Positive electrode for nonaqueous electrolyte secondary battery, and method for manufacturing positive electrode for nonaqueous electrolyte secondary battery
The positive electrode for non-aqueous electrolyte secondary batteries, featuring a lithium-containing transition metal composite oxide with a sulfonic acid compound and uniformly distributed PTFE, addresses the limitations of existing technologies by improving output and cycle characteristics through reduced reaction resistance and enhanced electrolyte diffusivity.
Patent Information
- Application Number
- PCT/JP2024/013759
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional techniques for non-aqueous electrolyte secondary batteries fail to adequately improve output characteristics while maintaining good cycle characteristics, particularly due to issues with reaction resistance and diffusivity in the positive electrode mixture layer.
A positive electrode with a lithium-containing transition metal composite oxide active material, coated with a sulfonic acid compound and uniformly distributed PTFE, where the PTFE content is carefully controlled across the thickness of the mixture layer to enhance electrolyte diffusivity and reaction distribution.
This configuration improves both output characteristics and cycle stability by reducing reaction resistance and ensuring uniform electrolyte distribution, resulting in a non-aqueous electrolyte secondary battery with enhanced performance.
Smart Images

Figure JP2024013759_31102024_PF_FP_ABST
Abstract
Description
Positive electrode for non-aqueous electrolyte secondary battery and method for manufacturing the positive electrode for non-aqueous electrolyte secondary battery
[0001] The present disclosure relates to a positive electrode for a non-aqueous electrolyte secondary battery and a method for manufacturing a positive electrode for a non-aqueous electrolyte secondary battery.
[0002] In recent years, the applications of non-aqueous electrolyte secondary batteries have expanded to include power sources for electric vehicles and power storage devices for utilizing natural energy. Since the positive electrode significantly affects battery characteristics, including battery capacity, output characteristics, and cycle characteristics, much research has been conducted on the positive electrode. Patent Document 1 discloses a positive electrode for a non-aqueous electrolyte secondary battery that uses, as a positive electrode active material, a lithium-containing transition metal composite oxide having a low-solubility Li salt scattered on its surface, with the aim of reducing reaction resistance during storage at high temperatures.
[0003] Japanese Patent Application Laid-Open No. 2019-169286
[0004] In non-aqueous electrolyte secondary batteries, improving output characteristics while maintaining good cycle characteristics is an important issue. Conventional techniques including those described in Patent Document 1 have not been able to adequately address such issues, and there is still much room for improvement.
[0005] A positive electrode for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure is a positive electrode for a non-aqueous electrolyte secondary battery having a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core, the positive electrode mixture layer including a positive electrode active material and PTFE, the positive electrode active material including a lithium-containing transition metal composite oxide having a layered structure, and the lithium-containing transition metal composite oxide is represented by the general formula Li x Ni a Co b Mn c M d O 2-y(wherein 0.8<x<1.2, 0.75≦a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr), and the secondary particles are formed by aggregation of primary particles, and a sulfonic acid compound represented by formula (I) is present on the surfaces of the secondary particles, and when the positive electrode mixture layer is divided into three equal parts in the thickness direction and defined as a first region, a second region, and a third region from the positive electrode core side, the PTFE content (s) in the first region, the PTFE content (t) in the second region, and the PTFE content (u) in the third region satisfy (u−s) / (s+t+u)≦±10%. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)
[0006] According to the positive electrode for a non-aqueous electrolyte secondary battery of one aspect of the present disclosure, it is possible to provide a non-aqueous electrolyte secondary battery with improved output characteristics while ensuring good cycle characteristics.
[0007] Fig. 1 is a longitudinal cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment; Fig. 2 is a cross-sectional view of a positive electrode according to an embodiment; Fig. 3 is a view showing a mixing step in a process for producing a positive electrode according to an embodiment; Fig. 4 is a view showing a stretching step in a process for producing a positive electrode according to an embodiment; Fig. 5 is a view showing a bonding step in a process for producing a positive electrode according to an embodiment.
[0008] The layered rock salt structure of a lithium-containing transition metal composite oxide has a transition metal layer such as Ni, a Li layer, and an oxygen layer, and the charge / discharge reaction of the battery progresses as Li ions present in the Li layer reversibly enter and exit. Generally, lithium nickel oxide-based lithium-containing transition metal composite oxides containing Ni as a main component are known as high-capacity positive electrode active materials. From the viewpoint of increasing the capacity of the battery, the Ni content in the lithium-containing transition metal composite oxide is preferably 75 mol % or more relative to the total number of moles of metal elements excluding Li.
[0009] As a result of the inventors' investigations, it has been found that by adding a sulfonic acid compound represented by the above formula (I) to the surface of secondary particles of a lithium-containing transition metal composite oxide used as a positive electrode active material, a nonaqueous electrolyte secondary battery with improved output characteristics can be realized. This is thought to be because the reaction resistance at the positive electrode is reduced by the function of the sulfonic acid compound. However, the presence of the sulfonic acid compound has led to a new problem: reduced cycle characteristics. This is thought to be because the mere presence of a sulfonic acid compound on the surface of the secondary particles does not improve the diffusibility of the nonaqueous electrolyte in the positive electrode mixture layer, resulting in a distribution of the reaction in the thickness direction of the positive electrode mixture layer.
[0010] The inventors further conducted extensive research and discovered that by uniformly dispersing polytetrafluoroethylene (PTFE) in the positive electrode mixture layer while maintaining a sulfonic acid compound on the surface of secondary particles of a lithium-containing transition metal composite oxide, a nonaqueous electrolyte secondary battery with improved output characteristics and cycle characteristics can be realized. More specifically, when the positive electrode mixture layer is divided into three equal parts in the thickness direction, separated into a first region, a second region, and a third region from the positive electrode core side, the PTFE content (s) in the first region, the PTFE content (t) in the second region, and the PTFE content (u) in the third region satisfy the relationship (u-s) / (s+t+u)≦±10%. Uniformly dispersing PTFE in the positive electrode mixture layer improves the diffusibility of the nonaqueous electrolyte in the positive electrode mixture layer, resulting in a more uniform distribution of the reaction in the thickness direction of the positive electrode mixture layer. As a result, the cycle characteristics of the battery are improved.
[0011] Hereinafter, an example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail with reference to the drawings. Note that configurations obtained by selectively combining the components of the multiple embodiments and variations described below are included within the scope of the present disclosure. Furthermore, in this specification, "to" refers to a range that includes the upper and lower limits before and after "to."
[0012] In the following, a cylindrical battery in which a wound electrode assembly 14 is housed in a cylindrical, bottomed exterior body 16 is exemplified as a nonaqueous electrolyte secondary battery; however, the exterior body of the battery is not limited to a cylindrical exterior body. The nonaqueous electrolyte secondary battery according to the present disclosure may be, for example, a prismatic battery with a prismatic exterior body, a coin-shaped battery with a coin-shaped exterior body, or a pouch-type battery with an exterior body composed of a laminate sheet including a metal layer and a resin layer. Furthermore, the electrode assembly is not limited to a wound type, but may also be a stacked type electrode assembly in which multiple positive electrodes and multiple negative electrodes are alternately stacked with separators interposed therebetween. Furthermore, the design of the nonaqueous electrolyte secondary battery according to the present disclosure is not limited to the design of the exemplified nonaqueous electrolyte secondary battery, and known nonaqueous electrolyte secondary battery designs may also be applied.
[0013] FIG. 1 is an axial cross-sectional view of a cylindrical nonaqueous electrolyte secondary battery 10 according to an embodiment. As shown in FIG. 1 , the nonaqueous electrolyte secondary battery 10 includes a wound electrode assembly 14, a nonaqueous electrolyte, and an exterior body 16 that accommodates the electrode assembly 14 and the nonaqueous electrolyte. The electrode assembly 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a wound structure in which the positive electrode 11 and the negative electrode 12 are spirally wound with the separator 13 interposed therebetween. The exterior body 16 is a cylindrical metal container with a bottom that is open on one axial side, and the opening of the exterior body 16 is closed by a sealing body 17. Hereinafter, for convenience of explanation, the sealing body 17 side of the battery will be referred to as the top, and the bottom side of the exterior body 16 will be referred to as the bottom.
[0014] The positive electrode 11, negative electrode 12, and separator 13 that make up the electrode assembly 14 are all rectangular, elongated bodies that are spirally wound in the longitudinal direction and stacked alternately in the radial direction of the electrode assembly 14. The separator 13 isolates the positive electrode 11 and the negative electrode 12 from each other. The negative electrode 12 is disposed, for example, so as to sandwich the positive electrode 11. The electrode assembly 14 includes a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like. In the electrode assembly 14, the longitudinal direction of the positive electrode 11 and the negative electrode 12 is the winding direction, and the lateral direction of the positive electrode 11 and the negative electrode 12 is the axial direction. That is, the lateral end faces of the positive electrode 11 and the negative electrode 12 form the axial end faces of the electrode assembly 14.
[0015] Insulating plates 18 and 19 are disposed above and below the electrode body 14. In the example shown in Fig. 1 , the positive electrode lead 20 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and the negative electrode lead 21 passes outside the insulating plate 19 and extends toward the bottom side of the exterior body 16. The positive electrode lead 20 is connected to the underside of an internal terminal plate 23 of the sealing body 17 by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the internal terminal plate 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the exterior body 16 by welding or the like, and the exterior body 16 serves as the negative electrode terminal.
[0016] A gasket 28 is provided between the exterior body 16 and the sealing body 17 to ensure airtightness inside the battery. The exterior body 16 has a groove 22 formed on its side surface that protrudes inward and supports the sealing body 17. The groove 22 is preferably formed in an annular shape along the circumferential direction of the exterior body 16, and supports the sealing body 17 on its top surface. The sealing body 17 is fixed to the top of the exterior body 16 by the groove 22 and the open end of the exterior body 16 that is crimped to the sealing body 17.
[0017] The sealing body 17 has a structure in which, in order from the electrode body 14 side, an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked. Each member constituting the sealing body 17 has, for example, a disk or ring shape, and each member except for the insulating member 25 is electrically connected to one another. The lower valve body 24 and the upper valve body 26 are connected at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0018] The positive electrode 11, the negative electrode 12, the separator 13, and the nonaqueous electrolyte that constitute the nonaqueous electrolyte secondary battery 10 will be described in detail below, with the positive electrode 11 being particularly described below.
[0019] 2, the positive electrode 11 has a positive electrode core 30 and a positive electrode mixture layer 31 formed on the surface of the positive electrode core 30. The positive electrode mixture layer 31 is preferably formed on both sides of the positive electrode core 30. The positive electrode core 30 can be made of a foil of a metal such as aluminum or an aluminum alloy that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface layer. The thickness of the positive electrode core 30 is, for example, 10 μm to 30 μm.
[0020] The positive electrode mixture layer 31 contains a positive electrode active material and PTFE as a binder. The thickness of the positive electrode mixture layer 31 is, for example, 10 μm to 150 μm on one side of the positive electrode core 30. The positive electrode mixture layer 31 may also contain a conductive agent. Examples of conductive agents contained in the positive electrode mixture layer 31 include carbon black (CB) such as acetylene black (AB) and ketjen black, carbon nanotubes (CNT), graphene, graphite, and other carbon-based particles. The particle diameter of the conductive agent is, for example, 0.01 μm to 0.1 μm. This allows the conductive agent to penetrate and adhere to recesses on the surface of the positive electrode active material. The content of the conductive agent in the positive electrode mixture layer 31 can be, for example, 0.001% by mass to 5.0% by mass, particularly 0.01% by mass to 2.5% by mass. In particular, when carbon nanotubes are used as the conductive agent, the amount of conductive agent can be reduced.
[0021] The positive electrode active material includes a lithium-containing transition metal composite oxide having a layered structure. The lithium-containing transition metal composite oxide is a secondary particle formed by aggregation of primary particles. The particle size of the primary particles constituting the secondary particles of the lithium-containing transition metal composite oxide is, for example, 0.02 μm to 2 μm. The particle size of the primary particles is measured as the diameter of the circumscribed circle in a particle image observed with a scanning electron microscope (SEM). The average particle size of the secondary particles of the lithium-containing transition metal composite oxide is, for example, 2 μm to 30 μm. Here, the average particle size refers to the volume-based median diameter (D50). D50 refers to the particle size at which the cumulative frequency in the volume-based particle size distribution is 50% from the smallest particle size, and is also referred to as the median diameter. The particle size distribution of the secondary particles of the lithium-containing transition metal composite oxide can be measured using a laser diffraction particle size distribution analyzer (e.g., MT3000II, manufactured by Microtrac-Bell Corporation) using water as a dispersion medium.
[0022] The lithium-containing transition metal composite oxide has a layered structure. Examples of the layered structure of the lithium-containing transition metal composite oxide include a layered structure belonging to the space group R-3m and a layered structure belonging to the space group C2 / m. From the viewpoints of increasing capacity and stabilizing the crystal structure, the lithium-containing transition metal composite oxide preferably has a layered structure belonging to the space group R-3m. The layered structure of the lithium-containing transition metal composite oxide may include a transition metal layer and a Li layer.
[0023] The lithium-containing transition metal composite oxide has the general formula Li x Ni a Co b Mn c M d O 2-y (wherein 0.8<x<1.2, 0.75≦a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr). The positive electrode active material may contain a composite oxide other than the lithium-containing transition metal composite oxide represented by the above general formula. The content of the positive electrode active material is, for example, 90% by mass or more with respect to the mass of the positive electrode mixture layer.
[0024] By setting the Ni content in the lithium-containing transition metal composite oxide to 75 mol % to 95 mol %, a battery with a high capacity can be obtained. The higher the Ni content, the higher the capacity of the battery. The content of the elements constituting the lithium-containing transition metal composite oxide can be measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), or the like.
[0025] The content of Co in the lithium-containing transition metal composite oxide is 0 mol % to 15 mol %, and Co is an optional component. In other words, the lithium-containing transition metal composite oxide does not need to contain Co. By containing Co, the lithium-containing transition metal composite oxide can improve the heat resistance of the battery.
[0026] The content of Mn in the lithium-containing transition metal composite oxide is 0 mol % to 25 mol %, and Mn is an optional component. In other words, the lithium-containing transition metal composite oxide does not necessarily contain Mn. By containing Mn, the lithium-containing transition metal composite oxide can stabilize its crystal structure.
[0027] The content of M (M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr) in the lithium-containing transition metal composite oxide is 0 mol % to 10 mol %, and M is an optional component. In other words, the lithium-containing transition metal composite oxide does not necessarily contain M.
[0028] The sulfonic acid compound represented by formula (I) is present on the surface of the secondary particles of the lithium-containing transition metal composite oxide. In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2. A is preferably a Group 1 element. Among these, Li or Na is more preferred, and Li is particularly preferred.
[0029] The sulfonic acid compound may be present so as to coat at least a portion of the surface of the secondary particles of the lithium-containing transition metal composite oxide, or may be present so as to coat the entire surface of the secondary particles. The sulfonic acid compound may also be present on the surface of the primary particles of the lithium-containing transition metal composite oxide. The presence of the sulfonic acid compound on the surface of the secondary particles of the lithium-containing transition metal composite oxide reduces the reaction resistance in the positive electrode, making it possible to increase the charge / discharge depth. As a result, the output characteristics of the battery can be improved.
[0030] In formula (I), R is preferably an alkyl group. The number of carbon atoms in the alkyl group is preferably 5 or less, more preferably 3 or less. From the viewpoint of reducing reaction resistance, a suitable example of R is an alkyl group having 3 or less carbon atoms, and among these, A is preferably a methyl group. In R, some of the hydrogen atoms bonded to the carbon may be substituted with fluorine. In addition, n in formula (I) is preferably 1.
[0031] Specific examples of the sulfonic acid compound include lithium methanesulfonate, lithium ethanesulfonate, lithium propanesulfonate, sodium methanesulfonate, sodium ethanesulfonate, magnesium methanesulfonate, lithium fluoromethanesulfonate, etc. Among these, at least one selected from the group consisting of lithium methanesulfonate, lithium ethanesulfonate, and sodium methanesulfonate is preferred, with lithium methanesulfonate being particularly preferred.
[0032] The sulfonic acid compound reduces the reaction resistance in the positive electrode 11. This reduction in resistance allows for a deeper charge / discharge depth, improving output characteristics. Even a very small amount of sulfonic acid compound can achieve this effect, but it is preferable for the sulfonic acid compound to be present on the secondary particle surface of the composite oxide in an amount of 0.1% by mass or more relative to the mass of the lithium-containing transition metal composite oxide. The upper limit of the sulfonic acid compound content is not particularly limited, but from the viewpoint of cycle characteristics, 2.0% by mass relative to the mass of the lithium-containing transition metal composite oxide is preferred. Therefore, an example of a suitable range for the amount of sulfonic acid compound is 0.1% by mass to 2.0% by mass relative to the mass of the lithium-containing transition metal composite oxide.
[0033] The presence of the sulfonic acid compound on the surface of the secondary particles of the lithium-containing transition metal composite oxide can be confirmed by Fourier transform infrared spectroscopy (FT-IR). In the infrared absorption spectrum obtained by FT-IR, the positive electrode active material containing lithium methanesulfonate exhibits, for example, a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It has an absorption peak around 1238 cm -1 , 1175 cm -1 , 1065 cm -1 The peak around 785 cm is due to the SO stretching vibration of lithium methanesulfonate. -1 The peak around 1000 nm is a peak due to the C-S stretching vibration derived from lithium methanesulfonate. Note that the presence of a positive electrode active material containing a sulfonic acid compound other than lithium methanesulfonate can also be confirmed from the absorption peak derived from the sulfonic acid compound in the infrared absorption spectrum.
[0034] The presence of the sulfonic acid compound can also be confirmed by X-ray photoelectron spectroscopy (XPS). In the spectrum obtained by XPS, a peak with a binding energy of approximately 165 to 170 eV and an intensity (c / s) of 200 to 1000 is observed for the positive electrode active material containing lithium methanesulfonate. The presence of the sulfonic acid compound on the secondary particle surface of the lithium-containing transition metal composite oxide can also be confirmed by ICP, atomic absorption spectroscopy, synchrotron XRD measurement, TOF-SIMS, etc.
[0035] In addition to the sulfonic acid compound, a metal compound may be present on the surface of the secondary particles of the lithium-containing transition metal composite oxide. The metal compound contains, for example, one or more metal elements selected from the group consisting of Sr, Ca, W, Zr, rare earth elements, and Al. Examples of the Sr-containing compound include SrO, Sr(OH), and the like. 2 and SrCO 3 Examples of compounds containing Ca include CaO and Ca(OH). 2 and CaCO 3 Examples of compounds containing W include WO 3 Examples of the compound containing Al include Al 2 O 3 Examples of compounds containing Zr include ZrO 2 , Zr(OH) 4 , Zr(CO 3 ) 2 and Zr(SO 4 ) 2 ・4H 2 Examples of rare earth-containing compounds include oxides, hydroxides, carbonates, sulfates, nitrates, and phosphates of rare earth elements. The metal compound may contain a plurality of types of these metal elements, and examples thereof include SrAlO 4 , CaAlO 4 The metal compound may further contain Li, and an example thereof is lithium tungstate.
[0036] A nonmetallic compound may be present on the surface of the lithium-containing transition metal composite oxide. The nonmetallic compound contains, for example, one or more nonmetallic elements selected from the group consisting of P and B. Examples of the P-containing compound include Li, 3-x H x P.O. 4 (0≦x≦3) can be exemplified. 3 BO 3 , Li 3 BO 3 , Li 2 B 4 O 7 Examples include:
[0037] Here, the alkali content of the positive electrode active material determined by the Warder method is preferably 150 μmol / g or less, more preferably 125 μmol / g or less, and even more preferably 100 μmol / g or less. In this case, the reaction between excess Li in the positive electrode active material and the non-aqueous electrolyte is suppressed, and the generation of various gases such as carbon dioxide, hydrogen carbonate, and CO gas during charge and discharge can be reduced. As a result, battery expansion during charge and discharge is suppressed. Furthermore, the alkali content determined by the Warder method may be 5 μmol / g or more, or may be 10 μmol / g or more. Therefore, the range of the alkali content determined by the Warder method is preferably 5 μmol / g to 150 μmol / g, more preferably 5 μmol / g to 125 μmol / g, and even more preferably 5 μmol / g to 100 μmol / g. The amount of alkali determined by the Warder method may be 10 μmol / g to 150 μmol / g, 10 μmol / g to 125 μmol / g, or 10 μmol / g to 100 μmol / g. The amount of alkali contained in the positive electrode active material can be reduced by carrying out a washing step in the manufacturing process of the positive electrode active material, which will be described later. Examples of the alkali component contained in the positive electrode active material include lithium hydroxide (LiOH), lithium carbonate (Li 2 CO 3Lithium hydroxide and lithium carbonate may be present at the interface between primary particles inside the composite oxide particles and on the surface of secondary particles formed by aggregation of primary particles.
[0038] The specific method for quantifying the alkaline component extracted from the positive electrode active material is as follows. (1) 1 g of the positive electrode active material is added to 30 ml of pure water and stirred to prepare a suspension in which the positive electrode active material is dispersed in water. (2) The suspension is filtered, and pure water is added to the suspension to make a total volume of 70 ml, obtaining a filtrate containing the water-soluble alkaline component eluted from the positive electrode active material. (3) While measuring the pH of the filtrate, hydrochloric acid is added dropwise to the filtrate. The amount of hydrochloric acid (titration amount) X mol / g consumed up to the first inflection point (near pH 8) on the pH curve and the amount of hydrochloric acid (titration amount) Y mol / g consumed up to the second inflection point (near pH 4) are calculated. The inflection points are the peak positions of the differential value with respect to the titration amount. (4) Here, the value X - (Y - X) is the alkaline amount.
[0039] The positive electrode active material, which is one example of the embodiment, can be produced by the following method: Note that the production method described here is only an example, and the method for producing the positive electrode active material is not limited to this method.
[0040] The manufacturing process of the positive electrode active material includes a synthesis step of mixing a metal oxide with a Li compound or the like to obtain a mixture and calcining the mixture to obtain a lithium-containing transition metal composite oxide; a washing step of washing the calcined product with water and dehydrating it to obtain a cake-like composition; a drying step of drying the cake-like composition to obtain a powder-like composition; and an addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition or the powder-like composition.
[0041] In the synthesis step, for example, a metal oxide containing 75 mol% to 95 mol% of Ni, 0 mol% to 15 mol% of Co, 0 mol% to 25 mol% of Mn, and 0 mol% to 10 mol% of M (M is at least one element selected from W, Mg, Mo, Nb, Ti, Si, Al, and Zr) is mixed with a Li compound to obtain a mixture.
[0042] The metal oxide can be obtained, for example, by adding an alkaline solution such as sodium hydroxide dropwise to a stirred solution of a metal salt containing Ni and an arbitrary metal element (Co, Mn, M, etc.) to adjust the pH to the alkaline side (e.g., 8.5 to 12.5) to precipitate (co-precipitate) a composite hydroxide containing Ni and the arbitrary metal element, and then heat-treating the composite hydroxide. The heat-treatment temperature is not particularly limited, but is, for example, in the range of 250°C to 600°C.
[0043] Examples of Li compounds include Li 2 CO 3 , LiOH, Li 2 O 2 , Li 2 O, LiNO 3 , LiNO 2 , Li 2 SO 4 , LiOH·H 2 Examples of the metal oxide include O, LiH, and LiF. In order to facilitate adjustment of the above-mentioned parameters to the ranges specified above, the mixing ratio of the metal oxide and the Li compound is preferably such that the molar ratio of the total amount of metal elements in the metal oxide to Li falls within a range of 1:0.8 to 1:1.2, and more preferably 1:1.0 to 1:1.1.
[0044] Next, the synthesis step includes a calcination step in which the resulting mixture is calcined. The calcination step is a multi-stage calcination step that includes at least a first calcination step in which the mixture is calcined at 300°C to 680°C under an oxygen stream, and a second calcination step in which the calcined product obtained by the first calcination step is calcined at a temperature exceeding 680°C under an oxygen stream. In the first calcination step, the temperature is increased to a first set temperature of 680°C or less at a first temperature increase rate of 0.2°C / min to 4.5°C / min. In the second calcination step, the temperature is increased to a second set temperature of 900°C or less at a first temperature increase rate of 0.5°C / min to 3.5°C / min. Note that multiple first and second temperature increase rates may be set for each temperature range as long as they are within the above-specified range.
[0045] The holding time of the first set temperature in the first firing step is preferably 5 hours or less, more preferably 3 hours or less. The holding time of the first set temperature is the time during which the first set temperature is maintained after reaching the first set temperature, and the holding time may be zero. The holding time of the second set temperature in the second firing step is preferably 1 hour to 10 hours, more preferably 1 hour to 5 hours. The holding time of the second set temperature is the time during which the second set temperature is maintained after reaching the second set temperature. The firing of the mixture is carried out, for example, in an oxygen stream with an oxygen concentration of 60% or more, and the flow rate of the oxygen stream is set to 10 cm / min. 3 The flow rate shall be 0.2 mL / min to 4 mL / min per kg of the mixture or 0.3 L / min or more per kg of the mixture.
[0046] In the washing step, the lithium-containing transition metal composite oxide is washed with water and dehydrated to obtain a cake-like composition. The particulate lithium-containing transition metal composite oxide obtained in the synthesis step can be used. By washing with water, unreacted lithium compounds added in the synthesis step and impurities other than the lithium compounds can be removed. When washing with water, for example, 300 g to 5000 g of lithium-containing transition metal composite oxide is added to 1 L of water. Note that water washing may be repeated multiple times. Dehydration after water washing can be performed, for example, using a filter press.
[0047] In the drying step, the cake-like composition obtained in the washing step is dried to obtain a powdery composition. The drying step may be performed in a vacuum atmosphere. The drying conditions are, for example, 150°C to 400°C and 0.5 hours to 15 hours.
[0048] In the adding step, at least one of a sulfonic acid compound and a sulfonic acid solution is added to the cake-like composition obtained in the washing step or the powder-like composition obtained in the drying step. This allows the sulfonic acid compound to adhere to the surface of the lithium-containing transition metal composite oxide. It is preferable to add at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition. The sulfonic acid compound to be added may be in the form of either a powder or a solution. The sulfonic acid solution is, for example, a methanesulfonic acid solution obtained by dissolving methanesulfonic acid in water. Li compounds remain in the cake-like composition, and these remaining Li compounds are dissolved in the water contained in the cake-like composition. Therefore, even when a sulfonic acid solution is added, a sulfonic acid compound containing Li is formed. To more easily achieve the effects of the present application, a Li compound or a Li compound solution may be added to the cake-like composition or the powder-like composition together with the sulfonic acid solution, or a mixed solution prepared by premixing the sulfonic acid solution with the Li compound or the Li compound solution may be added to the cake-like composition or the powder-like composition. The Li compound is, for example, LiOH, and the Li compound solution is, for example, a LiOH solution prepared by dissolving LiOH in water. The amounts of the Li compound and the sulfonic acid solution added to the cake-like composition preferably satisfy the relationship of 0≦Li compound / sulfonic acid≦1.3 in molar ratio. The amount of the sulfonic acid compound or sulfonic acid added is preferably 0.1% by mass to 1% by mass, more preferably 0.3% by mass to 0.8% by mass, relative to the mass of the lithium-containing transition metal composite oxide. The concentrations of the sulfonic acid solution and the sulfonic acid compound solution are, for example, 0.5% by mass to 40% by mass. The addition step may be carried out during the washing step, after the washing step, during the drying step, or after the drying step, and the timing of the addition step can be changed as appropriate.
[0049] A metal compound containing one or more metal elements selected from the group consisting of Sr, Ca, W, Zr, rare earth elements, and Al, and a nonmetallic compound containing one or more nonmetallic elements selected from the group consisting of P and B can be attached to the surface of the lithium-containing transition metal composite oxide by adding the raw material of the metal compound or nonmetallic compound during the synthesis process, after the synthesis process, during the cleaning process, after the cleaning process, during the drying process, after the drying process, or during the addition process. 2 , Sr(OH) 2 ・8H 2 O, SrO, SrCo 3 , SrSO 4 , Sr(NO 3 ) 2、 SrCl 2 , SrAlO 4 Examples of Ca raw materials include Ca(OH) 2 , CaO, CaCO 3 , CaSO 4 , Ca(NO 3 ) 2、 CaCl 2 , CaAlO 4 The Zr raw material is Zr(OH) 4 , ZrO 2 , Zr(CO 3 ) 2 , Zr(SO 4 ) 2 ・4H 2 Examples of rare earth raw materials include oxides, hydroxides, and carbonates of rare earth elements. Examples of W raw materials include tungsten oxide (WO 3 ), lithium tungstate (Li 2 WO 4 , Li 4 WO 5 , Li 6 W 2 O 9 As the W raw material, a solution containing W may be used. As the Al raw material, Al 2 O 3、 Al(OH) 3、 Al 2 (SO 4 ) 3The P raw material may be Al derived from a lithium-containing transition metal composite oxide. 3-x H x P.O. 4 (0≦x≦3) and the like. 3 BO 3 , Li 3 BO 3 , Li 2 B 4 O 7 These compounds may be pulverized to appropriately change the particle shape or particle size, or may be used as hydrates with the water content adjusted.
[0050] The PTFE contained in the positive electrode mixture layer 31 is a dry powder, not a powder dispersed in a dispersion such as water. This allows the positive electrode mixture layer to be produced by a dry process described below. In addition to PTFE, the positive electrode mixture layer 31 may also contain a binder that does not fibrillate (fiberize), such as polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), nitrile-butadiene rubber (NBR), polyimide resin, acrylic resin, or polyolefin resin. The positive electrode mixture layer 31 may also contain a fibrillating binder other than PTFE, as long as it does not impair the objectives of the present disclosure.
[0051] The PTFE content in the positive electrode mixture layer 31 is preferably 0.05% by mass to 5% by mass, and more preferably 1% by mass to 3% by mass. In this case, the diffusibility of the nonaqueous electrolyte in the positive electrode mixture layer is further improved, and the reaction distribution in the thickness direction of the positive electrode mixture layer is more uniform. As a result, the cycle characteristics of the battery are significantly improved. PTFE adheres to the particle surfaces of the positive electrode active material and is entangled with the positive electrode active material. In other words, the positive electrode active material is held in place by the PTFE present in a network structure.
[0052] PTFE includes fibrillated (fiberized) PTFE fibers. PTFE fibers are formed by fibrillating PTFE raw material (PTFE particles) that belongs to a fibrillable fine powder through a mixing step described below. The median diameter of the PTFE fibers is preferably 2 μm to 20 μm. The median diameter of the PTFE fibers can be measured with a particle size distribution analyzer. A median diameter of the PTFE fibers of 2 μm to 20 μm means that the PTFE fibers are finely divided into PTFE particles.
[0053] As described above, most PTFE particles are fibrillated to form PTFE fibers, but PTFE may contain PTFE particles that remain unfibrillated. The PTFE particles may be secondary particles. The average particle size of the PTFE particles is, for example, 100 μm to 700 μm, preferably 100 μm to 500 μm, and more preferably 100 μm to 400 μm. The average particle size of the PTFE particles can be determined by observing the particles of the PTFE raw material with an SEM. Specifically, the external shapes of 100 randomly selected particles are identified, and the major axis (longest diameter) of each of the 100 particles is determined, and the average value is taken as the average particle size of the PTFE particles.
[0054] The PTFE contains, for example, fibrous particles having an aspect ratio of 1.5 or more, at a rate of 20% or more relative to the total particles, and the average major axis size of the fibrous particles is 1 μm to 20 μm. By using the PTFE containing the fibrous particles, it is possible to produce a positive electrode mixture layer that has good moldability and high breaking strength.
[0055] The ratio of fibrous particles to all particles can be calculated as follows: (1) PTFE containing fibrous particles is imaged using a scanning electron microscope (SEM). The imaging magnification can be, for example, 300 to 1000 times. (2) The image is imported into a computer, and all particles are separated into fibrous particles and particles with an aspect ratio of less than 1.5 using image analysis software such as ImageJ. (3) The number of fibrous particles is divided by the number of all particles, i.e., the sum of the number of fibrous particles and the number of particles with an aspect ratio of less than 1.5, to calculate the ratio of fibrous particles to all particles.
[0056] The average major axis size of the fibrous particles can be calculated, similar to the calculation of the ratio of the fibrous particles to the total particles described above, by analyzing the SEM image with image analysis software, measuring the major axis size (major axis length) of 100 fibrous particles with an aspect ratio of 1.5 or more, and averaging the measured values.
[0057] The average aspect ratio of the fibrous particles may be 2 to 20. The average aspect ratio of the fibrous particles can be calculated, similarly to the calculation of the average major axis size described above, by analyzing SEM images with image analysis software, measuring the aspect ratios (major axis / minor axis) of 100 fibrous particles having an aspect ratio of 1.5 or more, and averaging the measured values.
[0058] PTFE containing fibrous particles can be produced by fibrillating PTFE raw material (PTFE particles), a fine powder that can be fibrillated, using a dry grinder such as a jet mill grinder. The PTFE raw material may be secondary particles. The average particle size of the PTFE raw material is, for example, 100 μm to 700 μm, preferably 100 μm to 500 μm, and more preferably 100 μm to 400 μm. The average particle size of the PTFE raw material can be determined by observing the PTFE raw material particles with an SEM. Specifically, the outer shapes of 100 randomly selected particles are identified, and the major axis (longest diameter) of each of the 100 particles is determined, and the average value is taken as the average particle size of the PTFE raw material. When producing PTFE powder containing fibrous particles using a jet mill grinder, the ratio of fibrous particles to all particles can be adjusted to 20% or more by appropriately adjusting the supply rate of the PTFE raw material, the grinding pressure, etc.
[0059] Here, when the positive electrode mixture layer 31 is divided into three equal parts in the thickness direction and, from the positive electrode core 30 side, is divided into a first region, a second region, and a third region, the PTFE content (s) in the first region, the PTFE content (t) in the second region, and the PTFE content (u) in the third region preferably satisfy (u-s) / (s+t+u)≦±10%, and more preferably satisfy (u-s) / (s+t+u)≦±5%. As a result, PTFE is present substantially uniformly throughout the thickness direction of the positive electrode mixture layer 31, without being ubiquitous in some areas. Note that, by using a dry process described later, PTFE can be present substantially uniformly throughout the positive electrode mixture layer 31.
[0060] Furthermore, the positive electrode mixture layer 31 preferably has a mixture resistance of 20 Ωcm or less. This can improve the output characteristics of the battery. The mixture resistance is the resistance of the positive electrode mixture layer 31 only. The mixture resistance can be measured, for example, using an electrode resistance measurement system manufactured by Hioki E.E. Corporation, as follows: (1) Prepare a positive electrode 11 cut to a size of 20 mm x 50 mm. (2) Measure the thickness of the positive electrode mixture layer 31 and the thickness of the positive electrode core 30, and input them as measurement parameters into the measurement conditions. (3) Select appropriate main current and voltage ranges. (4) Set the positive electrode 11 in a predetermined position, contact it with a probe, and measure the mixture resistance.
[0061] The positive electrode 11, which is an example of the embodiment, can be manufactured by the following method. Note that the manufacturing method described here is just an example, and the manufacturing method of the positive electrode 11 is not limited to this method.
[0062] 3 to 5 are diagrams schematically illustrating the manufacturing process of a positive electrode 11 according to an embodiment. The manufacturing method of the positive electrode 11 includes a mixing step shown in FIG. 3, a stretching step shown in FIG. 4, and a bonding step shown in FIG. 5. In the mixing step, a positive electrode active material and PTFE are mixed to produce positive electrode mixture particles 32 having a solids concentration of substantially 100%. In the stretching step, the positive electrode mixture particles 32 are kneaded and stretched to form a sheet, thereby producing a positive electrode mixture sheet 33. In the bonding step, the positive electrode 11 is produced by bonding the positive electrode mixture sheet 33 to a positive electrode core 30.
[0063] The manufacturing method of the positive electrode 11 is a dry process for manufacturing the positive electrode 11 using a positive electrode mixture layer 31 having a solid content concentration of substantially 100%. The dry process is a process in which the positive electrode active material particles and the binder particles are mixed without using a solvent, that is, the positive electrode active material and the binder are mixed in a state in which the solid content concentration of the positive electrode 11 is substantially 100%. The manufacturing method of the positive electrode 11 according to the present disclosure does not require the use of a solvent as in the conventional manufacturing method of the positive electrode 11. Here, "no need to use a solvent" means not only that a solvent is not required as a raw material, but also that a solvent drying process is not required, and exhaust equipment and the like related to the drying process are also not required.
[0064] In the mixing step, as shown in FIG. 3 , raw materials such as a positive electrode active material, PTFE, and a conductive agent are mixed in a mixer 40 to produce positive electrode mixture particles 32. The mixer 40 can be, for example, a conventional mechanical agitator mixer. Specific examples of suitable mixers 40 include devices capable of applying mechanical shear force, such as cutter mills, pin mills, bead mills, microparticle composite devices (devices in which shear force is generated between a specially shaped rotor rotating at high speed inside a tank and an impact plate), granulators, and kneaders such as twin-screw extrusion mixers and planetary mixers. Of these, cutter mills, microparticle composite devices, granulators, and twin-screw extrusion mixers are preferred. This allows the PTFE to be fibrillated while the raw materials are mixed. The processing time of the mixing step (the time during which shear force is applied to the materials) is preferably within 15 minutes, and can be, for example, 0.5 to 10 minutes. If the processing time is too long, the amount of conductive agent incorporated into the PTFE increases. In this case, the conductivity of the positive electrode mixture sheet is significantly reduced, and the resistance increases, adversely affecting the battery characteristics.
[0065] The mixing step may include a step of mixing a positive electrode active material and a conductive agent to prepare a coated positive electrode active material, and a step of mixing the coated positive electrode active material with PTFE. By using a coated positive electrode active material prepared by mixing a positive electrode active material and a conductive agent, the time required to mix the coated positive electrode active material and PTFE can be shortened. This reduces the amount of conductive agent incorporated into PTFE. The coverage of the conductive agent on the surface of the coated positive electrode active material is, for example, 10% to 60%. It is preferable that the surface of the coated positive electrode active material has irregularities, and the conductive agent penetrates and adheres to the recesses in the irregularities. This makes it difficult for the conductive agent on the surface of the coated positive electrode active material to be absorbed by PTFE during the mixing process of the coated positive electrode active material and PTFE.
[0066] The dry mixing of the positive electrode active material and the conductive agent may be performed, for example, by mechanofusion. Mechanofusion is a dry processing method carried out in a mechanofusion reactor having a cylindrical chamber equipped with a compression tool and rotating at high speed. The conductive agent and the positive electrode active material are placed in the chamber, and by rotating the chamber, the particles are pressed against each other and against the chamber wall. The use of a compression tool and the generation of centrifugal force by high-speed rotation promotes adhesion and bonding between the conductive agent and the positive electrode active material. Examples of mechanofusion reactors include the "Nobilta" (registered trademark) or "Mechanofusion" (registered trademark) crushers manufactured by Hosokawa Micron Corporation (Japan), the "Hybridizer" (trademark) crusher manufactured by Nara Machinery Works, Ltd., the "Balance Gran" crusher manufactured by Freund Turbo Corporation, and the "COMPOSI" crusher manufactured by Nippon Coke & Engineering Co., Ltd.
[0067] Next, in the stretching step, as shown in FIG. 4 , the positive electrode mixture particles 32 are kneaded and stretched using a pair of rolls 41 to form a sheet. The pair of rolls 41 are arranged with a predetermined gap between them and rotate in the same direction. The positive electrode mixture particles 32 are supplied to the gap between the pair of rolls 41, and are compressed by the pair of rolls 41 and stretched into a sheet. The linear pressure applied by the pair of rolls 41 is, for example, 1 t / cm to 3 t / cm. The pair of rolls 41 have, for example, the same roll diameter. The temperature of the pair of rolls 41 is not particularly limited and may be, for example, room temperature or higher.
[0068] The obtained positive electrode mixture sheet 33 is passed again between the pair of rolls 41, whereby the PTFE is loosened and dispersed. In other words, by passing the positive electrode mixture particles 32 between the pair of rolls 41 two or more times, the in-plane dispersion of the PTFE is improved. The number of times that the positive electrode mixture particles 32 and the positive electrode mixture sheet 33 formed from the positive electrode mixture particles 32 are passed between the pair of rolls 41 is preferably 2 to 50 times, more preferably 3 to 40 times, and particularly preferably 5 to 20 times. The stretching step is not limited to a method using only one pair of rolls, and may include a step of stretching using another pair of rolls having a different roll diameter, circumferential speed, gap, etc.
[0069] The thickness of the positive electrode mixture sheet 33 obtained after the stretching step can be controlled by, for example, the gap between the pair of rolls 41, the circumferential speed, the number of stretching treatments, etc. In the stretching step, it is preferable to form the positive electrode mixture particles 32 into a sheet using a pair of rolls 41 whose circumferential speed ratio differs by two or more times. By making the circumferential speed ratio of the pair of rolls 41 different, for example, it becomes easier to thin the positive electrode mixture sheet 33, improving productivity. The density of the positive electrode active material in the positive electrode mixture sheet 33 is, for example, 3.2 g / cm 3 ~4.0 g / cm 3 be.
[0070] Next, in the bonding step, as shown in FIG. 5 , the positive electrode mixture sheet 33 is bonded to the positive electrode core 30, thereby obtaining a positive electrode 11 in which a mixture layer made of the positive electrode mixture layer 31 is provided on the surface of the positive electrode core 30. While FIG. 5 shows a state in which the positive electrode mixture layer 31 is bonded to only one surface of the positive electrode core 30, it is preferable that the positive electrode mixture layer 31 be bonded to both surfaces of the positive electrode core 30. Two positive electrode mixture layers 31 may be bonded to both surfaces of the positive electrode core 30 simultaneously, or one may be bonded to one surface of the positive electrode core 30 and then the other may be bonded to the other surface. Furthermore, the positive electrode mixture sheet 33 may be bonded to the positive electrode core 30 via an adhesive layer or the like.
[0071] In the laminating step, the positive electrode mixture sheet 33 is laminated to the surface of the positive electrode core 30 using a pair of rolls 42. The pair of rolls 42, for example, have the same roll diameter, are arranged with a predetermined gap between them, and rotate in the same direction at the same peripheral speed. The temperature of the pair of rolls 42 is, for example, 25°C to 300°C. The linear pressure applied by the pair of rolls 42 is preferably 0.1 t / cm to 5 t / cm, and more preferably 0.2 t / cm to 3 t / cm.
[0072] [Negative Electrode] The negative electrode 12 may have, for example, a negative electrode core and a negative electrode mixture layer formed on the surface of the negative electrode core, or a metal Li foil may be used as the negative electrode 12. Alternatively, the negative electrode 12 may have a negative electrode core, and lithium metal may be deposited on the surface of the negative electrode core upon charging. When the negative electrode 12 has a negative electrode mixture layer, the negative electrode mixture layer is preferably formed on both sides of the negative electrode core. The negative electrode core may be made of a foil of a metal that is stable within the potential range of the negative electrode 12, such as copper or a copper alloy, or a film with such a metal disposed on the surface layer. The thickness of the negative electrode core is, for example, 5 μm to 30 μm. The negative electrode mixture layer includes, for example, a negative electrode active material and a binder. The thickness of the negative electrode mixture layer is, for example, 10 μm to 150 μm on one side of the negative electrode core. The negative electrode 12 can be produced, for example, by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, etc. to the surface of a negative electrode core, drying the coating, and then rolling it to form a negative electrode mixture layer on both sides of the negative electrode core.
[0073] The negative electrode active material contained in the negative electrode mixture layer is not particularly limited as long as it can reversibly absorb and release lithium ions, and generally, carbon materials such as graphite are used. Graphite may be any of natural graphite such as flake graphite, lump graphite, and amorphous graphite, or artificial graphite such as lump artificial graphite and graphitized mesophase carbon microbeads. Furthermore, metals that alloy with Li, such as Si and Sn, metal compounds containing Si, Sn, and lithium-titanium composite oxides may also be used as the negative electrode active material. Furthermore, those provided with a carbon coating may also be used. For example, SiO x (0.5≦x≦1.6) or Li 2y SiO (2+y) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0<y<2) may be used in combination with graphite.
[0074] Examples of binders contained in the negative electrode mixture layer include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.
[0075] [Separator] A porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have a single-layer structure or a multi-layer structure. Furthermore, a highly heat-resistant resin layer such as an aramid resin may be formed on the surface of the separator 13.
[0076] A filler layer containing an inorganic filler may be formed at the interface between the separator 13 and at least one of the positive electrode 11 and the negative electrode 12. Examples of inorganic fillers include oxides and phosphate compounds containing metal elements such as Ti, Al, Si, and Mg. The filler layer can be formed by applying a slurry containing the filler to the surface of the positive electrode 11, the negative electrode 12, or the separator 13.
[0077] [Non-aqueous electrolyte] The non-aqueous electrolyte has ion conductivity (for example, lithium ion conductivity). The non-aqueous electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.
[0078] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent that can be used include esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen atoms in these solvents are substituted with halogen atoms such as fluorine. Examples of the halogen-substituted compound include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylic acid esters such as methyl fluoropropionate (FMP).
[0079] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylic acid esters such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).
[0080] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, and methyl phenyl ether. and chain ethers such as ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
[0081] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiClO 4 , LiBF 4 , LiPF 6 , LiAlCl 4 , LiSbF 6 , LiSCN, LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiB 10 Cl 10 , lower aliphatic lithium carboxylates, LiCl, LiBr, LiI, phosphates, borates, and imide salts. Examples of phosphates include lithium difluorophosphate (LiPO 2 F 2Examples of the borate salt include lithium bis(oxalato)borate (LiBOB) and lithium difluoro(oxalato)borate (LiDFFOB). Examples of the imide salt include lithium bisfluorosulfonylimide (LiN(FSO 2 ) 2 ), lithium bistrifluoromethanesulfonyl imide (LiN(CF 3 SO 2 ) 2 ), lithium trifluoromethanesulfonate nonafluorobutanesulfonate imide (LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 )), lithium bispentafluoroethanesulfonyl imide (LiN(C 2 F 5 SO 2 ) 2 Among these, LiPF is preferred from the viewpoint of ionic conductivity, electrochemical stability, etc. 6 The concentration of the lithium salt may be, for example, 4 mol or less, or 3 mol or less, preferably 1.8 mol or less, and more preferably 0.8 to 1.8 mol per liter of the non-aqueous solvent.
[0082] The non-aqueous electrolyte may contain an additive such as an unsaturated carbonate ester, an acid anhydride, a phenol compound, a benzene compound, a nitrile compound, an isocyanate compound, a sultone compound, a sulfate compound, a borate ester compound, a phosphate ester compound, or a phosphite ester compound.
[0083] Examples of unsaturated cyclic carbonates include vinylene carbonate, 4-methylvinylene carbonate, 4,5-dimethylvinylene carbonate, 4-ethylvinylene carbonate, 4,5-diethylvinylene carbonate, 4-propylvinylene carbonate, 4,5-dipropylvinylene carbonate, 4-phenylvinylene carbonate, 4,5-diphenylvinylene carbonate, vinylethylene carbonate, and divinylethylene carbonate. One type of unsaturated cyclic carbonate may be used alone, or two or more types may be used in combination. Some of the hydrogen atoms in the unsaturated cyclic carbonate may be substituted with fluorine atoms. The acid anhydride may be an anhydride formed by intermolecular condensation of multiple carboxylic acid molecules, but is preferably an acid anhydride of a polycarboxylic acid. Examples of polycarboxylic acid anhydrides include succinic anhydride, maleic anhydride, and phthalic anhydride.
[0084] Examples of phenol compounds include phenol, hydroxytoluene, etc. Examples of benzene compounds include fluorobenzene, hexafluorobenzene, cyclohexylbenzene (CHB), etc.
[0085] Examples of nitrile compounds include adiponitrile, pimelonitrile, propionitrile, and succinonitrile. Examples of isocyanate compounds include methyl isocyanate (MIC), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), and bisisocyanatomethylcyclohexane (BIMCH). Examples of sultone compounds include propane sultone and propene sultone. Examples of sulfate compounds include ethylene sulfate, ethylene sulfite, dimethyl sulfate, and lithium fluorosulfate. Examples of borate ester compounds include trimethyl borate and tris(trimethylsilyl)borate. Examples of phosphate ester compounds include trimethyl phosphate and tris(trimethylsilyl)phosphate. Examples of phosphite ester compounds include trimethyl phosphite and tris(trimethylsilyl)phosphite.
[0086] As the solid electrolyte, for example, a solid or gel-like polymer electrolyte, an inorganic solid electrolyte, etc. can be used. As the inorganic solid electrolyte, a material known in all-solid-state lithium ion secondary batteries, etc. (for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a halogen-based solid electrolyte, etc.) can be used. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs the non-aqueous solvent and gels is used. As the polymer material, for example, a fluororesin, an acrylic resin, a polyether resin, etc. can be used.
[0087] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0088] Example 1 Preparation of Positive Electrode Active Material [Ni 0.90 Co 0.05 Al 0.05 ](OH) 2The composite hydroxide represented by the formula (1) was calcined at 500°C for 8 hours to obtain a metal oxide containing Ni, Co, and Al. Next, lithium hydroxide monohydrate (LiOH·H) was added to the composite hydroxide represented by the formula (1) so that the molar ratio of Li to the total amount of Ni, Co, and Al was 1:1.03. 2 O) was mixed to obtain a mixture. Then, this mixture was placed under an oxygen flow (10 cm) with an oxygen concentration of 95%. 3 The mixture was heated from room temperature to 650°C at a temperature increase rate of 2.0°C / min under a temperature of 2 mL / min per kg of the mixture and 5 L / min per kg of the mixture, and then heated from 650°C to 740°C at a temperature increase rate of 0.5°C / min to obtain a lithium-containing transition metal composite oxide (synthesis step).
[0089] Water was added to the obtained lithium-containing transition metal composite oxide so that the slurry concentration was 1500 g / L, and the mixture was stirred for 15 minutes and filtered to obtain a cake-like composition (washing step). Powdered lithium methanesulfonate was then added to the obtained cake-like composition (addition step). The obtained cake-like composition was then dried under vacuum at 180°C for 2 hours to obtain a powder-like composition (drying step). The amount of lithium methanesulfonate added was 0.1 mass% relative to the total mass of the lithium-containing transition metal composite oxide. Furthermore, Fourier transform infrared spectroscopy (FT-IR) confirmed the presence of lithium methanesulfonate on the surface of the secondary particles of the lithium-containing transition metal composite oxide. The amount of alkaline component in the positive electrode active material determined by the above-described method was 50 μmol / g.
[0090] [Preparation of Positive Electrode] The positive electrode of Example 1 was prepared through a process (dry process) in which positive electrode active material particles and binder particles were mixed without using a solvent. More specifically, a lithium-containing transition metal composite oxide, acetylene black (AB), and PTFE particles were added to a mixer (Osaka Chemical, Wonder Crusher) in a mass ratio of 100:1:2, and mixed at room temperature for 5 minutes at a rotation speed of 3 (mixing step). The rotation speed of the Wonder Crusher was 28,000 rpm, the maximum rotation speed of 10. This mixing process resulted in positive electrode mixture particles in which the positive electrode active material and PTFE were uniformly dispersed. The resulting positive electrode mixture had a solids concentration of 100%.
[0091] The obtained positive electrode mixture particles were passed through a pair of rolls five times and stretched while being kneaded to prepare a positive electrode mixture sheet (stretching step). The peripheral speed ratio of the pair of rolls was set to 1:3, and the thickness of the positive electrode mixture sheet was adjusted to approximately 100 μm. The prepared positive electrode mixture sheet was then placed on the surface of a positive electrode core, and the laminate of the positive electrode mixture sheet and the positive electrode core was pressed (linear pressure: 1.0 t / cm) using two rolls to obtain a positive electrode (lamination step). Note that an aluminum alloy foil was used as the positive electrode core.
[0092] For the prepared positive electrode, the positive electrode mixture layer was divided into three equal parts in the thickness direction, and the first, second, and third regions were measured from the positive electrode core side. The transition metal content and fluorine (F) content were measured in each region by energy dispersive XRD (EDS). Then, from the ratio of the fluorine content to the transition metal content, the PTFE content (s) in the first region, the PTFE content (t) in the second region, and the PTFE content (u) in the third region were calculated. In the positive electrode of Example 1, s, t, and u were 32%, 33%, and 35%, respectively, and (u-s) / (s+t+u) was 3%.
[0093] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF 6 ) was dissolved in the solution to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0094] [Preparation of Test Cell] A positive electrode lead was attached to the exposed portion of the positive electrode, and a negative electrode lead was attached to the lithium metal foil serving as the negative electrode. The positive electrode and the negative electrode were spirally wound with a polyolefin separator interposed therebetween to prepare a wound electrode assembly. This electrode assembly was housed in an exterior body made of an aluminum laminate sheet, and the nonaqueous electrolyte was poured into the exterior body. The opening of the exterior body was then sealed to obtain a test cell.
[0095] [Evaluation of Output Characteristics] The test cell was subjected to constant current charging at 0.2 C in a temperature environment of 25°C until the battery voltage reached 4.3 V (vs. Li), and constant voltage charging at 4.3 V until the current value reached 0.02 C. After a 1-hour pause, the cell was discharged at a constant current of 0.2 C until the battery voltage reached 2.5 V, as an initial charge / discharge. Next, the cell was again subjected to constant current charging at 0.2 C until the battery voltage reached 4.3 V, and constant voltage charging at 4.3 V until the current value reached 0.02 C. After a 1-hour pause, the cell was discharged at 1 C until the battery voltage reached 2.5 V, and then further discharged at 0.01 C until the battery voltage reached 2.5 V. The initial output was calculated using the following formula: Initial output = 1 C discharge capacity / (1 C discharge capacity + 0.01 C discharge capacity).
[0096] [Evaluation of cycle characteristics] The test cell was charged to 4.3 V (vs. Li) at a constant current of 0.2 C in a temperature environment of 25°C, and then charged to 0.02 C at a constant voltage of 4.3 V. Thereafter, the test cell was discharged to 2.5 V at a constant current of 0.2 C. This charge / discharge cycle constituted one cycle, and this cycle was repeated 30 times. The capacity retention rate was calculated using the following formula: Capacity retention rate = (discharge capacity at 30th cycle / discharge capacity at 1st cycle) x 100
[0097] [Evaluation of Gas Generation Amount] The test cell was charged to 4.3 V (vs. Li) at a constant current of 0.2 C in a temperature environment of 25 °C, and then constant-voltage charged at 4.3 V until the current value reached 0.01 C, completing the charge. After a 10-minute pause, the cell was discharged to 2.5 V at a constant current of 0.1 C. After two charge / discharge cycles, the volume of the test cell, which had undergone only one charge cycle, was measured using the buoyancy method (Archimedes method). The pause between cycles was 10 minutes. The charged test cell was stored in a thermostatic chamber at 85 °C for 3 hours. After storage, the test cell was cooled to room temperature and the volume was measured again using the buoyancy method. The difference between the volume before and after storage was taken as the amount of gas generation, normalized per 1 g of positive electrode active material.
[0098] Example 2 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing the positive electrode active material, the amount of lithium methanesulfonate added was 0.5 mass % relative to the total mass of the lithium-containing transition metal composite oxide.
[0099] Example 3 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing the positive electrode active material, the amount of lithium methanesulfonate added was 1.0 mass % relative to the total mass of the lithium-containing transition metal composite oxide.
[0100] Example 4 A test cell was prepared and evaluated in the same manner as in Example 1, except that in the addition step of preparing the positive electrode active material, a lithium methanesulfonate solution prepared by dissolving lithium methanesulfonate in pure water was added instead of powdered lithium methanesulfonate, and the amount of lithium methanesulfonate added was 0.5% by mass relative to the total mass of the lithium-containing transition metal composite oxide. The concentration of the added lithium methanesulfonate solution was 10% by mass, and the lithium methanesulfonate solution was added so that the amount of lithium methanesulfonate added was as described above.
[0101] Example 5 A test cell was prepared and evaluated in the same manner as in Example 1, except that in the addition step of preparing the positive electrode active material, a diluted solution of methanesulfonic acid was added instead of powdered lithium methanesulfonate, and the amount of methanesulfonic acid added was 0.5 mass% relative to the total mass of the lithium-containing transition metal composite oxide. The concentration of the added methanesulfonic acid solution was 10 mass%, and the methanesulfonic acid solution was added so that the amount of methanesulfonic acid added was as described above.
[0102] Example 6 A test cell was prepared and evaluated in the same manner as in Example 1, except that in the addition step of preparing the positive electrode active material, a solution containing methanesulfonic acid and LiOH (hereinafter referred to as a methanesulfonic acid + LiOH solution) prepared by dissolving methanesulfonic acid and LiOH in pure water at a molar ratio of 1:0.5 was added instead of powdered lithium methanesulfonate, and the amount of lithium methanesulfonate added was 0.5 mass% relative to the total mass of the lithium-containing transition metal composite oxide. The concentration of the added methanesulfonic acid + LiOH solution was 10 mass%, and the methanesulfonic acid + LiOH solution was added so that the amount of lithium methanesulfonate added was as described above.
[0103] Example 7 A test cell was prepared and evaluated in the same manner as in Example 1, except that in the addition step of preparing the positive electrode active material, a methanesulfonic acid + LiOH solution prepared by dissolving methanesulfonic acid and LiOH in pure water at a molar ratio of 1:1 was added instead of powdered lithium methanesulfonate, and the amount of lithium methanesulfonate added was 0.5 mass% relative to the total mass of the lithium-containing transition metal composite oxide. The concentration of the added methanesulfonic acid + LiOH solution was 10 mass%, and the methanesulfonic acid + LiOH solution was added so that the amount of lithium methanesulfonate added was as described above.
[0104] Example 8 A test cell was prepared and evaluated in the same manner as in Example 1, except that in the addition step of preparing the positive electrode active material, a lithium ethanesulfonate solution prepared by dissolving lithium ethanesulfonate in pure water was added instead of powdered lithium methanesulfonate, and the amount of lithium ethanesulfonate added relative to the total mass of the lithium-containing transition metal composite oxide was 0.5% by mass. The concentration of the added lithium ethanesulfonate solution was 10% by mass, and the lithium ethanesulfonate solution was added so that the amount of lithium ethanesulfonate added was as described above. The presence of lithium ethanesulfonate on the surface of the positive electrode active material was confirmed by Fourier transform infrared spectroscopy (FT-IR).
[0105] Example 9 A test cell was prepared and evaluated in the same manner as in Example 1, except that in the addition step of preparing the positive electrode active material, a sodium methanesulfonate solution prepared by dissolving sodium methanesulfonate in pure water was added instead of powdered lithium methanesulfonate, and the amount of sodium methanesulfonate added relative to the total mass of the sodium-containing composite oxide was 0.5% by mass. The concentration of the added sodium methanesulfonate solution was 10% by mass, and the sodium methanesulfonate solution was added so that the amount of sodium methanesulfonate added was as described above. The presence of sodium methanesulfonate on the surface of the positive electrode active material was confirmed by Fourier transform infrared spectroscopy (FT-IR).
[0106] Example 10 A test cell was prepared and evaluated in the same manner as in Example 4, except that in the preparation of the positive electrode active material, the water washing step was not performed and the amount of lithium methanesulfonate added relative to the total mass of the lithium-containing transition metal composite oxide in the addition step was 0.1 mass %. The amount of the alkaline component in the positive electrode active material was 300 μmol / g.
[0107] Example 11 A test cell was prepared and evaluated in the same manner as in Example 4, except that in the preparation of the positive electrode active material, the water washing step was not performed and the amount of lithium methanesulfonate added relative to the total mass of the lithium-containing transition metal composite oxide in the addition step was 0.5 mass %. The amount of the alkaline component in the positive electrode active material was 200 μmol / g.
[0108] Comparative Example 1: In the preparation of the positive electrode active material, the addition process was not performed. Instead of the dry process described above, the positive electrode was prepared by a process (wet process) in which the positive electrode active material particles and the binder particles were mixed using a solvent. More specifically, in the preparation of the positive electrode, the positive electrode active material, acetylene black (AB), and polyvinylidene fluoride were mixed in a mass ratio of 92:5:3, and a positive electrode mixture slurry was prepared using N-methyl-2-pyrrolidone (NMP) as a dispersion medium. The positive electrode mixture slurry was then applied to a positive electrode core made of aluminum foil, the coating was dried and compressed, and the positive electrode core was cut to a predetermined electrode size to obtain a positive electrode in which a positive electrode mixture layer was disposed on both sides of the positive electrode core. A test cell was prepared and evaluated in the same manner as in Example 1, except for the above steps.
[0109] Comparative Example 2 A test cell was prepared and evaluated in the same manner as in Example 1, except that in the addition step of preparing the positive electrode active material, the amount of lithium methanesulfonate added relative to the total mass of the lithium-containing transition metal composite oxide was 0.5% by mass, and in preparing the positive electrode, the positive electrode was prepared via a wet process rather than a dry process. More specifically, in preparing the positive electrode, the positive electrode active material, acetylene black (AB), and polyvinylidene fluoride were mixed in a mass ratio of 92:5:3, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode mixture slurry. The positive electrode mixture slurry was then applied to a positive electrode core made of aluminum foil, the coating was dried and compressed, and the positive electrode core was cut to a predetermined electrode size to obtain a positive electrode in which a positive electrode mixture layer was disposed on both sides of the positive electrode core.
[0110] Comparative Example 3 A test cell was produced and evaluated in the same manner as in Example 1, except that the addition step was not carried out in the production of the positive electrode active material.
[0111] Comparative Example 4 A test cell was produced and evaluated in the same manner as in Example 1, except that the addition step was not carried out in the production of the positive electrode active material.
[0112] Comparative Example 5 A test cell was produced and evaluated in the same manner as in Example 4, except that in the addition step of producing a positive electrode active material, a 10 mass % lithium succinate solution was added instead of the methanesulfonic acid solution, and the amount of lithium succinate added was 0.5 mass % with respect to the total mass of the lithium-containing transition metal composite oxide.
[0113] <Comparative Example 6> A test cell was produced and evaluated in the same manner as in Example 4, except that in the addition step of producing a positive electrode active material, a 10 mass % lithium oxalate solution was added instead of the methanesulfonic acid solution, and the amount of lithium oxalate added relative to the total mass of the lithium-containing transition metal composite oxide was 0.5 mass %.
[0114] Table 1 shows the initial output, capacity retention, and gas increase of the test cells of Examples 1 to 11 and Comparative Examples 1 to 6. Table 1 also shows the presence or absence of a water washing step in the preparation of the positive electrode active material, the added compounds, the addition method, the addition amount, the amount of alkali in the positive electrode active material, the positive electrode coating method, and the PTFE contents (s, t, u) of the first, second, and third regions in the positive electrode mixture layer. The initial output, capacity retention, and gas increase of the test cells of Examples 1 to 11 and Comparative Examples 1 to 6 shown in Table 1 are expressed relative to the initial output, capacity retention, and gas increase of the test cell of Comparative Example 1, which are set to 100. A larger initial output value indicates better output characteristics, and a larger capacity retention value indicates better cycle characteristics during high-rate charging.
[0115]
[0116] As shown in Table 1, the test cells of the examples have improved initial output while ensuring a sufficient capacity retention rate, compared to the test cells of the comparative examples. In other words, by having a sulfonic acid compound present on the surfaces of the secondary particles and by having the PTFE content distribution in the positive electrode mixture layer satisfy (u-s) / (s+t+u)≦±10%, a nonaqueous electrolyte secondary battery with improved cycle characteristics and output characteristics can be provided.
[0117] On the other hand, the test cell of Comparative Example 2, in which the positive electrode was produced by a wet process and the PTFE content distribution was (u-s) / (s+t+u)>±10% while lithium sulfonate was present on the surface of the secondary particles, had an improved initial output but a worsened capacity retention rate compared to the test cell of Comparative Example 1. This is presumably because the mere presence of lithium sulfonate on the surface of the secondary particles does not improve the diffusibility of the non-aqueous electrolyte in the positive electrode mixture layer, resulting in a distribution of reaction in the thickness direction of the positive electrode mixture layer.
[0118] Furthermore, the test cells of Comparative Examples 3 and 4, in which the positive electrode was produced by a dry process and the PTFE content distribution satisfied (u-s) / (s+t+u)≦±10% but no lithium sulfonate was present on the surface of the secondary particles, showed improved capacity retention but no improved initial output compared to the test cell of Comparative Example 1. Furthermore, the test cells of Comparative Examples 5 and 6, in which lithium succinate or lithium oxalate was present on the surface of the secondary particles instead of lithium sulfonate, showed improved capacity retention but no improved initial output compared to the test cell of Comparative Example 1.
[0119] Example 12 In the synthesis process for producing a positive electrode active material, the composition of the composite hydroxide was changed to [Ni 0.90 Mn 0.10 ](OH) 2 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step, the amount of lithium methanesulfonate added was changed to 0.5 mass % relative to the total mass of the lithium-containing transition metal composite oxide.
[0120] Example 13 In the synthesis process for producing a positive electrode active material, the composition of the composite hydroxide was changed to [Ni 0.90 Mn 0.10 ](OH) 2 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step, the amount of lithium methanesulfonate added was changed to 0.5 mass % relative to the total mass of the lithium-containing transition metal composite oxide.
[0121] Comparative Example 7 In the synthesis step of producing the positive electrode active material, the composition of the composite hydroxide was changed to [Ni 0.90 Mn 0.10 ](OH) 2 A test cell was prepared and evaluated in the same manner as in Comparative Example 1, except that the temperature was changed to
[0122] Comparative Example 8 In the synthesis step of producing the positive electrode active material, the composition of the composite hydroxide was changed to [Ni 0.90 Mn 0.10 ](OH) 2A test cell was produced and evaluated in the same manner as in Comparative Example 1, except that in the addition step of producing the positive electrode active material, the amount of lithium methanesulfonate added was changed to 0.5 mass% with respect to the total mass of the lithium-containing transition metal composite oxide.
[0123] Comparative Example 9 In the synthesis step of producing the positive electrode active material, the composition of the composite hydroxide was changed to [Ni 0.90 Mn 0.10 ](OH) 2 A test cell was produced and evaluated in the same manner as in Example 1, except that the addition step was not carried out.
[0124] The initial output, capacity retention rate, and gas increase rate of the test cells of Examples 12 and 13 and Comparative Examples 7 to 9 are shown in Table 2. Table 2 also shows whether a water washing step was performed in the preparation of the positive electrode active material, the added compounds, the addition method, the addition amount, the amount of alkali in the positive electrode active material, the positive electrode coating method, and the PTFE contents (s, t, u) of the first, second, and third regions in the positive electrode mixture layer. The initial output, capacity retention rate, and gas increase rate of the test cells of Examples 12 and 13 and Comparative Examples 7 to 9 shown in Table 2 are expressed relative to the initial output, capacity retention rate, and gas increase rate of the test cell of Comparative Example 7, which are set to 100.
[0125]
[0126] As shown in Table 2, the test cells of the examples have improved initial output while ensuring capacity retention, compared to the test cells of the comparative examples. In other words, by having a sulfonic acid compound present on the surfaces of the secondary particles and having the PTFE content distribution in the positive electrode mixture layer satisfy (u-s) / (s+t+u)≦±10%, it is possible to provide a nonaqueous electrolyte secondary battery with improved output characteristics while ensuring cycle characteristics.
[0127] The present disclosure will be further described by the following embodiments. Configuration 1: A positive electrode for a non-aqueous electrolyte secondary battery, having a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core, the positive electrode mixture layer including a positive electrode active material and PTFE, the positive electrode active material including a lithium-containing transition metal composite oxide having a layered structure, the lithium-containing transition metal composite oxide being represented by the general formula Li x Nia Co b Mn c M d O 2-y (wherein 0.80<x<1.2, 0.75≦a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr), and the secondary particles are formed by agglomeration of primary particles, and the surfaces of the secondary particles are provided with a compound represented by formula (I): A positive electrode for a non-aqueous electrolyte secondary battery, wherein a sulfonic acid compound is present, and when the positive electrode mixture layer is divided into three equal parts in a thickness direction into a first region, a second region, and a third region from the positive electrode core side, the PTFE content (s) in the first region, the PTFE content (t) in the second region, and the PTFE content (u) in the third region satisfy (u−s) / (s+t+u)≦±10%. (wherein A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) Configuration 2: A positive electrode for a non-aqueous electrolyte secondary battery according to Configuration 1, wherein the positive electrode active material has an alkali content of 150 μmol / g or less as measured by the Warder method. Configuration 3: A positive electrode for a non-aqueous electrolyte secondary battery according to Configuration 1 or 2, wherein the PTFE contains fibrous particles having an aspect ratio of 1.5 or more in a proportion of 20% or more relative to all particles, the fibrous particles having an average major axis size of 1 μm or more and 20 μm or less. Configuration 4: A positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 3, wherein the positive electrode active material comprises a coated positive electrode active material in which a conductive agent is adhered to the surfaces of the secondary particles, and a coverage of the conductive agent on the surface of the coated positive electrode active material is 10% to 60%. Configuration 5: The positive electrode for a non-aqueous electrolyte secondary battery according to Configuration 4, wherein the coated positive electrode active material has an uneven surface, and the conductive agent penetrates and adheres to recesses in the uneven surface. Configuration 6: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 5, wherein the positive electrode mixture layer has a mixture resistance of 20 Ωcm or less. Configuration 7: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 6, wherein A is a Group 1 element. Configuration 8: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 7, wherein A is Li. Configuration 9: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 8, wherein R is an alkyl group. Configuration 10: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 9, wherein R is a methyl group. Aspect 11: The positive electrode for a nonaqueous electrolyte secondary battery according to any one of Aspects 1 to 10, wherein the amount of the sulfonic acid compound present on the surface of the lithium-containing transition metal composite oxide is 0.1 mass % or more and 2 mass % or less, based on the mass of the lithium-containing transition metal composite oxide.Configuration 12: A method for manufacturing a positive electrode for a non-aqueous electrolyte secondary battery, comprising: a mixing step of mixing a positive electrode active material including a lithium-containing transition metal composite oxide in which a sulfonic acid compound represented by formula (I) is present on the surfaces of secondary particles with PTFE to prepare positive electrode mixture layer particles having a solids concentration of substantially 100%; a stretching step of passing the positive electrode mixture layer particles between a pair of rolls two or more times to knead and stretch them to prepare a positive electrode mixture layer sheet; and a laminating step of laminating the positive electrode mixture layer sheet to a core to prepare an electrode. (wherein A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)
[0128] REFERENCE SIGNS LIST 10 Non-aqueous electrolyte secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode body, 16 Exterior body, 17 Sealing body, 18, 19 Insulating plate, 20 Positive electrode lead, 21 Negative electrode lead, 22 Grooved portion, 23 Internal terminal plate, 24 Lower valve body, 25 Insulating member, 26 Upper valve body, 27 Cap, 28 Gasket, 30 Positive electrode core, 31 Positive electrode mixture layer, 32 Positive electrode mixture particles, 33 Positive electrode mixture sheet, 40 Mixer, 41, 42 Rolls
Claims
1. A positive electrode for a non-aqueous electrolyte secondary battery having a positive electrode core and a positive electrode mixture layer formed on a surface of the positive electrode core, the positive electrode mixture layer including a positive electrode active material and PTFE, the positive electrode active material including a lithium-containing transition metal composite oxide having a layered structure, the lithium-containing transition metal composite oxide being represented by the general formula Li x Ni a Co b Mn c M d O 2-y (wherein 0.8<x<1.2, 0.75≦a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr), and the secondary particles are formed by agglomeration of primary particles, and a sulfonic acid compound represented by formula (I) is present on the surface of the secondary particles, A positive electrode for a nonaqueous electrolyte secondary battery, in which, when the positive electrode mixture layer is divided into three equal parts in a thickness direction into a first region, a second region, and a third region from the positive electrode core side, the PTFE content (s) in the first region, the PTFE content (t) in the second region, and the PTFE content (u) in the third region satisfy (u-s) / (s+t+u)≦±10%. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) 2. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the positive electrode active material has an alkali content of 150 μmol / g or less as measured by the Warder method.
3. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the PTFE contains fibrous particles having an aspect ratio of 1.5 or more in a proportion of 20% or more of all particles, and the average major axis size of the fibrous particles is 1 μm or more and 20 μm or less.
4. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the positive electrode active material includes a coated positive electrode active material having a conductive agent attached to a surface thereof, and a coverage rate of the conductive agent on the surface of the coated positive electrode active material is 10% to 60%.
5. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 4, wherein the secondary particles of the coated positive electrode active material have uneven surfaces, and the conductive agent penetrates and adheres to the recesses of the uneven surfaces.
6. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the positive electrode mixture layer has a mixture resistance of 20 Ωcm or less.
7. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein A is a Group 1 element.
8. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein A is Li.
9. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein R is an alkyl group.
10. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein R is a methyl group.
11. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the amount of the sulfonic acid compound present on the surface of the lithium-containing transition metal composite oxide is 0.1 mass % or more and 2 mass % or less, based on the mass of the lithium-containing transition metal composite oxide.
12. A method for manufacturing a positive electrode for a non-aqueous electrolyte secondary battery, comprising: a mixing step of mixing a positive electrode active material including a lithium-containing transition metal composite oxide having a sulfonic acid compound represented by formula (I) present on the surfaces of secondary particles with PTFE to prepare positive electrode mixture layer particles having a solid content concentration of substantially 100%; a stretching step of passing the positive electrode mixture layer particles between a pair of rolls two or more times to knead and stretch them to prepare a positive electrode mixture layer sheet; and a bonding step of bonding the positive electrode mixture layer sheet to a core body to prepare an electrode. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)
Citation Information
Patent Citations
High-nickel composite positive electrode material as well as preparation method and application thereof
CN109616657A
Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery
JP2019169286A
Electrode and method for producing electrode
WO2022070542A1
Electrode and electrode manufacturing method
WO2022113498A1
Single-crystal high-nickel positive electrode material and preparation method therefor and application thereof
WO2022227494A1