Gas-barrier nylon composite material, and preparation method therefor and use thereof

By using a combination of polyol and cyclodextrin and an impact modifier in the high-pressure hydrogen storage tank lining material, the problems of melt collapse and reduced barrier properties during the molding process are solved, and wall thickness uniformity and gas resistance are achieved. The barrier properties are improved and the heat aging resistance of the storage tank is enhanced.

WO2024222713A1PCT designated stage expired Publication Date: 2024-10-31DONGHUA UNIV +1

Patent Information

Application Number
PCT/CN2024/089450
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing high-pressure hydrogen storage tank lining materials are prone to melt collapse or cracking during the molding process, and the addition of impact modifiers will reduce gas barrier properties and accelerate material aging, making the storage tank prone to cracking.

Method used

A gas barrier nylon composite material combining polyhydroxy compounds with cyclodextrin or its derivatives is prepared through a twin-screw extruder to form a quasi-crosslinked structure to improve elasticity and barrier properties, and is combined with an impact modifier to improve toughness and Heat aging resistance.

Benefits of technology

The wall thickness uniformity, gas barrier properties and heat aging resistance of the high-pressure hydrogen storage tank lining material are achieved, melt rupture and barrier property decline are avoided, and the stability and performance of the storage tank are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024089450-FTAPPB-I100001
    Figure PCTCN2024089450-FTAPPB-I100001
  • Figure PCTCN2024089450-FTAPPB-I100002
    Figure PCTCN2024089450-FTAPPB-I100002
  • Figure PCTCN2024089450-FTAPPB-I100003
    Figure PCTCN2024089450-FTAPPB-I100003
Patent Text Reader

Abstract

Disclosed in the present invention is a gas-barrier nylon composite material, comprising the following components in parts by weight: 60 parts of PA6; 0-30 parts of an impact modifier; 2.5-20 parts of a polyhydroxy compound; and 2.5-6 parts of cyclodextrin or a derivative thereof. In the present invention, by means of compounding of a polyhydroxy compound and cyclodextrin or a derivative thereof, degradation in hydrogen-barrier property caused by addition of an impact modifier can be mitigated. Thus, the gas-barrier nylon composite material of the present invention has the advantages of a good hydrogen-barrier property and good high-temperature aging resistance, and a finished piece having a uniform wall thickness can be obtained by means of a blow molding process.
Need to check novelty before this filing date? Find Prior Art

Description

A gas barrier nylon composite material and its preparation method and application Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a gas barrier nylon composite material and a preparation method and application thereof. Background Art

[0002] In recent years, the world has been actively researching and rapidly developing fuel cell vehicles (FCVs) to address energy crises and climate change caused by greenhouse gases. These vehicles utilize fuel cells that generate electricity through an electrochemical reaction between hydrogen and oxygen in the air, providing continuous power to the engine. Although hydrogen produces significantly more energy per unit mass than gasoline, and the reaction product is water, hydrogen is a gas at room temperature with a low energy density. Therefore, pressurization is required to increase its energy density and extend the range of fuel cell vehicles. Therefore, the availability of high-pressure hydrogen storage tanks determines the practicality of FCVs.

[0003] The number of tanks and the pressure in a fuel cell vehicle determine the amount of gas carried. To achieve high-pressure gas storage and reduce tank weight, high-pressure hydrogen tank technology is undergoing continuous innovation. Because hydrogen has smaller molecules than air, methane, and other gases, it more easily penetrates resin. High-pressure hydrogen also creates greater strain on the lining material, and repeated filling and degassing can easily cause material fatigue and cracking. Polycaprolactam (PA6), with its high crystallinity, effectively inhibits hydrogen permeation.

[0004] In the existing technology, the lining materials of high-pressure hydrogen storage tanks have the following difficulties:

[0005] First, the molding methods for producing high-pressure hydrogen storage tank lining materials using polymer compositions include injection molding, rotational molding, and extrusion blow molding. Blow molding is often used to mold large, hollow parts. However, melt collapse or fracture during blow molding can lead to molding failure. Therefore, hydrogen storage tank linings must have uniform wall thickness and be free of cracks.

[0006] Second, existing hydrogen storage tank linings utilize impact modifiers to improve toughness. However, during the charging and degassing process, or during the operation of a fuel vehicle, the system heat causes aging. In particular, the elastomer in the impact modifier typically ages before the polyamide substrate, resulting in a decrease in toughness. This factor accelerates cracking at weak points during repeated charging and degassing. Therefore, improving the heat aging resistance of high-pressure hydrogen storage tank lining materials is a key parameter. Furthermore, the addition of impact modifiers can disrupt the gas barrier structure, thereby reducing the gas barrier properties of PA6. Therefore, improving this reduction in gas barrier properties caused by the addition of impact modifiers is a key industry concern.

[0007] Summary of the Invention

[0008] The purpose of the present invention is to overcome the above technical defects and provide a gas barrier nylon composite material suitable for the lining of high-pressure gas storage tanks, which has the advantages of being suitable for blow molding, having good heat aging resistance and good hydrogen barrier properties.

[0009] The present invention is achieved through the following technical solutions:

[0010] A gas barrier nylon composite material, comprising the following components in parts by weight:

[0011] Preferably, the weight ratio of the polyol to cyclodextrin or its derivative is (3-4): 1. Under the preferred ratio, the gas barrier property is better.

[0012] Optionally, the relative viscosity of the PA6 is 2.7 to 4.5. The relative viscosity is measured according to ISO 307 by dissolving PA6 in 98% concentrated sulfuric acid using an Ubbelohde viscometer.

[0013] Optionally, the cyclodextrin or its derivative is selected from at least one of β-cyclodextrin, γ-cyclodextrin, hydroxypropyl-β-cyclodextrin, sulfobutyl ether-β-cyclodextrin, disaccharide-β-cyclodextrin, methyl-β-cyclodextrin or hydroxyethyl-β-cyclodextrin.

[0014] The polyol is selected from at least one of a polyol containing two hydroxyl functional groups, a polyol containing three hydroxyl functional groups, a polyol containing at least four hydroxyl functional groups, and a polyol polymer containing at least four hydroxyl functional groups;

[0015] Preferably, the polyol is selected from polyol polymers containing at least four hydroxyl functional groups.

[0016] Optionally, the polyhydroxy compound containing two hydroxyl functional groups is at least one selected from 1,2-ethylene glycol, 1,3-propylene glycol, 2,3-butylene glycol, 1,5-pentanediol, 2,2-dimethyl-1,3-propylene glycol, and polyether glycols;

[0017] The polyol containing three hydroxyl groups is selected from glycerol, trimethylolpropane, 2,3-bis(2′-hydroxyethyl)cyclohexane-1-ol, 1,2,6-hexanetriol, 1,1,1-tris-(hydroxymethyl)ethane, 3-(2′-hydroxyethoxy)propane-1,2-diol, 3-(2′-hydroxypropoxy)propane-1,2-diol, 2-(2′-hydroxyethoxy)hexane-1,2-diol, 6-(2′-hydroxypropoxy)hexane-1,2-diol, 1,1,1-tris[(2′-hydroxyethoxy) at least one of: 1,1,1-tris[(2′-hydroxypropoxy)methyl]propane, 1,1,1-tris(4′-hydroxyphenyl)ethane, 1,1,1-tris(hydroxyphenyl)propane, 1,1,3-tris(dihydroxy-3-methylphenyl)propane, 1,1,4-tris(dihydroxyphenyl)butane, 1,1,5-tris(hydroxyphenyl)-3-methylpentane, di(trimethylolpropane), trimethylolpropane ethoxylates, trimethylolpropane propoxylates, and trihydroxy polyether compounds;

[0018] The polyol containing at least four hydroxyl functional groups is selected from at least one of 1,1,3,3-tetrakis(methoxy)propane, pentaerythritol, dipentaerythritol, and tripentaerythritol;

[0019] The polyhydroxy polymer containing at least four hydroxyl functional groups is at least one selected from polyvinyl alcohol, ethylene vinyl alcohol copolymer, and dendritic hyperbranched polyester.

[0020] Optionally, the impact modifier is selected from at least one of maleic anhydride grafted ethylene-octene copolymer, polyethylene, polypropylene, polybutene, polyisoprene, ethylene-propylene rubber, ethylene-propylene-butadiene rubber, maleic anhydride grafted linear low density polyethylene, ethylene-butene rubber, ethylene-acrylate rubber, butadiene-styrene rubber, butadiene-acrylate rubber, ethylene-octene rubber, butadiene acrylonitrile rubber, ethylene-acrylic acid polymer, ethylene-vinyl acetate polymer, ethylene-acrylate polymer, maleic anhydride grafted ethylene-butene copolymer, acrylonitrile-butadiene-styrene copolymer, styrene-ethylene-butadiene-styrene block copolymer, ethylene-n-butyl acrylate-glycidyl methacrylate, styrene-butadiene-styrene copolymer, and methacrylate-butadiene-styrene type core / shell elastomers.

[0021] It is also possible to decide whether to add 0-5 parts of an auxiliary agent according to actual needs. The auxiliary agent is selected from at least one of an antioxidant, a lubricant, and a weathering agent.

[0022] The antioxidant may be a hindered phenol antioxidant (such as Irganox 1098) or a phosphite antioxidant (such as PEP-36).

[0023] The lubricant may be an ester lubricant or the like.

[0024] The weathering agent may be an anti-ultraviolet agent or the like.

[0025] The preparation method of the gas barrier nylon composite material of the present invention comprises the following steps: uniformly mixing the components according to the proportion, extruding and granulating the components through a twin-screw extruder, with the screw temperature ranging from 210 to 250° C. and the rotation speed ranging from 200 to 500 rpm, to obtain the gas barrier nylon composite material.

[0026] The gas barrier nylon composite material of the present invention is used for lining of high-pressure gas storage tanks.

[0027] The present invention has the following beneficial effects

[0028] The polyhydroxy structure on the outer edge of the cyclodextrin molecular structure is combined with PA6 through hydrogen bonding. The multi-functional groups provided together with the polyhydroxy compounds provide intermolecular hydrogen bonding force with the PA6 polymer chain, forming a quasi-cross-linked structure, which is beneficial to improving the elastic storage modulus of the melt, especially under low-frequency shear or stretching. It corresponds to the ability to resist tensile deformation of the melt during extrusion and blow molding, is not prone to melt fracture during blow molding, and a product with uniform wall thickness is obtained.

[0029] Cyclodextrins possess a unique ring structure, forming a hydrophilic outer edge and a hydrophobic inner cavity. This allows them to capture hydrogen molecules attempting to penetrate the material through van der Waals interactions within the hydrophobic cavity. Furthermore, the dense structure formed by the polyol also helps to block the passage of gas molecules. Dispersed around the impact modifier, it can mitigate the decrease in hydrogen barrier properties caused by the addition of the impact modifier. This barrier property, while effective against low-molecular-weight hydrogen molecules, also provides the same effectiveness against larger oxygen molecules, thus preventing, to a certain extent, the toughness loss caused by high-temperature aging of the internal impact modifier. DETAILED DESCRIPTION

[0030] The present invention will be described in detail below with reference to specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those skilled in the art, several variations and improvements can be made without departing from the scope of the present invention. These all fall within the scope of protection of the present invention.

[0031] The raw materials used in the examples of the present invention and the comparative examples are as follows:

[0032] PA6: Ultramid B40L, relative viscosity 3.8, BASF;

[0033] Impact modifier A: maleic anhydride grafted ethylene-octene copolymer (mPOE), purchased from DuPont, brand Fusabond N493;

[0034] Impact modifier B: maleic anhydride grafted linear low-density polyethylene (mLLDPE), purchased from UBE, brand name UBE BOND F3000;

[0035] Impact modifier C: maleic anhydride grafted ethylene butene copolymer (mEBA), purchased from Mitsui Chemicals, TAFMER MH5020;

[0036] Impact modifier D: ethylene-n-butyl acrylate-glycidyl methacrylate (E-nBA-GMA), purchased from DuPont with the brand name Elvaloy PTW.

[0037] 1,5-Pentanediol: Sigma-Aldrich;

[0038] Glycerol: Sigma-Aldrich;

[0039] Pentaerythritol: Charmor PM40, purchased from Perstorp.

[0040] Polyvinyl alcohol A: purchased from Kuraray;

[0041] Polyvinyl alcohol B: purchased from Shanghai Yingjia.

[0042] Ethylene vinyl alcohol copolymer: purchased from Changchun Group.

[0043] β-cyclodextrin: Sigma-Aldrich;

[0044] γ-Cyclodextrin: Sigma-Aldrich.

[0045] Preparation method of gas barrier nylon composite material of embodiment and comparative example: According to the ratio, each component is mixed uniformly, and granulated by extrusion through a twin-screw extruder, with the screw temperature range of 210-250°C and the speed range of 300-400rpm to obtain PA6 composite material.

[0046] Various test methods:

[0047] (1) Gas barrier properties: The granulated sample is injection molded into a 100×100×1mm sample, adapted to the gas permeability test cavity to be taken as a disc, and the sample is installed between two cavities to form a sealed system. The gas exchange between the two cavities is only allowed to be achieved through the sample, one cavity is the target high-pressure gas (hydrogen) generation end, and the other cavity is the target gas permeation collection end. The amount of gas passing through the sample per unit area per unit time is recorded as the gas permeability, unit cm 3 / (m 2 *day). In this system, gas permeability is a characteristic of the sample itself. The material permeability needs to take into account the sample thickness and the partial pressure of the target gas. That is, permeability coefficient = gas permeability × sample thickness / target gas partial pressure, unit is cm 3 cm / (cm 2 ·s·cmHg). The specific test conditions are relative humidity of 0%, test temperature of 23°C, helium partial pressure of 0.5MPa, and sample thickness of 1mm. The gas barrier properties are classified as follows:

[0048] Permeability ≤2.5×10 -11 , level 1;

[0049] 2.5×10 -11 <Permeability<5.0×10 -11 , level 2;

[0050] 5.0×10 -11 <Permeability≤2.5×10 -10 , level 3;

[0051] 2.5×10 -10 <Permeability, level 4;

[0052] (Permeability unit: cm 3 cm / (cm 2 ·s·cmHg)).

[0053] (2) Heat aging resistance: Unnotched impact strength was tested according to ISO 179, and the initial unnotched impact strength was measured. The aging temperature was 150°C, and the aging cycle was 1000 hours. The unnotched impact strength after aging was measured. Retention rate = unnotched impact strength after aging / initial unnotched impact strength * 100%.

[0054] (3) Wall thickness uniformity: The evaluation was conducted using the HAAKE PolyLab OS multifunctional torque rheometer with an annular extrusion die; the extrusion temperature was 250-280°C, the rotation speed was 250 rpm, and after extruding a sample of about 8-10 cm, the bottom of the extruded sample was clamped with tweezers. The high-pressure gas valve connected to the core layer pipe of the annular die was opened, nitrogen was filled in, and the gas valve pressure was adjusted to control the gas flow rate at 0.15 m / s. 3 / min, and after inflating for 5 seconds, close the valve. Wait for the inflated extrudate to cool to room temperature, then remove the blow-molded sample from the extrusion die. To measure wall thickness, cut the blow-molded sample in the middle perpendicular to the extrusion direction. Measure each point on the cross-section, divided equally into eight parts, and calculate the relative deviation (in %). Based on the relative deviation, the sample is rated as follows:

[0055] Relative deviation ≤5%, level 1;

[0056] 5%<relative deviation≤10%, Level 2;

[0057] 10%<relative deviation≤20%, level 3;

[0058] 20%<relative deviation≤30%, Level 4;

[0059] Relative deviation>30%, level 5.

[0060] Table 1: Content (parts by weight) of each component of gas barrier nylon composite materials of Examples 1-7 and test results

[0061] In Example 1-4, the gas barrier property and wall thickness uniformity as well as the heat aging resistance can be significantly improved by compounding 1,5-pentanediol / β-cyclodextrin.

[0062] Table 2: Content (parts by weight) of each component of gas barrier nylon composite materials of Examples 8-15 and test results

[0063] As can be seen from Examples 8-12, the preferred content of the polyol is 12-17 parts.

[0064] It can be seen from Examples 10 / 13-15 that the preferred weight ratio of the polyhydroxy compound to the cyclodextrin or its derivative is (3-4):1.

[0065] Table 3: Content (parts by weight) of each component of gas barrier nylon composite materials of Examples 16-20 and test results

[0066] As can be seen from Examples 9 / 16-19, polyhydroxy polymers containing at least four hydroxyl functional groups are preferred, as they have higher gas barrier properties and thus stronger resistance to heat and oxidation.

[0067] Table 4: Comparative Example Gas Barrier Nylon Composite Material Component Content (Parts by Weight) and Test Results

[0068] Comparative Examples 1-5 show that the content of polyol / cyclodextrin is outside the scope of the present invention, and it is impossible to ensure that the hydrogen barrier properties, thermal oxygen aging resistance, and uniformity of the wall thickness of the blow-molded parts meet the requirements.

[0069] It can be seen from Comparative Examples 6 / 7 that an increase in the impact modifier content will destroy the gas barrier structure of the nylon composite material and the uniformity of the wall thickness, and will also lead to a decrease in the retention rate of the unnotched impact strength.

Claims

1. A gas barrier nylon composite material, characterized in that: By weight, it includes the following components:

2. The gas barrier nylon composite material according to claim 1, characterized in that: The content of the polyhydroxy compound is 12-17 parts; the weight ratio of the polyhydroxy compound to cyclodextrin or its derivative is (3-4):

1.

3. The gas barrier nylon composite material according to claim 1, characterized in that: The relative viscosity of the PA6 is 2.7-4.

5.

4. The gas barrier nylon composite material according to claim 1, characterized in that: The cyclodextrin or its derivative is selected from at least one of β-cyclodextrin, γ-cyclodextrin, hydroxypropyl-β-cyclodextrin, sulfobutyl ether-β-cyclodextrin, disaccharide-β-cyclodextrin, methyl-β-cyclodextrin or hydroxyethyl-β-cyclodextrin.

5. The gas barrier nylon composite material according to claim 1, characterized in that: The polyhydroxy compound is selected from at least one of a polyhydroxy compound containing two hydroxyl functional groups, a polyhydroxy compound containing three hydroxyl functional groups, a polyhydroxy compound containing at least four hydroxyl functional groups, and a polyhydroxy polymer containing at least four hydroxyl functional groups; preferably, the polyhydroxy compound is selected from a polyhydroxy polymer containing at least four hydroxyl functional groups.

6. The gas barrier nylon composite material according to claim 5, characterized in that: The polyhydroxy compound containing two hydroxyl functional groups is selected from at least one of 1,2-ethylene glycol, 1,3-propylene glycol, 2,3-butylene glycol, 1,5-pentanediol, 2,2-dimethyl-1,3-propylene glycol, and polyether glycols; the polyhydroxy compound containing three hydroxyl functional groups is selected from glycerol, trimethylolpropane, 2,3-di(2′-hydroxyethyl)cyclohexane-1-ol, 1,2,6-hexanetriol, 1,1,1-tri-(hydroxymethyl)ethane, 3-(2′-hydroxyethoxy)propane-1,2-diol, 3-(2′-hydroxypropoxy)propane-1,2-diol, 2-(2′-hydroxyethoxy)hexane-1,2-diol, 6-(2′-hydroxypropoxy)hexane-1,2-diol, 1,1,1-tri[(2′-hydroxyethoxy)methyl]ethane, 1,1,1-tri[ At least one of [(2′-hydroxypropoxy)methyl] propane, 1,1,1-tri(4′-hydroxyphenyl)ethane, 1,1,1-tri(hydroxyphenyl)propane, 1,1,3-tri(dihydroxy-3-methylphenyl)propane, 1,1,4-tri(dihydroxyphenyl)butane, 1,1,5-tri(hydroxyphenyl)-3-methylpentane, di(trimethylolpropane), trimethylolpropane ethoxylates, trimethylolpropane propoxylates, and trihydroxy polyether compounds; the polyhydroxy compound containing at least four hydroxyl functional groups is selected from at least one of 1,1,3,3-tetra(methoxy)propane, pentaerythritol, dipentaerythritol, and tripentaerythritol; the polyhydroxy polymer containing at least four hydroxyl functional groups is selected from at least one of polyvinyl alcohol, ethylene vinyl alcohol copolymer, and dendritic hyperbranched polyester.

7. The gas barrier nylon composite material according to claim 1, characterized in that: The impact modifier is selected from at least one of maleic anhydride grafted ethylene-octene copolymer, polyethylene, polypropylene, polybutene, polyisoprene, ethylene-propylene rubber, ethylene-propylene-butadiene rubber, maleic anhydride grafted linear low density polyethylene, ethylene-butene rubber, ethylene-acrylate rubber, butadiene-styrene rubber, butadiene-acrylate rubber, ethylene-octene rubber, butadiene acrylonitrile rubber, ethylene-acrylic acid polymer, ethylene-vinyl acetate polymer, ethylene-acrylate polymer, maleic anhydride grafted ethylene butene copolymer, acrylonitrile-butadiene-styrene copolymer, styrene-ethylene-butadiene-styrene block copolymer, ethylene-butyl acrylate-glycidyl methacrylate, styrene-butadiene-styrene copolymer, and methacrylate-butadiene-styrene type core / shell elastomer.

8. The gas barrier nylon composite material according to claim 1, characterized in that: By weight, the invention also includes 0-5 parts of auxiliary agents, wherein the auxiliary agents are selected from at least one of antioxidants, lubricants and weathering agents.

9. The method for preparing the gas barrier nylon composite material according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: mixing the components uniformly according to the proportion, extruding and granulating the components through a twin-screw extruder, wherein the screw temperature range is 210-250° C. and the rotation speed range is 200-500 rpm, so as to obtain a gas barrier nylon composite material.

10. Use of the gas barrier nylon composite material according to any one of claims 1 to 8, characterized in that: Used for lining of high pressure gas storage tanks.

Citation Information

Patent Citations

  • Polyamide resin composition for hydrogen gas storage containers or hydrogen gas preparation pipes

    CN110511560A

  • Gas barrier nylon composite material as well as preparation method and application thereof

    CN116987380A

  • Method for storing hydrogen, hydrogen clathrate compound and production method thereof

    US20040230084A1

  • Barrier material comprising a thermoplastic and a compatible cyclodextrin derivative

    US5492947A

Cited By

  • Preparation method and application of acrylate PVC impact modifier

    CN120192463A