Battery shell, battery cell, battery and electric apparatus

By applying an insulating coating to the connection welds of the power battery casing, the problems of weld corrosion and the complex folding process of the insulating protective film are solved, achieving more reliable insulation and anti-corrosion protection.

WO2024222508A1PCT designated stage expired Publication Date: 2024-10-31CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/087777
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-15
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The connection welds on the end faces of existing power battery casings are easily corroded, the folding and covering process of the insulation protective film is complicated and the anti-corrosion protection fails.

Method used

The insulating coating is used to cover the connection welds to simplify the coating process of the insulating protective film and ensure that the coating reliably covers the welds to prevent corrosion.

Benefits of technology

It improves the insulation and anti-corrosion properties of the battery case, simplifies process operations, and avoids weld corrosion and protection failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024087777_31102024_PF_FP_ABST
    Figure CN2024087777_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A battery shell, a battery cell, a battery and an electric apparatus. The battery shell comprises a shell side wall and a shell end wall, which are mutually connected, wherein an attachment weld is provided at the joint between the shell side wall and the shell end wall and is positioned at an end face of the battery shell. The battery shell further comprises an insulating protective film and an insulating coating, wherein the outer side of the shell side wall is connected to the insulating protective film, and the outer side of the attachment weld is covered with the insulating coating. The battery shell provided in the embodiment of the present application covers the attachment weld in the form of the insulating coating for protection, and the insulating protective film is thus not required to be turned over, such that the coating process of the insulating protective film is simpler to operate, and the problem of the attachment weld being corroded can be more reliably ameliorated.
Need to check novelty before this filing date? Find Prior Art

Description

Battery housing, battery cells, batteries and electrical equipment

[0001] This application claims priority to Chinese patent application number 202310458369.6, filed with the Chinese Patent Office on April 25, 2023, entitled “Battery Housing, Battery Cell, Battery and Electrical Equipment,” the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of battery technology, and in particular to a battery housing, a battery cell, a battery, and an electrical device. Background Art

[0003] In current power batteries, an insulating protective film is typically applied to the sides of the battery casing for insulation and corrosion protection. Because the end welds of the battery casing are susceptible to corrosion, the insulating protective film is typically folded over and then applied to cover the welds. However, this method of folding the insulating protective film over the welds is complex to operate and can easily ineffectively protect the welds from corrosion.

[0004] Summary of the Invention

[0005] In view of the above problems, the present application provides a battery housing, a battery cell, a battery and an electrical device, wherein the insulating protective film coating process is simpler to operate and can more reliably improve the problem of corrosion of the connecting welds.

[0006] The embodiment of the present application is implemented as follows:

[0007] In the first aspect, an embodiment of the present application provides a battery shell, comprising a shell side wall and a shell end wall connected to each other, wherein the connection between the shell side wall and the shell end wall has a connecting weld, and the connecting weld is located on the end face of the battery shell; wherein, it also includes an insulating protective film and an insulating coating, the outer side of the shell side wall is connected to the insulating protective film, and the outer side of the connecting weld is covered with an insulating coating.

[0008] In the battery case provided in the embodiments of the present application, the outer sidewalls of the case are insulated and protected against corrosion by an insulating protective film, and the connecting welds are protected against corrosion by an insulating coating. In this embodiment, the insulating protective film does not need to be folded over, making the insulating protective film coating process simpler. Furthermore, there is no risk of the insulating protective film's flange warping, which could render the connecting welds less resistant to corrosion. The coating more reliably covers the connecting welds, thereby more reliably improving the corrosion problem of the connecting welds.

[0009] In some embodiments, the edge region of the insulating protective film is connected to the insulating coating. In this embodiment, the insulating protective film and the insulating coating are connected so that there is no unprotected area between the insulating protective film and the insulating coating, thereby improving the insulation and corrosion resistance of the battery housing.

[0010] In some embodiments, the surface area of ​​the outer sidewall of the shell is S1, and the surface area of ​​the outer sidewall of the shell corresponding to the insulating protective film is S2, where S2 = S1 × (80% to 95%). In this embodiment, most of the area of ​​the shell sidewall corresponds to the insulating protective film, allowing the insulating protective film to better insulate and protect the shell sidewall.

[0011] In some embodiments, the ratio of the overlap between the ends of the insulating protective film along the circumference of the shell sidewall to the outer perimeter of the shell sidewall is (3-10):(145-750). In this embodiment, the two ends of the insulating protective film overlap by a certain dimension along the circumference of the shell sidewall. On the one hand, this allows the insulating protective film to effectively insulate and protect the shell sidewall along the entire circumference; on the other hand, it avoids excessive overlap between the two ends of the insulating protective film, which would lead to material waste and increased costs, and also avoids excessive impact on the energy density of the battery cell, the size of the battery shell, etc.

[0012] In some embodiments, the insulating coating comprises a first coating portion and a second coating portion that are interconnected. The first coating portion is located on the end face of the battery casing, with at least a portion of the first coating portion covering the outside of the connecting weld. The second coating portion is located on the outside of the casing sidewall and connected to the edge region of the insulating protective film. In this embodiment, the insulating coating is configured with the second coating portion located on the outside of the casing sidewall. The connection between the second coating portion and the edge region of the insulating protective film enables a more reliable and convenient connection between the insulating protective film and the insulating coating.

[0013] In some embodiments, the second portion of the coating covers the outer end of the shell sidewall, and at least a portion of the second portion of the coating is covered by the insulating protective film. In this embodiment, the second portion of the coating covers the outer side of the shell sidewall and is covered by the insulating protective film, that is, the second portion of the coating is located between the shell sidewall and the insulating protective film. During the manufacturing process, the second portion of the coating can be first sprayed on the outer side of the shell sidewall to form the second portion of the coating, and then the insulating protective film is glued and connected. This manufacturing process is easy to operate, and the second portion of the coating can be firmly connected to the outer side of the shell sidewall.

[0014] In some embodiments, at least a portion of the second portion of the coating covers the outer edge of the insulating protective film. In this embodiment, the second portion of the coating covers the outer side of the insulating protective film. During the manufacturing process, the insulating protective film can be first bonded and then sprayed to form the second portion of the coating, which facilitates better adhesion of the edge of the insulating protective film to the outer side of the shell sidewall.

[0015] In some embodiments, the end surface of the edge region of the insulating protective film is connected to the insulating coating. In this embodiment, the insulating coating can be formed by spraying only on the end surface of the battery housing. This preparation process is easy to operate and can save material for the insulating coating.

[0016] In some embodiments, the outer side of the shell end wall and the outer side of the connecting weld are both covered with an insulating coating. In this embodiment, the insulating coating covering the outer side of the shell end wall and the connecting weld can better protect the end face of the battery shell from corrosion, compared to only covering the outer side of the connecting weld with the insulating coating, and the manufacturing process is simpler.

[0017] In some embodiments, the insulating coating is annular and mainly covers the connecting welds, and does not need to cover the entire shell end wall, which can save the material of the insulating coating.

[0018] In some embodiments, the surface area of ​​the outer side of the shell sidewall is S1, and the surface area of ​​the area on the outer side of the shell sidewall corresponding to the second portion of the coating is S3, where S3 = S1 × (5% to 20%). In this embodiment, a certain surface area of ​​the shell sidewall corresponds to the second portion of the coating, that is, the second portion of the coating overlaps with the shell sidewall by a certain area. On the one hand, this allows for more reliable and convenient connection between the second portion of the coating and the edge area of ​​the insulating protective film; on the other hand, it avoids excessive overlap between the second portion of the coating and the shell sidewall, which would lead to material waste and increased costs, while also avoiding excessive impact on the energy density of the battery cell, the size of the battery shell, etc.

[0019] In some embodiments, along the height direction of the shell sidewall, the shell sidewall has a dimension H1, and the overlap dimension between the second portion of the coating and the insulating protective film is H2, where H2 = H1 × (2% to 10%). In this embodiment, the shell sidewall and the second portion of the coating overlap by a certain dimension along the height direction of the shell sidewall. This, on the one hand, enables a more reliable and convenient connection between the second portion of the coating and the insulating protective film; on the other hand, it avoids excessive overlap between the second portion of the coating and the insulating protective film, which would lead to material waste and increased costs, while also avoiding excessive impact on the energy density of the battery cell, the size of the battery shell, etc.

[0020] In some embodiments, the thickness of the insulating protective film is 50 μm to 120 μm. In this embodiment, the insulating protective film has an appropriate thickness to provide good insulation and corrosion resistance while avoiding excessive thickness that would lead to material waste and increased costs, and also avoid excessively affecting the energy density of the battery cell and the size of the battery housing.

[0021] In some embodiments, the thickness of the insulating coating is 50 μm to 120 μm. In this embodiment, the insulating coating has an appropriate thickness to provide good insulation and corrosion resistance while avoiding excessive thickness that would lead to material waste and increased costs, and also avoid excessively affecting the energy density of the battery cell and the size of the battery housing.

[0022] In some embodiments, the insulating protective film includes at least one connecting layer and at least one base film layer, wherein the insulating protective film is connected to the outer side of the shell sidewall via the connecting layer, and the surface of the insulating protective film away from the shell sidewall is the base film layer; wherein the connecting layer is formed by photocuring an adhesive layer including an adhesive, wherein the adhesive includes 60wt% to 95wt% of an acrylic resin, 3wt% to 35wt% of an active monomer, and 0.8wt% to 10wt% of a photoinitiator. In this embodiment, the insulating protective film is connected to the shell sidewall by photocuring an adhesive layer having an adhesive composition. wherein the adhesive comprises an acrylic resin as a primary component, which is combined with a specific amount of an active monomer and a photoinitiator. Under irradiation with light, the photoinitiator generates free radicals, causing the acrylic resin and the active monomer to form a complex. The complex continuously crosslinks, polymerizes, and solidifies into a film, forming a polyester-based three-dimensional network crosslinked body, which can provide good adhesion.

[0023] In some embodiments, the photoinitiator includes one or more of ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 1-hydroxycyclohexylphenyl ketone, 2-isopropylthioxanthone, 2-phenylbenzyl-2-dimethylamino-1-(4-morpholinobenzylphenyl)butanone, and 2-hydroxy-2-methyl-1-phenylpropanone. In this embodiment, the use of a specific type of acrylate monomer can make the polyester-based three-dimensional network cross-linked structure formed by photocuring have better density, thereby providing the insulating protective film with better rigidity and toughness.

[0024] In some embodiments, the total thickness of the base film layer is T1, and the total thickness of the adhesive layer is T2; wherein T2 = T1 × (50% to 150%); alternatively, T2 = T1 × (80% to 120%). In this embodiment, the adhesive layer and the base film layer meet an appropriate thickness ratio, so that the insulating protective film can achieve both good adhesion and insulation withstand voltage performance.

[0025] In some embodiments, the insulating coating comprises a photocured product of a UV-curable ink; wherein the UV-curable ink comprises 10 wt% to 30 wt% acrylic resin, 40 wt% to 80 wt% reactive monomer, 2 wt% to 10 wt% photoinitiator, ≤15 wt% hydrophobic monomer, ≤5 wt% coupling agent, and ≤10 wt% pigment; the reactive monomer has a viscosity of ≤10 cps at 50°C. In this embodiment, the insulating coating is formed by photocuring a UV-curable ink having a specific composition. Provided that the reactive monomer has a viscosity of ≤10 cps at 50°C and the aforementioned raw material ratios are met, the UV-curable ink can achieve a viscosity of ≤100 cps at 50°C. This allows the UV-curable ink to form an insulating coating precursor on the outside of the battery housing by spraying or printing. The insulating coating precursor is then cured by UV light to form an insulating coating, thereby improving the problem of poor insulation performance on the surface of the battery cell.

[0026] In some embodiments, the reactive monomer includes a first monomer, which is a monofunctional monomer. In this embodiment, the first monomer can improve the toughness of the insulating coating formed by UV-curable ink through UV curing.

[0027] In some embodiments, the reactive monomer further comprises a second monomer, wherein the second monomer has a functionality ≥ 2, and the mass of the second monomer is 30% to 50% of the mass of the first monomer. In this embodiment, the second monomer can increase the degree of crosslinking during curing of the UV-curable ink, and when the mass of the second monomer is 30% to 50% of the mass of the first monomer, the insulating coating can maintain both high mechanical properties and good toughness.

[0028] In some embodiments, the UV-curable ink includes 0.1 wt% to 15 wt% of a hydrophobic monomer, wherein the hydrophobic monomer has a contact angle with water of ≥90°. In this embodiment, the hydrophobic monomer can improve the wet-heat aging resistance and water resistance of the insulating coating formed by UV-curing the UV-curable ink.

[0029] In a second aspect, an embodiment of the present application provides a battery cell, comprising a battery housing as described in the above embodiment.

[0030] In a third aspect, an embodiment of the present application provides a battery, comprising a battery cell as described in the above embodiment.

[0031] In a fourth aspect, an embodiment of the present application provides an electrical device, comprising a battery housing or a battery cell as described in the above embodiment.

[0032] The above description is only an overview of the technical solutions of the embodiments of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.

[0034] FIG1 is a schematic structural diagram of a vehicle provided in some embodiments of the present application;

[0035] FIG2 is an exploded view of a battery provided in some embodiments of the present application;

[0036] FIG3 is an exploded view of a battery cell provided in some embodiments of the present application;

[0037] FIG4 is a schematic structural diagram of a first battery housing provided in some embodiments of the present application;

[0038] FIG5 is a schematic structural diagram of a second battery housing provided in some embodiments of the present application;

[0039] FIG6 is a schematic structural diagram of a third battery housing provided in some embodiments of the present application;

[0040] FIG7 is a diagram showing the corresponding relationship between the shell side wall and the insulating protective film in the unfolded state in some embodiments of the present application;

[0041] FIG8 is a schematic structural diagram of a fourth battery housing provided in some embodiments of the present application;

[0042] FIG9 is a diagram showing the corresponding relationship between the shell sidewall and the second portion of the coating in the expanded state in some embodiments of the present application;

[0043] FIG10 is a partial enlarged view of the X in FIG4 ;

[0044] FIG11 is a schematic diagram of the connection relationship between the first insulating protective film and the battery housing provided in some embodiments of the present application;

[0045] FIG12 is a schematic diagram of the connection relationship between the second insulating protective film and the battery housing provided in some embodiments of the present application;

[0046] FIG13 is a schematic structural diagram of a first insulating protective film before photocuring provided in some embodiments of the present application;

[0047] FIG14 is a schematic structural diagram of the first insulating protective film before photocuring provided in some embodiments of the present application.

[0048] Icon: 1000-vehicle; 100-battery; 200-controller; 300-motor; 10-housing; 11-first part; 12-second part; 13-accommodation space; 20-battery cell; 21-housing; 22-electrode assembly; 23-electrode terminal; 24-pressure relief structure; 211-battery housing; 212-cover; 2111-housing side wall; 2112-housing end wall; 2113-connecting weld; 2114-insulating protective film; 21141-connecting layer; 21142-base film layer; 21143-adhesive layer; 2115-insulating coating; 2115a-first part of coating; 2115b-second part of coating. DETAILED DESCRIPTION

[0049] To make the purpose, technical solutions and advantages of the examples of the present application clearer, the technical solutions in the examples of the present application will be described clearly and completely below. Where specific conditions are not specified in the examples, conventional conditions or conditions recommended by the manufacturer are used. Where the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0050] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.

[0051] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.

[0052] In the description of the embodiments of the present application, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features.

[0053] In the description of the embodiments of the present application, the orientations or positional relationships indicated by technical terms such as "inside" and "outside" are based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they cannot be understood as limitations on the embodiments of the present application.

[0054] In the description of the embodiments of this application, unless otherwise specified or limited, technical terms such as "installed," "connected," "connected," and "fixed" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integration; they can refer to direct connections or indirect connections through an intermediate medium. Those skilled in the art will understand the specific meanings of the above terms in the embodiments of this application based on specific circumstances.

[0055] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0056] In the embodiments of this application, the same reference numerals represent the same components, and for the sake of brevity, detailed descriptions of the same components in different embodiments are omitted. It should be understood that the heights, lengths, widths, and other dimensions of the various components in the embodiments of this application, as well as the overall heights, lengths, widths, and other dimensions of the integrated device shown in the drawings are merely illustrative and do not constitute any limitation on this application.

[0057] Currently, market developments indicate that power batteries are becoming increasingly widely used. They are not only used in energy storage systems such as hydropower, thermal, wind, and solar power plants, but are also widely used in electric vehicles like electric bicycles, electric motorcycles, and electric vehicles, as well as in military equipment and aerospace. As power battery applications continue to expand, market demand is also growing.

[0058] Battery casings (such as cylindrical battery casings) are generally made of steel, which is not resistant to slight acid and alkali corrosion and is prone to aging under the use environment.

[0059] Some currently proposed technical solutions employ a pressure-sensitive adhesive insulating protective film attached to the sides of the battery casing to meet insulation requirements during battery assembly while also providing corrosion protection. Because the end welds of the battery casing are susceptible to corrosion, in some cases the insulating protective film is primarily attached to the sidewalls of the battery casing, then folded over and attached to cover the welds.

[0060] However, when the insulating protective film is folded over to cover the connecting weld, the insulating protective film coating process is complicated to operate. Moreover, the folded edge of the insulating protective film used to cover the connecting weld is prone to warping, resulting in the failure of the anti-corrosion protection of the connecting weld, and the connecting weld on the end face of the battery shell is still easily corroded.

[0061] Based on this, the applicant designed a battery shell, in which the connecting welds on the end faces of the battery shell are covered with an insulating coating. There is no need to fold the insulating protective film, and the insulating protective film coating process is simpler to operate. Moreover, there is no problem of the insulating protective film's flange curling causing the corrosion protection of the connecting welds to fail. The connecting welds are more reliably covered in the form of a coating, thereby more reliably improving the problem of the connecting welds on the end faces of the battery shell being easily corroded.

[0062] In the present application, electrical equipment can be in various forms, for example, mobile phones, portable devices, laptops, battery vehicles, electric cars, ships, spacecraft, electric toys and electric tools, etc. For example, spacecraft include airplanes, rockets, space shuttles and spacecraft, etc. Electric toys include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys and electric airplane toys, etc. Electric tools include metal cutting power tools, grinding power tools, assembly power tools and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators and electric planers.

[0063] For the convenience of description, the following embodiments are described by taking a vehicle as an example of an electrical device in the embodiments of the present application.

[0064] Refer to Figure 1, which is a structural schematic diagram of a vehicle 1000 provided in some embodiments of the present application. The vehicle 1000 can be a fuel vehicle, a gas vehicle or a new energy vehicle. The new energy vehicle can be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. A battery 100 is provided inside the vehicle 1000, and the battery 100 can be provided at the bottom, head or tail of the vehicle 1000. The battery 100 can be used to power the vehicle 1000. For example, the battery 100 can serve as an operating power source for the vehicle 1000. The vehicle 1000 may also include a controller 200 and a motor 300. The controller 200 is used to control the battery 100 to power the motor 300, for example, for starting, navigating and driving the vehicle 1000.

[0065] In some embodiments of the present application, the battery 100 can not only serve as the operating power source of the vehicle 1000, but also serve as the driving power source of the vehicle 1000, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 1000.

[0066] In this application, a battery 100 refers to a single physical module that includes multiple battery cells 20 to provide higher voltage and capacity. It can be in the form of a battery pack, a battery module, etc. The battery 100 can include a housing 10 for enclosing the multiple battery cells 20. The housing 10 can prevent liquids or other foreign matter from affecting the charging or discharging of the battery cells 20.

[0067] Referring to FIG2 , FIG2 is an exploded view of a battery 100 provided in some embodiments of the present application. The battery 100 includes a housing 10 and a plurality of battery cells 20, wherein the plurality of battery cells 20 are housed in the housing 10. The housing 10 is used to house the battery cells 20, and the housing 10 can have various structures. In some embodiments, the housing 10 can include a first portion 11 and a second portion 12, wherein the first portion 11 and the second portion 12 overlap each other, and the first portion 11 and the second portion 12 jointly define a housing space 13 for accommodating the battery cells 20. The second portion 12 can be a hollow structure with one end open, and the first portion 11 is a plate-like structure, and the first portion 11 overlaps the open side of the second portion 12 to form the housing 10 with the housing space 13; the first portion 11 and the second portion 12 can also be hollow structures with one side open, and the open side of the first portion 11 overlaps the open side of the second portion 12 to form the housing 10 with the housing space 13. Of course, the first part 11 and the second part 12 can be in various shapes, such as a cylinder, a cuboid, etc.

[0068] In the battery 100, multiple battery cells 20 can be connected in series, in parallel, or in a hybrid configuration. A hybrid configuration refers to a combination of series and parallel connections among the multiple battery cells 20. Multiple battery cells 20 can be directly connected in series, in parallel, or in a hybrid configuration, and then the entire structure of the multiple battery cells 20 is housed within the housing 10. Alternatively, multiple battery cells 20 can be first connected in series, in parallel, or in a hybrid configuration to form a module, which is then connected in series, in parallel, or in a hybrid configuration to form a complete structure housed within the housing 10. The battery 100 may also include other structures. For example, multiple battery cells 20 can be electrically connected via a busbar to enable parallel, series, or hybrid connection of the multiple battery cells 20.

[0069] The battery cell 20 is the smallest unit that makes up the battery pack 100. The battery cell 20 can be a secondary battery 100 or a primary battery 100; it can also be a lithium-sulfur battery 100, a sodium-ion battery 100, or a magnesium-ion battery 100, but is not limited thereto.

[0070] 3 , the battery cell 20 may include a housing 21 , an electrode assembly 22 , and an electrolyte, and both the electrode assembly 22 and the electrolyte are accommodated in the housing 21 .

[0071] The outer shell 21 may include a battery shell 211 and a cover 212. The battery shell 211 is a component used to cooperate with the cover 212 to form an internal sealed space of the battery cell 20, wherein the formed sealed space can be used to accommodate the electrode assembly 22, electrolyte and other components. The cover 212 refers to a component that covers the opening of the battery shell 211 to isolate the internal environment of the battery cell 20 from the external environment. The shape of the cover 212 can be adapted to the shape of the battery shell 211 to cooperate with the battery shell 211. Functional components such as electrode terminals 23 and pressure relief structures 24 can also be provided on the cover 212. A sealing ring can be configured between the opening of the battery shell 211 and the cover 212 to achieve sealing between the battery shell 211 and the cover 212.

[0072] The battery housing 211 and the cover 212 can be selected from a variety of shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shapes of the battery housing 211 and the cover 212 can be determined according to the specific shape and size of the electrode assembly 22. The material of the battery housing 211 and the cover 212 can be selected from a variety of materials, such as but not limited to copper, iron, aluminum, stainless steel, aluminum alloy and other metals. The material of the sealing ring can be selected from a variety of materials, such as but not limited to PP (polypropylene), PC (polycarbonate), PET (polyethylene terephthalate) and other materials that are resistant to electrolyte corrosion, high toughness and fatigue resistance. A coating can be formed on the outer surface of the battery housing 211, and the material of the coating can be a variety of materials, such as but not limited to corrosion-resistant materials such as Ni and Cr.

[0073] The electrode assembly 22 may be composed of a positive electrode sheet, a negative electrode sheet, and a separator. The battery cell 20 primarily operates by the movement of metal ions between the positive electrode sheet and the negative electrode sheet.

[0074] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on the surface of the positive electrode current collector. The positive electrode current collector can be made of aluminum, and the positive electrode active material in the positive electrode active material layer can include lithium cobalt oxide, lithium iron phosphate, ternary lithium, lithium manganese oxide, lithium sulfur, and other positive electrode active material materials. The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector. The negative electrode current collector can be made of copper, and the negative electrode active material in the negative electrode active material layer can be carbon, silicon, and other negative electrode active material materials. In addition, the electrode assembly 22 can be a wound structure or a laminated structure, but the embodiments of the present application are not limited to this.

[0075] Next, the battery housing 211 , the battery cell 20 , the battery 100 and the electrical equipment proposed in the embodiment of the present application are described in detail.

[0076] Referring to Figures 4 to 7, in the first aspect, an embodiment of the present application provides a battery shell 211, comprising a shell side wall 2111 and a shell end wall 2112 connected to each other, and the connection between the shell side wall 2111 and the shell end wall 2112 has a connecting weld 2113, and the connecting weld 2113 is located on the end face of the battery shell 211; wherein, it also includes an insulating protective film 2114 and an insulating coating 2115, the outer side of the shell side wall 2111 is connected to the insulating protective film 2114, and the outer side of the connecting weld 2113 is covered with an insulating coating 2115.

[0077] The shell sidewall 2111 is an annular sidewall formed by a circle around the central axis of the battery shell 211. It has a hollow structure with openings at both ends. The internal cavity is used to accommodate the electrode assembly 22, electrolyte, and other components. The opening at one end is used to mate with the cover 212, and the opening at the other end is used to mate with the shell end wall 2112. The shape of the shell sidewall 2111 is not limited. In a cross section perpendicular to the central axis of the battery shell 211, the sidewall shape can be, for example, but not limited to, circular, rectangular, hexagonal, etc., for example, circular.

[0078] The end wall 2112 is a wall at the end of the battery housing 211 , and is, for example, a flat, thin-walled structure. The shape of the end wall 2112 corresponds to the opening of the side wall 2111 and is used to close the opening of the side wall 2111 .

[0079] The connecting weld 2113 refers to the solder structure formed between the shell end wall 2112 and the end of the shell side wall 2111 when the shell end wall 2112 is welded to the end of the shell side wall 2111 to close the opening at one end of the shell side wall 2111. The connecting weld 2113 extends along the circumference of the shell end wall 2112 and the shell side wall 2111 and forms an annular solder structure corresponding to the shapes of the shell end wall 2112 and the shell side wall 2111.

[0080] The outer side of the connection weld 2113 refers to a surface of the connection weld 2113 facing the outside of the battery case 211 .

[0081] The end face of the battery housing 211 refers to a face located at the end when the battery housing 211 is placed vertically, and includes a housing end wall 2112 and a connecting weld 2113 .

[0082] The insulating protective film 2114 refers to a film material having an insulating function, and may be a pressure-sensitive adhesive protective film, a light-curing protective film, or the like. It is connected to the outer side of the shell sidewall 2111, for example, but not limited to, by adhesive bonding. When the insulating protective film 2114 is connected to the outer side of the shell sidewall 2111, the insulating protective film 2114 may be connected only to the outer side of the shell sidewall 2111, or the insulating protective film 2114 may be additionally connected to the outer side of the shell end wall 2112 and / or the outer side of the connecting weld 2113.

[0083] The insulating coating 2115 is a coating having an insulating function, and is applied to the outside of the connection weld 2113 by, for example, but not limited to, spray coating, spin coating, or the like. When the outside of the connection weld 2113 is covered with the insulating coating 2115, the insulating coating 2115 may be applied only to the outside of the connection weld 2113, or may be applied to the outside of the shell end wall 2112 and / or the shell side wall 2111.

[0084] In the battery case 211 provided in the embodiment of the present application, the outer sidewall 2111 of the case is insulated and protected against corrosion by an insulating protective film 2114, and the connecting weld 2113 is insulated and protected against corrosion by an insulating coating 2115. In this embodiment, there is no need to fold the insulating protective film 2114, making the insulating protective film 2114 coating process simpler. Furthermore, there is no problem of the insulating protective film 2114's flange warping causing the connecting weld 2113's anti-corrosion protection to fail. The coating can more reliably cover the connecting weld 2113, thereby more reliably improving the problem of corrosion at the connecting weld 2113.

[0085] In some embodiments, an edge region of the insulating protection film 2114 is connected to the insulating coating 2115 .

[0086] The edge area of ​​the insulating protective film 2114 refers to the portion of the insulating protective film 2114 close to the end face of the battery shell 211 where the shell end wall 2112 is provided. The edge area of ​​the insulating protective film 2114 can be connected to the insulating coating 2115 through the inner side face, as shown in Figure 4; the edge area of ​​the insulating protective film 2114 can also be connected to the insulating coating 2115 through the outer side face, as shown in Figure 5; the edge area of ​​the insulating protective film 2114 can also be connected to the insulating coating 2115 through the end face, as shown in Figure 6.

[0087] In an embodiment of the present application, the connection between the edge area of ​​the insulating protective film 2114 and the insulating coating 2115 means that the two are seamlessly connected, that is, the two are connected along the circumference of the shell end wall 2112 so that there is no uncovered and protected area on the shell side wall 2111 between the two.

[0088] In this embodiment, the insulating protective film 2114 is connected to the insulating coating 2115 so that there is no uninsulated area between the insulating protective film 2114 and the insulating coating 2115, and the insulation and corrosion resistance of the battery housing 211 are better.

[0089] 7 , in some embodiments, the surface area of ​​the outer side of the shell sidewall 2111 is S1 , and the surface area of ​​the outer side of the shell sidewall 2111 corresponding to the insulating protective film 2114 is S2 , where S2 = S1 × (80% to 95%).

[0090] The surface area of ​​the outer side of the shell sidewall 2111 refers to the surface area of ​​the area corresponding to the central angle of 360° in the shell sidewall 2111. In other words, if the two ends of the shell sidewall 2111 overlap along the circumference of the shell sidewall 2111, the area of ​​the overlapping area is not counted twice.

[0091] The area on the outer side of the shell sidewall 2111 corresponding to the insulating protective film 2114 refers to the area where the insulating protective film 2114 is projected onto the outer side of the shell sidewall 2111. Similarly, if the two ends of the insulating protective film 2114 overlap along the circumference of the shell sidewall 2111, the area of ​​the overlapping area is not counted twice.

[0092] As an example, the percentage of S2 in S1 is, for example, but not limited to, any one of 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94% and 95%, or a range of values ​​between any two of them.

[0093] In this embodiment, most areas of the shell side wall 2111 correspond to the insulating protective film 2114 , so that the insulating protective film 2114 can better insulate and protect the shell side wall 2111 from corrosion.

[0094] In some embodiments, along the circumference of the shell sidewall 2111 , the ratio of the overlapping dimensions of the two ends of the insulating protection film 2114 to the outer perimeter of the shell sidewall 2111 is (3-10):(145-750).

[0095] The direction of the overlapping dimension of the two ends of the insulating protective film 2114 is the same as the direction in which the insulating protective film 2114 extends along the circumference of the shell sidewall 2111. When determining the outer perimeter of the shell sidewall 2111, if the two ends of the shell sidewall 2111 overlap, the length of the overlapping area is not double-counted.

[0096] In the first example, the shell sidewall 2111 is cylindrical, and the ratio of the overlapped dimension of the two ends of the insulating protective film 2114 to the outer perimeter of the shell sidewall 2111 is (3-10):(145-200). Alternatively, the outer perimeter of the shell sidewall 2111 is, for example, 145 mm to 200 mm, and the overlapped dimension of the two ends of the insulating protective film 2114 is, for example, 3 mm to 10 mm.

[0097] In the second example, the shell sidewall 2111 is in the form of a square shell, and the ratio of the overlapping dimension of the two ends of the insulating protective film 2114 to the outer perimeter of the shell sidewall 2111 is (3-10):(400-750), and further optionally (3-10):(400-500). Optionally, the outer perimeter of the shell sidewall 2111 is, for example, 400 mm to 750 mm, and further optionally 400 mm to 500 mm, and the overlapping dimension of the two ends of the insulating protective film 2114 is, for example, 3 mm to 10 mm.

[0098] As an example, the overlapping size of the two ends of the insulating protective film 2114 is, for example but not limited to, any point value among 3mm, 4mm, 5mm, 6mm, 7mm, 8mm, 9mm and 10mm, or a range value between any two of them.

[0099] In this embodiment, the two ends of the insulating protective film 2114 overlap to a certain extent along the circumference of the shell side wall 2111. On the one hand, the insulating protective film 2114 effectively insulates and protects the shell side wall 2111 in the entire circumference; on the other hand, it avoids excessive overlap of the two ends of the insulating protective film 2114, which may lead to material waste and increased costs, and at the same time avoids excessive impact on the energy density of the battery cell 20, the size of the battery shell 211, etc.

[0100] Referring to Figures 4, 5 and 8, in some embodiments, the insulating coating 2115 has a first coating portion 2115a and a second coating portion 2115b that are connected to each other, the first coating portion 2115a is located on the end face of the battery shell 211, at least a portion of the first coating portion 2115a covers the outside of the connecting weld 2113, and the second coating portion 2115b is located on the outside of the shell side wall 2111 and is connected to the edge area of ​​the insulating protective film 2114.

[0101] The first coating portion 2115a and the second coating portion 2115b are both part of the insulating coating 2115. The main difference between the two is the location. The materials of the two can be the same or different.

[0102] The first portion 2115a of the coating can only cover the outside of the connecting weld 2113, as shown in Figures 4 and 5; when a portion of the first portion 2115a of the coating covers the outside of the connecting weld 2113, other areas of the first portion 2115a of the coating can also cover other areas of the end face of the battery shell 211, for example, it can also cover at least a portion of the outside of the shell end wall 2112, as shown in Figure 8.

[0103] The second portion 2115b of the coating can be directly connected to the outer side of the shell side wall 2111. In this way, the second portion 2115b of the coating can be connected to the inner side of the edge area of ​​the insulating protective film 2114 through the outer side surface, as shown in Figure 4; the second portion 2115b of the coating can also be indirectly connected to the outer side of the shell side wall 2111. In this way, the insulating protective film 2114 can be directly connected to the outer side of the shell side wall 2111, and the second portion 2115b of the coating can be connected to the outer side of the edge area of ​​the insulating protective film 2114 through the inner side surface, as shown in Figure 5.

[0104] In this embodiment, the insulating coating 2115 is configured with a second coating portion 2115b located on the outside of the shell side wall 2111. The second coating portion 2115b is connected to the edge area of ​​the insulating protective film 2114, which can more reliably and conveniently achieve the connection between the insulating protective film 2114 and the insulating coating 2115.

[0105] 4 , in some embodiments, the second coating portion 2115 b covers the outer end portion of the shell sidewall 2111 , and at least a portion of the second coating portion 2115 b is covered by the insulating protection film 2114 .

[0106] In this embodiment, the second portion 2115b of the coating is covered on the outer side of the shell side wall 2111 and is covered by the insulating protective film 2114, that is, the second portion 2115b of the coating is located between the shell side wall 2111 and the insulating protective film 2114. In the preparation process, the second portion 2115b of the coating can be first sprayed on the outer side of the shell side wall 2111 and then glued to connect the insulating protective film 2114. The preparation process is easy to operate, and the second portion 2115b of the coating can be more firmly connected to the outer side of the shell side wall 2111.

[0107] 5 , in some embodiments, at least a portion of the second portion 2115 b of the coating layer covers an outer side of an edge region of the insulating protection film 2114 .

[0108] In this embodiment, the second portion 2115b of the coating covers the outside of the insulating protective film 2114. In the preparation process, the insulating protective film 2114 can be first glued and connected and then sprayed to form the second portion 2115b of the coating, so that the edge area of ​​the insulating protective film 2114 can better fit with the outside of the shell side wall 2111.

[0109] 6 , in some embodiments, an end surface of an edge region of the insulating protection film 2114 is connected to the insulating coating 2115 .

[0110] In this embodiment, the insulating coating 2115 can be formed by spraying only on the end surface of the battery housing 211 . This preparation process is easy to operate and can save material for the insulating coating 2115 .

[0111] 8 , in some embodiments, the outer side of the shell end wall 2112 and the outer side of the connection weld 2113 are both covered by an insulating coating 2115 .

[0112] In this embodiment, the insulating coating 2115 covers the outer side of the shell end wall 2112 and the connecting weld 2113. Compared with only covering the outer side of the connecting weld 2113 with the insulating coating 2115, the end face of the battery shell 211 can be better protected from corrosion, and the preparation process is simpler.

[0113] In some embodiments, the insulating coating 2115 is annular.

[0114] A ring refers to a structure that is connected end to end and is hollow inside. The shape of the ring in the extension direction is not limited to a circle, and can also be a square, or other regular or irregular shapes.

[0115] The extension paths of the insulating coating 2115 and the connecting weld 2113 are close so that the insulating coating 2115 can cover the connecting weld 2113, but the extension paths of the two are not limited to being identical. For example, if the extension path of the connecting weld 2113 is a square, the extension path of the insulating coating 2115 can be similar to the square, circular, etc.; if the extension path of the connecting weld 2113 is a circular, the extension path of the insulating coating 2115 can also be similar to the square, circular, etc.

[0116] In this embodiment, the insulating coating 2115 is annular and mainly covers the connecting weld 2113 . It does not need to cover the entire shell end wall 2112 , which can save material for the insulating coating 2115 .

[0117] 9 , in some embodiments, the surface area of ​​the outer side of the shell sidewall 2111 is S1, and the surface area of ​​the outer side of the shell sidewall 2111 corresponding to the second portion 2115b of the coating is S3, where S3 = S1×(5% to 20%).

[0118] The area on the outer side of the shell sidewall 2111 corresponding to the second portion 2115 b of the coating layer refers to the area on the outer side of the shell sidewall 2111 where the second portion 2115 b of the coating layer is projected onto.

[0119] As an example, the percentage of S3 in S1 is, for example but not limited to, any one of 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% and 20%, or a range of values ​​between any two of them.

[0120] In this embodiment, a certain surface area in the shell side wall 2111 corresponds to the second portion 2115b of the coating, that is, the second portion 2115b of the coating overlaps with the shell side wall 2111 by a certain area. On the one hand, it can more reliably and conveniently achieve the connection between the second portion 2115b of the coating and the edge area of ​​the insulating protective film 2114; on the other hand, it avoids excessive overlap between the second portion 2115b of the coating and the shell side wall 2111, resulting in material waste and increased costs, while avoiding excessive impact on the energy density of the battery cell 20, the size of the battery shell 211, etc.

[0121] 4 and 10 , in some embodiments, along the height direction of the shell sidewall 2111 , the size of the shell sidewall 2111 is H1 , and the overlapping size of the second portion 2115 b of the coating and the insulating protection film 2114 is H2 , where H2 = H1 × (2% to 10%).

[0122] As an example, the ratio of H2 / H1 is, for example but not limited to, any one of 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% and 10%, or a range of values ​​between any two of them.

[0123] In this embodiment, the shell side wall 2111 and the second portion 2115b of the coating overlap by a certain size along the height direction of the shell side wall 2111. On the one hand, the connection between the second portion 2115b of the coating and the insulating protective film 2114 can be achieved more reliably and conveniently; on the other hand, excessive overlap between the second portion 2115b of the coating and the insulating protective film 2114 is avoided, which may lead to waste of materials and increased costs, while also avoiding excessive impact on the energy density of the battery cell 20, the size of the battery shell 211, etc.

[0124] In some embodiments, the thickness of the insulating protection film 2114 is 50 μm to 120 μm.

[0125] The thickness of the insulating protective film 2114 refers to the dimension of the insulating protective film 2114 perpendicular to the surface to which it is attached. In other words, the thickness of the insulating protective film 2114 refers to the dimension of the insulating protective film 2114 perpendicular to the sidewall 2111 of the battery housing 211, in a specified cross-section of the battery housing 211. A specified cross-section is a cross-section passing through and parallel to the central axis of the battery housing 211. For a cylindrical battery housing 211, for example, a specified cross-section is a cross-section passing through and parallel to the axis of the cylinder.

[0126] As an example, the thickness of the insulating protection film 2114 is, for example but not limited to, any one of 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm and 120 μm, or a range between any two thereof.

[0127] In this embodiment, the insulating protective film 2114 has a suitable thickness, which can exert good insulation and corrosion resistance, while avoiding excessive thickness that leads to material waste and increased costs, and avoids excessive impact on the energy density of the battery cell 20, the size of the battery shell 211, etc.

[0128] In some embodiments, the thickness of the insulating coating 2115 is 50 μm to 120 μm.

[0129] The thickness of the insulating coating 2115 refers to the dimension of the insulating coating 2115 perpendicular to the surface to which it is attached. Taking the thickness of the second portion 2115b of the coating as an example, it refers to the dimension of the second portion 2115b of the coating perpendicular to the sidewall 2111 of the battery housing 211 in a specified cross-section. The specified cross-section refers to a cross-section passing through and parallel to the central axis of the battery housing 211.

[0130] As an example, the thickness of the insulating coating 2115 is, for example but not limited to, any one of 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm and 120 μm, or a range of values ​​between any two thereof.

[0131] In this embodiment, the insulating coating 2115 has a suitable thickness, which can exert good insulation and corrosion resistance, while avoiding excessive thickness that leads to material waste and increased costs, and avoids excessive impact on the energy density of the battery cell 20, the size of the battery shell 211, etc.

[0132] In some technical solutions, a pressure-sensitive adhesive insulating protective film 2114 is attached to the side of the battery housing 211 to meet the insulation requirements during battery 100 assembly and provide corrosion protection. However, the current pressure-sensitive insulating protective film 2114 has low bonding strength to the surface of the battery housing 211, posing a risk of interlaminar failure under harsh operating conditions.

[0133] Based on this, some embodiments of the present application provide an insulating protective film 2114 including a specific adhesive as a raw material. The adhesive includes a specific content of acrylic resin, an active monomer and a photoinitiator, and illustratively also includes a suitable content of a coupling agent. Additives and pigments can also be added as needed. The additives include, but are not limited to, one or more of a leveling agent, a plasticizer, a stabilizer and an inhibitor. The adhesive is used for the adhesive layer 21143 of the insulating film. The adhesive layer 21143 forms a connecting layer 21141 in the insulating protective film 2114 under the action of light curing, which is bonded to the surface of the battery shell 211. A polyester three-dimensional network cross-linked body is formed in the connecting layer 21141, which can provide better adhesion to the insulating protective film 2114 and improve the bonding strength between the insulating protective film 2114 and the surface of the battery shell 211.

[0134] The following is a description of some exemplary embodiments of the insulating protection film 2114 .

[0135] In some embodiments, the insulating protective film 2114 includes at least one connecting layer 21141 and at least one base film layer 21142. The insulating protective film 2114 is connected to the outer side of the shell side wall 2111 through the connecting layer 21141, and the surface layer of the insulating protective film 2114 away from the shell side wall 2111 is the base film layer 21142; wherein, the connecting layer 21141 is formed by photocuring an adhesive layer 21143 including an adhesive, and the adhesive includes 60wt% to 95wt% of acrylic resin, 3wt% to 35wt% of active monomer and 0.8wt% to 10wt% of photoinitiator.

[0136] The base film layer 21142 is a film layer with insulating properties, such as an insulating polyester film PET.

[0137] Optionally, the adhesive includes: 60 wt% to 88 wt% of acrylic resin, 10 wt% to 20 wt% of active monomer, 2 wt% to 5 wt% of photoinitiator, ≤5 wt% of coupling agent, and ≤10 wt% of pigment.

[0138] Acrylic resin is a polymer obtained by polymerizing acrylic acid or acrylic acid derivatives as monomers, or a polymer obtained by copolymerizing acrylic acid or acrylic acid derivatives with other unsaturated compounds.

[0139] The type of acrylic resin is not limited, for example, including one or more of ARONIX M-7100, ARONIX M-8030, ARONIX M-8060, ARONIX M-90, AgiSyn 720, NeoRad P-56, allnex unsaturated polyester resin UVECOAT@9010, allnex unsaturated polyester resin UVECOAT@2100 and allnex unsaturated polyester resin UVECOAT@3005.

[0140] The content of acrylic resin in the adhesive is, for example but not limited to, any one of 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, 80wt%, 85wt%, 90wt% and 95wt% or a range between any two of them.

[0141] The reactive monomer is a material that can improve the rheological properties of the oligomer formed during the light curing process of the adhesive, and can include one or more reactive monomers with monofunctionality, difunctionality, trifunctionality, and higher functionality.

[0142] The content of the active monomer in the adhesive is, for example but not limited to, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt% and 35wt%, any one of the values ​​or the range between any two of them.

[0143] Photoinitiator, also known as photosensitizer or photocuring agent, is a type of compound that can absorb energy of a certain wavelength in the ultraviolet light region (250nm~420nm) or visible light region (400nm~800nm), generate free radicals, cations, etc., thereby initiating monomer polymerization, cross-linking and curing.

[0144] The content of the photoinitiator in the adhesive is, for example but not limited to, any one of 0.8wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt% and 10wt%, or a range between any two of them.

[0145] In this embodiment, an adhesive layer 21143 with an adhesive of a specific composition is photocured to form a connecting layer 21141 to achieve the connection between the insulating protective film 2114 and the shell side wall 2111, wherein the adhesive is mainly composed of acrylic resin, and the acrylic resin is combined with a specific content of active monomers and photoinitiators. Under the irradiation of light, free radicals are generated by the photoinitiator, so that the acrylic resin and the active monomers form a complex. The complex is continuously cross-linked, polymerized and cured into a film, forming a polyester three-dimensional network cross-linked body, which can provide better adhesion.

[0146] In some embodiments, the adhesive includes 60 wt % to 88 wt % of an acrylic resin, 8 wt % to 28 wt % of a reactive monomer, and 2 wt % to 8 wt % of a photoinitiator.

[0147] Optionally, the adhesive includes: 60 wt% to 88 wt% of acrylic resin, 10 wt% to 20 wt% of active monomer, and 2 wt% to 5 wt% of photoinitiator.

[0148] It should be noted that, in the embodiments of the present application, when the contents of the above components are within a specific range, if the total is less than 100%, it means that other components such as solvents and additives may also be present in the adhesive.

[0149] In this embodiment, the acrylic resin, the active monomer and the photoinitiator have a more appropriate usage ratio, and can have good bonding strength, toughness and insulation withstand voltage performance.

[0150] In some embodiments, the reactive monomer comprises an acrylate monomer.

[0151] The acrylate monomer refers to a monomer of acrylic acid or an acrylic acid derivative.

[0152] In this embodiment, the acrylate monomer can make the polyester three-dimensional network cross-linked body formed by photocuring have better density, and can provide the insulating protection film 2114 with better rigidity and toughness.

[0153] In some embodiments, the acrylate monomer includes one or more of isobornyl acrylate, trimethylolpropane triacrylate, diethylene glycol diacrylate, dimethylolethane triacrylate, tripropylene glycol diacrylate, 2-ethylethyl acrylate, β-hydroxyethyl methacrylate, dipentaerythritol pentaacrylate, 2-methoxyethyl acrylate, bisphenol alpha dimethacrylate, 1,6-hexanediol diacrylate, and tetrahydrofuran acrylate.

[0154] In some exemplary embodiments, the acrylate monomer includes one or more of dimethylolethane triacrylate, bisphenol α dimethacrylate, tetrahydrofuran acrylate, and diethylene glycol diacrylate.

[0155] In this embodiment, a specific type of acrylic ester monomer is used to make the polyester three-dimensional network cross-linked body formed by photocuring have better density, thereby providing better rigidity and toughness for the insulating protective film 2114.

[0156] In some embodiments, the photoinitiator includes one or more of ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 1-hydroxycyclohexylphenyl ketone, 2-isopropylthioxanthone, 2-phenylbenzyl-2-dimethylamino-1-(4-morpholinobenzylphenyl)butanone, and 2-hydroxy-2-methyl-1-phenylpropanone.

[0157] In this embodiment, a specific type of acrylic ester monomer is used to make the polyester three-dimensional network cross-linked body formed by photocuring have better density, thereby providing better rigidity and toughness for the insulating protective film 2114.

[0158] In some embodiments, the photoinitiator includes at least two of ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 1-hydroxycyclohexylphenyl ketone, 2-isopropylthioxanthone, 2-phenylbenzyl-2-dimethylamino-1-(4-morpholinobenzylphenyl)butanone, and 2-hydroxy-2-methyl-1-phenylpropanone.

[0159] In some exemplary embodiments, the photoinitiator includes at least two of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-isopropylthioxanthone, and 1-hydroxycyclohexylphenyl ketone.

[0160] In this embodiment, at least two specific types of photoinitiators are used. The photoinitiators can cover a wider UV absorption wavelength and can better initiate the cross-linking and curing of the adhesive under ultraviolet light, so that the adhesive can have a higher degree of curing under ultraviolet light, thereby providing better adhesion and rigidity for the insulating protective film 2114.

[0161] In some embodiments, the photoinitiator includes 1-hydroxycyclohexyl phenyl ketone. Optionally, the mass proportion of 1-hydroxycyclohexyl phenyl ketone in the photoinitiator is, for example, 80 wt% to 95 wt%, such as, but not limited to, any one of 80 wt%, 81 wt%, 82 wt%, 83 wt%, 84 wt%, 85 wt%, 86 wt%, 87 wt%, 88 wt%, 89 wt%, 90 wt%, 91 wt%, 92 wt%, 93 wt%, 94 wt% and 95 wt%, or a range between any two of the above.

[0162] In some exemplary embodiments, the photoinitiator includes 1-hydroxycyclohexylphenyl ketone and ethyl 2,4,6-trimethylbenzoylphenylphosphonate.

[0163] In this embodiment, at least two specific types of photoinitiators are used, and at least 1-hydroxycyclohexyl phenyl ketone is contained, which can better initiate the cross-linking and curing of the adhesive under ultraviolet light, so that the adhesive can have a higher degree of curing under ultraviolet light, thereby providing better adhesion and rigidity for the insulating protective film 2114.

[0164] In some embodiments, ≤ 5 wt % of a coupling agent is also included.

[0165] Coupling agents are a class of substances with two functional groups of different properties, one is an inorganic-philic group and the other is an organic-philic group.

[0166] The content of the coupling agent in the adhesive is, for example but not limited to, any one of 0 wt %, 1 wt %, 2 wt %, 3 wt %, 4 wt % and 5 wt %, or a range between any two of them.

[0167] In the embodiments of the present application, the content of the coupling agent in the adhesive may be 0, and it may be selected whether to add the coupling agent as needed.

[0168] In this embodiment, the adhesive further includes a certain amount of coupling agent, which can provide a bridging effect and provide the insulating protective film 2114 with better adhesion and insulation withstand voltage performance.

[0169] In some embodiments, the coupling agent includes one or more of aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-methacryloxypropyltrimethoxysilane.

[0170] KH-550 is aminopropyltriethoxysilane, KH-560 is γ-glycidoxypropyltrimethoxysilane, and KH-570 is γ-methacryloyloxypropyltrimethoxysilane.

[0171] In this embodiment, a specific type of coupling agent is used to provide a better bridging effect, which can effectively provide better adhesion and insulation withstand voltage performance for the insulating protective film 2114, so that the insulating protective film 2114 has higher peel strength and smaller flange lift height.

[0172] In some embodiments, ≤ 10 wt % of pigment is also included.

[0173] Pigments can be used to dye the adhesive, thereby obtaining an insulating protective film 2114 of a target color. Examples of target colors include benzidine yellow, phthalocyanine blue, permanent red, pink, sapphire, or sun-fast crimson. Examples of pigments include one or more of azo pigments, phthalocyanine pigments, quinacridone pigments, isoindolinone pigments, isoindolinoline pigments, benzimidazolone pigments, dioxazine pigments, perylene pigments, peronone pigments, anthraquinone pigments, anthrapyrimidine pigments, and indanthrene pigments.

[0174] The content of the pigment in the adhesive is, for example but not limited to, any one of 0wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% and 10wt%, or a range between any two of them.

[0175] In the embodiments of the present application, the content of pigment in the adhesive may be 0, and it may be selected whether to add pigment as needed.

[0176] In this embodiment, the adhesive further includes a certain amount of pigment, which can dye the adhesive to an appropriate degree to achieve the target color.

[0177] In an embodiment of the present application, the connecting layer 21141 is formed by photocuring the adhesive layer 21143. The difference between the two lies in the cross-linking between the raw materials. The connecting layer 21141 and the adhesive layer 21143 are similar in size. Unless otherwise specified, it can be considered that the connecting layer 21141 and the adhesive layer 21143 are equal in size.

[0178] In some embodiments, the total thickness of the base film layer 21142 is T1, and the total thickness of the adhesive layer 21143 is T2; wherein, T2 = T1×(50% to 150%); optionally, T2 = T1×(80% to 120%).

[0179] As an example, the ratio of T1 and T2 is expressed as a percentage, such as but not limited to any point value of 50%, 60%, 70%, 80%, 90%, 100%, 110% and 120%, or a range of values ​​between any two.

[0180] In this embodiment, the adhesive layer 21143 and the base film layer 21142 meet a suitable thickness ratio, so that the connecting layer 21141 and the base film layer 21142 meet a suitable thickness ratio, so that the insulating protective film 2114 can take into account both good adhesion and insulation withstand voltage performance.

[0181] In some embodiments, the thickness of the single adhesive layer 21143 is T2′; wherein T2′ is ≤ 60 μm.

[0182] As an example, the thickness T2' of the single adhesive layer 21143 is, but is not limited to, any one of 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm and 60 μm, or a range between any two of them.

[0183] In this embodiment, the thickness of the single adhesive layer 21143 is below a certain standard, which is conducive to the adhesive in the adhesive layer 21143 to cure faster under the irradiation of light. While the adhesive layer 21143 can provide better adhesion, it avoids the adhesive layer 21143 being too thick, resulting in excess performance and affecting the production rhythm.

[0184] 5 and 6 , in some embodiments, the thickness of the single-layer base film layer 21142 is T1′; wherein, 25 μm≤T1′≤80 μm; optionally, 40 μm≤T1′≤60 μm.

[0185] As an example, the thickness T1' of the single-layer base membrane layer 21142 is any point value of 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, 75μm and 80μm, or a range value between any two of them.

[0186] In this embodiment, the thickness of the single-layer base film layer 21142 is within a certain range. While the base film layer 21142 can exert good insulation and voltage resistance performance, it avoids the base film layer 21142 being too thick to cause excess performance and affect the production rhythm.

[0187] The following is a description of some exemplary embodiments of the insulating protection film 2114 .

[0188] In some embodiments, the insulating coating 2115 includes a photocured product of a UV-curable ink; wherein the UV-curable ink includes 10wt% to 30wt% acrylic resin, 40wt% to 80wt% active monomer, 2wt% to 10wt% photoinitiator, ≤15wt% hydrophobic monomer, ≤5wt% coupling agent and ≤10wt% pigment; the viscosity of the active monomer at 50°C is ≤10cps.

[0189] Among them, the acrylic resin is selected from any one or more of EBECRYL 572 (functionality 3, number average molecular weight 1500) of the United States, EBECRYL 800 (functionality 4, number average molecular weight 780) of the United States, EBECRYL 837 (functionality 6, number average molecular weight 2700) of the United States, AgiSyn 707 (functionality 4, number average molecular weight 4700) of the Netherlands, AgiSyn 720 (functionality 4, number average molecular weight 1000) of the Netherlands and NeoRad P-56 (functionality 6, number average molecular weight 1800) of the Netherlands.

[0190] The photoinitiator is selected from any one or more of 1-hydroxycyclohexylphenyl ketone, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, (2,4,6-trimethylbenzoyl)diphenylphosphine oxide, 2-isopropylthioxanthone, 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone and 2-hydroxy-2-methyl-1-phenylpropanone.

[0191] In this embodiment, an insulating coating 2115 is formed by photocuring a UV-curable ink having a specific composition. Under the premise that the viscosity of the active monomer at 50°C is ≤10cps and the above-mentioned raw material ratio is met, the UV-curable ink can achieve a viscosity at 50°C of ≤100cps, so that the UV-curable ink can form an insulating coating 2115 precursor on the outside of the battery shell 211 by spraying or printing. The insulating coating 2115 precursor is cured by UV light to form the insulating coating 2115, thereby improving the problem of poor insulation performance on the surface of the battery cell 20.

[0192] Optionally, the viscosity of the reactive monomer at 50° C. is ≤ 8 cps.

[0193] On the premise that the active monomer satisfies the viscosity of ≤8cps at 50°C and meets the above raw material ratio, the UV-curable ink can achieve a viscosity of ≤80cps at 50°C.

[0194] According to some embodiments of the present application, optionally, the active monomer includes any one or more of isobornyl acrylate, tetramethylene acrylate, bisphenol α dimethacrylate, 2-ethyl acrylate, β-hydroxyethyl methacrylate, 2-methoxyethyl acrylate, tripropylene glycol diacrylate, diethylene glycol diacrylate, 1,6-hexanediol diacrylate, dimethylolethane triacrylate, trimethylolpropane triacrylate, 3-ethoxylated trimethylolpropane triacrylate, pentaerythritol pentaacrylate and dipentaerythritol pentaacrylate.

[0195] The viscosity of the reactive monomer at 50° C. is ≤10 cps, which can make the viscosity of the prepared UV-curable ink at 50° C. ≤100 cps, thereby making the UV-curable ink meet the requirements of spraying or printing.

[0196] The viscosity of the reactive monomer and the prepared external light curing ink at 50°C can be obtained by testing with reference to the GB / T 2794 method.

[0197] In some embodiments, the reactive monomer includes a first monomer, and the first monomer is a monofunctional monomer.

[0198] The functionality of the monofunctional monomer, ie, the first monomer, is 1.

[0199] In this embodiment, the first monomer can improve the toughness of the insulating coating 2115 formed by UV-curable ink through UV-curing.

[0200] According to some embodiments of the present application, optionally, the first monomer includes any one or more of isobornyl acrylate, tetramethylene acrylate, bisphenol α dimethacrylate, 2-ethyl acrylate, β-hydroxyethyl methacrylate and 2-methoxyethyl acrylate.

[0201] The above monomer is a monofunctional monomer, which can improve the toughness of the insulating coating 2115 formed by UV-curing the UV-curable ink.

[0202] In some embodiments, the reactive monomer further comprises a second monomer, the functionality of the second monomer is ≥2, and the mass of the second monomer is 30% to 50% of the mass of the first monomer.

[0203] As an example, the weight of the second monomer is 30%, 35%, 40%, 45%, or 50% of the weight of the first monomer.

[0204] In this embodiment, the second monomer can increase the degree of cross-linking during curing of the UV-curable ink, and when the mass of the second monomer is 30% to 50% of the mass of the first monomer, the insulating coating 2115 can maintain both high mechanical properties and good toughness.

[0205] According to some embodiments of the present application, optionally, the second monomer includes any one or more of tripropylene glycol diacrylate, diethylene glycol diacrylate, 1,6-hexanediol diacrylate, dimethylolethane triacrylate, trimethylolpropane triacrylate, 3-ethoxylated trimethylolpropane triacrylate, pentaerythritol pentaacrylate and dipentaerythritol pentaacrylate.

[0206] The functionality of the above monomers is ≥2, which can improve the cross-linking degree of the UV-curable ink during curing and enable the insulating coating 2115 to maintain both high mechanical properties and good toughness.

[0207] In some embodiments, the UV-curable ink includes 0.1 wt % to 15 wt % of a hydrophobic monomer, and the contact angle of the hydrophobic monomer with water is ≥90°.

[0208] In this embodiment, the hydrophobic monomer can improve the moisture-heat aging resistance and water resistance of the insulating coating 2115 formed by UV-curable ink through UV curing.

[0209] According to some embodiments of the present application, optionally, the hydrophobic monomer includes any one or more of trifluoroethyl (meth)acrylate, hexafluorobutyl (meth)acrylate, dodecafluoroheptyl methacrylate, tetrafluoropropanol methacrylate, γ-methacryloyloxypropyltrimethoxysilane, α-methacryloyloxymethyltrimethylsilane and trimethylsilyl methacrylate.

[0210] The above monomer is a hydrophobic monomer, which can improve the heat and moisture aging resistance and water resistance of the insulating coating 2115 formed by UV-curing ink through UV curing.

[0211] According to some embodiments of the present application, optionally, the UV curable ink includes 0.2 wt % to 5 wt % of a coupling agent.

[0212] The coupling agent can enhance the adhesion of the insulating coating 2115 formed by UV-curing ink through UV-curing to the main body of the battery 100 shell 21 and the structural adhesive.

[0213] According to some embodiments of the present application, optionally, the coupling agent includes any one or more of KH-550, KH-560 and KH-570.

[0214] The coupling agent can enhance the adhesion of the insulating coating 2115 formed by UV-curable ink through UV-curing to the main body of the battery 100 shell 21 and the structural adhesive.

[0215] According to some embodiments of the present application, optionally, the UV curable ink includes 1 wt% to 10 wt% of pigment.

[0216] The pigment can dye the insulating coating 2115 to obtain the insulating coating 2115 of a target color.

[0217] Target colors include benzidine yellow, phthalocyanine blue, permanent red, pink, ruby ​​red, or light-fast crimson.

[0218] The pigment includes any one or more of azo pigments, phthalocyanine pigments, quinacridone pigments, isoindolinone pigments, isoindolinone pigments, benzimidazolone pigments, dioxazine pigments, perylene pigments, perinone pigments, anthraquinone pigments, anthrapyrimidine pigments and indanthrene pigments.

[0219] An embodiment of the present application also provides a method for preparing a battery shell 211, and the process of connecting the insulating protective film 2114 includes: providing a connecting unit having an adhesive layer 21143 and a base film layer 21142, connecting the outermost adhesive layer 21143 of the connecting unit to the outer side of the shell side wall 2111, and allowing the adhesive layer 21143 to be photocured to form a connecting layer 21141.

[0220] In some embodiments, the connecting unit is illuminated and cut, and then the outer side of the shell side wall 2111 is coated with the connecting unit, and then left to solidify.

[0221] In some embodiments, the connection unit is cut, the outer side of the shell side wall 2111 is coated with the connection unit, and then the connection unit is illuminated and then left to solidify.

[0222] An embodiment of the present application also provides a method for preparing a battery shell 211, and the process of connecting the insulating coating 2115 includes: using the ultraviolet light-curing ink of the above embodiment as a raw material, inkjet printing is performed on the target area of ​​the end face of the battery shell 211 where the shell end wall is provided to form an insulating coating 2115 precursor; and the insulating coating 2115 precursor is cured by ultraviolet light irradiation to form an insulating coating 2115.

[0223] In the embodiment of the present application, the insulating protective film 2114 may be connected first and then the insulating coating 2115 ; or the insulating coating 2115 may be connected first and then the insulating protective film 2114 .

[0224] In the embodiment of the present application, when the insulating protective film 2114 and the insulating coating 2115 are photocured, the photocuring process exemplarily includes the following conditions: the UV light source is selected as UVLED, and the wavelength of 365nm, 385nm or 405nm is selected according to the absorption wavelength of the photoinitiator. The UV activation energy is selected as 500mJ / cm 2 ~10000mJ / cm 2 , the activation time is 0.1s to 10s; further, the UV activation energy is selected to be 1000mJ / cm 2 ~6000mJ / cm 2 The activation time is 1s to 6s.

[0225] Referring to FIG. 4 , in some embodiments of the present application, the insulating coating 2115 includes a first coating portion 2115a and a second coating portion 2115b that are interconnected. The second coating portion 2115b covers the outer end of the shell sidewall 2111, and at least a portion of the second coating portion 2115b is covered by the insulating protective film 2114. The insulating coating 2115 is annular in shape, corresponding to the connecting weld 2113. The outer side of the connecting weld 2113 is covered by the first coating portion 2115a, while the outer side of the shell end wall 2112 is not covered by the first coating portion 2115a.

[0226] Referring to FIG. 8 , in some embodiments of the present application, the insulating coating 2115 includes a first coating portion 2115a and a second coating portion 2115b that are interconnected. The second coating portion 2115b covers the outer end of the shell sidewall 2111, and at least a portion of the second coating portion 2115b is covered by an insulating protective film 2114. The outer side of the shell end wall 2112 and the outer side of the connecting weld 2113 are both covered by the first coating portion 2115a.

[0227] In a second aspect, an embodiment of the present application provides a battery cell 20 , comprising a battery housing 211 as described in the above embodiment.

[0228] In a third aspect, an embodiment of the present application provides a battery 100 including the battery cell 20 according to the above embodiment.

[0229] In a fourth aspect, an embodiment of the present application provides an electrical device, including a battery housing 211 or a battery cell 20 as described in the above embodiment.

[0230] Some specific embodiments are listed below to better illustrate the present application.

[0231] Test Example 1

[0232] 11 and 12 , an insulating protective film 2114 is connected to the case side wall 2111 of the battery case 211 .

[0233] The adhesive layer 21143 is made of 75 wt% acrylic resin, 17 wt% reactive monomer, 5 wt% photoinitiator, 2.5 wt% coupling agent, and 0.5 wt% pigment. The reactive monomer is UVECOAT@2100, an allnex unsaturated polyester resin. The reactive monomer is tetrahydrofuran acrylate, the photoinitiator is ethyl 2,4,6-trimethylbenzoylphenylphosphonate and 1-hydroxycyclohexylphenyl ketone in a 9:1 ratio by weight, and the coupling agent is KH-550. The target pigment color is phthalocyanine blue.

[0234] The arrangement structure and thickness of the base film layer 21142 in the insulating protective film 2114 and the adhesive layer 21143 forming the connecting layer 21141 are shown in Table 1.1. The light source in the process of photocuring the adhesive layer 21143 is selected as UVLED, and the absorption band is selected as the 370nm band. The other conditions are shown in Table 1.1.

[0235] Table 1.1 Insulation protective film structure and light curing conditions

[0236] Test Example 2

[0237] 11 , an insulating protective film 2114 is connected to the case side wall 2111 of the battery case 211 .

[0238] The insulating protective film 2114 has a base film layer 21142 and an adhesive layer 21143 forming the connecting layer 21141, each with a thickness of 50 μm. The light source for the photocuring of the adhesive layer 21143 is a UV LED, with an absorption band of 370 nm. The UV activation energy is 4500 mJ / cm 2 , the activation time is 3s.

[0239] The types of adhesive components used in each example are shown in Table 2.1, and the amounts of adhesive components used in each example are shown in Table 2.2. The acrylic resin used in each example is UVECOAT@2100, an unsaturated polyester resin from Allnex.

[0240] Table 2.1 Component types of adhesives in various examples

[0241] Table 2.2 Component dosage of adhesive in each embodiment

[0242] In addition, Example 2.22 of Test Example 2 also provides an adhesive comprising 10 wt % of acrylic acid, 15 wt % of methyl acrylate, 17 wt % of methyl methacrylate, 25 wt % of butyl acrylate, 30 wt % of ethyl acetate, 0.5 wt % of benzoyl peroxide, and 2.5 wt % of sodium dodecylbenzenesulfonate.

[0243] Test Example 3

[0244] An insulating coating 2115 is formed on the end wall of the battery case 211 .

[0245] The insulating coating 2115 is formed by ultraviolet curing ink. The ultraviolet curing ink is cured by ultraviolet light, and the intensity of ultraviolet light is 2000mW / cm 2 ~5000mW / cm 2 , the ultraviolet light irradiation time is 2s~20s, and the wavelength of ultraviolet light is 350nm~400nm.

[0246] The amount of components used in the UV-curable ink of each embodiment is shown in Table 3.1, and the type of components used in the UV-curable ink of each embodiment is shown in Table 3.2.

[0247] Table 3.1 Component dosage of UV curable ink in each example

[0248] Table 3.2 Components of UV-curable inks in various examples

[0249] Performance Testing

[0250] The performance of the corresponding insulating protective films and insulating coatings in Test Examples 1 to 3 were tested. The results corresponding to Test Example 1 are shown in Table 1.2, the results corresponding to Test Example 2 are shown in Tables 2.3 and 2.4, and the results corresponding to Test Example 3 are shown in Table 3.3.

[0251] The performance test method of the insulating protective film is as follows:

[0252] 1. Anti-flaring and warping performance

[0253] Bend the insulating film 90° and attach it to the aluminum shell of the battery cell. The bending length is 4mm. Observe the degree of warping and measure the height of the warping edge.

[0254] 2. Adhesion

[0255] Testing was performed according to the GB / T 9286-1998 method. An insulating protective film was adhered to the surface of a 150 x 100 mm aluminum plate and placed on a horizontal, rigid surface. A grid knife was used to cut perpendicular to the sample, ensuring that all cuts penetrated the substrate surface. An equal number of cuts were then made at 90° angles to the original cut lines to form a grid. The surface was then brushed several times with a soft brush. Transparent tape was applied over the grid, flattened, and removed. The adhesion of the insulating protective film was determined using the adhesion grading chart, and the 180° peel strength was recorded.

[0256] 3. Shear strength

[0257] Standard aluminum sheets with insulating protective film were overlapped with structural adhesive and tested according to GB / T 7124 method.

[0258] 4. Aging test

[0259] Place a standard aluminum sheet with an insulating protective film under 85°C / 85% humidity conditions for 1000 hours, and test the shear strength of the insulating protective film after aging. Record this as the shear strength after aging.

[0260] 5. Insulation withstand voltage test

[0261] Cut the insulating protective film into 5×5cm rectangular strips and stick them on the surface of the aluminum plate. Use an insulation withstand voltage tester to perform a 2700V, 60s withstand voltage test. If the leakage current is ≤0.1mA, it passes and the result is expressed as "OK"; if the leakage current is greater than 0.1mA, it fails and the result is expressed as "NG".

[0262] The performance test method of the insulating coating is as follows:

[0263] 1. Viscosity

[0264] Tested according to GB / T 2794 method.

[0265] 2. Shear strength

[0266] Standard aluminum sheets with insulation coatings were overlapped with structural adhesive and tested according to the GB / T 7124 method.

[0267] 3. Insulation withstand voltage test

[0268] The insulating coating was cut into 5×5cm rectangular strips and attached to the surface of the aluminum plate. An insulation withstand voltage test was performed using a 2700V, 60s withstand voltage test. The test passed if the leakage current was ≤0.1mA.

[0269] 4. Adhesion

[0270] Test according to GB / T 9286-1998. Adhere the insulating coating to the surface of a 150 x 100 mm aluminum plate and place it on a horizontal, rigid surface. Use a grid knife to cut perpendicular to the sample, ensuring all cuts penetrate the substrate surface. Then, make the same number of cuts at 90° angles to the original cut lines to form a grid. Then, use a soft brush to brush the surface several times. Apply transparent tape over the grid, flatten it, and remove the tape. Refer to the Adhesion Grading Chart for the adhesion of the insulating coating.

[0271] 5. Aging test

[0272] A standard aluminum sheet with an insulating coating was placed under 85°C / 85% for 1000 hours to test the shear strength and adhesion of the insulating coating after aging.

[0273] 6. Water test

[0274] Place a standard aluminum sheet with insulating coating in 85℃ deionized water for 1000h, take it out and wipe off the water, then dry it in the air, and test the adhesion and insulation withstand voltage performance of the insulating coating.

[0275] 7. Flexibility test

[0276] Refer to GB / T 6742 for assessment. Bend the test specimens coated with insulating coatings 180° on mandrels of different diameters and report the minimum curvature diameter at which the insulating coating does not crack or peel off.

[0277]

[0278] The performance test results and brief analysis are as follows:

[0279] Table 1.2 Performance test results of insulation protective film

[0280] According to Table 1.1 and Table 1.2, a brief analysis is as follows:

[0281] In Examples 1.1 to 1.3, the adhesive layer and base film layer have suitable thicknesses, and the insulating protective film has good shear strength, aging resistance, and anti-flagging performance. Within a certain range, as the thickness of the adhesive layer and base film layer increases, the shear strength, aging resistance, and anti-flagging performance of the insulating protective film gradually increase.

[0282] In Examples 1.1 to 1.2 and 1.4, the thickness of the adhesive layer is similar, and Example 1.1 and Example 1.2 have a more suitable base film layer thickness. The shear strength and aging resistance of the insulating protective films of Example 1.1 and Example 1.2 are better.

[0283] In Examples 1.4 and 1.5, the total thickness of the adhesive layer and the base film layer is the same. In Example 1.5, the adhesive layer and the base film layer are each provided with two layers. Compared with Example 1.4 in which the adhesive layer and the base film layer are each provided with only one layer, the shear strength and anti-aging performance of the insulating protective film of Example 1.5 are better.

[0284] Table 2.3. Performance test results of the insulating protective film of each embodiment

[0285] Table 2.4. Performance test results of the insulating protective film of each embodiment

[0286] According to Tables 2.1 to 2.4, a brief analysis is as follows:

[0287] In Examples 2.1 to 2.3, the components of the adhesive meet the appropriate types and amounts. Compared with Example 2.22, the peel strength, shear strength and shear strength after aging of the insulating protective film are significantly improved.

[0288] In Examples 2.3 through 2.6, and 2.21, the acrylic resin content in the adhesive varied, while the mass ratios of the other components remained consistent. Compared to Example 2.3, Examples 2.4 and 2.21 contained lower amounts of acrylic resin, resulting in Example 2.3 exhibiting higher peel strength, shear strength, aged shear strength, and dielectric withstand voltage performance. Examples 2.5 and 2.6 contained higher amounts of acrylic resin, resulting in Example 2.3 exhibiting even higher dielectric withstand voltage performance.

[0289] In Examples 2.3 and 2.7 through 2.10, the active monomer content in the adhesive varied, while the mass ratios of the remaining components remained consistent. Compared to Example 2.3, Examples 2.7 and 2.8 contained lower amounts of active monomer, resulting in Example 2.3 exhibiting lower flange lift heights, higher peel strength, higher shear strength, and higher shear strength after aging. In Examples 2.9 and 2.10, the active monomer content was higher, resulting in Example 3 exhibiting lower flange lift heights. Furthermore, compared to Examples 2.3 and 2.7 through 2.10, Examples 2.3 and 2.8 through 2.9 all exhibited higher edge pressure resistance.

[0290] In Examples 2.3 and 2.11 to 2.14, the photoinitiator content in the adhesive varied, while the mass ratios of the other components remained consistent. Compared to Example 2.3, Examples 2.11 and 2.12 contained lower levels of photoinitiator, resulting in Example 2.3 exhibiting lower flange lift heights, higher peel strength, higher shear strength, higher shear strength after aging, and higher edge pressure resistance. Examples 2.13 and 2.14 contained higher levels of photoinitiator, resulting in Example 3 exhibiting lower flange lift heights. Furthermore, compared to Examples 2.3 and 2.11 to 2.14, Example 2.3 and Examples 2.12 to 2.13 all exhibited higher edge pressure resistance.

[0291] In Examples 2.3, 2.15, and 2.16, the coupling agent content in the adhesive varied, while the mass ratios of the other components remained consistent. Compared to Example 2.3, Examples 2.15 and 2.16 contained higher amounts of coupling agent, resulting in Example 2.3 exhibiting higher peel strength, higher shear strength, and higher aged shear strength. Furthermore, compared to Example 2.1, Examples 2.3 and 2.15 exhibited higher insulation pressure resistance.

[0292] In Examples 2.3, 2.17 and 2.19, the adhesives of Examples 2.17 and 2.19 use only one photoinitiator, and the peel strength, shear strength and shear strength after aging of the insulating protective film in Example 2.3 are higher.

[0293] In Examples 2.3, 2.18 and 2.20, the adhesives of Examples 2.18 and 2.20 do not contain a coupling agent, the insulating protective film in Example 2.3 has higher peel strength and insulation withstand voltage performance, and the flange warping height is lower.

[0294] Table 3.3 Properties of UV-curable inks in various examples

[0295] According to Tables 3.1 to 3.3, a brief analysis is as follows:

[0296] By comparing Examples 3.1 to 3.26 and Examples 3.27 to 3.29, it can be seen that the first monomer and the second monomer of Examples 3.1 to 3.26 are both active monomers with a viscosity of ≤10 cps at 50°C and meet the ratio relationship, and the viscosity of the obtained UV-curable ink at 50°C is ≤100 cps; the first monomer of Example 3.27 is an active monomer with a viscosity of >10 cps at 50°C (lauryl methacrylate, with a viscosity of 47 cps at 50°C), and the viscosity of the obtained UV-curable ink at 50°C is as high as 186 cps; the second monomer of Example 3.28 is an active monomer with a viscosity of >10 cps at 50°C (lauryl methacrylate, with a viscosity of 47 cps at 50°C). An active monomer with a viscosity of >10cps at 50°C (ethoxylated bisphenol A dimethacrylate, with a viscosity of 39cps at 50°C) is selected, and the viscosity of the obtained UV-curable ink at 50°C is as high as 153cps; in Example 3.29, the first monomer is an active monomer with a viscosity of >10cps at 50°C (lauryl methacrylate, with a viscosity of 47cps at 50°C), and the second monomer is an active monomer with a viscosity of >10cps at 50°C (ethoxylated bisphenol A dimethacrylate, with a viscosity of 39cps at 50°C), and the viscosity of the obtained UV-curable ink at 50°C is as high as 357cps.

[0297] From the comparison between Example 3.1 and Example 3.23, it can be seen that Example 3.23 does not have the second monomer. Compared with Example 3.1, Example 3.1 has better insulation withstand voltage and higher shear strength.

[0298] From the comparison between Example 3.1 and Example 3.24, it can be seen that Example 3.24 does not have the first monomer. Compared with Example 3.1, Example 1 has better flexibility.

[0299] From the comparison between Example 3.1 and Example 3.25, it can be seen that Example 3.25 does not have a hydrophobic monomer. Compared with Example 3.1, Example 3.1 has better adhesion when immersed in water at 85°C and better insulation withstand voltage when immersed in water at 85°C.

[0300] From the comparison between Example 3.1 and Example 3.26, it can be seen that Example 3.26 does not contain a coupling agent. Compared with Example 3.1, Example 3.1 has better adhesion when immersed in water at 85°C and better insulation withstand voltage when immersed in water at 85°C.

[0301] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A battery housing, wherein: It comprises a shell side wall and a shell end wall connected to each other, wherein the connection between the shell side wall and the shell end wall has a connecting weld, and the connecting weld is located on the end surface of the battery shell; Among them, it also includes an insulating protective film and an insulating coating. The outer side of the shell side wall is connected to the insulating protective film, and the outer side of the connecting weld is covered with the insulating coating.

2. The battery casing according to claim 1, wherein: An edge region of the insulating protection film is connected to the insulating coating layer.

3. The battery casing according to claim 1, wherein: The surface area of ​​the outer side of the shell side wall is S1, and the surface area of ​​the region on the outer side of the shell side wall corresponding to the insulating protection film is S2, S2 = S1 × (80% to 95%).

4. The battery case according to any one of claims 1 to 3, wherein Along the circumferential direction of the shell side wall, the ratio of the overlapping dimensions of the two ends of the insulating protection film to the outer circumference of the shell side wall is (3-10): (145-750).

5. The battery case according to any one of claims 1 to 4, wherein The insulating coating comprises a first coating portion and a second coating portion which are connected to each other, wherein the first coating portion is located at the end face of the battery shell, and at least a portion of the first coating portion covers the outside of the connecting weld, and the second coating portion is located at the outside of the shell side wall and connected to the edge area of ​​the insulating protective film.

6. The battery case according to claim 5, wherein: The second portion of the coating covers the outer end portion of the shell side wall, and at least a portion of the second portion of the coating is covered by the insulating protection film.

7. The battery case according to claim 5, wherein: At least a portion of the second portion of the coating covers the outer side of the edge region of the insulating protection film.

8. The battery case according to any one of claims 1 to 4, wherein An end surface of an edge region of the insulating protection film is connected to the insulating coating layer.

9. The battery case according to any one of claims 1 to 8, wherein The outer side of the shell end wall and the outer side of the connecting weld are both covered by the insulating coating.

10. The battery case according to any one of claims 1 to 8, wherein The insulating coating is ring-shaped.

11. The battery case according to any one of claims 5 to 7, wherein: The surface area of ​​the outer side of the shell side wall is S1, and the surface area of ​​the region on the outer side of the shell side wall corresponding to the second portion of the coating is S3, S3 = S1 x (5% to 20%).

12. The battery case according to any one of claims 5 to 7 and 11, wherein Along the height direction of the shell side wall, the size of the shell side wall is H1, and the overlapping size of the second portion of the coating and the insulating protection film is H2, H2 = H1 × (2% to 10%).

13. The battery case according to any one of claims 1 to 12, wherein: The thickness of the insulating protection film is 50 μm to 120 μm.

14. The battery case according to any one of claims 1 to 13, wherein: The thickness of the insulating coating is 50 μm to 120 μm.

15. The battery case according to any one of claims 1 to 14, wherein The insulating protective film includes at least one connecting layer and at least one base film layer, the insulating protective film is connected to the outer side of the shell side wall through the connecting layer, and the surface layer of the insulating protective film away from the shell side wall is the base film layer; The connection layer is formed by photocuring an adhesive layer including an adhesive, wherein the adhesive includes 60wt% to 95wt% of acrylic resin, 3wt% to 35wt% of active monomers and 0.8wt% to 10wt% of photoinitiator.

16. The battery casing according to claim 15, wherein: The photoinitiator includes one or more of ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 1-hydroxycyclohexylphenyl ketone, 2-isopropylthioxanthone, 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone and 2-hydroxy-2-methyl-1-phenylacetone.

17. The battery casing according to claim 15 or 16, wherein: The total thickness of the base film layer is T1, and the total thickness of the adhesive layer is T2; Wherein, T2 = T1 × (50% to 150%); Optionally, T2=T1×(80% to 120%).

18. The battery case according to any one of claims 1 to 17, wherein The insulating coating comprises a photocured product of an ultraviolet light curing ink; The UV curable ink comprises 10wt% to 30wt% acrylic resin, 40wt% to 80wt% active monomer, 2wt% to 10wt% photoinitiator, ≤15wt% hydrophobic monomer, ≤5wt% coupling agent and ≤10wt% pigment; the viscosity of the active monomer at 50°C is ≤10cps.

19. The battery casing according to claim 18, wherein: The active monomer includes a first monomer, and the first monomer is a monofunctional monomer.

20. The battery casing according to claim 19, wherein: The active monomer further includes a second monomer, the functionality of the second monomer is ≥2, and the mass of the second monomer is 30% to 50% of the mass of the first monomer.

21. The battery case according to any one of claims 18 to 20, wherein The ultraviolet curable ink comprises 0.1wt% to 15wt% of a hydrophobic monomer, and the contact angle between the hydrophobic monomer and water is ≥90°.

22. A battery cell, wherein: The invention comprises the battery casing according to any one of claims 1 to 21.

23. A battery, wherein: Comprising the battery cell as claimed in claim 22.

24. An electrical device, wherein: It comprises the battery housing as claimed in claim 22 or the battery cell as claimed in claim 23.

Citation Information

Patent Citations

  • Shell, secondary battery, battery pack, vehicle and manufacturing method of secondary battery

    CN112331963A

  • Insulation shell structure and adopt lithium ion power batteries of this insulation shell structure

    CN204927359U

  • Battery box body, battery pack and power utilization device

    CN217768703U

  • Battery monomer, battery and electric device

    CN217823188U

  • Battery and battery shell thereof

    CN218385436U