 minutes to 50 minutes.
[0024] In one embodiment of the present invention, the weight ratio of the waste rubber reducing material to the waste rubber is 2:98 to 15:85.
[0025] Based on the above, the present invention provides a method for preparing a waste rubber reduction material and a method for reducing waste rubber. This method can help rearrange the rubber structure, returning it to its pre-vulcanized state. The waste rubber reduction method of the present invention can reduce waste rubber under low-temperature conditions (50°C to 100°C), avoiding the high-temperature conditions used in prior art, thereby avoiding the problems encountered in conventional heat treatment. This prevents the problem of deterioration in physical properties and reduces recycling costs, while also improving the applicability of the reduced product and avoiding the generation of toxic gases, thereby providing environmental advantages. DETAILED DESCRIPTION
[0026] Hereinafter, embodiments of the present invention will be described in detail. However, these embodiments are merely illustrative and the present invention is not limited thereto.
[0027] In this document, the term "range from one value to another value" is used as a summary to avoid listing all values within the range. Therefore, a description of a specific numerical range encompasses any value within that range and any smaller numerical range defined by that value, just as if the value and smaller numerical range were listed in the specification.
[0028] The method for preparing a waste rubber reduction material of the present invention comprises the following steps: An accelerator material, processing oil, and filler particles are mixed using a high-speed dry powder mixer, wherein the processing oil adheres to the accelerator material. The filler particles then coat the accelerator material, which is adhered to the processing oil, to form composite particles. An unvulcanized rubber-plastic polymer is then bonded to the composite particles using a kneading device. The composite particles are then surface-treated with a surface treatment material, and a dispersing material is added and mixed to form the waste rubber reduction material. The waste rubber reduction material can then be extruded in the form of masterbatches, sheets, films, or blocks.
[0029] In this embodiment, the accelerator material may include thiazoles, thioureas, sulfenamides, thiurams, or dithiocarbamates, with the accelerator material particle size ranging, for example, from 100 μm to 3000 μm. The process oil may include paraffin-based, cycloalkyl-based, or aromatic-based process oils. The filler particles may include inorganic filler particles such as calcium carbonate, calcium sulfate, or magnesium carbonate, with the filler particle size ranging, for example, from 0.1 μm to 15 μm. Based on 100 wt% of the total waste rubber reduction material, the filler material content may be, for example, from 10 wt% to 25 wt%, the accelerator material content may be, for example, from 5 wt% to 40 wt%, and the process oil content may be, for example, from 0.1 wt% to 3 wt%. The addition of the process oil softens the accelerator material, allowing the filler particles to effectively encapsulate the accelerator material, forming composite particles. This reduces degradation or oxidation of the accelerator material due to mechanical forces or localized high temperatures during the reduction material preparation process. Because the unvulcanized rubber polymer has unsaturated double bonds, coating the accelerator material can also prevent the accelerator material from chemically reacting with the unsaturated double bonds during the preparation process, which would cause the effectiveness of the accelerator material to decrease.
[0030] In this embodiment, the unvulcanized rubber-plastic polymer may include unvulcanized, pre-crosslinked rubber, such as natural rubber (NR), isoprene rubber (IR), butyl rubber (IIR), polybutadiene rubber (BR), nitrile rubber (NBR), ethylene propylene rubber (EPDM), chloroprene rubber (CR), styrene butadiene rubber (SBR), or uncrosslinked ethylene-vinyl acetate copolymer (EVA). The unvulcanized rubber-plastic polymer may comprise, for example, 15 to 50 weight percent of the total weight of the waste rubber recovery material as 100 weight percent. This provides suitable bonding properties for bonding the composite particles containing the accelerator material and sufficient compatibility for the subsequent recovery of the waste rubber.
[0031] In this embodiment, the surface treatment material may include a titanate coupling agent, an alkoxysilane coupling agent, a methacryloyl coupling agent, an amino coupling agent, a thiol coupling agent, or a combination thereof. The surface treatment process temperature is, for example, 40°C to 90°C, and the treatment time is, for example, 5 to 10 minutes. Based on 100% by weight of the total weight of the recycled waste rubber material, the surface treatment material content is, for example, 2% to 5% by weight. The surface treatment process can improve the mixing uniformity between the unvulcanized rubber polymer and the outer filler material of the composite particles.
[0032] In this embodiment, the dispersing material may include polyethylene wax, stearic acid, or oxidized polyethylene wax. Based on 100% by weight of the total weight of the recycled waste rubber material, the dispersing material content is, for example, 0.5% to 5% by weight. This ensures smooth and uniform dispersion during composite material processing, while minimizing mechanical losses caused by excessive current load during operation.
[0033] The present invention also provides a method for reducing waste rubber, comprising the following steps: mixing a waste rubber reducing material with waste rubber under mechanical force to destroy the vulcanized waste rubber and restore the workability of the waste rubber. The waste rubber reducing material is prepared by the above-mentioned method for preparing the waste rubber reducing material.
[0034] In this embodiment, the operating temperature of the waste rubber reduction method is, for example, 50°C to 100°C, and the operating time is, for example, 20 minutes to 50 minutes. The weight ratio of the waste rubber reduction material to the waste rubber is, for example, 2:98 to 15:85. In order to improve the efficiency of waste rubber reduction, a crushing pre-treatment may also be used. The crushing pre-treatment method may be, for example: grinding or water jet grinding the waste rubber at room temperature or low temperature conditions to process the waste rubber into fine powder and increase its specific surface area for reaction. The processing equipment used in the waste rubber reduction method may include a two-roll mill, a kneader, or a high-speed mixing machine (Banbury mixer). The waste rubber is reduced through shearing mechanical force, rearranging the rubber structure and returning it to its pre-vulcanization state.
[0035] The following experimental examples are used to illustrate the method for preparing the waste rubber reduction material and the method for reducing waste rubber according to the present invention. However, the following experimental examples are not intended to limit the present invention.
[0036] Experimental example
[0037] In order to demonstrate that the waste rubber reduction material proposed in the present invention can restore waste rubber to its pre-vulcanization state and retain more than 70% of its pre-treatment physical properties and strength, the following experimental example is specifically described.
[0038] Evaluation methods for rubber properties
[0039] Specific gravity: Measured using a hydrometer to compare raw rubber and reduced rubber.
[0040] Hardness: Measured using a durometer, comparing raw rubber and reduced rubber.
[0041] Tensile Strength: Measured using a universal testing machine. Compare the raw rubber and the reduced rubber. Place them in a tensile test fixture, enter the corresponding parameters in the software, and start the testing machine to read their tensile strength.
[0042] Elongation: Measured using a universal testing machine. Compare the raw rubber and the reduced rubber. Place them in a tensile test fixture. Enter the corresponding parameters in the software, start the testing machine, and read the elongation.
[0043] Preparation of waste rubber reduction materials
[0044] 1155g of thiazole accelerator powder (Brand: Xinsheng International Co., Ltd., Model: MBT) was dispersed in a high-speed dry powder mixer at room temperature (500rpm). 12g of naphthenic process oil was slowly added dropwise (over 2-3 minutes) while dispersing and mixing. 660g of calcium carbonate (Brand: Peilin Enterprise Co., Ltd., Model: M3001, average particle size 10-12μm) was then added to coat the accelerator material to produce composite particles. 890g of unvulcanized butyl rubber polymer (Brand: Lanxess, Model: RB402) was placed in the tank of another mixer (Brand: Li Na Machinery Industrial Co., Ltd., Model: 3L Testing Machine) and kneaded for 10 minutes at a set temperature of 40-50°C and a set speed of 10 rpm. Next, the composite particles, 90 grams of a silane coupling agent (Brand: Topco Electronics Co., Ltd., Model: KBM-403), and 110 grams of polyethylene wax (Brand: Zhongbo Chemical Co., Ltd., Model: PE-WAX) were added to a kneading mixer in batches and kneaded for 10 minutes to form a mass. The mass was then transferred to an extruder pelletizer (Brand: Lira Machinery Co., Ltd.) to produce a masterbatch of the reduced waste rubber material.
[0045] Reduction and re-vulcanization of waste rubber
[0046] Example 1: Styrene-butadiene rubber (SBR)
[0047] Vulcanized styrene-butadiene rubber (SBR) scraps from the production process (provided by Changhong Rubber Co., Ltd.) were collected and crushed on a double-roll mixer. When the operating temperature reached 75°C, 5wt% of the waste rubber reducing material was added, based on the total weight of the waste rubber and waste rubber reducing material (100wt%). The reduction process was continued on the double-roll mixer at 75°C for 20 minutes to complete the reduction of the SBR.
[0048] The reduced styrene-butadiene rubber was re-vulcanized at 170° C. for 5 minutes by adding 2.5 wt % sulfur, 1.8 wt % dibenzothiazole disulfide, and 0.3 wt % tetramethylthiuram disulfide (based on the total amount of the reduced rubber as 100 wt %).
[0049] The re-vulcanization evaluation results are shown in Table 1. Compared to a manufacturer's styrene-butadiene rubber sample (vulcanized raw rubber), the waste rubber reduction material proposed in this invention can be reduced and re-vulcanized while retaining over 70% of its physical properties, with hardness, tensile stress, tensile strain, and specific gravity similar to those of the vulcanized raw rubber.
[0050] Table 1
[0051] Example 2: Natural rubber (NR)
[0052] The method is similar to that of Example 1. Vulcanized natural rubber scraps provided by Changhong Rubber Industry Co., Ltd. are crushed and the waste rubber is reduced on a double-roller mixer.
[0053] The reduced natural rubber was similarly added with 2.5 wt% sulfur, 1.8 wt% dibenzothiazole disulfide, and 0.3 wt% tetramethylthiuram disulfide and re-vulcanized at high temperature. The re-vulcanization operation was carried out at 175° C. for 3 minutes.
[0054] The evaluation results of resulfurization are shown in Table 2 below.
[0055] Table 2
[0056] Reduction and re-bridging of EVA foam
[0057] Example 3: Ethylene vinyl acetate foam (EVA foam)
[0058] The method is similar to Example 1. The manufacturer Qimeng Industrial Co., Ltd. provides scraps of expanded EVA foam (model: L-2500NN), which are crushed and reduced in a double-roller mixer.
[0059] The reduced EVA was re-foamed by adding 3.0 wt% of azodicarbonamide and 0.8 wt% of dicumyl peroxide (based on the total amount of the reduced EVA as 100 wt%) as a blowing agent and a bridging agent, respectively. The re-foaming operation was carried out at a temperature of 170° C. and a pressure of 15 MPa for 7 minutes.
[0060] The physical property evaluation results of EV A re-cross-linked foaming are shown in Table 3 below.
[0061] Table 3
[0062] In summary, the present invention provides a method for preparing a waste rubber reduction material and a method for reducing waste rubber. The method for reducing waste rubber can help rearrange the structure of the rubber and return it to its pre-vulcanization state. The method for reducing waste rubber of the present invention can reduce waste rubber under low temperature conditions (70°C to 80°C), avoiding the high temperature conditions in the prior art, and thus avoiding the problems encountered in conventional heat treatment. In this way, the problem of physical property degradation can be avoided and the recycling cost can be reduced, the applicability of the reduced product can be improved, and the generation of toxic gases can be avoided, thereby having green energy and environmental protection advantages. The method for preparing a waste rubber reduction material of the present invention uses an accelerator to rearrange the rubber structure and return it to its pre-vulcanization state, and retain more than 70% of the strength of the physical properties before treatment. Therefore, it can make full use of discarded rubber resources, alleviate the shortage of rubber resources, protect the ecological environment, and develop a circular economy.
Claims
1. A method for preparing a waste rubber reduction material, characterized in that: include: Using a high-speed dry powder mixer to mix the accelerator material, processing oil and filler material particles, wherein the processing oil adheres to the accelerator material, and then the filler material particles cover the accelerator material adhered to the processing oil to form composite particles; as well as The unvulcanized rubber-plastic polymer is bonded to the composite particles by using a kneading device, and then a surface treatment process is performed by using a surface treatment material, and a dispersing material is added and mixed to form a waste rubber reduction material.
2. The method for preparing waste rubber reduction materials according to claim 1, characterized in that: The method also includes extruding the waste rubber reduced material in the form of master batch, sheet, film or block.
3. The method for preparing waste rubber reduction materials according to claim 1, characterized in that: The accelerator material includes thiazoles, thioureas, sulfenamides, thiurams or dithiocarbamates.
4. The method for preparing waste rubber reduction materials according to claim 1, characterized in that: The process oil includes paraffin-based, cycloalkyl-based or aromatic-based process oil.
5. The method for preparing waste rubber reduction materials according to claim 1, characterized in that: The filler material particles include inorganic filler material particles, and the inorganic filler material particles include calcium carbonate, calcium sulfate or magnesium carbonate.
6. The method for preparing waste rubber reduction materials according to claim 1, characterized in that: The particle size of the accelerator material is 100 μm to 3000 μm.
7. The method for preparing waste rubber reduction materials according to claim 1, characterized in that: The size of the filler material particles is 0.1 μm to 15 μm.
8. The method for preparing waste rubber reduction materials according to claim 1, characterized in that: Based on the total amount of the waste rubber reduction material as 100wt%, the content of the filler material particles is 10wt% to 25wt%, the content of the accelerator material is 5wt% to 40wt%, the content of the unvulcanized rubber and plastic polymer is 15wt% to 50wt%, the content of the processing oil is 0.1wt% to 3wt%, the content of the surface treatment material is 2wt% to 5wt%, and the content of the dispersed material is 0.5wt% to 5wt%.
9. The method for preparing waste rubber reduction materials according to claim 1, characterized in that: The unvulcanized rubber and plastic polymer includes natural rubber, isoprene rubber, butyl rubber, polybutadiene rubber, nitrile rubber, ethylene propylene rubber, chloroprene rubber, styrene butadiene rubber or unbridged ethylene-vinyl acetate copolymer.
10. The method for preparing waste rubber reduction materials according to claim 1, characterized in that: The surface treatment material includes a titanate coupling agent, an alkoxysilane coupling agent, a methacryloxy coupling agent, an amino coupling agent, a mercapto coupling agent or a combination thereof.
11. The method for preparing waste rubber reduction materials according to claim 1, characterized in that: The surface treatment process has a treatment temperature of 40° C. to 90° C. and a treatment time of 5 minutes to 10 minutes.
12. The method for preparing waste rubber reduction materials according to claim 1, characterized in that: The dispersing material includes polyethylene wax, stearic acid or oxidized polyethylene wax.
13. A method for reducing waste rubber, characterized in that: include: The waste rubber reducing material is mixed with the waste rubber under the action of mechanical force to destroy the vulcanized waste rubber and restore the processability of the waste rubber. The waste rubber reduced material is prepared by the method for preparing the waste rubber reduced material according to any one of claims 1 to 12.
14. The method for reducing waste rubber according to claim 13, characterized in that: The operating temperature of the waste rubber reduction method is 50° C. to 100° C., and the operating time is 20 minutes to 50 minutes.
15. The method for reducing waste rubber according to claim 13, characterized in that: The weight ratio of the waste rubber reducing material to the waste rubber is 2:98 to 15:85.
Citation Information
Patent Citations
Compound accelerator pre-dispersing master batch particles for rubber and preparation method of compound accelerator pre-dispersing master batch particles
CN105602120A
Vulcanization accelerator master batch and preparation method thereof
CN105733053A
Pre-dispersed rubber master batch particle for integrated accelerant and preparation method thereof
CN109054199A
Environment-friendly rubber accelerator ZDTP pre-dispersion masterbatch particle and preparation method thereof
CN112662079A
Improvement in and relating to the receiving of naural and synthetic rubber
CN1127271A