Electrode and battery
By incorporating an insulating layer with controlled porosity and particle size bonded to the active material layer in the battery electrode, the internal resistance is reduced, enhancing battery performance and energy density.
Patent Information
- Application Number
- PCT/JP2024/009797
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional battery electrodes face challenges in suppressing the increase in internal resistance, which affects battery performance.
The electrode configuration includes a current collecting layer, an active material layer, and an insulating layer with specific porosity and particle diameter ranges, where the insulating layer is strategically bonded to the active material layer to minimize overlap and enhance electrolyte retention, thereby reducing internal resistance.
This configuration effectively suppresses the increase in internal resistance, ensuring smooth lithium ion propagation and maintaining energy density, resulting in improved battery performance.
Smart Images

Figure JP2024009797_31102024_PF_FP_ABST
Abstract
Description
Electrodes and batteries
[0001] The present invention relates to an electrode and a battery.
[0002] BACKGROUND ART Conventionally, there has been known a technique relating to an electrode in which an insulating layer is coated on an active material layer bonded to a current collecting layer and then bonded thereto (see, for example, Patent Document 1).
[0003] Japanese Patent Application Laid-Open No. 2020-061226
[0004] There is a demand for suppressing an increase in the internal resistance of the battery.
[0005] The electrode of the present invention has a current collecting layer, an active material layer, and an insulating layer. The active material layer is laminated and bonded to the current collecting layer and contains an active material. The insulating layer is laminated and bonded to the active material layer and contains an insulating material. The insulating material has an average particle diameter of 0.5 μm or more and 5.0 μm or less. The insulating layer has a porosity of 25% or more and 70% or less. The insulating layer and the active material layer overlap by 0.001% or more and 30% or less along the stacking direction.
[0006] The battery of the present invention includes a positive electrode, a negative electrode, and an insulator provided between the positive electrode and the negative electrode. At least one of the positive electrode and the negative electrode is the electrode.
[0007] It is possible to obtain an electrode in which an increase in internal resistance is suppressed, and a battery including such an electrode.
[0008] 1 is a perspective view showing a battery 1 of a first embodiment. 2 is a perspective view showing a charging / discharging body 10 of the battery 1. 3 is a cross-sectional view showing the charging / discharging body 10 at 3A-3B in FIG. 2. 4 is a cross-sectional view showing the charging / discharging body 10 in region 4 in FIG. 3. 5 is a side view schematically showing a method for manufacturing a positive electrode 100. 6 is a top view schematically showing a state in which a slurry is applied to the positive electrode current collecting layer 110 in FIG.
[0009] Embodiments for carrying out the present invention will be described with reference to the drawings. To facilitate understanding of each embodiment, the size and proportions of components may be exaggerated in each drawing. In cross-sectional views of active material layers, etc., adjacent active materials are shown not in contact with each other to illustrate the binders and additives surrounding the active materials. In each drawing, identical components are assigned the same reference numerals. The arrows indicate the short-side direction X of the stacked positive electrode 100, negative electrode 200, and separator 300. The arrows indicate the long-side direction Y of the stacked positive electrode 100, negative electrode 200, and separator 300. The arrows indicate the stacking direction Z of the stacked positive electrode 100, negative electrode 200, and separator 300.
[0010] The electrode in the embodiment corresponding to the present invention will be described as a positive electrode. The electrode in the embodiment corresponding to the present invention also includes a negative electrode. The battery 1 in the embodiment corresponding to the present invention will be described as a rectangular parallelepiped battery. The battery 1 in the embodiment corresponding to the present invention also includes a cylindrical battery.
[0011] (Configuration of Battery 1 Including Positive Electrode 100 of First Embodiment) The configuration of a battery 1 including a positive electrode 100 of the first embodiment will be described with reference to FIGS. 1 to 4. FIG.
[0012] Fig. 1 is a perspective view showing a battery 1 of the first embodiment. Fig. 2 is a perspective view showing a charging / discharging body 10 of the battery 1. Fig. 3 is a cross-sectional view showing the charging / discharging body 10 at 3A-3B in Fig. 2. Fig. 4 is a cross-sectional view showing the charging / discharging body 10 in region 4 in Fig. 3.
[0013] The battery 1 is, for example, a lithium ion secondary battery. As shown in Figures 1 to 4, the battery 1 includes a charge / discharge unit 10, an exterior body 50, and external terminals 60. The main components included in the battery 1 will be described below.
[0014] The charge / discharge unit 10 is charged and discharged. The charge / discharge unit 10 shown in FIGS. 2 and 3 includes a positive electrode 100, a negative electrode 200, a separator 300, and an electrolyte (so-called electrolytic solution). The charge / discharge unit 10 is formed, for example, by stacking the positive electrode 100, the negative electrode 200, and two separators 300 in this order, and then winding them into a rectangular parallelepiped shape. In the charge / discharge unit 10, the electrolyte is permeated, particularly into the separator 300. The charge / discharge unit 10 is covered with an insulating sheet in a state where the positive electrode current collector and the negative electrode current collector are joined together.
[0015] As shown in FIG. 3 , the positive electrode 100 (electrode) includes a positive electrode current collecting layer 110 , a positive electrode active material layer 120 , and an insulating layer 130 .
[0016] The positive electrode current collecting layer 110 (current collecting layer) is configured, for example, in a long shape. That is, the positive electrode current collecting layer 110 is formed in a foil shape. A positive electrode current collecting portion 110a is provided along the longitudinal direction Y at one end of the positive electrode current collecting layer 110 in the short direction X. The positive electrode current collecting layer 110 is formed, for example, from aluminum or an aluminum alloy. For example, JIS standard A3003 is used for the positive electrode current collecting layer 110. A3003 is a non-heat-treated type Al-Mn-based alloy. The thickness of the positive electrode current collecting layer 110 along the stacking direction Z is, for example, 10 μm. The thickness of the positive electrode current collecting layer 110 is selected, for example, from the range of 5 μm to 30 μm.
[0017] The positive electrode active material layer 120 (active material layer) is provided on the positive electrode current collecting layer 110. The positive electrode active material layers 120 are laminated and bonded to both sides of the positive electrode current collecting layer 110, facing each other along the lamination direction Z. The thickness of the positive electrode active material layer 120 along the lamination direction Z is, for example, 30 μm or 40 μm. The thickness of the positive electrode active material layer 120 is selected, for example, within the range of 10 μm to 200 μm.
[0018] The positive electrode active material layer 120 contains a positive electrode active material 121 , a positive electrode binder 122 , and a positive electrode conductive additive 123 .
[0019] The positive electrode active material 121 (active material) is, for example, a lithium-containing composite oxide. The lithium-containing composite oxide is, for example, a metal element such as nickel (Ni), cobalt (Co), or manganese (Mn), and lithium (Li). The positive electrode active material 121 is formed in a particulate form. The average particle diameter (D50) of the positive electrode active material 121 is, for example, 25 μm. The average particle diameter (D50) of the positive electrode active material 121 is selected, for example, within the range of 1 μm to 50 μm.
[0020] The positive electrode binder 122 bonds the positive electrode active material 121 together. For example, polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyethylene (PE), polystyrene, polybutadiene, polyacrylonitrile, polyvinyl fluoride, polypropylene fluoride, polychloroprene fluoride, butyl rubber, nitrile rubber, styrene butadiene rubber (SBR), polysulfide rubber, nitrocellulose, cyanoethyl cellulose, various latexes, acrylic resins, or mixtures thereof are used for the positive electrode binder 122.
[0021] The positive electrode conductive additive 123 improves the characteristics of the positive electrode 100. The positive electrode conductive additive 123 is mixed with the positive electrode active material 121 and increases the electrical conductivity between the positive electrode current collecting layer 110 and the positive electrode active material 121. That is, the positive electrode conductive additive 123 ensures a conductive path between the positive electrode current collecting layer 110 and the positive electrode active material 121 in the positive electrode 100. The positive electrode conductive additive 123 is, for example, a carbon-based material. The carbon-based material is, for example, crystalline carbon, amorphous carbon, or a mixture thereof. The crystalline carbon is, for example, artificial graphite, natural graphite, or a mixture thereof. The natural graphite is, for example, flake graphite, lump graphite, or amorphous graphite. The amorphous carbon is, for example, carbon black. The carbon black is, for example, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, or a mixture thereof.
[0022] As shown in FIG. 4 , the insulating layer 130 is laminated and bonded to the positive electrode active material layer 120. The insulating layer 130 has a porosity of 25% or more and 70% or less. The porosity corresponds to the electrolyte retention rate. The insulating layer 130 overlaps the positive electrode active material layer 120 by 0.001% or more and 30% or less along the stacking direction Z. The 0.001% or more and 30% or less represents a volume ratio. The insulating layer 130 has a thickness along the stacking direction Z of 1.0 μm or more and 10.0 μm or less. As shown in FIG. 4 , a region of the insulating layer 130 having a thickness t2 along the stacking direction Z and a region of the positive electrode active material layer 120 having a thickness t1 along the stacking direction Z partially overlap with each other in a region of a thickness t3 along the stacking direction Z. The insulating layer 130 suppresses the intrusion of foreign matter into the positive electrode 100.
[0023] As shown in FIG. 4, the insulating layer 130 includes an insulating material 131, a binder 132, and an additive material 133.
[0024] The insulating material 131 is an inorganic or organic material. The insulating material 131 is, for example, boehmite or alumina. The insulating material 131 is formed in a particulate form. The average particle diameter (D50) of the insulating material 131 is 0.5 μm or more and 5.0 μm. The average particle diameter (D50) of the insulating material 131 is, for example, 1.2 μm. The insulating material 131 has insulating properties. It is preferable that the insulating material 131 has heat resistance. The ratio of the insulating material 131 in the insulating layer 130 is, for example, 98%.
[0025] The binder 132 bonds the insulating materials 131 together. Examples of the binder 132 include polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyethylene (PE), polystyrene, polybutadiene, polyacrylonitrile, polyvinyl fluoride, polypropylene fluoride, polychloroprene fluoride, butyl rubber, nitrile rubber, styrene butadiene rubber (SBR), polysulfide rubber, nitrocellulose, cyanoethyl cellulose, various latexes, acrylic resins, and mixtures thereof. The binder 132 is, for example, PVdF. The binder 132 has insulating properties. The ratio of the binder 132 in the insulating layer 130 is, for example, 1.9%.
[0026] The additive 133, for example, uniformly disperses the insulating material 131 and the binder 132. The additive 133 is, for example, a dispersant. The dispersant is, for example, a carboxylic acid compound. The ratio of the additive 133 in the insulating layer 130 is, for example, 0.1%. The additive 133 is not essential for the insulating layer 130.
[0027] As shown in FIG. 3 , the negative electrode 200 includes a negative electrode current collecting layer 210 and a negative electrode active material layer 220 .
[0028] The negative electrode current collecting layer 210 is configured, for example, in an elongated shape. That is, the negative electrode current collecting layer 210 is formed in a foil shape. A negative electrode current collecting portion 210a is provided along the longitudinal direction Y at one end of the negative electrode current collecting layer 210 in the short side direction X. The negative electrode current collecting portion 210a of the negative electrode current collecting layer 210 faces the positive electrode current collecting portion 110a of the positive electrode current collecting layer 110 in the short side direction X. The negative electrode current collecting layer 210 is formed, for example, from copper or a copper alloy. The thickness of the negative electrode current collecting layer 210 along the stacking direction Z is, for example, 10 μm. The thickness of the negative electrode current collecting layer 210 is selected, for example, within a range of 5 μm to 30 μm.
[0029] The negative electrode active material layer 220 is provided on the negative electrode current collecting layer 210. The negative electrode active material layers 220 are bonded to both sides of the negative electrode current collecting layer 210 and face each other along the stacking direction Z. The negative electrode active material layer 220 has a greater width along the short-side direction X than the positive electrode active material layer 120. When the negative electrode 200 faces the positive electrode 100 via the separator 300, both ends of the negative electrode active material layer 220 in the short-side direction X are located further outward in the short-side direction X than both ends of the positive electrode active material layer 120 in the short-side direction X. The thickness of the negative electrode active material layer 220 along the stacking direction Z is, for example, 30 μm or 40 μm. The thickness of the negative electrode active material layer 220 is selected, for example, within a range of 10 μm to 200 μm.
[0030] The negative electrode active material layer 220 contains a negative electrode active material 221 and a negative electrode binder 222. The negative electrode active material layer 220 may also contain a negative electrode conductive additive 223.
[0031] The negative electrode active material 221 is made of, for example, carbon. The carbon is, for example, graphite, non-graphitizable carbon (hard carbon), or easily graphitizable carbon (soft carbon). The graphite is, for example, natural graphite or artificial graphite. The natural graphite is, for example, flake graphite, lump graphite, or amorphous graphite. The negative electrode active material 221 is formed in a particulate form. The average particle size (D50) of the negative electrode active material 221 is, for example, 25 μm. The average particle size (D50) of the negative electrode active material 221 is selected, for example, within the range of 1 μm to 50 μm.
[0032] The negative electrode binder 222 bonds the negative electrode active material 221 together. For the negative electrode binder 222, for example, the same material as the positive electrode binder 122 is used.
[0033] The negative electrode conductive additive 223 improves the characteristics of the negative electrode 200. The negative electrode conductive additive 223 is mixed with the negative electrode active material 221 and disposed therein to increase the electrical conductivity between the negative electrode current collecting layer 210 and the negative electrode active material 221. That is, the negative electrode conductive additive 223 ensures a conductive path between the negative electrode current collecting layer 210 and the negative electrode active material 221 in the negative electrode 200.
[0034] The negative electrode 200 may include an insulating layer that covers the negative electrode active material layer 220. The insulating layer has heat resistance. The insulating layer contains, for example, an inorganic material or an organic material and a binder. The inorganic material is, for example, alumina particles.
[0035] The separator 300 (insulator) insulates the positive electrode 100 from the negative electrode 200. The insulating layer 130 of the positive electrode 100 faces the negative electrode 200 in the stacking direction Z via the separator 300. The separator 300 also holds an electrolyte (so-called electrolytic solution). The separator 300 is formed in an elongated shape. The separator 300 has a width in the short-side direction X that is greater than that of the negative electrode active material layer 220. When the positive electrode 100 and the negative electrode 200 face each other via the separator 300, both ends of the positive electrode active material layer 120 in the short-side direction X and both ends of the negative electrode active material layer 220 in the short-side direction X are located within the range of the separator 300 along the short-side direction X. The thickness of the separator 300 along the stacking direction Z is, for example, 20 μm. The thickness of the separator 300 is selected within the range of 5 μm to 60 μm, for example.
[0036] 3, the separator 300 is made of a porous material. Examples of the porous material include polyethylene, polypropylene, polyester, cellulose, and polyamide. The separator 300 may be made of a laminate of multiple different porous materials.
[0037] The separator 300 may include an insulating layer. The insulating layer has heat resistance. The insulating layer contains, for example, an inorganic material or an organic material and a binder. The inorganic material is, for example, alumina particles.
[0038] The electrolyte allows lithium ions to flow between the positive electrode 100 and the negative electrode 200. The electrolyte is also called an electrolytic solution.
[0039] The electrolyte contains an organic solvent and a lithium salt, and may contain an additive.
[0040] The organic solvent may be, for example, a carbonate ester such as ethylene carbonate. The lithium salt may be, for example, lithium hexafluorophosphate (LiPF 6 ) is used as the additive. For example, lithium hexafluorophosphate (LiPF 6 ) is used.
[0041] The exterior body 50 houses the charging / discharging unit 10. As shown in FIG. 1 , the exterior body 50 includes a container 51, a lid 52, a filling tap 53, and a split valve 54. The container 51 is formed in a rectangular parallelepiped shape. The container 51 houses the charging / discharging unit 10. The lid 52 is welded to the container 51. The lid 52 has a filling hole. The filling hole is a hole for injecting an electrolyte (so-called electrolytic solution) into the interior of the battery 1. The filling tap 53 is attached to the filling hole of the lid 52. After the electrolyte is injected into the interior of the battery 1 through the filling hole, the filling tap 53 is inserted into the filling hole and welded. The lid 52 has a split valve 54. The split valve 54 is formed integrally with the lid 52. The split valve 54 splits outward from the battery 1 when the internal pressure of the battery 1 exceeds a predetermined value.
[0042] The external terminals 60 relay the input and output of power between the current collectors provided inside the battery 1 and electrical equipment provided outside the battery 1. The electrical equipment is, for example, a relay or inverter provided in the vehicle. Furthermore, the external terminals 60 provided on one battery 1 are electrically connected to the external terminals 60 provided on other batteries 1 via bus bars or the like, relaying the input and output of power between the one battery 1 and the other batteries 1. As shown in FIG. 1 , the external terminals 60 include a positive terminal 61 and a negative terminal 62. The positive terminal 61 is electrically connected to the positive current collecting portion 110a of the positive current collecting layer 110 via a positive current collecting plate. The positive terminal 61 is attached to the lid 52 via a positive electrode insulating member. The negative terminal 62 is electrically connected to the negative current collecting portion 210a of the negative current collecting layer 210 via a negative current collecting plate. The negative terminal 62 is attached to the lid 52 via a negative electrode insulating member.
[0043] (Method for manufacturing the positive electrode 100 of the first embodiment) A method for manufacturing the positive electrode 100 will be described with reference to Fig. 5 and Fig. 6. Fig. 5 is a side view that schematically shows the method for manufacturing the positive electrode 100. Fig. 6 is a top view that schematically shows the state in which the slurry is applied to the positive electrode current collecting layer 110 of Fig. 5.
[0044] In the method for manufacturing the positive electrode 100, a coating step involves coating a positive electrode active material layer slurry 1100 and an insulating layer slurry 1200. In the coating step, the positive electrode active material layer slurry 1100 is coated onto the positive electrode current collecting layer 110. In addition, in the coating step, the insulating layer slurry 1200 is coated onto the positive electrode active material layer slurry 1100.
[0045] The positive electrode active material layer slurry 1100 used in the coating step contains a solvent in addition to the components that make up the positive electrode active material layer 120. The components that make up the positive electrode active material layer 120 include a positive electrode active material 121, a positive electrode binder 122, and a positive electrode conductive additive 123. The solvent disperses the components contained in the positive electrode active material layer 120. For example, a solvent that is vaporizable at a temperature equal to or higher than room temperature is used. For example, the solvent is N-methyl-2-pyrrolidone (NMP).
[0046] The insulating layer slurry 1200 used in the coating process contains a solvent in addition to the components that make up the insulating layer 130. The solvent disperses the insulating material 131, binder 132, and other materials contained in the insulating layer 130. The solvent used is, for example, one that evaporates at temperatures above room temperature. The solvent is, for example, N-methyl-2-pyrrolidone (NMP).
[0047] As shown in FIG. 5, the manufacturing apparatus 1000 for the positive electrode 100 includes a conveying section 1010, a coating section 1020, a drying section 1030, and a rolling section 1040.
[0048] 5, the conveying unit 1010 conveys the members that constitute the positive electrode 100. The conveying unit 1010 includes a conveying roller 1011.
[0049] The conveying unit 1010 conveys the positive electrode current collecting layer 110 wound around a first roller (not shown) to the coating unit 1020, the drying unit 1030, and the rolling unit 1040 via conveying rollers 1011 and the like. The conveying unit 1010 winds the positive electrode current collecting layer 110, in which the positive electrode active material layer 120 and the insulating layer 130 are bonded, around a second roller (not shown). When the second roller to which the positive electrode current collecting layer 110 is attached rotates, the conveying roller 1011 and the first roller in contact with the positive electrode current collecting layer 110 also rotate, conveying the positive electrode current collecting layer 110. The conveying direction H of the positive electrode current collecting layer 110 corresponds to the longitudinal direction Y of the positive electrode current collecting layer 110.
[0050] 5, the coating unit 1020 applies slurry to the positive electrode current collecting layer 110 and the like. The coating unit 1020 includes a first coating head 1021, a first liquid feed pipe 1022, a second coating head 1023, and a second liquid feed pipe 1024.
[0051] As shown in FIGS. 5 and 6 , the first coating head 1021 is provided along the conveying direction H of the positive electrode current collecting layer 110, i.e., along the short direction X perpendicular to the longitudinal direction Y of the positive electrode current collecting layer 110. An elongated opening is formed in the first coating head 1021. The elongated opening is connected to a first liquid supply pipe 1022. The positive electrode active material layer slurry 1100 is supplied to the first coating head 1021 from a tank (not shown) via a pump (not shown) and the first liquid supply pipe 1022. The first coating head 1021 faces the conveying roller 1011 across the positive electrode current collecting layer 110. The first coating head 1021 applies the positive electrode active material layer slurry 1100 to the positive electrode current collecting layer 110 while the positive electrode current collecting layer 110 is being conveyed.
[0052] As shown in FIGS. 5 and 6 , the second coating head 1023 is provided along the short-side direction X of the positive electrode current collecting layer 110. The second coating head 1023 is aligned with the first coating head 1021 along the conveyance direction H of the positive electrode current collecting layer 110. The second coating head 1023 is located downstream of the first coating head 1021 in the conveyance direction H of the positive electrode current collecting layer 110. An elongated opening is formed in the second coating head 1023. The elongated opening is connected to a second liquid feed pipe 1024. The insulating layer slurry 1200 is supplied to the second coating head 1023 from a tank (not shown) via a pump (not shown) and the second liquid feed pipe 1024. The second coating head 1023 faces the conveyance roller 1011 with the positive electrode current collecting layer 110 interposed therebetween. The second coating head 1023 coats the insulating layer slurry 1200 onto the positive electrode active material layer slurry 1100 while the positive electrode current collecting layer 110 is being transported. That is, the insulating layer slurry 1200 is coated so as to cover the positive electrode active material layer slurry 1100. The insulating layer slurry 1200 may be coated onto the positive electrode current collecting layer 110 so as to extend beyond the end of the positive electrode active material layer slurry 1100 in the short direction X and along the longitudinal direction Y of the positive electrode active material layer slurry.
[0053] 5 , the drying unit 1030 dries the slurry. The drying unit 1030 is provided downstream of the coating unit 1020 in the conveying direction H of the positive electrode current collecting layer 110. The drying unit 1030 includes a dryer 1031.
[0054] As shown in Fig. 5 , the dryer 1031 is provided along the transport direction H of the positive electrode current collecting layer 110, i.e., the longitudinal direction Y of the positive electrode current collecting layer 110. The dryer 1031 dries the positive electrode active material layer slurry 1100 and the insulating layer slurry 1200 while the positive electrode current collecting layer 110 is being transported. The dryer 1031 is equipped with a plurality of heat sources along the transport direction H of the positive electrode current collecting layer 110. The dryer 1031 uses the multiple heat sources to dry the positive electrode active material layer slurry 1100 and the insulating layer slurry 1200 under a plurality of conditions.
[0055] In the drying section 1030, the solvent in the positive electrode active material layer slurry 1100 evaporates, thereby forming the positive electrode active material layer 120. The NMP contained in the positive electrode active material layer slurry 1100 evaporates, thereby drying the positive electrode active material layer slurry 1100. As the positive electrode active material layer slurry 1100 dries, the thickness of the positive electrode active material layer slurry 1100 along the stacking direction Z decreases. The positive electrode active material layer 120 is bonded to the positive electrode current collecting layer 110. The solvent in the insulating layer slurry 1200 evaporates, thereby forming the insulating layer 130. The NMP contained in the insulating layer slurry 1200 evaporates, thereby drying the insulating layer slurry 1200. As the insulating layer slurry 1200 dries, the thickness of the insulating layer slurry 1200 along the stacking direction Z decreases. The insulating layer 130 is bonded to the positive electrode active material layer 120.
[0056] 5 , the rolling unit 1040 rolls the positive electrode current collecting layer 110, the positive electrode active material layer 120, and the insulating layer 130, which are bonded together. The rolling unit 1040 is provided downstream of the drying unit 1030 in the conveying direction H of the positive electrode current collecting layer 110. The rolling unit 1040 includes a rolling roller 1041 and a driven roller 1042.
[0057] As shown in FIG. 5 , the rolling roller 1041 is provided along the widthwise direction X of the positive electrode current collecting layer 110. The rolling roller 1041 faces the insulating layer 130 of the positive electrode 100. As shown in FIG. 5 , the driven roller 1042 is provided along the widthwise direction X of the positive electrode current collecting layer 110. The driven roller 1042 faces the rolling roller 1041 across the positive electrode 100. The driven roller 1042 faces the positive electrode current collecting layer 110 of the positive electrode 100. The rolling unit 1040 determines the thicknesses of the positive electrode active material layer 120 and the insulating layer 130 by the distance between the rolling roller 1041 and the driven roller 1042.
[0058] In the method for manufacturing the positive electrode 100, the configuration described with reference to FIGS. 5 and 6 is a configuration in which the positive electrode active material layer 120 and the insulating layer 130 are bonded to one surface of the positive electrode current collecting layer 110. That is, the method for manufacturing the positive electrode 100 shown in FIGS. 5 and 6 is a so-called single-sided coating method for manufacturing the positive electrode 100. On the other hand, as shown in FIG. 3, for example, the positive electrode 100 has the positive electrode active material layer 120 and the insulating layer 130 bonded to both surfaces of the positive electrode current collecting layer 110. That is, the positive electrode 100 shown in FIG. 3 is configured by so-called double-sided coating. Therefore, in the method for manufacturing the positive electrode 100, after the configuration described with reference to FIGS. 5 and 6, the positive electrode active material layer 120 and the insulating layer 130 are bonded to the other surface of the positive electrode active material layer 120.
[0059] (Comparative Experimental Results of Positive Electrode 100 of First Embodiment and Comparative Positive Electrode) The comparative experimental results of the positive electrode 100 of the first embodiment and comparative positive electrodes will be described with reference to Table 1.
[0060]
[0061] The insulating layers under conditions 1 and 2 correspond to the insulating layer 130 of the positive electrode 100 of the embodiment. On the other hand, the insulating layers under conditions 3 and 4 correspond to the insulating layer of the positive electrode of the comparative example.
[0062] Under condition 1, the ratio of insulating material 131 in insulating layer 130 was set to 98%. Also, under condition 1, the ratio of binder 132 in insulating layer 130 was set to 1.9%. Under condition 1, the ratio of solids in insulating layer slurry 1200 was set to 30%. The solids consisted of insulating material 131, binder 132, and additive 133. Under condition 1, the viscosity of insulating layer slurry 1200 was 325 mPa·s.
[0063] Under condition 2, unlike condition 1, the solid content ratio in insulating layer slurry 1200 was set to 15%. That is, under condition 2, the proportion of solvent in insulating layer slurry 1200 was increased compared to condition 1. Under condition 2, the viscosity of insulating layer slurry 1200 became 100 mPa·s.
[0064] Under condition 3, unlike condition 1, the ratio of insulating material in the insulating layer was set to 99.5%. Also, under condition 3, the ratio of binder in the insulating layer was set to 0.4%. That is, under condition 3, the ratio of insulating material in the insulating layer was increased and the ratio of binder was decreased compared to condition 1. Under condition 3, the viscosity of the insulating layer slurry was 100 mPa s.
[0065] Unlike condition 1, condition 4 had a 90% insulating material ratio in the insulating layer. Also, condition 4 had a 9.9% binder ratio in the insulating layer. That is, condition 4 had a reduced insulating material ratio and an increased binder ratio in the insulating layer compared to condition 1. Condition 4 had a viscosity of 800 mPa s or higher.
[0066] Under condition 5, unlike condition 1, the solid content ratio in insulating layer slurry 1200 was set to 10%. That is, under condition 5, the proportion of solvent in insulating layer slurry 1200 was increased compared to conditions 1 and 2. Under condition 5, the viscosity of insulating layer slurry 1200 became 3 mPa·s.
[0067] The insulating layer 130 under condition 1 was sufficiently bonded to the positive electrode active material layer 120. The insulating layer 130 under condition 1 had a very good interface with the positive electrode active material layer 120. That is, the insulating layer 130 under condition 1 overlapped the positive electrode active material layer 120 relatively little. The positive electrode 100 provided with the insulating layer 130 under condition 1 was able to suppress an increase in resistance.
[0068] The insulating layer 130 under condition 2 was sufficiently bonded to the positive electrode active material layer 120. The insulating layer 130 under condition 2 had a good interface with the positive electrode active material layer 120. That is, the insulating layer 130 under condition 2 overlapped the positive electrode active material layer 120 relatively little. The positive electrode 100 provided with the insulating layer 130 under condition 2 was able to suppress an increase in resistance.
[0069] The insulating layer 130 under condition 3 could not be sufficiently bonded to the positive electrode active material layer 120. This is because, under condition 3, the ratio of insulating material in the insulating layer was increased and the ratio of binder was decreased compared to condition 1. If the binder ratio is too low, it is difficult to fix the insulating layer to the positive electrode active material layer. The insulating layer 130 under condition 3 had a good interface with the positive electrode active material layer 120. The positive electrode 100 provided with the insulating layer 130 under condition 3 was able to suppress an increase in resistance.
[0070] The insulating layer 130 under condition 4 was sufficiently bonded to the positive electrode active material layer 120. The insulating layer 130 under condition 4 had an extremely good interface with the positive electrode active material layer 120. That is, the insulating layer 130 under condition 4 overlapped the positive electrode active material layer 120 relatively little. The positive electrode 100 provided with the insulating layer 130 under condition 4 was unable to suppress an increase in resistance. This is because, compared to condition 1, under condition 4 the proportion of insulating material in the insulating layer was reduced and the proportion of binder was increased. The binder does not contribute to the battery reaction.
[0071] The insulating layer 130 under condition 5 was not sufficiently bonded to the positive electrode active material layer 120. The insulating layer 130 under condition 5 had an unsatisfactory interface with the positive electrode active material layer 120. That is, the insulating layer 130 under condition 5 overlapped the positive electrode active material layer 120 relatively frequently. The reason for this is that the viscosity of the insulating layer slurry 1200 under condition 5 was very low (3 mPa s). The positive electrode 100 provided with the insulating layer 130 under condition 5 was unable to suppress an increase in resistance.
[0072] (Effects of the Battery 1 Including the Positive Electrode 100 of the First Embodiment) The effects of the battery 1 including the positive electrode 100 of the first embodiment will be described.
[0073] (1), (6), and (7) The positive electrode 100 (electrode) has an insulating layer 130 (insulating layer). The insulating layer 130 is laminated and bonded to the positive electrode active material layer 120 (active material layer) and includes an insulating material 131 having insulating properties. The insulating material 131 has an average particle diameter (D50) of 0.5 μm or more and 5.0 μm or less. The insulating layer 130 has a porosity of 25% or more and 70% or less. The insulating layer 130 and the positive electrode active material layer 120 overlap each other by 0.001% or more and 30% or less along the stacking direction Z. The overlap between the insulating layer 130 and the positive electrode active material layer 120 is based on a volume ratio. With this configuration, the overlap of the insulating layer 130, which does not contribute to the battery reaction, with the positive electrode active material layer 120, which contributes to the battery reaction, can be suppressed to a certain level or less. Furthermore, with this configuration, the insulating layer 130 can be sufficiently impregnated with the electrolyte solution, allowing smooth propagation of lithium ions. As a result, a positive electrode 100 in which an increase in internal resistance is suppressed can be obtained. Furthermore, with this configuration, a battery 1 including a positive electrode 100 in which an increase in internal resistance is suppressed can be obtained.
[0074] (2) The insulating layer 130 and the positive electrode active material layer 120 overlap each other by 1% or less along the stacking direction Z. With this configuration, the overlap between the insulating layer 130 and the positive electrode active material layer 120 is suppressed to 1% or less, so that a positive electrode 100 can be obtained in which an increase in internal resistance is further suppressed.
[0075] (3) The insulating layer 130 and the positive electrode active material layer 120 overlap each other by 0.5% or less along the stacking direction Z. With this configuration, the overlap between the insulating layer 130 and the positive electrode active material layer 120 is suppressed to 0.5% or less, and therefore, a positive electrode 100 can be obtained in which an increase in internal resistance is further suppressed.
[0076] (4) The insulating material 131 contains boehmite or alumina. With this configuration, the insulating material 131 can be made of a versatile material.
[0077] (5) The insulating layer 130 has a thickness in the stacking direction Z of 1.0 μm or more and 10.0 μm or less. With this configuration, the proportion of the insulating layer 130 in the positive electrode 100 can be suppressed to a certain percentage or less. As a result, the energy density of the positive electrode 100 can be maintained at a certain level or more.
[0078] (8) The insulating layer 130 faces the negative electrode 200 in the stacking direction Z, with the separator 300 (insulator) interposed therebetween. With this configuration, the separator 300 can complement the insulation between the positive electrode 100 and the negative electrode 200.
[0079] (Battery of Other Embodiments) The battery of the present invention is not limited to the configuration of the battery described in the embodiments, and can be configured appropriately based on the content described in the claims.
[0080] The embodiments are described in detail or simply to make the present invention easier to understand, and do not necessarily include all of the components described, or may include components not shown. Also, some of the components of the embodiments may be deleted, replaced with components of other embodiments, or combined with components of other embodiments.
[0081] In the electrode (positive electrode) of the present invention, the positive electrode active material is not limited to nickel (Ni), cobalt (Co), and manganese (Mn)-based materials. The positive electrode active material of the present invention may be, for example, iron (olivine)-based.
[0082] In the electrode (negative electrode) of the present invention, the negative electrode active material is not limited to a carbon-based material, but may be, for example, a silicon-based material.
[0083] The battery of the present invention is not limited to a configuration in which the charge / discharge body is sealed by a container and a lid, but can be applied to a configuration in which the charge / discharge body is sealed by a laminate film.
[0084] The battery of the present invention is not limited to a lithium-ion battery, but can be applied to, for example, a nickel-metal hydride battery.
[0085] The battery of the present invention is not limited to a secondary battery, but can be applied to a primary battery.
[0086] In the battery of the present invention, the charge / discharge body is not limited to a wound type in which a positive electrode, a separator, and a negative electrode each formed in a long shape are bundled and wound up. A stacked type in which a positive electrode, a separator, and a negative electrode each formed in a rectangular shape are alternately stacked can be used as the charge / discharge body of the battery of the present invention.
[0087] In the battery of the present invention, the charge / discharge body may be a stacked type in which a plurality of relatively short positive electrodes and a plurality of short negative electrodes are alternately arranged facing each other with the separator interposed therebetween, with the separator being folded and stacked.
[0088] In the battery of the present invention, the charging / discharging body is not limited to a rectangular parallelepiped type, and a cylindrical or columnar type may also be used as the charging / discharging body of the battery of the present invention.
[0089] In the battery of the present invention, the charge / discharge body is not limited to a configuration in which an insulating separator is provided between the positive electrode and the negative electrode. The battery of the present invention can also be applied to a configuration in which an insulating layer is provided on at least one of the positive electrode and the negative electrode without providing a separator. Such a configuration corresponds to a so-called separatorless configuration.
[0090] The battery of the present invention is not limited to a configuration in which only one charging / discharging element is provided, but can be applied to a configuration in which two or more charging / discharging elements are provided.
[0091] The electrodes (positive and negative electrodes) of the present invention are not limited to a configuration in which the ends of the current collecting layer are joined to the current collecting plate. The electrodes of the battery of the present invention can be applied to a type in which electrode tabs protruding outward from the edges of the current collecting layer are joined to the current collecting plate.
[0092] The electrodes (positive electrode, negative electrode) of the present invention are not limited to a configuration in which active material layers are bonded to both sides of a current collecting layer, and may be configured to have an active material layer bonded to only one side of a current collecting layer.
[0093] The method for producing electrodes (positive electrode, negative electrode) of the present invention is not limited to a configuration in which an active material layer and an insulating layer are formed by simultaneously applying and drying an active material layer slurry and an insulating layer slurry. The method for producing electrodes (positive electrode, negative electrode) of the present invention can also be applied to a configuration in which an active material layer is first formed by applying and drying an active material layer slurry to a current collecting layer. In such a configuration, an insulating layer is then formed by applying and drying an insulating layer slurry to an active material layer.
[0094] The method for manufacturing electrodes (positive electrode, negative electrode) of the present invention is not limited to a configuration in which the first coating head and the second coating head are provided independently, but can be applied to a configuration in which the first coating head and the second coating head are integrated.
[0095] LIST OF SYMBOLS 1 Battery, 10 Charger / Discharger, 50 Exterior, 51 Container, 52 Lid, 53 Injection plug, 54 Cleavage valve, 60 External terminal, 61 Positive electrode terminal, 62 Negative electrode terminal, 100 Positive electrode (electrode), 110 Positive electrode current collector layer (current collector layer), 110a Positive electrode current collector, 120 Positive electrode active material layer (active material layer), 121 Positive electrode active material (active material), 122 Positive electrode binder, 123 Positive electrode conductive additive, 130 Insulating layer, 131 Insulating material, 132 Binder, 133 Additive, 200 Negative electrode, 210 Negative electrode current collector layer, 210a Negative electrode current collector, 220 Negative electrode active material layer, 221 Negative electrode active material, 222 Negative electrode binder, 223 Negative electrode conductive additive, 300 Separator (insulator), 1000 Manufacturing apparatus, 1010 Conveying section, 1011 Conveying roller, 1020 Coating section, 1021 First coating head, 1022 First liquid supply pipe, 1023 Second coating head, 1024 Second liquid supply pipe, 1030 Drying section, 1031 Dryer, 1040 Rolling section, 1041 Rolling roller, 1042 Driven roller, 1100 Positive electrode active material layer slurry, 1200 Insulating layer slurry, t1 Thickness (along the stacking direction Z of the positive electrode active material layer 120), t2 Thickness (along the stacking direction Z of the insulating layer 130), t3 Thickness (of the portion where the region of thickness t1 and the region of thickness t2 overlap along the stacking direction Z), X: short side direction (of the positive electrode 100, the negative electrode 200, and the separator 300), Y: longitudinal direction (of the positive electrode 100, the negative electrode 200, and the separator 300), Z: stacking direction (of the positive electrode 100, the negative electrode 200, and the separator 300), H: transport direction (longitudinal direction Y) (of the positive electrode 100, the negative electrode 200, and the separator 300).
Claims
1. An electrode comprising: a current collecting layer; an active material layer laminated and joined to the current collecting layer and containing an active material; and an insulating layer laminated and joined to the active material layer and containing an insulating material, wherein the insulating material has an average particle diameter of 0.5 μm or more and 5.0 μm or more, the insulating layer has a porosity of 25% or more and 70% or less, and the insulating layer and the active material layer overlap by 0.001% or more and 30% or less along the stacking direction.
2. The electrode according to claim 1, wherein the insulating layer and the active material layer overlap each other by 1% or less along the stacking direction.
3. The electrode according to claim 1, wherein the insulating layer and the active material layer overlap each other by 0.5% or less along the stacking direction.
4. The electrode of claim 1, wherein the insulating material comprises boehmite or alumina.
5. The electrode according to claim 1, wherein the insulating layer has a thickness in the stacking direction of 1.0 μm or more and 10.0 μm or less.
6. The electrode according to claim 1, wherein the current collecting layer is a positive electrode current collecting layer, and the active material layer is a positive electrode active material layer containing a positive electrode active material.
7. A battery comprising: a positive electrode; and a negative electrode, wherein at least one of the positive electrode and the negative electrode has a current collecting layer, an active material layer laminated and joined with the current collecting layer and containing an active material, and an insulating layer laminated and joined with the active material layer and containing an insulating material, wherein the insulating material has an average particle diameter of 0.5 μm or more and 5.0 μm, the insulating layer has a porosity of 25% or more and 70% or less, the insulating layer and the active material layer overlap with each other by 0.001% or more and 30% or less along the stacking direction, and the insulating layer of the positive electrode faces the negative electrode along the stacking direction, or the insulating layer of the negative electrode faces the positive electrode along the stacking direction.
8. The battery according to claim 7, further comprising an insulator provided between the positive electrode and the negative electrode, wherein the insulating layer of the positive electrode faces the negative electrode in the stacking direction via the insulator, or the insulating layer of the negative electrode faces the positive electrode in the stacking direction via the insulator.
Citation Information
Patent Citations
Electrode, electrode device, and non-aqueous electrolyte solution electric storage device
JP2020061226A
Electrode for lithium ion secondary battery and lithium ion secondary battery
JP2020140896A
Negative electrode, lithium ion secondary battery, method for manufacturing negative electrode for lithium ion secondary battery, and method for manufacturing negative electrode sheet for lithium ion secondary battery
JP2021197249A