Solar cell and preparation method therefor, photovoltaic module, and electric device

By arranging a boron-hydrogen doped layer and a boron-doped polysilicon layer on the N-type silicon substrate of the solar cell to replace the aluminum oxide passivation layer, the problem of poor passivation effect caused by burn-through is solved, and the electrical performance and photovoltaic performance are improved. conversion efficiency.

WO2024222721A1PCT designated stage expired Publication Date: 2024-10-31TONGWEI SOLAR ENERGY (MEISHAN) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/089488
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing solar cells need to burn through the aluminum oxide passivation layer during the passivation process, resulting in poor passivation effect and limited electrical performance, which affects photoelectric conversion efficiency.

Method used

A boron-hydrogen doped layer, a first tunnel oxide layer and a boron-doped polysilicon layer are sequentially placed on an N-type silicon substrate. Through the joint action of these film layers, the aluminum oxide layer is replaced to achieve better passivation effect and conductivity. , to avoid the burn-through process, the electrode can achieve current conduction by contacting the boron-doped polysilicon layer.

Benefits of technology

It improves the electrical performance and photoelectric conversion efficiency of solar cells, takes into account chemical passivation and field passivation, reduces carrier recombination, and enhances the passivation effect without destroying the passivation structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024089488_31102024_PF_FP_ABST
    Figure CN2024089488_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of photovoltaic power generation, and in particular to a solar cell and a preparation method therefor, a photovoltaic module, and an electric device. The solar cell (100) comprises: an N-type silicon substrate (6), wherein the N-type silicon substrate (6) has a first surface and a second surface that are arranged opposite to each other, and the first surface is a light-incident surface; a boron-hydrogen doped layer (5), a first tunneling oxide layer (4), a boron-doped polycrystalline silicon layer (3) and a first anti-reflection layer (2) that are sequentially stacked on the first surface of the N-type silicon substrate (6); a second tunneling oxide layer (7), a phosphorus-doped polycrystalline silicon layer (8) and a second anti-reflection layer (9) that are sequentially stacked on the second surface of the N-type silicon substrate (6); first electrodes (1) that pass through the first anti-reflection layer (2) and are then in ohmic contact with the boron-doped polycrystalline silicon layer (3); and second electrodes (10) in ohmic contact with the second tunneling oxide layer (7). The solar cell not only can improve the passivation effect, but also facilitates improvement of the electrical performance and the photoelectric conversion efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Solar cell and preparation method thereof, photovoltaic module, and electrical equipment

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 26, 2023, with application number 2023104617565 and invention name “A solar cell and its preparation method, photovoltaic module, and electrical equipment”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present invention relates to the technical field of photovoltaic power generation, and in particular to a solar cell and a preparation method thereof, a photovoltaic module, and electrical equipment. Background Art

[0003] Existing solar cells require passivation on the front to reduce surface recombination and thus improve the photoelectric conversion efficiency. The existing passivation process usually forms an aluminum oxide passivation layer on the front of the substrate. Since aluminum oxide is not conductive, the front electrons cannot be directly transmitted through the aluminum oxide layer. Instead, a high-temperature sintering process is required to burn through the aluminum oxide passivation layer and all the film layers above it to achieve contact between the metal electrode and the substrate, thereby achieving current conduction. However, this method of burning through the aluminum oxide passivation layer not only affects the passivation effect of the aluminum oxide passivation layer burn-through position and the surrounding area, but is also not conducive to improving the electrical performance of the solar cell and affects the photoelectric conversion efficiency.

[0004] Summary of the Invention

[0005] An embodiment of the present invention discloses a solar cell, which can improve the passivation effect, electrical performance and photoelectric conversion efficiency without burning through the passivation structure.

[0006] To achieve the above-mentioned object, the present invention discloses a solar cell, comprising: an N-type silicon substrate having a first surface and a second surface disposed opposite to each other, the first surface being a light incident surface; a boron-hydrogen doped layer, a first tunneling oxide layer, a boron-doped polysilicon layer, and a first anti-reflection layer sequentially stacked on the first surface of the N-type silicon substrate;

[0007] A second tunneling oxide layer, a phosphorus-doped polysilicon layer, and a second anti-reflection layer are sequentially stacked on the second surface of the N-type silicon substrate;

[0008] a first electrode, penetrating the first anti-reflection layer and making ohmic contact with the boron-doped polysilicon layer;

[0009] The second electrode is in ohmic contact with the second tunneling oxide layer.

[0010] As an optional implementation, in an embodiment of the present invention, the boron-doped polysilicon layer is doped with hydrogen, and / or the phosphorus-doped polysilicon layer is doped with hydrogen.

[0011] As an optional implementation, in an embodiment of the present invention, the first tunneling oxide layer is a silicon oxide layer; and / or,

[0012] The second tunneling oxide layer is a silicon oxide layer; and / or,

[0013] The first anti-reflection layer is a silicon nitride layer; and / or,

[0014] The second anti-reflection layer is a silicon nitride layer.

[0015] As an optional implementation manner, in an embodiment of the present invention, the thickness of the first tunneling oxide layer is 1 nm to 2 nm; and / or,

[0016] The thickness of the boron-doped polysilicon layer is 1 nm to 30 nm.

[0017] As an optional implementation, in an embodiment of the present invention, the junction depth of the boron hydride doped layer is 0.8 μm to 1.5 μm; and / or,

[0018] The sheet resistance of the boron hydride doped layer is 105Ω / sq to 145Ω / sq; and / or,

[0019] The concentration of boron in the boron-hydrogen doped layer is 1×10 19 N / cm 2 ~2×10 19 N / cm 2 .

[0020] In a second aspect, the present application provides a method for preparing the back-contact solar cell according to the first aspect, the method comprising the following steps:

[0021] Providing the N-type silicon substrate that has been textured;

[0022] forming the boron hydride doped layer on the first surface;

[0023] Cleaning to remove the wraparound of the second surface;

[0024] forming the second tunneling oxide layer on the second surface;

[0025] forming a phosphorus-doped amorphous silicon layer on a surface of the second tunnel oxide layer away from the N-type silicon substrate;

[0026] forming a first tunneling oxide layer on a surface of the boron hydride doped layer away from the N-type silicon substrate;

[0027] forming a boron-doped amorphous silicon layer on a surface of the first tunnel oxide layer away from the N-type silicon substrate;

[0028] Annealing to convert the boron-doped amorphous silicon layer and the phosphorus-doped amorphous silicon layer into the boron-doped polysilicon layer and the phosphorus-doped polysilicon layer;

[0029] forming the first anti-reflection layer on the surface of the boron-doped polysilicon layer away from the N-type silicon substrate, and forming the second anti-reflection layer on the surface of the phosphorus-doped polysilicon layer away from the N-type silicon substrate;

[0030] Post-processing allows the first electrode to penetrate the first anti-reflection layer and make ohmic contact with the boron-doped polysilicon layer, and allows the second electrode to penetrate the second anti-reflection layer and the phosphorus-doped polysilicon layer and make ohmic contact with the second tunneling oxide layer.

[0031] As an optional embodiment, in an embodiment of the present invention, in the step of forming the second tunneling oxide layer on the second surface, nitrous oxide and nitrogen are introduced to deposit the second tunneling oxide layer, wherein the nitrogen flow rate is 30,000 sccm to 70,000 sccm, the nitrous oxide flow rate is 8,000 sccm to 9,000 sccm, the deposition temperature is 550°C to 650°C, the deposition pressure is 2,500 mTorr to 3,000 mTorr, and the deposition time is 3 min to 4 min.

[0032] As an optional embodiment, in an embodiment of the present invention, in the step of forming the first tunneling oxide layer on the surface of the boron hydride doped layer away from the N-type silicon substrate, nitrous oxide and nitrogen are introduced to deposit the first tunneling oxide layer, wherein the nitrogen flow rate is 30,000 sccm to 70,000 sccm, the nitrous oxide flow rate is 8,000 sccm to 9,000 sccm, the deposition temperature is 550°C to 650°C, the deposition pressure is 2,500 mTorr to 3,000 mTorr, and the deposition time is 3 min to 4 min.

[0033] As an optional implementation, in an embodiment of the present invention, the solar cell is prepared by chemical vapor deposition;

[0034] Wherein, in the step of forming the boron hydride doped layer on the first surface, the boron hydride compound is ionized to

[0035] forming the boron hydride doped layer on the first surface; and / or,

[0036] In the step of forming a boron-doped amorphous silicon layer on a surface of the first tunneling oxide layer facing away from the N-type silicon substrate, ionizing a silicon hydride compound and a boron hydride compound to form a boron-doped amorphous silicon layer on a surface of the first tunneling oxide layer facing away from the N-type silicon substrate; and / or

[0037] In the step of forming a phosphorus-doped amorphous silicon layer on a surface of the second tunnel oxide layer facing away from the N-type silicon substrate, silicon hydride and phosphorus hydride are ionized to form a phosphorus-doped amorphous silicon layer on a surface of the second tunnel oxide layer facing away from the N-type silicon substrate.

[0038] As an optional embodiment, in an embodiment of the present invention, in the step of ionizing the boron hydride compound to form the boron hydride doped layer on the first surface, the flow rate of the boron hydride compound is 700sccm~800sccm, the nitrogen flow rate is 10000sccm~15000sccm, the RF power is 7000W~7500W, the pressure is 2500mTorr~3000mTorr, the temperature is 800℃~850℃, and the ionization time is 14min~16min.

[0039] As an optional embodiment, in an embodiment of the present invention, in the step of ionizing the silicon hydride and the phosphorus hydride to form a phosphorus-doped amorphous silicon layer on the surface of the second tunneling oxide layer away from the N-type silicon substrate, the flow rate of the silicon hydride is 2000sccm~3000sccm, the flow rate of the phosphorus hydride is 700sccm~800sccm, the flow rate of the nitrogen is 8000sccm~10000sccm, the RF power is 7000W~7500W, the pressure is 2500mTorr~3000mTorr, the temperature is 550℃~650℃, and the ionization time is 10min~12min.

[0040] As an optional embodiment, in an embodiment of the present invention, in the step of ionizing the silicon hydride compound and the boron hydride compound to form a boron-doped amorphous silicon layer on the surface of the first tunneling oxide layer away from the N-type silicon substrate, the flow rate of the silicon hydride compound is 2000sccm~3000sccm, the flow rate of the boron hydride compound is 700sccm~800sccm, the nitrogen flow rate is 8000sccm~10000sccm, the RF power is 7000W~7500W, the pressure is 2500mTorr~3000mTorr, the temperature is 550℃~650℃, and the ionization time is 10min~12min.

[0041] In a third aspect, the present application provides a photovoltaic module, wherein the photovoltaic module is prepared by connecting solar cells in series or in parallel, and the solar cells are prepared by the preparation method described in the second aspect.

[0042] In a fourth aspect, the present application provides an electrical device, wherein the electrical device includes a solar cell, and the solar cell is prepared by the preparation method described in the second aspect.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] Unlike the prior art solution that uses an aluminum oxide layer for passivation, the solar cell of the embodiment of the present invention sequentially arranges a boron-hydrogen doped layer, a first tunneling oxide layer, and a boron-doped polysilicon layer on the light-incident surface of the N-type silicon substrate. Through the combined action of these layers, not only can they replace the aluminum oxide layer to achieve a better passivation effect, but they also have better electrical conductivity, avoiding the problem of multiple film layers needing to be burned through in subsequent processes, which in turn affects the passivation effect and electrical performance. Among them, the first tunneling oxide layer and the boron-doped polysilicon layer can produce a quantum tunneling effect to form a tunneling channel for electron transmission, which is conductive, without the need to burn through the first tunneling oxide layer and the boron-doped polysilicon layer. The electrode contacts the boron-doped polysilicon layer to achieve current conduction, which can effectively provide electrical performance.

[0045] In addition, on the first hand, the boron-doped polysilicon layer and the first tunneling oxide layer can both form a potential barrier to block the transmission of holes, and can replace the aluminum oxide passivation layer to block holes from reaching the N-type silicon substrate for recombination, thereby reducing oxidation defects and achieving field passivation. On the second hand, the boron-hydrogen doped layer close to the N-type silicon substrate is doped with hydrogen, which can quickly saturate the unsaturated dangling bonds on the surface of the N-type silicon substrate at a relatively short distance, thereby achieving chemical passivation and reducing carrier recombination. As a result, the solar cell of the present application can not only achieve layer-by-layer passivation, taking into account both chemical passivation and field passivation, but also improve the electrical performance as much as possible without destroying the passivation structure, and can improve the photoelectric conversion efficiency of the solar cell in many aspects. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0047] FIG1 is a schematic structural diagram of a solar cell disclosed in Example 1 of the present invention;

[0048] FIG2 is a flow chart of a method for preparing a solar cell disclosed in an embodiment of the present invention.

[0049] Icon: 100, solar cell; 1, first electrode; 2, first anti-reflection layer; 3, boron-doped polysilicon layer; 4, first tunneling oxide layer; 5, boron-hydrogen-doped layer; 6, N-type silicon substrate; 7, second tunneling oxide layer; 8, phosphorus-doped polysilicon layer; 9, second anti-reflection layer; 10, second electrode. DETAILED DESCRIPTION

[0050] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts shall fall within the scope of protection of the present invention.

[0051] In the present invention, terms such as "upper," "lower," "left," "right," "front," "back," "top," "bottom," "inner," "outer," "center," "vertical," "horizontal," "transverse," and "longitudinal" indicate positions or locations based on the positions or locations shown in the accompanying drawings. These terms are primarily intended to better describe the present invention and its embodiments and are not intended to limit the devices, elements, or components indicated to having a specific orientation, or to being constructed or operated in a specific orientation.

[0052] Furthermore, some of the above terms may be used to express other meanings besides indicating a position or location. For example, the term "on" may also be used to indicate a dependency or connection in certain circumstances. Those skilled in the art will understand the specific meanings of these terms in the present invention based on the specific circumstances.

[0053] Furthermore, the terms "installed," "disposed," "provided with," "connected," and "connected" should be interpreted broadly. For example, they can refer to fixed connections, removable connections, or integral structures; mechanical connections or electrical connections; direct connections or indirect connections through an intermediary; or internal communication between two devices, elements, or components. Those skilled in the art will understand the specific meanings of these terms in the present invention based on specific circumstances.

[0054] Furthermore, the terms "first," "second," etc., are primarily used to distinguish between different devices, elements, or components (which may or may not be of the same type and configuration), and are not intended to indicate or imply the relative importance or quantity of the devices, elements, or components indicated. Unless otherwise specified, "plurality" means two or more.

[0055] The technical solution of the present invention will be further described below in conjunction with embodiments and drawings.

[0056] Impurities adsorbed on the front of the solar cell and surface defects such as dangling bonds formed by broken bonds on the silicon substrate surface will become carrier recombination centers, reducing the photoelectric conversion efficiency. Related technologies will set an aluminum oxide passivation layer on its front to play a passivation role and reduce surface recombination. However, the aluminum oxide passivation layer cannot conduct electrons. It is necessary to match the burn-through slurry and high-temperature sintering process until the aluminum oxide passivation layer is completely burned through, and the electrode is in direct contact with the silicon substrate to complete the current conduction. This process that destroys the passivation structure has harsh and complex processing conditions and is difficult to control; it also reduces the passivation effect of the location where the aluminum oxide passivation layer is burned through and the surrounding area, which is not conducive to improving the electrical performance and photoelectric conversion efficiency of the solar cell.

[0057] Based on this, in its first aspect, the present application provides a solar cell comprising: an N-type silicon substrate having a first and a second surface disposed opposite each other, the first surface being a light-incident surface; a boron-hydrogen-doped layer, a first tunneling oxide layer, a boron-doped polysilicon layer, and a first anti-reflection layer stacked in sequence on the first surface of the N-type silicon substrate; and a second tunneling oxide layer, a phosphorus-doped polysilicon layer, and a second anti-reflection layer stacked in sequence on the second surface of the N-type silicon substrate. The solar cell also comprises a first electrode and a second electrode, the first electrode penetrating the first anti-reflection layer to form an ohmic contact with the boron-doped polysilicon layer; and the second electrode forming an ohmic contact with the second tunneling oxide layer. The present application provides a passivation structure on the front side of the solar cell, comprising the boron-hydrogen-doped layer, the first tunneling oxide layer, and the boron-doped polysilicon layer, to replace the aluminum oxide passivation layer. This structure not only achieves better passivation than an aluminum oxide passivation layer, but also enables current conduction without damaging the passivation structure, effectively improving electrical performance and photoelectric conversion efficiency.

[0058] It should be noted that the boron-hydrogen doped layer in the present application refers to a boron-doped layer doped with hydrogen, that is, a doped layer containing both boron and hydrogen elements is deposited on an N-type silicon substrate.

[0059] Specifically, the first tunneling oxide layer and the boron-doped polysilicon layer can achieve a quantum tunneling effect, forming a tunneling channel for electron transmission. Electrons can move through the first tunneling oxide layer, the boron-doped polysilicon layer, and the boron-hydrogen-doped layer toward the N-type silicon substrate, thus achieving conductivity. Without burning through the first tunneling oxide layer and the boron-doped polysilicon layer, the electrodes can conduct current simply by contacting the boron-doped polysilicon layer. This further reduces the local contact area of ​​the electrodes in the solar cell, further reducing recombination at the electrode contact point, reducing front-side transmission losses, and effectively improving electrical performance.

[0060] In addition, on the one hand, the barrier height caused by the boron-doped polysilicon layer and the first tunnel oxide layer to the holes can block the transmission of holes, and the interaction between the two layers prevents the holes from reaching the surface of the N-type silicon substrate for recombination, thereby achieving the effect of field passivation. On the other hand, the boron-hydrogen doped layer close to the N-type silicon substrate is doped with hydrogen ions, which can fully saturate the unsaturated dangling bonds on the surface of the N-type silicon substrate at a relatively short distance, thereby achieving chemical passivation, reducing surface defects, and reducing recombination. Therefore, the solar cell of the present application can effectively improve the passivation effect, reduce the recombination of surface defects and carriers, and improve electrical performance and photoelectric conversion efficiency without destroying the passivation structure.

[0061] In some embodiments, the first tunneling oxide layer is a silicon oxide layer, and the second tunneling oxide layer is a silicon oxide layer; the first anti-reflection layer is a silicon nitride layer, and the second anti-reflection layer is a silicon nitride layer. The use of the same material for both the first and second tunneling oxide layers is silicon oxide, and both the first and second anti-reflection layers are silicon nitride. These materials provide a higher optical compatibility with sunlight within the visible light band, enabling better passivation and enhanced absorption of incident light.

[0062] In some embodiments, the boron-doped polysilicon layer is doped with hydrogen, and the phosphorus-doped polysilicon layer is doped with hydrogen. Free hydrogen in the boron-doped and phosphorus-doped polysilicon layers can occupy dangling bond vacancies, thereby achieving a chemical passivation effect. The front and back surfaces of the solar cell contain a multilayer hydrogen-rich structure, which can further enhance the passivation effect.

[0063] In some embodiments, the thickness of the first tunneling oxide layer is 1 nm to 2 nm; and / or the thickness of the boron-doped polysilicon layer is 1 nm to 30 nm. When the thickness of the first tunneling oxide layer and the boron-doped polysilicon layer is controlled within the above range, both can improve the field passivation effect, reduce recombination, and improve electrical and optical properties. When the thickness of the first tunneling oxide layer is controlled within the above range, the thickness of the first tunneling oxide layer is extremely thin, which has almost no effect on the transport of carriers, and effectively improves the open circuit voltage and short-circuit current. When the thickness of the boron-doped polysilicon layer is controlled within the above range, the tunneling probability of the carriers can be guaranteed, which is beneficial to improving the open circuit voltage and photoelectric conversion efficiency.

[0064] Preferably, the thickness of the first tunnel oxide layer is 1 nm to 2 nm and the thickness of the boron-doped polysilicon layer is 1 nm to 30 nm.

[0065] For example, the thickness of the first tunnel oxide layer may be any value within the aforementioned range, including but not limited to 1 nm, 1.1 nm, 1.2 nm, 1.3 nm, 1.4 nm, 1.5 nm, 1.6 nm, 1.7 nm, 1.8 nm, 1.9 nm, 2 nm, etc. The thickness of the boron-doped polysilicon layer may be any value within the aforementioned range, including but not limited to 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 10 nm, 12 nm, 14 nm, 16 nm, 18 nm, 20 nm, 22 nm, 24 nm, 26 nm, 28 nm, 30 nm, etc.

[0066] In some embodiments, the junction depth of the boron hydride doped layer is 0.8 μm to 1.5 μm, and / or the sheet resistance of the boron hydride doped layer is 105 Ω / sq to 145 Ω / sq, and / or the concentration of the boron element in the boron hydride doped layer is 1×10 19 N / cm 2 ~2×10 19 N / cm 2 By controlling the junction depth, square resistance and boron doping concentration of the boron-hydrogen doped layer within the above ranges, the contact resistance between the PN junction and the electrode is effectively reduced, which can increase the fill factor and improve the conversion efficiency of the solar cell.

[0067] Preferably, the junction depth of the boron hydride doped layer is 0.8 μm to 1.5 μm, the sheet resistance of the boron hydride doped layer is 105Ω / sq to 145Ω / sq, and the boron doping concentration is 1×10 19 N / cm 2 ~2×10 19 N / cm 2 .

[0068] For example, the junction depth of the boron hydride doped layer may be any value within the above range, including but not limited to 0.8 nm, 0.9 nm, 1 nm, 1.1 nm, 1.2 nm, 1.3 nm, 1.4 nm, 1.5 nm, etc. The sheet resistance of the boron hydride doped layer may be any value within the above range, including but not limited to 105 Ω / sq, 110 Ω / sq, 115 Ω / sq, 120 Ω / sq, 125 Ω / sq, 130 Ω / sq, 135 Ω / sq, 140 Ω / sq, 145 Ω / sq, etc. The boron doping concentration may be any value within the above range, including but not limited to 1×10 19 N / cm 2 , 1.1×10 19 N / cm 2 , 1.2×10 19 N / cm 2 , 1.3×10 19 N / cm 2 , 1.4×10 19N / cm 2 , 1.5×10 19 N / cm 2 , 1.6×10 19 N / cm 2 , 1.7×10 19 N / cm 2 , 1.8×10 19 N / cm 2 , 1.9×10 19 N / cm 2 , 2×10 19 N / cm 2 wait.

[0069] In a second aspect, referring to FIG. 2 , the present application provides a method for preparing a solar cell according to the first aspect, the method comprising the following steps:

[0070] Provide N-type silicon substrate after texturing treatment;

[0071] forming a boron hydride doped layer on the first surface;

[0072] Cleaning to remove the second side wraparound;

[0073] forming a second tunnel oxide layer on the second surface;

[0074] forming a phosphorus-doped amorphous silicon layer on a surface of the second tunnel oxide layer facing away from the N-type silicon substrate;

[0075] forming a first tunneling oxide layer on a surface of the boron-hydrogen doped layer facing away from the N-type silicon substrate;

[0076] forming a boron-doped amorphous silicon layer on a surface of the first tunnel oxide layer facing away from the N-type silicon substrate;

[0077] Annealing to convert the boron-doped amorphous silicon layer and the phosphorus-doped amorphous silicon layer into a boron-doped polysilicon layer and a phosphorus-doped polysilicon layer;

[0078] forming a first anti-reflection layer on a surface of the boron-doped polysilicon layer facing away from the N-type silicon substrate, and forming a second anti-reflection layer on a surface of the phosphorus-doped polysilicon layer facing away from the N-type silicon substrate;

[0079] Post-processing allows the first electrode to penetrate the first anti-reflection layer and make ohmic contact with the boron-doped polysilicon layer, and allows the second electrode to penetrate the second anti-reflection layer and the phosphorus-doped polysilicon layer and make ohmic contact with the second tunneling oxide layer.

[0080] In the boron-doped layer fabrication process, boron chloride (BCl₃) or boron bromide (BBr₃) is typically used to form the boron-doped layer through a boron diffusion process. These substances are introduced into a tubular diffusion furnace, where they react with oxygen to form boron oxide (B₂O₃). Nitrogen is then used to distribute the B₂O₃ across the surface of the N-type silicon substrate, where it reacts with the silicon to complete the boron doping. Due to the low solubility of boron in silicon, the deposition process requires high flow rates of nitrogen and oxygen, supplemented by a high propulsion temperature, to achieve boron doping. Furthermore, chlorides are highly corrosive, while bromides are highly viscous. The B₂O₃ formed during the doping process is adhesive and adheres to the surface of the tubular diffusion furnace, resulting in varying stresses within the furnace tubes and the risk of breakage over extended periods. The combination of high temperatures and the B₂O₃ content shortens the furnace tubes' service life, leading to high material and equipment costs. Furthermore, after the boron-doped layer is applied to the surface of the N-type silicon substrate, the semi-finished product must be transferred to other equipment for subsequent passivation treatment, resulting in a large number of equipment and lengthy process steps. For solar cells that require passivation on both the front and back sides of the N-type silicon substrate, the process flow is further extended, further increasing production costs. Existing solar cell production suffers from drawbacks such as high gas and energy consumption, severe equipment wear, multiple equipment requirements, and a complex manufacturing process.

[0081] In some embodiments, solar cells may be fabricated using chemical vapor deposition methods, such as LCVD (Laser-chemical CVD), RFCVD (Radio Frequency CVD), and PECVD (Plasma Enhanced CVD).

[0082] Taking PECVD as an example, PECVD and other related plasma preparation processes offer the advantages of low deposition temperature, low gas consumption, and low energy consumption. However, PECVD is primarily affected by pressure and RF power, making it difficult to control the doping concentration during the boron doping process. It is generally used to produce boron-doped polysilicon layers where the doping concentration requirement is not very high. Furthermore, inherent process flaws in PECVD can cause contamination, resulting in a high level of impurities and residues, which can seriously affect the quality of the boron-doped layer.

[0083] In order to prepare a high-quality boron hydride doped layer by PECVD and reduce process pollution, this application mainly regulates the gas flow rate and doping temperature prepared by the PECVD method to prepare the boron hydride doped layer, and performs a cleaning immediately after the boron hydride doped layer is completed, which can effectively improve the above problems.

[0084] The preparation method of the present invention will be described in detail below in order of steps.

[0085] In the step of providing an N-type silicon substrate that has been textured, the N-type silicon substrate is textured and cleaned using a 1% to 3% by volume NaOH aqueous solution for texture, and the N-type silicon wafer is cleaned for 30s to 60s using a 25% to 40% by volume H2O2 solution and a 1% to 5% by volume KOH aqueous solution to remove various pollutants and mechanical damage layers.

[0086] In some embodiments, in the step of forming a boron-hydrogen doped layer on the first surface, a boron-hydrogen compound is ionized to form a boron-hydrogen doped layer on the first surface; and / or, in the step of forming a boron-doped amorphous silicon layer on the surface of the first tunneling oxide layer facing away from the N-type silicon substrate, a silicon-hydrogen compound and a boron-hydrogen compound are ionized to form a boron-doped amorphous silicon layer on the surface of the first tunneling oxide layer facing away from the N-type silicon substrate; and / or, in the step of forming a phosphorus-doped amorphous silicon layer on the surface of the second tunneling oxide layer facing away from the N-type silicon substrate, a silicon-hydrogen compound and a phosphorus-hydrogen compound are ionized to form a phosphorus-doped amorphous silicon layer on the surface of the second tunneling oxide layer facing away from the N-type silicon substrate.

[0087] Boron hydride compounds refer to compounds containing, but not limited to, boron and hydrogen, such as monoborane and diborane. Silicon hydride compounds refer to compounds containing, but not limited to, silicon and hydrogen, such as monosilane, disilane, and trisilane. Phosphine hydride compounds refer to compounds containing, but not limited to, phosphorus and hydrogen, such as phosphine and tetrahydrophosphine. Preferably, the boron hydride is diborane, the silicon hydride is monosilane, and the phosphine hydride is phosphine. These preferred materials are safe, reliable, inexpensive, and compatible with chemical vapor deposition processes.

[0088] In the step of forming a boron-hydrogen doped layer on the first surface, a boron-hydrogen compound is ionized to form the boron-hydrogen doped layer on the first surface. Taking diborane as an example, diborane can be ionized to form boron ions and hydrogen ions. The boron ions dope the surface of the N-type silicon substrate, while the hydrogen ions passivate dangling bonds on the surface of the N-type silicon substrate. Thus, a boron-hydrogen doped layer with a chemical passivation effect is formed on the light-incident surface of the N-type silicon substrate.

[0089] In some embodiments, in the step of forming the boron hydride doped layer on the first surface, the flow rate of the boron hydride compound is 700 sccm to 800 sccm, the flow rate of the nitrogen is 10,000 sccm to 15,000 sccm; and / or, the RF power is 7,000 W to 7,500 W, the pressure is 2,500 mTorr to 3,000 mTorr, the temperature is 650° C. to 750° C., and the ionization time is 14 min to 16 min. The above parameters are coordinated with each other so that the junction depth of the boron hydride doped layer is maintained at 0.8 μm to 1.5 μm, and the boron doping concentration is maintained at 1×10 19 N / cm 2 ~2×10 19 N / cm2 , so that the sheet resistance of the boron-doped layer is maintained at 105Ω / sq~145Ω / sq. This ensures that the boron-hydrogen doped layer has better deposition quality, improves the passivation effect of the boron-hydrogen doped layer, reduces surface defects, and improves optical and electrical properties. The specific influencing factors are as follows:

[0090] The gas flow rate affects the content of boron and hydrogen in the boron-hydrogen doped layer. Excessive or insufficient gas flow rate will affect the deposition thickness of the boron-hydrogen doped layer and the doping concentration of the boron element, thereby improving the film quality of the boron-hydrogen doped layer. Exemplarily, the flow rate of the boron hydride compound is any value within the above range, including but not limited to: 700 sccm, 710 sccm, 720 sccm, 730 sccm, 740 sccm, 750 sccm, 760 sccm, 770 sccm, 780 sccm, 790 sccm, 800 sccm, etc. The nitrogen flow rate is any value within the above range, including but not limited to: 10,000 sccm, 11,000 sccm, 12,000 sccm, 13,000 sccm, 14,000 sccm, 15,000 sccm, etc.

[0091] Controlling the temperature within a suitable range can, on the one hand, reduce the introduction of defects and impurities, and on the other hand, provide thermodynamic momentum for hydrogen ions, facilitating the migration of ionized hydrogen ions to the surface of the N-type silicon substrate, saturating the dangling bonds on the surface and further reducing defect density. The temperature can be any value within the above range, including but not limited to 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, etc.

[0092] Low pressure reduces the number of boron hydride compounds participating in the reaction per unit volume, which is detrimental to the ionization rate. However, excessive pressure intensifies the plasma polymerization reaction generated by ionization, leading to irregular plasma doping on the surface of the N-type silicon substrate and increasing surface defects on the N-type silicon substrate. Excessive pressure also reduces the density of the deposited boron hydride doped layer and creates numerous surface defects, causing carrier recombination and reducing photoelectric conversion efficiency. The pressure can be any value within the above range, including but not limited to 2500mTorr, 2600mTorr, 2700mTorr, 2800mTorr, 2900mTorr, and 3000mTorr.

[0093] Increasing the RF power increases the energy of the bombarding ions, resulting in a denser and more uniform boron hydride-doped layer, which improves the deposition quality of the boron hydride-doped layer. When the RF power increases to a certain range, the boron hydride compounds are almost completely ionized, and the deposition rate gradually stabilizes. However, higher RF powers can cause greater damage to the N-type silicon substrate. The RF power can be any value within the above range, including but not limited to: 7000W, 7100W, 7200W, 7300W, 7400W, 7500W, etc.

[0094] The ionization time affects the junction depth of the boron hydride doped layer. The ionization time can be any value within the above range, including but not limited to 14 minutes, 14.1 minutes, 14.2 minutes, 14.3 minutes, 14.4 minutes, 14.5 minutes, 14.6 minutes, 14.7 minutes, 14.8 minutes, 14.9 minutes, 15 minutes, 15.1 minutes, 15.2 minutes, 15.3 minutes, 15.4 minutes, 15.5 minutes, 15.6 minutes, 15.7 minutes, 15.8 minutes, 15.9 minutes, 16 minutes, etc.

[0095] When a boron hydride doped layer is prepared on the first surface of an N-type silicon substrate by ionization, the boron ions diffused on the front surface will also diffuse to the second surface. If not removed, this will cause leakage failure of the solar cell and edge defects and hidden cracks on the N-type silicon substrate. In the step of removing the diffusion on the second surface, an inorganic base or etching acid is used to etch and polish the second surface and edge of the N-type silicon substrate, controlling the reflectivity of the second surface to 40% to 50%. As a result, the flatness of the second surface is increased after etching and polishing, which increases the reflection of long wavelengths, promotes the secondary absorption of incident light, and can increase the short-circuit current. At the same time, due to the reduction in the specific surface area of ​​the back surface, the back recombination is reduced and the back passivation effect can be improved.

[0096] Optionally, the inorganic base may be sodium hydroxide and / or potassium hydroxide, etc., and the etching acid may be hydrofluoric acid and / or nitric acid and / or sulfuric acid, etc., which can be adjusted according to process requirements.

[0097] In the step of forming the second tunneling oxide layer on the second surface, the formation of a silicon dioxide layer is taken as an example. In some embodiments, in the step of forming the second tunneling oxide layer on the second surface, nitrous oxide and nitrogen are introduced to deposit the second tunneling oxide layer, wherein the nitrous oxide can generate oxygen and react with the silicon in the N-type silicon substrate for deposition. The nitrogen flow rate is 30,000 sccm to 70,000 sccm, and the nitrous oxide flow rate is 8,000 sccm to 9,000 sccm; and / or, the deposition temperature is 550°C to 650°C, the deposition pressure is 2,500 mTorr to 3,000 mTorr, and the deposition time is 3 min to 4 min. Nitrous oxide can decompose to generate oxygen when ionized, and the oxygen and the silicon in the N-type silicon substrate can form a silicon dioxide tunneling oxide layer.

[0098] Illustratively, the flow rate of nitrogen is any point value within the above range, including but not limited to: 30,000 sccm, 40,000 sccm, 50,000 sccm, 60,000 sccm, 70,000 sccm, etc.

[0099] The flow rate of nitrous oxide is any point value within the above range, including but not limited to: 8000 sccm, 8100 sccm, 8200 sccm, 8300 sccm, 8400 sccm, 8500 sccm, 8600 sccm, 8700 sccm, 8800 sccm, 8900 sccm, 9000 sccm, etc.

[0100] The temperature may be any value within the above range, including but not limited to 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, etc.

[0101] The pressure is any value within the above range, including but not limited to 2500mTorr, 2600mTorr, 2700mTorr, 2800mTorr, 2900mTorr, 3000mTorr, etc.

[0102] The ionization time can be any value within the above range, including but not limited to 3 min, 3.1 min, 3.2 min, 3.3 min, 3.4 min, 3.5 min, 3.6 min, 3.7 min, 3.8 min, 3.9 min, 4 min, etc.

[0103] In the step of forming a phosphorus-doped amorphous silicon layer on the surface of the second tunneling oxide layer away from the N-type silicon substrate, silicon hydrogen compounds and phosphorus hydrogen compounds are ionized to form a phosphorus-doped amorphous silicon layer on the surface of the second tunneling oxide layer away from the N-type silicon substrate. Take the silicon hydrogen compound as monosilane and the phosphorus hydrogen compound as phosphine as an example. Phosphine can be ionized into phosphorus ions and hydrogen ions, and monosilane can be ionized into silicon ions and hydrogen ions. Phosphorus completes the doping of the second surface of the N-type silicon substrate in an ionic state, and hydrogen ions complete the passivation of the dangling bonds on the surface of the N-type silicon substrate. In this step, the square resistance of the phosphorus-doped amorphous silicon layer is controlled to be 90Ω / sq to 130Ω / sq, and the concentration range of phosphorus doping is 2×10 20 N / cm 2 ~3×10 20 N / cm 2 .

[0104] In some embodiments, the flow rate of the silicon hydride compound is 2000 sccm to 3000 sccm, the flow rate of the phosphorus hydride compound is 700 sccm to 800 sccm, and the flow rate of nitrogen is 8000 sccm to 10000 sccm; and / or, the RF power is 7000 W to 7500 W, the pressure is 2500 mTorr to 3000 mTorr, the temperature is 550° C. to 650° C., and the ionization time is 10 min to 12 min.

[0105] Illustratively, the flow rate of the silicon hydride compound is any value within the above range, including but not limited to 2000 sccm, 2500 sccm, 2600 sccm, 2700 sccm, 2800 sccm, 2900 sccm, 3000 sccm, etc.

[0106] The flow rate of the phosphorus hydrogen compound is any value within the above range, including but not limited to: 700 sccm, 710 sccm, 720 sccm, 730 sccm, 740 sccm, 750 sccm, 760 sccm, 770 sccm, 780 sccm, 790 sccm, 800 sccm, etc.

[0107] The flow rate of nitrogen gas may be any value within the above range, including but not limited to: 8000 sccm, 8500 sccm, 9000 sccm, 9500 sccm, 10000 sccm, etc.

[0108] The RF power can be any value within the above range, including but not limited to: 7000W, 7100W, 7200W, 7300W, 7400W, 7500W, etc.

[0109] The deposition pressure is any value within the above range, including but not limited to 2500 mTorr, 2600 mTorr, 2700 mTorr, 2800 mTorr, 2900 mTorr, 3000 mTorr, etc.

[0110] The temperature may be any value within the above range, including but not limited to 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, etc.

[0111] The ionization time can be any value within the above range, including but not limited to 10 min, 10.1 min, 10.2 min, 10.3 min, 10.4 min, 10.5 min, 10.6 min, 10.7 min, 10.8 min, 10.9 min, 11, 11.5 min, 12 min, etc.

[0112] In some embodiments, a first tunneling oxide layer is formed on the surface of the boron hydride-doped layer facing away from the N-type silicon substrate. Nitrous oxide decomposes under ionization to produce oxygen, which reacts with silicon in the N-type silicon substrate to form a silicon dioxide tunneling oxide layer. In some embodiments, the nitrogen flow rate is 30,000 sccm to 70,000 sccm, and the nitrous oxide flow rate is 8,000 sccm to 9,000 sccm; and / or the deposition temperature is 550°C to 650°C, the deposition pressure is 2,500 mTorr to 3,000 mTorr, and the deposition time is 3 to 4 minutes.

[0113] Illustratively, the flow rate of nitrogen is any point value within the above range, including but not limited to: 30,000 sccm, 40,000 sccm, 50,000 sccm, 60,000 sccm, 70,000 sccm, etc.

[0114] The flow rate of nitrous oxide is any point value within the above range, including but not limited to: 8000 sccm, 8100 sccm, 8200 sccm, 8300 sccm, 8400 sccm, 8500 sccm, 8600 sccm, 8700 sccm, 8800 sccm, 8900 sccm, 9000 sccm, etc.

[0115] The temperature may be any value within the above range, including but not limited to 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, etc.

[0116] The pressure is any value within the above range, including but not limited to 2500mTorr, 2600mTorr, 2700mTorr, 2800mTorr, 2900mTorr, 3000mTorr, etc.

[0117] The ionization time can be any value within the above range, including but not limited to 3 min, 3.1 min, 3.2 min, 3.3 min, 3.4 min, 3.5 min, 3.6 min, 3.7 min, 3.8 min, 3.9 min, 4 min, etc.

[0118] In some embodiments, during the step of forming a boron-doped amorphous silicon layer on the surface of the first tunneling oxide layer facing away from the N-type silicon substrate, a silicon hydride compound and a boron hydride compound are ionized to form a boron-doped amorphous silicon layer on the surface of the first tunneling oxide layer facing away from the N-type silicon substrate. For example, the silicon hydride compound is monosilane, and the boron hydride compound is diborane. Phosphine can be ionized into phosphorus ions and hydrogen ions, and diborane can be ionized into boron ions and hydrogen ions. Boron, in its ionic state, accomplishes doping on the second surface of the N-type silicon substrate, while the hydrogen ions passivate dangling bonds on the surface of the N-type silicon substrate.

[0119] In some embodiments, the flow rate of the silicon hydride compound is 2000sccm~3000sccm, the flow rate of the boron hydride compound is 700sccm~800sccm, and the nitrogen flow rate is 8000sccm~10000sccm; and / or, the RF power is 7000W~7500W, the pressure is 2500mTorr~3000mTorr, the temperature is 550℃~650℃, and the ionization time is 10min~12min.

[0120] Illustratively, the flow rate of the silicon hydride compound is any point value within the above range, including but not limited to: 2000 sccm, 2500 sccm, 2600 sccm, 2700 sccm, 2800 sccm, 2900 sccm, 3000 sccm, etc.

[0121] The flow rate of the boron hydride compound is any point value within the above range, including but not limited to: 700 sccm, 710 sccm, 720 sccm, 730 sccm, 740 sccm, 750 sccm, 760 sccm, 770 sccm, 780 sccm, 790 sccm, 800 sccm, etc.

[0122] The flow rate of nitrogen gas can be any value within the above range, including but not limited to: 8000 sccm, 8500 sccm, 9000 sccm, 9500 sccm, 10000 sccm, etc.

[0123] The RF power can be any value within the above range, including but not limited to: 7000W, 7100W, 7200W, 7300W, 7400W, 7500W, etc.

[0124] The deposition pressure is any value within the above range, including but not limited to 2500mTorr, 2600mTorr, 2700mTorr, 2800mTorr, 2900mTorr, 3000mTorr, etc.

[0125] The temperature may be any value within the above range, including but not limited to 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, etc.

[0126] The ionization time can be any value within the above range, including but not limited to 10 min, 10.1 min, 10.2 min, 10.3 min, 10.4 min, 10.5 min, 10.6 min, 10.7 min, 10.8 min, 10.9 min, 11 min, 11.5 min, 12 min, etc.

[0127] It should also be noted that before forming the boron-hydrogen doped layer on the first surface, the N-type silicon substrate can be oxidized to form a mask to limit the boron doping area. After forming the boron-hydrogen doped layer on the first surface, before proceeding to subsequent steps, the entire ionization environment can be purged at a constant temperature to remove impurity gases to prevent interference with subsequent steps.

[0128] After a phosphorus-doped amorphous silicon layer is formed on the surface of the second tunnel oxide layer facing away from the N-type silicon substrate, the phosphorus diffused from the first surface of the N-type silicon substrate and its edge is cleaned. The entire ionization environment can also be purged at a constant temperature to remove impurity gases to avoid interference with subsequent steps.

[0129] After a boron-doped amorphous silicon layer is formed on the surface of the first tunnel oxide layer facing away from the N-type silicon substrate, the second surface of the N-type silicon substrate and the boron diffused at its edge are cleaned and etched to remove the surrounding diffusion.

[0130] In the post-processing step of allowing the first electrode to penetrate the first anti-reflection layer and make ohmic contact with the boron-doped polysilicon layer, and allowing the second electrode to penetrate the second anti-reflection layer and make ohmic contact with the phosphorus-doped polysilicon layer and the second tunneling oxide layer, the first electrode is a positive electrode and the second electrode is a negative electrode.

[0131] In summary, the preparation of all film structures of the solar cell of the present application can be done by ionization, and the production can be completed in only one PECVD device, which reduces gas consumption, energy consumption and equipment loss, reduces the number of machines, reduces process steps, effectively reduces the difficulty of maintenance for production line personnel, and can effectively reduce production costs and improve production efficiency. In addition, it is precisely because of the use of the ionization method to prepare the above-mentioned film layers that the boron-hydrogen doped layer, the boron-doped amorphous silicon layer, and the phosphorus-doped amorphous silicon layer are all rich in hydrogen elements. When annealing to form polycrystalline silicon, the hydrogen elements can obtain power to transfer to the surface of the N-type silicon substrate, saturate the dangling bonds, reduce the defect density, reduce recombination, and improve the photoelectric conversion efficiency.

[0132] In a third aspect, the present application provides a photovoltaic module, which is a solar cell prepared in the second aspect, or a plurality of solar cells connected in series or in parallel.

[0133] In a fourth aspect, the present application also provides an electrical device, which includes the solar cell prepared in the second aspect. The electrical device can be a communication base station, a photovoltaic power station, a household appliance, a traffic light, etc.

[0134] The following is a detailed introduction to the solution of this application using specific embodiments:

[0135] Example 1

[0136] Referring to FIG. 1 , an embodiment of the present application provides a solar cell 100, including:

[0137] An N-type silicon substrate 6, the N-type silicon substrate 6 having a first surface and a second surface disposed opposite to each other, the first surface being a light incident surface;

[0138] The boron-hydrogen doped layer 5, the first tunneling oxide layer 4 is a silicon dioxide layer, the boron-doped polysilicon layer 3 and the first anti-reflection layer 2 is a silicon nitride layer stacked in sequence on the first surface of the N-type silicon substrate 6. The junction depth of the boron-hydrogen doped layer 5 is 1.2 μm, and the boron doping concentration is 1.5×10 19 N / cm 2 ; The thickness of the first tunnel oxide layer 4 is 1.2 nm, and the thickness of the boron-doped polysilicon layer 3 is 15 nm;

[0139] The second tunneling oxide layer 7 is a silicon oxide layer, the phosphorus-doped polysilicon layer 8 and the second anti-reflection layer 9 are a silicon nitride layer stacked sequentially on the second surface of the N-type silicon substrate 6;

[0140] A first electrode 1 is formed to penetrate the first anti-reflection layer 2 and to make ohmic contact with the boron-doped polysilicon layer 3. The first electrode 1 is a positive electrode.

[0141] The second electrode 10 penetrates the second anti-reflection layer 9 and the phosphorus-doped polysilicon layer 8 and comes into ohmic contact with the second tunneling oxide layer 7 . The second electrode 10 is a negative electrode.

[0142] The present invention also provides a method for preparing the solar cell 100, which comprises the following steps:

[0143] Providing an N-type silicon substrate that has been textured: performing texturing and cleaning on the N-type silicon substrate, using a 1% by volume NaOH aqueous solution for texturing, and using a 25% by volume H2O2 solution and a 1% by volume KOH aqueous solution to clean the N-type silicon wafer for 30 seconds;

[0144] Forming a boron hydride doped layer on the first surface: In a nitrogen atmosphere, diborane was ionized to form a boron hydride doped layer on the first surface, wherein the diborane flow rate was 750 sccm, the nitrogen flow rate was 12000 sccm, the ionization RF power was 7200 W, the ionization pressure was 2700 mTorr, the ionization temperature was 700°C, and the ionization time was 15 minutes.

[0145] Cleaning to remove the deflection of the second surface, using a mixed aqueous solution of NaOH and KOH to remove the deflection of the second surface and its edges;

[0146] A second tunneling oxide layer was formed on the second surface: in a nitrogen atmosphere, nitrous oxide was introduced to generate oxygen to react with silicon in the N-type silicon substrate. The second tunneling oxide layer was a silicon dioxide layer. The nitrogen flow rate was 50,000 seem, the nitrous oxide flow rate was 8,500 seem, the deposition temperature was 600°C, the deposition pressure was 2,700 mTorr, and the deposition time was 3.5 minutes.

[0147] forming a phosphorus-doped amorphous silicon layer on a surface of the second tunnel oxide layer facing away from the N-type silicon substrate: ionizing a silicon hydride compound and a phosphorus hydride compound in a nitrogen atmosphere to form a phosphorus-doped amorphous silicon layer on a surface of the second tunnel oxide layer facing away from the N-type silicon substrate, wherein the flow rate of monosilane is 2500 sccm, the flow rate of phosphine is 750 sccm, the flow rate of nitrogen is 9000 sccm, the radio frequency power is 7200 W, the pressure is 2700 mTorr, the temperature is 600° C., and the ionization time is 11 minutes;

[0148] A first tunneling oxide layer was formed on the surface of the boron hydride doped layer facing away from the N-type silicon substrate. Nitrous oxide was introduced into the layer in a nitrogen atmosphere to generate oxygen to react with silicon in the N-type silicon substrate. The first tunneling oxide layer was a silicon oxide layer. The nitrogen flow rate was 50,000 seem, the nitrous oxide flow rate was 8,500 seem, the deposition temperature was 600°C, the deposition pressure was 2,700 mTorr, and the deposition time was 3.5 minutes.

[0149] forming a boron-doped amorphous silicon layer on a surface of the first tunnel oxide layer facing away from the N-type silicon substrate: ionizing a silicon hydride compound and a boron hydride compound in a nitrogen atmosphere to form a boron-doped amorphous silicon layer on a surface of the first tunnel oxide layer facing away from the N-type silicon substrate, wherein the flow rate of monosilane is 2500 sccm, the flow rate of diborane is 750 sccm, the flow rate of nitrogen is 8000 sccm, the radio frequency power is 7200 W, the pressure is 2700 mTorr, the temperature is 600° C., and the ionization time is 11 minutes;

[0150] Annealing to convert the boron-doped amorphous silicon layer and the phosphorus-doped amorphous silicon layer into a boron-doped polysilicon layer and a phosphorus-doped polysilicon layer;

[0151] forming a first anti-reflection layer on a surface of the boron-doped polysilicon layer facing away from the N-type silicon substrate, and forming a second anti-reflection layer on a surface of the phosphorus-doped polysilicon layer facing away from the N-type silicon substrate, wherein both the first anti-reflection layer and the second anti-reflection layer are silicon nitride layers;

[0152] Post-processing allows the first electrode to penetrate the first anti-reflection layer and then make ohmic contact with the boron-doped polysilicon layer, and allows the second electrode to make ohmic contact with the second tunneling oxide layer. The first electrode is a positive electrode and the second electrode is a negative electrode.

[0153] Example 2

[0154] The difference between Example 2 and Example 1 is that in the step of preparing the boron hydride doped layer in Example 2, the flow rate of diborane is 700 sccm, the flow rate of nitrogen is 10,000 sccm, the ionization temperature is 650°C, the RF power is 7,000 W, the deposition pressure is 2,500 mTorr, and the deposition time is 14 minutes. The rest is the same as in Example 1.

[0155] Example 3

[0156] The difference between Example 3 and Example 1 is that in the step of preparing the boron hydride doped layer in Example 2, the diborane flow rate is 800 sccm, the nitrogen flow rate is 15000 sccm, the ionization temperature is 750°C, the RF power is 7500W, the deposition pressure is 3000 mTorr, and the deposition time is 16 minutes. The rest is consistent with Example 1.

[0157] Example 4

[0158] The only difference between Example 4 and Example 1 is that the diborane flow rate in Example 4 is 600 sccm, and the rest is consistent with Example 1.

[0159] Example 5

[0160] The only difference between Example 5 and Example 1 is that the diborane flow rate in Example 5 is 900 sccm, and the rest is the same as Example 5.

[0161] The only difference between Example 6 and Example 1 is that the ionization temperature of Example 6 is 500° C., and the rest is consistent with Example 1.

[0162] Example 7

[0163] The only difference between Example 7 and Example 1 is that the ionization temperature of Example 7 is 800° C., and the rest is consistent with Example 1.

[0164] Example 8

[0165] Example 8 provides a passivated contact cell. Comparative Example 4 does not perform cleaning after the boron hydride doping layer is prepared to remove the flexure on the second surface. The rest is consistent with Example 1.

[0166] Comparative Example 1

[0167] Comparative Example 1 provides a passivated contact cell. The only difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not set a boron-doped polysilicon layer and a first tunneling oxide layer, but sets an aluminum oxide passivation layer. The preparation method directly deposits the aluminum oxide passivation layer on the boron-hydrogen doped layer, and the rest is consistent with Example 1.

[0168] Comparative Example 2

[0169] Comparative Example 1 provides a passivated contact cell. The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 uses boron chloride BCl3 to perform boron diffusion junction to form a boron diffusion layer, and the rest is consistent with Example 1.

[0170] The passivated contact cells provided in the examples and comparative examples were subjected to Auger recombination testing and performance testing of open circuit voltage, short circuit current, and fill factor using a Halm test and sorting device. The Halm machine is a device that simulates sunlight and is equipped with an electronic load, data acquisition, and computing equipment to test the electrical properties of photovoltaic devices, such as Eta, Voc, Isc, FF, Rs, and Rsh, which are used to reflect the performance of solar cells. The silicon wafers used for the control tests were 182 mm in size and the calibrated light intensity was 1000 ± 50 W / m 2 , the experimental test results are as follows, where Eta represents Auger recombination, Voc represents open circuit voltage, Isc represents short circuit current, FF represents fill factor, Rs represents series resistance, and Rsh is shunt resistance.

[0171] Using SIMS (secondary ion mass spectrometry), a high-energy primary ion beam is bombarded on the surface of the solar cell, causing the surface molecules to absorb energy and sputter from the surface to produce secondary ions. These secondary ions are collected and analyzed by a mass analyzer to obtain a map of the hydrogen content.

[0172] Table 1. Parameters of the preparation process of the boron hydride doped layer

[0173] Table 2. Performance test results of solar cells

[0174] Eta represents the photoelectric conversion efficiency. Voc represents the open-circuit voltage, Isc represents the short-circuit current, and FF represents the fill factor. The higher the above three, the fewer surface defects in the solar cell, the less carrier recombination, and the more effective the photoelectric conversion efficiency. Rs represents the series resistance. Rsh is the parallel resistance. The bypass resistance indicates leakage failure. The higher the parallel resistance, the less leakage. Rsh also indicates the formation of the PN junction. The higher the parallel resistance, the better the quality of the PN junction. A higher hydrogen content (%) indicates a better passivation effect.

[0175] Combined with Table 1 and Table 2, compared with Example 1, Example 4 and Example 5 have the following characteristics: the flow rate of diborane in Example 4 is lower than the flow rate range, and the flow rate of Example 5 is higher than the flow rate range. The various performance data of Example 1 are different from those of Example 4 and Example 5, indicating that controlling the flow rate of diborane within an appropriate range can improve the film formation quality of the boron-hydrogen doped layer, thereby improving the passivation effect and various photo / electrochemical properties.

[0176] Compared with Example 1, Example 6 and Example 7 have an ionization temperature lower than the temperature range, and an ionization temperature higher than the temperature range. The various performance data of Example 1 are different from those of Example 6 and Example 7, indicating that controlling the temperature can effectively reduce the introduction of defects and contamination in the boron hydride doped layer, reduce recombination centers, and improve the passivation effect, thereby also improving the photoelectric conversion efficiency.

[0177] Compared with Example 1, Example 8 does not perform a cleaning step to remove contaminants and defects after the boron hydride doped layer is formed, so the film quality of the boron hydride doped layer is reduced, and the passivation effect is reduced.

[0178] Compared with Comparative Example 1, Example 1 shows a higher parallel resistance than Comparative Example 1. This is because the boron hydride-doped layer is doped with a large amount of hydrogen atoms during the PN junction formation process, resulting in a better passivation effect and a higher-quality PN junction. The passivation structure in Comparative Example 1 is an aluminum oxide passivation layer. Because the aluminum oxide passivation layer requires perforations, this affects both electrical performance and passivation effectiveness, resulting in lower performance than in Example 1.

[0179] Compared with Example 1 and Comparative Example 2, Comparative Example 2 uses conventional technology to make the boron diffusion layer, does not introduce a large amount of hydrogen element, and the hydrogen content is significantly reduced, the passivation effect is reduced, there are more defects and recombination centers, and the photoelectric conversion efficiency is reduced.

[0180] The above is a detailed introduction to a solar cell and its preparation method, photovoltaic module, and electrical equipment disclosed in the embodiments of the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the solar cell and its preparation method, photovoltaic module, electrical equipment and its core ideas of the present invention: At the same time, for general technical personnel in this field, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the contents of this specification should not be understood as limiting the present invention.

Claims

1. A solar cell, characterized in that: The solar cell comprises: An N-type silicon substrate, the N-type silicon substrate having a first surface and a second surface disposed opposite to each other, the first surface being a light incident surface; A boron-hydrogen doped layer, a first tunneling oxide layer, a boron-doped polysilicon layer and a first anti-reflection layer are sequentially stacked on the first surface of the N-type silicon substrate; A second tunneling oxide layer, a phosphorus-doped polysilicon layer, and a second anti-reflection layer are sequentially stacked on the second surface of the N-type silicon substrate; a first electrode, penetrating the first anti-reflection layer and making ohmic contact with the boron-doped polysilicon layer; The second electrode is in ohmic contact with the second tunneling oxide layer.

2. The solar cell according to claim 1, characterized in that: The boron-doped polysilicon layer is doped with hydrogen element.

3. The solar cell according to claim 1 or 2, characterized in that: The phosphorus-doped polysilicon layer is doped with hydrogen elements.

4. The solar cell according to any one of claims 1 to 3, characterized in that: The first tunneling oxide layer is a silicon oxide layer.

5. The solar cell according to any one of claims 1 to 4, characterized in that: The second tunneling oxide layer is a silicon oxide layer.

6. The solar cell according to any one of claims 1 to 5, characterized in that: The first anti-reflection layer is a silicon nitride layer.

7. The solar cell according to any one of claims 1 to 6, characterized in that: The second anti-reflection layer is a silicon nitride layer.

8. The solar cell according to any one of claims 1 to 7, characterized in that: The thickness of the first tunnel oxide layer is 1 nm to 2 nm.

9. The solar cell according to any one of claims 1 to 8, characterized in that: The thickness of the boron-doped polysilicon layer is 1 nm to 30 nm.

10. The solar cell according to any one of claims 1 to 9, characterized in that: The junction depth of the boron hydride doped layer is 0.8 μm to 1.5 μm.

11. The solar cell according to any one of claims 1 to 10, characterized in that: The sheet resistance of the boron hydride doped layer is 105Ω / sq to 145Ω / sq.

12. The solar cell according to any one of claims 1 to 11, characterized in that: The concentration of boron in the boron-hydrogen doped layer is 1×10 19 N / cm 2 ~2×10 19 N / cm 2 .

13. A method for preparing a solar cell, wherein the solar cell is the solar cell according to any one of claims 1 to 12, characterized in that: The preparation method comprises the following steps: Providing the N-type silicon substrate that has been textured; forming the boron hydride doped layer on the first surface; Cleaning to remove the wraparound of the second surface; forming the second tunneling oxide layer on the second surface; forming a phosphorus-doped amorphous silicon layer on a surface of the second tunnel oxide layer away from the N-type silicon substrate; forming the first tunneling oxide layer on a surface of the boron hydride doped layer away from the N-type silicon substrate; forming a boron-doped amorphous silicon layer on a surface of the first tunnel oxide layer away from the N-type silicon substrate; Annealing to convert the boron-doped amorphous silicon layer and the phosphorus-doped amorphous silicon layer into the boron-doped polysilicon layer and the phosphorus-doped polysilicon layer; forming the first anti-reflection layer on the surface of the boron-doped polysilicon layer away from the N-type silicon substrate, and forming the second anti-reflection layer on the surface of the phosphorus-doped polysilicon layer away from the N-type silicon substrate; The post-processing allows the first electrode to penetrate the first anti-reflection layer and make ohmic contact with the boron-doped polysilicon layer, and allows the second electrode to penetrate the second anti-reflection layer and the phosphorus-doped polysilicon layer and make ohmic contact with the second tunneling oxide layer. touch.

14. The preparation method according to claim 13, characterized in that: In the step of forming the second tunneling oxide layer on the second surface, nitrous oxide and nitrogen are introduced to deposit the second tunneling oxide layer, wherein the nitrogen flow rate is 30000sccm~70000sccm, the nitrous oxide flow rate is 8000sccm~9000sccm, the deposition temperature is 550℃~650℃, the deposition pressure is 2500mTorr~3000mTorr, and the deposition time is 3min~4min.

15. The preparation method according to claim 13 or 14, characterized in that: In the step of forming the first tunneling oxide layer on the surface of the boron hydride doped layer away from the N-type silicon substrate, nitrous oxide and nitrogen are introduced to deposit the first tunneling oxide layer, wherein the nitrogen flow rate is 30000sccm~70000sccm, the nitrous oxide flow rate is 8000sccm~9000sccm, the deposition temperature is 550℃~650℃, the deposition pressure is 2500mTorr~3000mTorr, and the deposition time is 3min~4min.

16. The preparation method according to any one of claims 13 to 15, characterized in that: The solar cell is prepared by chemical vapor deposition; Wherein, in the step of forming the boron hydride doped layer on the first surface, a boron hydride compound is ionized to form the boron hydride doped layer on the first surface.

17. The preparation method according to any one of claims 13 to 16, characterized in that: In the step of forming a boron-doped amorphous silicon layer on a surface of the first tunnel oxide layer away from the N-type silicon substrate, silicon hydride and boron hydride are ionized to form a boron-doped amorphous silicon layer on a surface of the first tunnel oxide layer away from the N-type silicon substrate.

18. The preparation method according to any one of claims 13 to 17, characterized in that: In the step of forming a phosphorus-doped amorphous silicon layer on a surface of the second tunnel oxide layer away from the N-type silicon substrate, silicon hydride and phosphorus hydride are ionized to form a phosphorus-doped amorphous silicon layer on a surface of the second tunnel oxide layer away from the N-type silicon substrate.

19. The preparation method according to any one of claims 16 to 18, characterized in that: In the step of ionizing the boron hydride compound to form the boron hydride doped layer on the first surface, the flow rate of the boron hydride compound is 700sccm~800sccm, the nitrogen flow rate is 10000sccm~15000sccm, the RF power is 7000W~7500W, the pressure is 2500mTorr~3000mTorr, the temperature is 800℃~850℃, and the ionization time is 14min~16min.

20. The preparation method according to any one of claims 16 to 19, characterized in that: In the step of ionizing the silicon hydride and the phosphorus hydride to form a phosphorus-doped amorphous silicon layer on the surface of the second tunneling oxide layer away from the N-type silicon substrate, the flow rate of the silicon hydride is 2000sccm~3000sccm, the flow rate of the phosphorus hydride is 700sccm~800sccm, the flow rate of nitrogen is 8000sccm~10000sccm, the RF power is 7000W~7500W, the pressure is 2500mTorr~3000mTorr, the temperature is 550℃~650℃, and the ionization time is 10min~12min.

21. The preparation method according to any one of claims 16 to 20, characterized in that: In the step of ionizing the silicon hydride compound and the boron hydride compound to form a boron-doped amorphous silicon layer on the surface of the first tunneling oxide layer away from the N-type silicon substrate, the flow rate of the silicon hydride compound is 2000sccm~3000sccm, the flow rate of the boron hydride compound is 700sccm~800sccm, the flow rate of nitrogen is 8000sccm~10000sccm, the RF power is 7000W~7500W, the pressure is 2500mTorr~3000mTorr, the temperature is 550℃~650℃, and the ionization time is 10min~12min.

22. A photovoltaic module, characterized in that: The photovoltaic module is prepared by connecting solar cells in series or in parallel, and the solar cells are prepared by the preparation method according to any one of claims 13 to 21.

23. An electrical device, comprising a solar cell, wherein the solar cell is prepared by the preparation method according to any one of claims 13 to 21.

Citation Information

Patent Citations

  • Double-sided passivation contact solar cell and manufacturing method thereof

    CN114883421A

  • N-TOPCon photovoltaic solar cell preparation method and solar cell

    CN114975643A

  • TOPCon battery and manufacturing method thereof

    CN115148857A

  • Preparation method of P-type passivation contact solar cell

    CN115332392A

  • Solar cell and preparation method thereof, photovoltaic module and electric equipment

    CN116417527A