Antimicrobial agent
The antibacterial agent utilizing simoncolite nanoparticles addresses the challenge of microorganism growth causing body and scalp odors by effectively inhibiting Corynebacterium, Moraxella, and Malassezia, providing a solution for odor reduction and skin health improvement in cosmetics.
Patent Information
- Application Number
- PCT/JP2024/004460
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-02-09
- Publication Date
- 2024-10-31
AI Technical Summary
Current technologies lack effective solutions for suppressing the growth and activity of microorganisms like Corynebacterium, Moraxella, and Malassezia, which cause body odor, scalp odor, and dry skin issues, with the antibacterial effects of existing agents like butterbur extract and straight-chain aliphatic aldehydes being partially studied, and simoncolite's potential uses unexplored.
Development of an antibacterial agent using simoncolite, a zinc chloride hydroxide hydrate, in nanoparticle form to inhibit the growth of these microorganisms, providing a new use for simoncolite and enhancing its antibacterial properties for cosmetic and deodorant applications.
The antibacterial agent effectively suppresses the activity and proliferation of Corynebacterium, Moraxella, and Malassezia, reducing body and scalp odors, inflammation, and dandruff, while offering a cosmetically pleasing and residue-free formulation.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
antibacterial agents
[0001] The present invention relates to an antibacterial agent, and in particular to an antibacterial agent that is incorporated into a deodorant cosmetic or a scalp care cosmetic (for preventing dandruff, itching, and scalp odor).
[0002] Various microorganisms known as resident skin flora live on the skin, forming a resident flora. While some microorganisms in the resident skin flora maintain healthy skin, others have adverse effects, such as causing rough skin and body odor. The composition ratio of these microorganisms fluctuates depending on changes in skin condition and physical condition. Among these adversely affecting resident skin flora, Corynebacterium, Moraxella, and Malassezia fungi are known to be responsible for body odor and scalp odor by breaking down components contained in sweat and sebum and synthesizing odorous compounds during proliferation. Corynebacterium is known to cause axillary odor and may also cause body odor, scalp odor, and foot odor. Moraxella is also responsible for the smell of damp laundry. Malassezia fungi are known to cause seborrheic alopecia when they overgrow on the scalp, and are known to cause scalp odor, scalp inflammation, dandruff, and itching. Therefore, progress is being made in the development of technologies for suppressing unpleasant odors such as body odor, scalp odor, and damp odor by inhibiting the growth and activity of these types of microorganisms. For example, Patent Document 1 proposes an anti-armpit odor agent and an anti-Malassezia agent that contain a fat-soluble extract of butterbur as an active ingredient, and Patent Document 2 proposes an agent for suppressing damp odor produced by Moraxella bacteria that contains a straight-chain aliphatic aldehyde having a specific number of carbon atoms as an active ingredient.
[0003] On the other hand, Simoncolite is a zinc chloride hydroxide hydrate composed of zinc, hydroxyl groups, and chlorine, and its chemical formula is Zn 5 (OH) 8 Cl 2 ・(H 2 O) nIt is a compound represented by the formula: It is a white crystalline powder insoluble in water and organic solvents, and is also known as basic zinc chloride or zinc chloride hydroxide. Simoncollite, a natural mineral, was announced as a new mineral in 1985 and named after Werner Simon and Kurt Kolle, who collected samples of simoncollite. To date, simoncollite has primarily been used as the main component of tetrabasic zinc chloride (TBZC), an animal feed additive, and is considered a desirable nutritional supplement for animals.
[0004] In recent years, research and development has been conducted into new uses and industrial production methods for Simonkolite. For example, Patent Document 3 reports a technology for using Simonkolite as a skin wound treatment agent, and Patent Document 4 reports a method for producing Simonkolite that can be used as an active ingredient in pharmaceuticals.
[0005] Japanese Patent Publication No. 2021-161043 Japanese Patent No. 5852313 Japanese Patent No. 6185215 International Publication No. 2018 / 105738
[0006] The above-mentioned Patent Document 1 reports that butterbur fat-soluble extract has antibacterial action against microorganisms that cause body odor, scalp odor, etc., and Patent Document 2 reports that straight-chain aliphatic aldehydes have the effect of inhibiting the production of 4-methyl-3-hexenoic acid, a substance that causes damp odor, by microorganisms that are capable of producing the same substance. However, no study has been conducted to date on the effect of simoncolite on this type of microorganism, and its effectiveness has been unknown.
[0007] Furthermore, Patent Document 3 reports the use of simoncolyte as a skin wound treatment agent, but the use of simoncolyte for suppressing body odor and scalp odor, preventing dandruff and itching of the scalp, etc. has not been investigated to date, and its effectiveness has been unknown.
[0008] Therefore, the present invention has been made in view of the above-mentioned points, and an object of the present invention is to provide a new use of Simoncolite.
[0009] As a result of extensive research into new functions of Simoncolyte, the present inventors discovered that Simoncolyte has antibacterial activity against microorganisms that cause body odor, scalp odor, and damp odor. Based on this finding, the present invention was completed. In order to solve the above problems, the antibacterial agent of the present invention is an antibacterial agent against at least one species of normal skin bacteria selected from the group consisting of the genera Corynebacterium, Moraxella, and Malassezia, and contains Simoncolyte as an active ingredient. Simoncolyte has antibacterial activity that inhibits the growth of normal skin bacteria of the genera Corynebacterium, Moraxella, and Malassezia. Therefore, it can inhibit the activity and growth of these microorganisms that cause body odor, scalp odor, and damp odor.
[0010] In addition, it is also preferable that the antibacterial agent of the present invention has nanoparticles of simoncollite. This reduces the rough feeling caused by the insoluble simoncollite, which is the antibacterial ingredient, when used in cosmetics and the like, and also makes it difficult for white residue to remain on the skin after application, resulting in a smooth feel in use and a cosmetically preferable appearance even after use. In this specification, nanoparticles refer to the 50% cumulative particle diameter (D) from the small particle side in the volume-based particle diameter distribution as determined by laser diffraction scattering method. 50 ) refers to particulate matter that is 1 nm or more and less than 800 nm.
[0011] The antibacterial agent of the present invention is also characterized in that Simoncolite has a 50% cumulative particle diameter (D 50 It is also preferable that the diameter of the simonkolite is 250 nm or less. 50 By making the nanoparticles 250 nm or less in size, when this antibacterial agent is blended into cosmetics, the rough feeling caused by Simoncolite is eliminated and the white residue on the skin after application is less likely to occur, resulting in a smooth feel in use and a cosmetically pleasing appearance even after use.
[0012] The deodorant cosmetic of the present invention also contains the antibacterial agent described above, which inhibits the activity and proliferation of microorganisms belonging to the genera Corynebacterium, Moraxella, and Malassezia, which cause body odor, scalp odor, and damp odor, thereby providing a deodorant cosmetic that can inhibit the generation of unpleasant odors such as body odor, scalp odor, and damp odor, thereby reducing these unpleasant odors.
[0013] The scalp care cosmetic of the present invention also contains the antibacterial agent described above, which has an antibacterial effect against fungi of the genus Malassezia, and thus can suppress scalp odor, inflammation, dandruff, and itching, thereby maintaining a healthy scalp.
[0014] The antibacterial agent of the present invention is an antibacterial agent against at least one microorganism selected from the group consisting of Corynebacterium, Moraxella, Malassezia, Staphylococcus, Pseudomonas, Candida, and Aspergillus, and contains simoncolyte as an active ingredient. Simoncolyte has an antibacterial effect of inhibiting the growth of microorganisms belonging to the genera Corynebacterium, Moraxella, Malassezia, Staphylococcus, Pseudomonas, Candida, and Aspergillus. Therefore, it can be used as an antibacterial agent that inhibits the activity and growth of these microorganisms.
[0015] The antibacterial product of the present invention contains the above-mentioned antibacterial agent. By incorporating this antibacterial agent into various products, antibacterial products having antibacterial activity against the above-mentioned microorganisms can be easily obtained.
[0016] According to the present invention, it is possible to provide an antibacterial agent, a deodorant cosmetic, a scalp care cosmetic, and an antibacterial product having the following excellent effects: (1) Simoncolyte has an antibacterial effect of inhibiting the growth of normal skin bacteria of the genera Corynebacterium, Moraxella, and Malassezia, and therefore can inhibit the activity and growth of these microorganisms that cause body odor, scalp odor, and damp odor, as well as the microorganisms that cause scalp odor, scalp inflammation, dandruff, and itching. (2) Simoncolyte inhibits the activity and growth of microorganisms that cause body odor, scalp odor, and damp odor, as well as the microorganisms that cause scalp odor, scalp inflammation, dandruff, and itching, and therefore can be suitably used as a functional ingredient in a deodorant cosmetic or a scalp care cosmetic. (3) Simoncolite has antibacterial properties that inhibit the growth of microorganisms belonging to the genera Corynebacterium, Moraxella, Malassezia, Staphylococcus, Pseudomonas, Candida, and Aspergillus. Therefore, by incorporating Simoncolite into materials or articles to which antibacterial properties are to be imparted, antibacterial products can be easily obtained.
[0017] 10A is a graph showing the antibacterial effect of a paper product impregnated with Simoncollite in Example 4, and FIG. 10B is a graph showing the antibacterial effect of a fabric product impregnated with Simoncollite in Example 4.
[0018] The antibacterial agent, deodorant cosmetic, scalp care cosmetic and antibacterial product of the present invention will be described below.
[0019] Simoncolite, which is the antibacterial component in the antibacterial agent, deodorant cosmetic, scalp care cosmetic or antibacterial product of the present invention, is a compound containing Zn 5 (OH) 8 Cl 2 ・(H 2 O) nSimoncollite refers to a white crystalline powder of zinc hydroxide chloride hydrate, represented by the formula: Simoncollite is generally available in the market as an industrially produced powder by the method shown in the above-mentioned Patent Document 4, and Simoncollite manufactured by JFE Mineral Co., Ltd. is a suitable example, but Simoncollite obtained by other production methods or Simoncollite derived from natural minerals can also be used. Furthermore, the Simoncollite used may have the same or different crystal grain phases (heterogeneous phases), or may be a mixture thereof.
[0020] In the present invention, the "antibacterial" effect means the ability to inhibit the growth of the target microorganisms, as compared to a control to which the antibacterial agent of the present invention is not added. The antibacterial effect can be measured by a known antibacterial test method, as shown in the examples below.
[0021] The antibacterial targets of the antibacterial agent according to the present invention are at least microorganisms that cause body odor, scalp odor, and damp odor, such as Corynebacterium bacteria, Moraxella bacteria, or Malassezia fungi. The antibacterial agent according to the present invention has excellent antibacterial activity against normal skin bacteria that cause body odor, etc., and can therefore be used in cosmetics for suppressing body odor (i.e., deodorants) or scalp care cosmetics for suppressing scalp odor and preventing scalp dandruff and itching. Examples of Corynebacterium bacteria include, but are not limited to, Corynebacterium striatum, Corynebacterium jeikeium, and Corynebacterium genitalium. Furthermore, examples of the Moraxella bacterium include, but are not limited to, Moraxella osloensis, and examples of the Malassezia fungi include, but are not limited to, Malassezia furfur, Malassezia globosa, and Malassezia restricta.
[0022] Furthermore, the antibacterial targets of the antibacterial agent of the present invention include Staphylococcus bacteria, Pseudomonas bacteria, Candida fungi, and Aspergillus fungi, in addition to the aforementioned Corynebacterium bacteria, Moraxella bacteria, and Malassezia fungi. The antibacterial agent of the present invention has antibacterial activity against these microorganisms and can therefore be used as an antibacterial agent for inhibiting the growth of these microorganisms. By incorporating this antibacterial agent into various products, antibacterial products having antibacterial activity against the above-mentioned microorganisms can be easily obtained. Examples of Staphylococcus bacteria include, but are not limited to, Staphylococcus aureus (Staphylococcus aureus). Furthermore, the Pseudomonas bacteria include, but are not limited to, Pseudomonas aeruginosa. Furthermore, the Candida fungi include, for example, Candida albicans, and the Aspergillus fungi include, for example, Aspergillus brasiliensis.
[0023] The simoncolite contained in the antibacterial agent of the present invention is preferably in the form of nanoparticles, in order to reduce the rough feeling caused by simoncolite when applied to the skin or scalp and the white residue on the skin after application, particularly when blended as an antibacterial agent in a deodorant cosmetic or a scalp care cosmetic. In this specification, nanoparticles refer to particles having a 50% cumulative particle diameter (D 50 In the present invention, from the viewpoint of further eliminating the roughness and white skin residue caused by Simonkolite, Simonkolite is used in a particle form having a 50% cumulative particle diameter (D 50 ) is preferably 500 nm or less, and further, the 90% cumulative particle diameter (D 90 ) is more preferably nanoparticles having a diameter of 800 nm or less.
[0024] The amount of simoncolyte contained in the antibacterial agent of the present invention and added, blended, or administered to an antibacterial target can be appropriately determined depending on the desired antibacterial effect, the target of addition or administration, the method of use, etc. From the viewpoint of its action and effect, for example, it is preferably 0.005 w / v% or more, more preferably 0.01 w / v% or more, and even more preferably 0.05 w / v% or more against bacteria of the genus Corynebacterium and Moraxella. Furthermore, for example, it is preferably 0.01 w / v% or more, more preferably 0.025 w / v% or more, and even more preferably 0.05 w / v% or more against bacteria of the genus Staphylococcus and Pseudomonas. For example, it is preferably 0.05 w / v% or more, more preferably 0.075 w / v% or more, and even more preferably 0.1 w / v% or more against fungi of the genus Malassezia, Candida, and Aspergillus.
[0025] The antibacterial agent of the present invention can be in any dosage form, such as solid, powder, suspension, or foam. However, from the viewpoint of ease of handling, it is preferably a suspension (slurry) in which Simoncolite is dispersed in a dispersion medium. The dispersion medium may be water, a water-miscible organic solvent, or a combination thereof. Examples of water-miscible organic solvents include water-miscible organic solvents such as alcohols (e.g., ethanol and propanol), ethers (e.g., tetrahydrofuran), esters (e.g., methyl acetate), and ketones (e.g., acetone). However, from the viewpoint of safety, ethanol is preferably used.
[0026] Furthermore, when the antibacterial agent of the present invention is prepared as a suspension (slurry), it is preferable to incorporate a dispersant to prevent Simoncolite from coagulating and precipitating in the suspension, making it difficult to redisperse. Examples of dispersants include ethylene oxide polymers, ethylene oxide-propylene oxide copolymers, cellulose derivatives, and combinations thereof. Specifically, although not particularly limited, polyethylene glycol, polypropylene glycol, ethylene oxide-propylene oxide copolymers, hydroxypropyl cellulose, hydroxypropyl methylcellulose, and hydroxyethyl cellulose are preferred. Of these, hydroxypropyl cellulose, polyethylene glycol 6000, hydroxypropyl methylcellulose, or combinations thereof are more preferred from the viewpoint of further improving the dispersibility of Simoncolite in the suspension. The amount of dispersant incorporated in the suspension is preferably 0.05% to 10% by mass, more preferably 0.1% to 5% by mass, from the viewpoint of improving dispersibility.
[0027] Furthermore, various components other than the dispersion medium and dispersant can be blended into the antibacterial agent of the present invention, as long as the effects of the present invention are not impaired. Examples of such components include surfactants, alcohols, thickeners, preservatives, preservative aids, excipients, fragrances, and colorants.
[0028] Next, a method for producing the antibacterial agent of the present invention will be described. The antibacterial agent may be composed solely of simoncollite, but by mixing it with other materials that constitute the antibacterial agent, an antibacterial agent containing simoncollite can be obtained. For example, when producing an antibacterial agent in the form of a suspension (slurry), the antibacterial agent can be obtained by adding simoncollite and, if necessary, a dispersant to a dispersion medium such as water and dispersing the mixture.
[0029] In addition, when Simoncollite is used to produce antibacterial agents in the form of nanoparticle suspensions (slurries), the crystals of Simoncollite that are commonly available have an average particle diameter (D 50Since the particle size of Simoncolite is as large as about 10 μm, it is necessary to pulverize it to nano-level size. For the pulverization process, wet pulverization is used because it is excellent for pulverizing to nano-level size. This will be explained in detail below.
[0030] (Mixing step) First, Simoncollite and a dispersion medium are mixed to obtain a suspension. As the dispersion medium, as described above, water, a water-miscible organic solvent, or a combination thereof is used. In this mixing step, it is also preferable to add the above-mentioned dispersant to the suspension so that the dispersant is contained in the suspension. This is because a slurry with improved dispersibility can be obtained by adding a dispersant to a suspension containing Simoncollite and introducing the suspension into an atomization device to atomize the Simoncollite.
[0031] (Stirring Step) Next, the suspension obtained by mixing the Simonkollite and the dispersion medium is stirred. This stirring step allows the Simonkollite in the suspension to become accustomed to the dispersion medium, thereby reducing the likelihood of clogging the flow channels and nozzles in the micronization device during the micronization process, facilitating the micronization of the Simonkollite. The stirring means is not particularly limited as long as it can stir the entire suspension, but for example, a propeller-type stirrer or a magnetic stirrer can be used. The stirring time is preferably 1 hour or more, more preferably 2 hours or more, in order to allow the Simonkollite to become accustomed to the dispersion medium. It is also preferable to add the above-mentioned dispersant to the suspension during this stirring step so that the dispersant is contained in the suspension. When a water-miscible organic solvent such as ethanol is selected as the dispersion medium, the micronization process can be performed without the stirring step.
[0032] (Micronization Treatment Step) In the micronization treatment step, the suspension is introduced into a micronization device to micronize the Simoncollite in the suspension to nano-level size. As the micronization device, a wet micronization device is used, for example, a high-pressure homogenizer type wet micronization device or a bead mill type wet micronization device. The micronization treatment is carried out until the Simoncollite reaches a 50% cumulative particle diameter (D 50 ) is preferably 500 nm or less, and further, the 90% cumulative particle diameter (D90 ) to nanoparticles of 800 nm or less. In the case of a high-pressure homogenizer-type device, the micronization treatment conditions include the chamber used, pressure, nozzle diameter, number of passes, and treatment time, while in the case of a bead mill-type device, the micronization treatment conditions include the material of the beads used, bead diameter, and treatment time. These treatment conditions can be appropriately set based on the specifications of the device used and the desired level of micronization. Furthermore, in this micronization treatment step, a preliminary grinding treatment may be performed in advance to roughly grind the Simonkolite in the suspension, followed by a further micronization treatment to further refine it. The preliminary grinding treatment can be performed using the same device as the above-mentioned micronization device. The Simonkolite in the suspension is roughly ground by reducing the treatment time, number of passes, pressure, etc., compared to the conditions for the main micronization treatment, or by increasing the nozzle diameter of the chamber used or the diameter of the beads used. This allows the 50% cumulative particle diameter (D 50 ) and it is possible to stably obtain Simoncolite with a uniform nanoparticle size.
[0033] (Solvent distillation step) In addition, when a water-miscible organic solvent such as ethanol is selected as the dispersion medium, the water-miscible organic solvent contained in the water-miscible organic solvent slurry after the micronization treatment is distilled off, and the dispersion medium can be replaced with another dispersion medium, specifically water. Specifically, as an example, water is added to the ethanol slurry after the micronization treatment, and the mixture is placed in a reduced pressure environment and subjected to steam distillation. As a result, the ethanol is distilled off, and a water slurry in which the micronized simoncolite is dispersed can be obtained.
[0034] The slurry obtained by the above-mentioned pulverization treatment step or distillation step can be used as an antibacterial agent as it is, or can be blended as an antibacterial agent in deodorant cosmetics or scalp care cosmetics. Furthermore, the slurry can be concentrated to form a concentrated liquid, or dried to form a fine powder, and these can also be used as antibacterial agents.
[0035] As described above, the antibacterial agent of the present invention has excellent antibacterial activity against normal skin bacteria that cause body odor, etc., and therefore can be incorporated into cosmetics for suppressing body odor (i.e., deodorants) or scalp care cosmetics for suppressing scalp odor and preventing scalp dandruff and itching.
[0036] The amount of simoncolyte blended as an antibacterial ingredient in the deodorant cosmetic or scalp care cosmetic according to the present invention can be appropriately set depending on the target antibacterial effect, formulation, dosage form, method of use, number of uses, etc., but from the viewpoint of its action and effect, for example, it is preferably 0.005 w / v% to 20 w / v%, more preferably 0.01 w / v% to 10 w / v%, and even more preferably 0.05 w / v% to 5 w / v% against bacteria of the genus Corynebacterium and Moraxella. Furthermore, for example, it is preferably 0.01 w / v% to 20 w / v%, more preferably 0.025 w / v% to 10 w / v%, and even more preferably 0.05 w / v% to 5 w / v% against bacteria of the genus Staphylococcus and Pseudomonas. For fungi of the genus Malassezia, the genus Candida, and the genus Aspergillus, the concentration is preferably 0.05 w / v% to 20 w / v%, more preferably 0.075 w / v% to 10 w / v%, and even more preferably 0.1 w / v% to 5 w / v%, for example.
[0037] The deodorant cosmetic or scalp care cosmetic of the present invention can be applied to various topical preparation dosage forms by conventionally used methods as dosage forms typically applied to the scalp or skin, and examples include liquids such as slurries and low-viscosity liquids, gels, emulsions, pastes, creams, solids, powders, foams, ointments, etc. The deodorant cosmetic or scalp care cosmetic of the present invention can be applied to any of cosmetics, quasi-drugs, and pharmaceuticals. Specific products include, but are not limited to, soaps, cleansers, body lotions, emulsions, gels, creams, and talcum powders, skin wipes, stick cosmetics, perfumes, bath additives, scalp lotions, shampoos, conditioners, treatments, hair tonics, and hair styling products.
[0038] The deodorant cosmetic or scalp care cosmetic of the present invention can also contain various ingredients commonly used in cosmetics and topical preparations, provided that the effects of the present invention are not impaired. Examples of such ingredients include antiperspirants, deodorants, alcohols, surfactants, thickeners, vitamins, amino acids, moisturizers, preservatives, preservative aids, fragrances, and colorants. Antibacterial ingredients other than simoncolite can also be added. Examples of other antibacterial ingredients include phenoxyethanol, isopropylmethylphenol, and benzalkonium chloride.
[0039] Furthermore, as described above, the antibacterial agent of the present invention has antibacterial activity against bacteria of the genus Corynebacterium, bacteria of the genus Moraxella, and fungi of the genus Malassezia, as well as bacteria of the genus Staphylococcus, bacteria of the genus Pseudomonas, fungi of the genus Candida, and fungi of the genus Aspergillus. Therefore, by incorporating this antibacterial agent into various products, antibacterial products having antibacterial activity against the above-mentioned microorganisms can be easily obtained.
[0040] Examples of antibacterial products include paper and cloth. Antibacterial products can be produced by incorporating Simoncollite into products to be imparted with antibacterial properties by methods such as addition, impregnation, spraying, or application. For example, paper or cloth products with antibacterial properties can be obtained by immersing paper or cloth in an antibacterial agent consisting of a Simoncollite-containing slurry and drying it. Note that the term "cloth" includes not only woven fabrics but also nonwoven fabrics. As an example, the Simoncollite concentration of the Simoncollite-containing slurry impregnating the target antibacterial product can be appropriately set depending on the target antibacterial effect, the control product, etc., but is preferably 0.05 w / v% or more, and more preferably 0.1 w / v% or more.
[0041] Next, the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.
[0042] Example 1 1. Examination of the Antibacterial Activity of Simoncolyte (1) In this example, the antibacterial activity of Simoncolyte against Corynebacterium bacteria, Moraxella bacteria, and Malassezia fungi, which are microorganisms that cause body odor, scalp odor, and damp odor, was examined.
[0043] [Preparation of Simoncollite Nanoparticle Water Slurry Sample a] 440 g of Simoncollite (JFE Mineral Corporation, lot number: S1J201) was added to 1,672 g of ion-exchanged water to obtain a suspension. This suspension was stirred for 3 hours at a stirring speed of 500 to 1,000 rpm using a propeller-type stirrer and then allowed to stand overnight. This Simoncollite water slurry (aqueous suspension) was introduced into a high-pressure homogenizer-type wet atomization device (Starburst Lab, manufactured by Sugino Machine Corporation) and subjected to a preliminary micronization treatment under the following conditions: chamber used: slit-type chamber, chamber nozzle diameter: 0.16 mm, pressure: 150 MPa, number of passes: 5 passes. After the preliminary micronization treatment, the chamber of the wet micronization device was changed to another slit-type chamber (model number: ESC-101, chamber nozzle diameter: smaller than 0.16 mm), and micronization treatment was carried out under conditions of a pressure of 150 MPa and a number of passes of 50 passes, to obtain an aqueous slurry sample a of Simonkollite nanoparticles (Simonkollite concentration: 21 w / w%) in which the Simonkollite particles had been micronized to nano-level sizes. When the particle size distribution of Simonkollite in this aqueous slurry was measured, the 50% cumulative particle size (D 50 ) is 160 nm, and the 90% cumulative particle diameter (D 90 ) was 478 nm.
[0044] The particle size distribution of Simoncollite was measured using a laser diffraction scattering particle size distribution analyzer (model number: Partica LA-960, manufactured by Horiba, Ltd.) with the refractive index parameter of Simoncollite crystals set to 1.700-0.000i and ion-exchanged water in which Simoncollite was dispersed as the dispersion medium. From the obtained particle size distribution, the 50% cumulative particle size (D 50 ) and 90% cumulative particle diameter (D 90 ) was sought.
[0045] [Antibacterial Activity Evaluation Test] An antibacterial activity evaluation test of Simoncolyte was carried out using the test microorganisms and culture media shown below. <Test microorganisms> Corynebacterium striatum NBRC15291 (Corynebacterium striatum) Corynebacterium jeikeium JCM9384 (Corynebacterium jeikeium) Moraxella osloensis NBRC113899 (Moraxella osloensis) Malassezia furfur NBRC10987 (Malassezia furfur) <Culture medium> Culture medium A: Mueller-Hinton agar medium {Muller-Hinton II broth ion preparation (product of Becton Dickinson) and 1.5% agar, powder (product of Fujifilm Wako Pure Chemical Industries, Ltd.)} Medium B: Columbia agar medium supplemented with 5% defibrinated sheep blood (Difco Columbia Blood Agar Base Medium (Becton Dickinson) and 5% defibrinated sheep blood (Cosmo Bio)) Medium C: Chromoagar Malassezia / Candida Live Medium (Kanto Chemical)
[0046] The test microorganisms stored at -70°C were inoculated onto agar medium and cultured at 32°C for 24 to 72 hours to restore them. Moraxella was restored using medium A (Mueller-Hinton agar medium), both Corynebacterium species were restored using medium B (Columbia agar medium supplemented with 5% defibrinated sheep blood), and Malassezia was restored using medium C (Chromoagar Malassezia / Candida live medium). Colonies of the grown test microorganisms were scraped off and suspended in sterilized saline (Otsuka Pharmaceutical Factory Co., Ltd. product) to a concentration equivalent to McFarland turbidity No. 0.5 (approximately 10 8 Each bacterial solution was serially diluted 10-fold with sterile physiological saline to prepare an inoculum.
[0047] On the other hand, when preparing Medium A and Medium B for the antibacterial activity evaluation test, each medium was prepared, heat-sterilized, and then cooled to approximately 60°C. A predetermined amount of the above-prepared Simoncollite nanoparticle aqueous slurry sample a (specific gravity: 1.20) was added to each medium and mixed to create agar plate media with Simoncollite nanoparticle concentrations of 0.025 w / v% and 0.050 w / v%. Furthermore, when preparing Medium C for the antibacterial activity evaluation test, since the medium was already sold as an agar plate medium, the above-prepared Simoncollite nanoparticle aqueous slurry sample a was appropriately diluted with sterilized water to create a diluted slurry, which was then applied to an agar medium to create Medium C with Simoncollite nanoparticle concentrations of 0.13 w / v% and 0.25 w / v%. For comparison, a medium containing no Simoncollite nanoparticles (0 w / v%) was also prepared.
[0048] Approximately 0.1 mL of each of the serially diluted inoculum solutions prepared as described above was smeared on a medium for the antibacterial activity evaluation test, and the medium was cultured at 32°C for 24 to 72 hours. As shown in Table 1 below, for Corynebacterium striatum, a bacterium of the genus Corynebacterium, the restoration medium was medium B (Columbia agar medium supplemented with 5% defibrinated sheep blood), but the antibacterial activity evaluation test was performed using both medium A (Mueller-Hinton agar medium) and medium B. After culture, the viable cell count was counted on the medium containing Simoncolyte nanoparticles, which had been smeared with the inoculum solution at a dilution ratio that resulted in tens to hundreds of viable cells in the medium without Simoncolyte nanoparticles. The results are shown in Table 1 below.
[0049]
[0050] These results demonstrate that Simoncolyte has excellent antibacterial activity against microorganisms of the genera Moraxella, Corynebacterium, and Malassezia. Simoncolyte can inhibit the growth of these odorous bacteria at a concentration of at least 0.025 w / v%, and can inhibit the growth of fungi of the genus Malassezia at a concentration of at least 0.13 w / v%.
[0051] [Example 2] 2. Examination of the Antibacterial Activity of Simoncollite (2) In this example, based on the results of Example 1 described above, the minimum inhibitory concentration (MIC) of Simoncollite against bacteria of the genus Corynebacterium, the genus Moraxella, and the genus Staphylococcus was measured by the broth microdilution method. Note that Staphylococcus aureus, used as the Staphylococcus bacterium, is also a type of normal skin flora. Furthermore, in this example, various samples with different Simoncollite particle sizes, samples containing a dispersant, and samples using Simoncollite containing a heterophase were prepared and tested to evaluate the antibacterial activity.
[0052] [Preparation of Simoncollite Water Slurry Sample b] 16 g of purified water was added to 4 g of Simoncollite (JFE Mineral Corporation, lot number: S1J201), and the mixture was stirred for 5 minutes using a vortex mixer to obtain Simoncollite water slurry sample b (Simoncollite concentration: 20 w / w%). When the particle size distribution of Simoncollite in this water slurry was measured, the 50% cumulative particle size (D 50 ) is 13700 nm (13.7 μm), 90% cumulative particle diameter (D 90 ) was 144,000 nm (144 μm).
[0053] [Preparation of Dispersant-Containing Water Slurry Sample c of Simoncollite Nanoparticles] 56 g of polyethylene glycol 6000 (PEG-6000P, product of Sanyo Chemical Industries, Ltd.) as a dispersant was dissolved in 1043 g of ion-exchanged water, and 280 g of Simoncollite (JFE Mineral Co., Ltd., lot number: S1J201) was added to this solution to obtain a suspension. This suspension was stirred for 2 hours at a stirring speed of 500 to 1000 rpm using a propeller stirrer and then allowed to stand overnight. This Simoncollite aqueous slurry (aqueous suspension) was treated under the same conditions and methods as the preliminary micronization and micronization treatments for the aqueous slurry sample a prepared in Example 1, except that the number of passes in the micronization treatment was changed to 40. This gave a PEG-containing water slurry sample c of Simoncollite nanoparticles in which the Simoncollite particles had been micronized to nano-level sizes (Simoncollite concentration: 20.3 w / w%). When the particle size distribution of the simoncollite in this water slurry was measured, the 50% cumulative particle size (D 50 ) is 206 nm, and the 90% cumulative particle diameter (D 90 ) was 444 nm.
[0054] [Preparation of a dispersant-containing aqueous slurry sample d of Simoncollite nanoparticles] 34.8 g of hydroxypropyl cellulose (HPC-L, Nippon Soda Co., Ltd.) as a dispersant was dissolved in 1531.2 g of ion-exchanged water, and 174 g of Simoncollite (JFE Mineral Corporation, lot number: S1J201) was added to this solution to obtain a suspension. This suspension was stirred for 2 hours at a stirring speed of 500 to 1000 rpm using a propeller-type stirrer and then allowed to stand overnight. This aqueous slurry (aqueous suspension) of Simoncollite was treated under the same conditions and methods as the preliminary micronization and micronization treatments of the aqueous slurry sample a prepared in Example 1 to obtain a HPC-containing slurry sample d of Simoncollite nanoparticles (Simoncollite concentration: 10 w / w%) in which the Simoncollite particles had been micronized to nano-level sizes. Measurement of the particle size distribution of Simoncollite in this aqueous slurry revealed a 50% cumulative particle size (D 50 ) is 152 nm, and the 90% cumulative particle diameter (D 90 ) was 730 nm.
[0055] [Preparation of Water Slurry Sample e Containing Dispersant for Heterophase-Containing Simoncollite Nanoparticles] Japanese Pharmacopoeia 40 g of polyethylene glycol 6000 (PEG-6000P, product of Sanyo Chemical Industries, Ltd.) as a dispersant was dissolved in 1600 g of absolute ethanol, and 400 g of Simoncollite (JFE Mineral Corporation, heterophase-containing preparation) was added to this solution and stirred to obtain a suspension. This suspension was introduced into a bead mill-type wet micronization device (MAX Nano Getter HFM06, product of Ashizawa Finetech Co., Ltd.) and pulverized for 40 minutes using 0.05 mm diameter PSZ beads. 485 g of absolute ethanol was then added and pulverized for an additional 10 minutes to perform a micronization treatment. This resulted in an ethanol slurry with a Simoncollite concentration of 15.8 w / w%. Measurement of the particle size distribution of Simoncollite in this ethanol slurry revealed a 50% cumulative particle size (D 50 ) is 136 nm, and the 90% cumulative particle diameter (D 90 39 g of purified water was added to 25 g of this ethanol slurry, and the ethanol was removed by steam distillation under reduced pressure. Purified water was then added to bring the total mass to 39 g, yielding a water slurry sample e (Simonkollite concentration: 10 w / w%) of heterogeneous simonkollite nanoparticles containing a dispersant.
[0056] [Measurement of Minimum Inhibitory Concentration (MIC)] MIC was measured using the test microorganisms and culture media shown below. MIC was measured with reference to Chemotherapy, "MIC Measurement Method by Broth Microdilution (Broth Microdilution Method)," Vol. 38, No. 1, pp. 103-105. <Test microorganisms> Staphylococcus aureus NCTC10788 (Staphylococcus aureus) Corynebacterium striatum NBRC15291 (Corynebacterium striatum) Corynebacterium jeikeium JCM9384 (Corynebacterium jeikeium) Moraxella osloensis NBRC113899 (Moraxella osloensis) <Culture medium> Restoration medium A: Mueller-Hinton agar medium {Muller-Hinton II broth ion preparation (product of Becton Dickinson) and 1.5% agar, powder (product of Fujifilm Wako Pure Chemical Industries, Ltd.)} Restoration medium B: Columbia agar medium supplemented with 5% defibrinated sheep blood {Difco Columbia Blood Agar Base Medium (product of Becton Dickinson) and 5% defibrinated sheep blood (product of Cosmo Bio)} Test medium D: Mueller-Hinton liquid medium {Kyokuto Mueller-Hinton Broth (product of Kyokuto Pharmaceutical Industries)} Test medium E: Mueller-Hinton liquid medium supplemented with horse lysed blood {Kyokuto Mueller-Hinton Broth supplemented with horse lysed blood (product of Kyokuto Pharmaceutical Industries)}
[0057] Test microorganisms stored at -70°C were inoculated into a revival medium and cultured at 32°C for 18 to 48 hours to revival. Staphylococcus aureus and Moraxella were revivalized using medium A (Mueller-Hinton agar medium), and both Corynebacterium species were revivalized using medium B (Columbia agar medium supplemented with 5% defibrinated sheep blood). Colonies of the grown test microorganisms were scraped off and suspended in sterilized saline (Otsuka Pharmaceutical Factory Co., Ltd. product) to a concentration equivalent to McFarland turbidity No. 0.5 (approximately 10 8 Each bacterial solution was diluted 10-fold with sterile saline (approximately 10 CFU / mL). 7 CFU / mL) was used as the inoculum.
[0058] To prepare test medium D and test medium E for MIC measurement, the simonkolyte water slurry samples a to e prepared in Example 1 and above were prepared with purified water to a simonkolyte concentration of 10 wt / w% (specific gravity 1.06), and then diluted approximately 10-fold with each medium to prepare a medium (simonkolyte concentration: 11,000 μg / mL). These were then sequentially diluted with medium to prepare test medium D and test medium E in a 2-fold dilution series. For comparison, test medium containing no simonkolyte (simonkolyte concentration: 0 μg / mL) was also prepared.
[0059] For the test, a U-bottom microplate (IWAKI Microplate 96-well with Lid, manufactured by AGC Technoglass) was used. Approximately 0.1 mL of test medium containing 11 μg / mL to 11,000 μg / mL of Simoncolyte and test medium without Simoncolyte were added per well in a two-fold dilution series. Approximately 0.005 mL of the inoculum solution prepared as described above was inoculated per well and cultured at 32°C for 18 to 48 hours. As shown in Table 2 below, Staphylococcus aureus was tested using Test Medium D, and Corynebacterium jeikeium was tested using Test Medium E, among the Corynebacterium species. Corynebacterium striatum and Moraxella osloensis were tested using both Test Medium D and Test Medium E. After the incubation, the growth of the bacteria in the control medium containing no simonkolyte was confirmed, and the MIC was determined as the lowest simonkolyte concentration in the well where no bacterial growth was visible to the naked eye. Here, since the simonkolyte itself causes turbidity when the amount of simonkolyte contained in the test medium increases, wells were set up to receive only the test medium but no inoculum, and it was confirmed that the turbidity caused by simonkolyte did not affect the determination of the MIC of simonkolyte.
[0060] Furthermore, the antibacterial effect was evaluated based on the determined MIC according to the following criteria: "+++" (excellent antibacterial effect): MIC less than 200 μg / mL. "++" (antibacterial effect): MIC 200 μg / mL or more and less than 1000 μg / mL. "+" (slight antibacterial effect): MIC 1000 μg / mL or more and less than 5000 μg / mL. "-" (no antibacterial effect): MIC 5000 μg / mL or more. The results are shown in Table 2 below. The notation in parentheses in each column is the evaluation result of the antibacterial effect.
[0061]
[0062] These results demonstrate that Simoncollite has excellent antibacterial effects against Staphylococcus aureus, Corynebacterium sp., and Moraxella sp. While no significant differences in antibacterial effects were observed among the added samples a to e, the antibacterial effect against Staphylococcus aureus was improved by forming Simoncollite into nanoparticles. Furthermore, even when a dispersant that improves the dispersibility of Simoncollite was added, it was found that the same level of antibacterial effect was maintained compared to samples without a dispersant. Furthermore, no difference in the excellent antibacterial effect was observed even when Simoncollite contained heterophase bodies.
[0063] Although not shown in Table 2, sample solutions containing 2% by mass of PEG 6000, which was blended into samples c and e as a dispersant, and HPC (hydroxypropyl cellulose), which was blended into sample d, were also prepared and diluted 10-fold with test medium, and the MIC was measured using a 2-fold dilution series. However, no antibacterial activity was observed in PEG 6000 or HPC.
[0064] Comparative Example 1 3. Study of the Antibacterial Activity of Simoncollite Water Slurry Supernatant Simoncollite is insoluble in water, but it is believed that a very small amount of zinc ions dissolves in water. Therefore, in this comparative example, to investigate whether the zinc ions dissolved in the Simoncollite water slurry contribute to Simoncollite's antibacterial effect, a supernatant of the Simoncollite water slurry was prepared, and the supernatant was serially diluted to measure the MIC. Specifically, each of Simoncollite water slurry samples a to c obtained in Examples 1 and 2 was prepared with purified water to a Simoncollite concentration of 10 wt% and then centrifuged at 1830 × g for 30 minutes (Model No. AX-521, manufactured by Tomy Seiko Co., Ltd.). The supernatant was collected and filtered through a membrane filter with a pore size of 0.22 μm (Millex (registered trademark)-GV filter, product of Merck), and a colorless, clear filtrate was obtained as the supernatant of aqueous slurry samples a to c with a simoncolite concentration of 10 w / w%.
[0065] The supernatants of aqueous slurry samples a to c, each containing a 10 wt% simonkolyte concentration, obtained as described above, were subjected to minimum inhibitory concentration measurements using the same test microorganisms and media as in Example 2. To prepare test medium D and test medium E for MIC measurements, the supernatants of aqueous slurry samples a to c, each containing a 10 wt% simonkolyte concentration, were diluted with each medium to create media containing aqueous slurry supernatants with a simonkolyte concentration equivalent to 11,000 μg / mL. These were then serially diluted with the medium to prepare test medium D and test medium E in a two-fold dilution series. For comparison, test media containing no supernatant were also prepared.
[0066] The test was performed using a U-bottom microplate. Approximately 0.1 mL of test medium containing aqueous slurry supernatant corresponding to Simonkolyte concentrations of 11 μg / mL to 11,000 μg / mL and test medium without aqueous slurry supernatant were added per well in a two-fold dilution series. Approximately 0.005 mL of an inoculum prepared as in Example 2 was inoculated per well and cultured at 32°C for 18 to 48 hours. After culture, bacterial growth was confirmed in the control medium without aqueous slurry supernatant. The MIC was determined as the minimum Simonkolyte concentration of the aqueous slurry corresponding to the aqueous slurry supernatant in the well where bacterial growth was not visually observed. In other words, the MIC in this comparative example indicates the Simonkolyte concentration of the aqueous slurry from which the supernatant was obtained. Furthermore, the antibacterial effect was evaluated based on the determined MIC in the same manner as in Example 2. The results are shown in Table 3 below.
[0067]
[0068] These results revealed that the supernatant of Simoncollite's aqueous slurry did not contain enough zinc ions to have an antibacterial effect against the microorganisms tested, and that it had no antibacterial effect at all. This made it clear that the excellent antibacterial effect of the Simoncollite aqueous slurry samples shown in Examples 1 and 2 was not due to the zinc ions liberated in the aqueous slurry, but was due to the Simoncollite itself. In other words, the test results of Comparative Example 1 and Example 2 showed that "Simoncollite itself" has an antibacterial effect.
[0069] [Example 3] 4. Examination of the Antibacterial Action of Simoncollite (3) In this example, the antibacterial activity of Simoncollite was examined against microbial species other than those for which the antibacterial effect has been examined so far: Pseudomonas aeruginosa, Candida albicans, Aspergillus brasiliensis, and Staphylococcus aureus, the antibacterial effect of which was also examined in Example 2. Specifically, the test was conducted as follows. The aqueous slurry sample a of Simoncollite prepared in Example 1 above was diluted with sterilized water to prepare a slurry with a Simoncollite concentration of 0.1 w / v %. This was then filled into a container, and the microorganisms shown in Table 4 below were inoculated into the container so as to achieve the viable cell count shown in Table 4, and the mixture was mixed uniformly.
[0070]
[0071] These samples were stored in the dark at 22.5±2.5°C for 28 days, and the viable cell count was measured on days 0, 14, and 28. The results on day 28 were used for evaluation, and the percentage of the number of bacteria at the start of the test was calculated, with 100 as the number of bacteria. The evaluation criteria were in accordance with the evaluation criteria (Category IB) specified in the Japanese Pharmacopoeia. Note that Candida is an important indicator reflecting antibacterial activity, and the same criteria as for bacteria were applied to it. The notation method for the viable cell count measurement results is shown in Table 5, and the viable cell count measurement results and evaluation results are shown in Table 6.
[0072]
[0073]
[0074] These results reveal that Simoncolite has antibacterial effects against Pseudomonas bacteria, Staphylococcus bacteria, Candida fungi, and Aspergillus fungi, and that it has antibacterial effects not only against the bacteria that have been studied so far, but also against fungi such as Candida and Aspergillus.
[0075] [Example 4] 5. Antibacterial Effect of Products Containing Simoncollite In this example, the antibacterial effect of paper and cloth impregnated with Simoncollite was investigated. Filter paper (No. 5B, manufactured by Advantec Toyo Co., Ltd.) and one-dollar bills were selected as the "paper" to be processed to contain Simoncollite. The paper was cut into 4 cm squares and then autoclaved at 121°C for 20 minutes. Furthermore, cellulose nonwoven fabric (BEMCOT (registered trademark) M-3II: manufactured by Asahi Kasei Corporation) was selected as the "cloth" to be processed to contain Simoncollite. The cloth was cut to approximately 0.4 g and then autoclaved at 121°C for 20 minutes.
[0076] The water slurry sample a of Simoncollite prepared in Example 1 above was diluted with physiological saline to prepare test solutions with Simoncollite concentrations of 0.05 w / v%, 0.13 w / v%, and 0.5 w / v%, respectively. Sterilized pieces of paper and cloth were immersed in these test solutions and physiological saline for at least one minute, then removed, and the excess liquid was removed and the pieces were air-dried on a clean bench for approximately 30 minutes. Of the paper pieces, only the 0.5 w / v% test solution was tested for one-dollar bills.
[0077] On the other hand, Staphylococcus aureus (Staphylococcus aureus NCTC10788 / ATCC6538: BIOBALL (registered trademark) product of bioMérieux) was used as the inoculum. 8 1 mL of the rehydration solution provided with the kit was added to the frozen cells, and after thorough stirring, the cells were diluted with nutrient broth (Solabia Biokar Diagnostics) to a concentration of approximately 2 × 10 5 To confirm the viable cell count, the mixture was diluted appropriately and spread on Mueller-Hinton agar medium (Mueller-Hinton II Broth Ion Preparation (Becton Dickinson) and 1.5% agar powder (Fujifilm Wako Pure Chemical Industries)), and cultured at 1-3 x 10 5 It was confirmed that the CFU / mL range was within the range of 2.7 × 10 5 CFU / mL).
[0078] After air-drying, the paper and cloth pieces were stained with Staphylococcus aureus (2.7 x 10 5CFU / mL) inoculum: 0.2 mL was inoculated into multiple locations using a micropipette and then placed in a 50 mL conical tube. For the 0-hour sample immediately after inoculation, 20 mL of saline was immediately added and vigorously stirred to perform washout. 1 mL of the washout solution was added to Mueller-Hinton liquid medium for serial dilutions, and 1 mL of each serial dilution was poured onto soft agar medium (1.2% Mueller-Hinton agar medium, ion-prepared, sterilized and stored in a water bath at 40-50 °C). After layering onto Mueller-Hinton agar medium, the medium solidified, and the mixture was placed in an incubator (35 °C) for overnight incubation, and the number of grown bacteria was measured. On the other hand, for a sample after 20 hours of incubation, a piece of paper or cloth inoculated with Staphylococcus aureus was placed in a 50 mL conical tube, the opening of the tube was covered with paraffin film, and the tube was placed in an incubator at 35 °C for approximately 20 hours. After 20 hours, 20 mL of physiological saline was added and vigorously stirred to wash out the bacteria. The number of bacteria that had grown in this washout solution was measured by the pour plate culture method using the same materials and method as for the washout solution of the 0-hour sample. The test on filter paper and nonwoven fabric was the average of three cases, and the test on banknotes was the average of two cases. It was also confirmed that the difference in the values of the individual test groups was within 10 times.
[0079] The antibacterial effect was evaluated based on the measured viable cell counts and the following criteria. The "number of grown bacteria" is the number of bacteria obtained by subtracting the number of viable bacteria immediately after inoculation from the number of viable bacteria 20 hours after incubation, expressed as a common logarithm, as shown in Table 7 below. "◎" (excellent antibacterial effect): (common logarithm of the number of grown bacteria in the control group) - (average common logarithm of the number of grown bacteria in the test group) is 3 or more. "○" (antibacterial effect): (common logarithm of the number of grown bacteria in the control group) - (average common logarithm of the number of grown bacteria in the test group) is 2 or more but less than 3. "×" (no antibacterial effect): (common logarithm of the number of grown bacteria in the control group) - (average common logarithm of the number of grown bacteria in the test group) is less than 2. The results are shown in Table 7 below and FIG. 1.
[0080]
[0081] These results show that paper and fabric products with antibacterial properties can be obtained simply by soaking paper or fabric in a Simoncollite-containing slurry and drying it. Furthermore, even a low Simoncollite concentration of 0.05 w / v% in the impregnation solution imparted antibacterial effects (especially to fabric products), and the higher the Simoncollite concentration in the impregnation solution, the higher the antibacterial activity (especially to paper products). This demonstrates that antibacterial products can be easily obtained by incorporating (adhering) Simoncollite into paper and fabric products.
[0082] [Example 5] 6. Preparation of deodorant cosmetics Aqueous slurry sample a of simoncollite nanoparticles obtained in Example 1: 10.0% by mass, dipropylene glycol: 10% by mass, propylene glycol-10 methyl glucose: 2% by mass, butylene glycol: 20% by mass, bisglyceryl ascorbate: 1% by mass, 1,2-hexanediol: 1% by mass, glycine: 1% by mass, arginine: 1% by mass, glycerin: 0.5% by mass, hydroxyethyl cellulose: 0.5% by mass, dextran: 0.5% by mass, hydroxypropyl cyclodextrin: 2% by mass, yuzu fruit extract: 0.2% by mass, rehmannia root extract: 0.2% by mass, acetyl tetrapeptide-3: 0.2% by mass, red clover flower extract: 0.2% by mass, biotin: 0.2% by mass, riboflavin: 0.2% by mass, pyridoxine HCl: 0.2% by mass, diglycyrrhizinate Potassium: 0.2% by mass, sodium acetyl hyaluronate: 0.2% by mass, hydrolyzed elastin: 0.2% by mass, cholesterol: 0.2% by mass, PEG-40 hydrogenated castor oil: 0.2% by mass, polyglyceryl-10 myristate: 0.2% by mass, diphenyl dimethicone: 0.2% by mass, bergamot fruit oil: 0.05% by mass, boswellia oil: 0.05% by mass, lime juice: 0.05% by mass, Orange juice: 0.05% by mass, lemon juice: 0.05% by mass, hawthorn extract: 0.05% by mass, jujube fruit extract: 0.05% by mass, grapefruit fruit extract: 0.05% by mass, apple fruit extract: 0.05% by mass, and the remainder water were mixed to obtain a slightly viscous, slightly peach-white suspension-like deodorant cosmetic with a refreshing scent (content of simoncolite in the lotion: 2.0% by mass).
[0083] [Example 6] 7. Preparation of a cosmetic (shampoo) for preventing and improving scalp dandruff, itching, or scalp odor Aqueous slurry sample a of simoncolite nanoparticles obtained in Example 1: 0.50% by mass, sodium lauroylmethylalanine: 2% by mass, cocamidopropyl betaine: 2% by mass, cocamidomethyl MEA: 0.5% by mass, glycerin: 10% by mass, 1,2-hexanediol: 0.5% by mass, citric acid: 1% by mass, lauryl glycoside: 2% by mass, bergamot fruit oil: 0.05% by mass, polyquaternium-1000: 0.05% by mass, hydroxybenzoates ... Oternium-10: 0.02% by mass, menthol: 0.2% by mass, hydroxypropyl cyclodextrin: 1.3% by mass, arginine: 1% by mass, dipropylene glycol: 10% by mass, kaolin: 2% by mass, glycine: 1% by mass, glycyrrhizinic acid 2K: 0.8% by mass, panthenol: 1% by mass, biotin: 0.1% by mass, riboflavin: 0.1% by mass, hydrolyzed keratin: 0.1% by mass, Hydrolyzed sodium hyaluronate: % by mass, shea butter: 2% by mass, hydrogenated lecithin: 0.2% by mass, 1,3-butylene glycol: 20% by mass, triethanolamine cocoyl glutamate: 3% by mass, hydrolyzed keratin (wool): 0.2% by mass, sodium lactate: 1% by mass, phytosterol: 0.1% by mass, N-stearoyldihydrosphingosine: 0.1% by mass, sodium lauraminopropionate: 2% by mass, sodium citrate: 0.1% by mass, sodium chloride: 1% by mass, persimmon tannin: 0.2% by mass, lactic acid: 0.1% by mass, pentylene glycol: 0.5% by mass, tocopherol: 0.1% by mass, tannic acid: 0.5% by mass, and the remainder water were mixed to obtain a slightly viscous, well-foaming scalp cleansing shampoo (content of the component as simoncolite in the shampoo: 0.1% by mass).
[0084] The present invention is not limited to the above-described embodiments or examples, and its technical scope also includes various modified designs within the scope that does not deviate from the gist of the invention described in the claims.
[0085] The antibacterial agent, deodorant cosmetic, cosmetic for preventing or improving scalp dandruff, itching or scalp odor, and antibacterial product of the present invention have excellent antibacterial activity and are therefore widely used not only in the fields of beauty and hair care.
Claims
1. An antibacterial agent containing simoncolite against at least one species of normal skin flora selected from the group consisting of Corynebacterium, Moraxella and Malassezia.
2. The antibacterial agent according to claim 1, wherein the simoncolite is in the form of nanoparticles.
3. The Simoncolite is a particle having a 50% cumulative particle size (D 50 2. The antibacterial agent according to claim 1, wherein the nanoparticles are 500 nm or less.
4. A deodorant cosmetic composition containing the antibacterial agent according to any one of claims 1 to 3.
5. A cosmetic composition for preventing or improving dandruff, itching or scalp odor, comprising the antibacterial agent according to any one of claims 1 to 3.
6. An antibacterial agent containing simoncolite against at least one microorganism selected from the group consisting of Corynebacterium, Moraxella, Malassezia, Staphylococcus, Pseudomonas, Candida and Aspergillus.
7. An antibacterial product containing the antibacterial agent according to claim 6.
Citation Information
Patent Citations
Method for preparing alkali zinc chloride nano-powder in hexagonal flake structures
CN102502783A
Antibacterial deodorant pet urinal mat and producing method thereof
CN108432642A
Flaky powder, production method of flaky powder, and flaky powder-containing cosmetic
JP2015038014A
Body odor component reducing agent and body odor suppressant using the same
JP2020026422A
Deodorant
JP2022190968A