Electrodeposition liquid and insulating coating film production method

By adding organic acid to the electrodeposition solution, the issue of fine cracks in anionic electrodeposition is resolved, resulting in high-quality insulating films with enhanced insulation properties.

WO2024224964A1PCT designated stage expired Publication Date: 2024-10-31MITSUBISHI MATERIALS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013773
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-02-07
Filing Date
2024-04-03
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The existing anionic electrodeposition method for forming insulating films on conductive substrates often results in fine cracks during the baking process, compromising the insulation properties of the films due to insufficient organic solvent content in the electrodeposition film.

Method used

Incorporating an appropriate amount of organic acid into the electrodeposition solution to optimize the organic solvent content in the film, thereby suppressing the occurrence of cracks and enhancing the insulation properties through pH buffering and improved resin-solvent compatibility.

Benefits of technology

The addition of organic acid effectively prevents minute cracks during the baking process, ensuring the formation of insulating films with superior insulation properties and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013773_31102024_PF_FP_ABST
    Figure JP2024013773_31102024_PF_FP_ABST
Patent Text Reader

Abstract

An electrodeposition liquid for electrodepositing an electrodeposition film on a conductive base material by anionic electrodeposition includes water, an organic solvent, a solid component, a neutralizing agent, and an organic acid. The solid component includes at least a polyimide-based resin. An insulating coating film production method for forming an insulating coating film on the surface of a base material includes: an electrodeposition film forming step (S02) for immersing the base material and a counter electrode in the electrodeposition liquid, and, by using the base material as a positive electrode and the counter electrode as a negative electrode, applying a voltage between the positive electrode and the negative electrode to form an electrodeposition film on the base material; and a baking process (S03) for baking the electrodeposition film.
Need to check novelty before this filing date? Find Prior Art

Description

Electrodeposition solution and method for producing insulating film

[0001] The present invention relates to an electrodeposition solution used for electrodepositing an electrodeposited film on a conductive substrate by anionic electrodeposition, and a method for producing an insulating film. This application claims priority based on Japanese Patent Application No. 2023-070843 filed on April 24, 2023, and Japanese Patent Application No. 2024-017133 filed on February 7, 2024, the contents of which are incorporated herein by reference.

[0002] Insulated conductors, which are made by covering a conductive substrate with an insulating coating made of an insulating resin, are widely used as conductive materials and heat sink materials for various electrical devices that require insulation. Various resins are used as constituent materials for the insulating coating. For example, Patent Document 1 discloses a material using a polyimide-based resin such as a polyamide-imide resin, and Patent Document 2 proposes a material using a mixed resin of a polyimide-based resin and a fluorine-based resin.

[0003] Electrodeposition is a known method for forming an insulating film made of such an insulating resin on the surface of a conductive substrate. The electrodeposition method involves immersing the substrate on which the insulating film is to be formed and a counter electrode in an electrodeposition solution in which the insulating film material is dispersed, and applying a voltage between the substrate and the counter electrode to deposit the insulating film material on the surface of the substrate. The formed electrodeposited film is then heated to bake the electrodeposited film onto the substrate, thereby forming the insulating film.

[0004] Electrodeposition methods include anionic electrodeposition, in which a voltage is applied to the substrate as an anode to form an insulating coating on the surface of the substrate, and cationic electrodeposition, in which a voltage is applied to the substrate as a cathode to form an insulating coating on the surface of the substrate.

[0005] Japanese Unexamined Patent Publication No. 2017-115120 (A) Japanese Unexamined Patent Application No. 2018-070663 (A)

[0006] The anionic electrodeposition solution used in anionic electrodeposition contains solid components including the resin described above, water, an organic solvent, and a neutralizer. When a voltage is applied, the pH decreases near the surface of the anode (substrate), and the solid components precipitate on the surface of the anode (substrate), forming an electrodeposited film. When the electrodeposited film formed on the surface of the anode is baked, fine cracks may occur, making it difficult to ensure the insulating properties of the insulating coating.

[0007] The present invention has been made in view of the above circumstances, and aims to provide an electrodeposition liquid that can suppress the occurrence of fine cracks when baking an electrodeposition film and can form an insulating film with excellent insulating properties, and a method for manufacturing an insulating film using this electrodeposition liquid.

[0008] In order to solve the above problems, the present inventors conducted extensive research and found that the fine cracks that occur when an electrodeposited film is baked are caused by an insufficient amount of organic solvent in the electrodeposited film, but that the insufficient amount of organic solvent in the electrodeposited film can be resolved by adding an appropriate amount of organic acid to the electrodeposition solution. Thus, the present inventors discovered that adding an appropriate amount of organic acid to the electrodeposition solution optimizes the amount of organic solvent in the electrodeposited film when solid components are deposited on the surface of the anode (substrate), making it possible to suppress the occurrence of fine cracks that occur during baking.

[0009] The present invention has been made based on the above-mentioned findings, and an electrodeposition liquid according to a first aspect of the present invention is an electrodeposition liquid for electrodepositing an electrodeposited film on a conductive substrate by anionic electrodeposition, and is characterized by containing water, an organic solvent, a solid component containing at least a polyimide-based resin, a neutralizing agent, and an organic acid.

[0010] The electrodeposition solution of the first aspect of the present invention contains an organic acid, which allows the amount of organic solvent contained in the electrodeposited film to be adjusted by the organic acid's pH buffering effect and its effect of influencing the compatibility between the resin and the organic solvent. This prevents a sudden drop in pH near the surface of the anode (substrate) and allows the electrodeposited film to contain a sufficient amount of organic solvent. This prevents the occurrence of fine cracks when the electrodeposited film is baked, allowing the formation of an insulating coating with high insulating properties.

[0011] The electrodeposition solution of Aspect 2 of the present invention is characterized in that, in the electrodeposition solution of Aspect 1 of the present invention, the organic acid contains any one of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid. Hydroxypropionic acid and hydroxybutyric acid, for example, exert their effects regardless of the position of the functional group, so even positional isomers are effective. The electrodeposition solution of Aspect 2 of the present invention contains the organic acid described above, which reliably prevents a rapid decrease in pH near the surface of the anode (substrate), allows the electrodeposition film to contain a sufficient amount of organic solvent, and effectively prevents cracks from occurring when the electrodeposition film is baked.

[0012] The electrodeposition solution of Aspect 3 of the present invention is characterized in that, in the electrodeposition solution of Aspect 1 or Aspect 2 of the present invention, the organic acid is two or more selected from formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid. Since the electrodeposition solution of Aspect 3 of the present invention contains two or more of the above-mentioned organic acids, it is possible to more effectively suppress a rapid decrease in pH near the surface of the anode (substrate), and it is possible to allow the electrodeposition film to contain a sufficient amount of organic solvent, thereby sufficiently suppressing the occurrence of cracks when the electrodeposition film is baked.

[0013] The electrodeposition solution of Aspect 4 of the present invention is the electrodeposition solution of any one of Aspects 1 to 3 of the present invention, characterized in that the organic acid contains a hydroxy acid. According to the electrodeposition solution of Aspect 4 of the present invention, since the organic acid contains a hydroxy acid, a sudden decrease in pH near the surface of the anode (substrate) can be more effectively suppressed, the electrodeposition film can be sufficiently impregnated with the organic solvent, and the occurrence of cracks when the electrodeposition film is baked can be sufficiently suppressed.

[0014] The electrodeposition solution of Aspect 5 of the present invention is characterized in that, in the electrodeposition solution of any one of Aspects 1 to 4 of the present invention, the concentration of the organic acid is in the range of 5 mg / L to 500 mg / L. According to the electrodeposition solution of Aspect 5 of the present invention, the concentration of the organic acid is in the range of 5 mg / L to 500 mg / L, so that an appropriate pH buffering effect can be exerted, the occurrence of cracks during baking of the electrodeposition film can be sufficiently suppressed, and the electrodeposition film can be stably formed.

[0015] The electrodeposition solution of Aspect 6 of the present invention is the electrodeposition solution of any one of Aspects 1 to 5 of the present invention, characterized in that the ratio A / B of the concentration A mg / L of the neutralizing agent to the concentration B mg / L of the organic acid is in the range of 5 to 500. According to the electrodeposition solution of Aspect 6 of the present invention, the ratio A / B of the concentration A mg / L of the neutralizing agent to the concentration B mg / L of the organic acid is in the range of 5 to 500, so that the action of the organic acid can suppress the occurrence of fine cracks during baking without inhibiting the action of the neutralizing agent.

[0016] The electrodeposition solution of Aspect 7 of the present invention is the electrodeposition solution of any one of Aspects 1 to 6 of the present invention, characterized in that the solid component further contains a fluororesin. According to the electrodeposition solution of Aspect 7 of the present invention, since the solid component contains a fluororesin together with a polyimide-based resin, it is possible to form an insulating film with particularly excellent insulating and dielectric properties. Furthermore, since it is more difficult to suppress cracking in an electrodeposition film containing a fluororesin than in the case of a polyimide-based resin alone, the addition of an organic acid is effective.

[0017] The method for producing an insulating coating according to aspect 8 of the present invention is a method for producing an insulating coating on the surface of a substrate, and is characterized by comprising: an electrodeposition film forming step of immersing the substrate and a counter electrode in the electrodeposition solution according to any one of aspects 1 to 7 of the present invention, and applying a voltage between the substrate as an anode and the counter electrode as a cathode to form an electrodeposition film on the substrate; and a baking step of baking the electrodeposition film.

[0018] The method for producing an insulating coating according to aspect 8 of the present invention includes an electrodeposition film formation step of forming an electrodeposition film using the electrodeposition solution according to any one of aspects 1 to 7 of the present invention, and a baking step of baking the electrodeposition film. This makes it possible to suppress the occurrence of fine cracks in the electrodeposition film during the baking step, and to stably produce an insulating coating with excellent insulating properties.

[0019] According to the present invention, it is possible to provide an electrodeposition liquid that can suppress the occurrence of fine cracks when baking an electrodeposited film and can form an insulating film with excellent insulating properties, and a method for producing an insulating film using this electrodeposition liquid.

[0020] FIG. 1 is a flow diagram showing a method for producing an insulating coating using an electrodeposition liquid according to an embodiment of the present invention.

[0021] An electrodeposition liquid and a method for producing an insulating coating according to one embodiment of the present invention will be described below. The electrodeposition liquid according to this embodiment is used when forming an electrodeposition film, which serves as a precursor to the insulating coating, on the surface of a conductive substrate. In this embodiment, the electrodeposition liquid is used in an anionic electrodeposition method in which a voltage is applied to the substrate, which serves as the anode, to form an insulating coating on the surface of the substrate, which serves as the anode.

[0022] The electrodeposition solution of this embodiment contains water, an organic solvent, a solid component, a neutralizing agent, and an organic acid. As described above, the electrodeposition solution of this embodiment is used in an anionic electrodeposition method, and therefore contains an amine as a neutralizing agent.

[0023] In this embodiment, the solid component contains at least a polyimide resin, and preferably contains two types of resin: a polyimide resin and a fluororesin. Examples of polyimide resins include polyamideimide, polyetherimide, and polyimide. Examples of fluororesins include polytetrafluoroethylene and perfluoroalkoxyalkane.

[0024] The average particle size of the solid component may be 50 nm or more and 500 nm or less, more preferably 50 nm or more and 450 nm or less, and even more preferably 50 nm or more and 300 nm or less, and the standard deviation of the particle size of the solid component may be 250 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less.

[0025] The water and organic solvent are used to disperse the solid components of the polyimide resin and fluorine resin. Examples of the organic solvent include N,N-dimethylacetamide, propylene carbonate, dimethyl sulfoxide, N,N-dimethylformamide, 4-butyrolactone, N-methyl-2-pyrrolidone, and N-methyl-2-pyrrolidone.

[0026] The water content in the electrodeposition solution is preferably 15% by mass or more, and more preferably 50% by mass or more. On the other hand, the water content in the electrodeposition solution is preferably 85% by mass or less, and more preferably 75% by mass or less. Furthermore, the organic solvent content in the electrodeposition solution is preferably 15% by mass or more, and more preferably 50% by mass or more. On the other hand, the organic solvent content in the electrodeposition solution is preferably 85% by mass or less, and more preferably 75% by mass or less.

[0027] The organic acid has a pH buffering effect and an effect of influencing the compatibility of the organic solvent with the resin (solid component). By adjusting the type and content of the organic acid, it is possible to control the amount of organic solvent contained in the electrodeposited film. Here, the organic acid preferably includes any of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid, and more preferably includes two or more selected from these. Furthermore, the organic acid preferably includes a hydroxy acid. Examples of hydroxy acids include glycololic acid, hydroxypropionic acid, hydroxybutyric acid, tartronic acid, and glyceric acid. Hydroxypropionic acid and hydroxybutyric acid, for example, exert their effects regardless of the position of the functional group, so even positional isomers can be effective.

[0028] In this embodiment, the concentration of the organic acid in the electrodeposition solution is preferably in the range of 5 mg / L or more and 500 mg / L or less. By setting the organic acid concentration to 5 mg / L or more, the pH buffering effect can be fully achieved, the organic solvent can be appropriately incorporated into the electrodeposition film, and the occurrence of fine cracks during baking can be accurately suppressed. On the other hand, by setting the organic acid concentration to 500 mg / L or less, swelling and a decrease in Coulomb efficiency due to excessive organic solvent being incorporated into the electrodeposition film can be prevented, and the electrodeposition film can be efficiently formed. The concentration of the organic acid in the electrodeposition solution is more preferably 10 mg / L or more, and even more preferably 20 mg / L or more. The concentration of the organic acid in the electrodeposition solution is more preferably 100 mg / L or less, and even more preferably 50 mg / L or less.

[0029] In this embodiment, the ratio A / B of the neutralizing agent concentration A mg / L to the organic acid concentration B mg / L is preferably in the range of 5 to 500. Organic acids undergo acid-base reactions with neutralizing agents consisting of amine compounds, which may inhibit the neutralizing agent's intended function of ionizing the resin. Therefore, in order to ensure the respective effects, it is preferable to set the ratio A / B of the neutralizing agent concentration A mg / L to the organic acid concentration B mg / L within the above-mentioned range. If the ratio A / B is less than 5, the resin ionization effect of the neutralizing agent is impaired, thereby compromising the stability of the solution. If the ratio A / B exceeds 500, the organic acid will not exert the desired effect, resulting in cracks in the film. It is more preferable that the ratio A / B of the neutralizing agent concentration A mg / L to the organic acid concentration B mg / L be 20 or more, and even more preferably 50 or more. Furthermore, the ratio A / B of the concentration of the neutralizing agent A mg / L to the concentration of the organic acid B mg / L is more preferably 400 or less, and even more preferably 200 or less.

[0030] Next, a method for producing an insulating film using an electrodeposition liquid according to this embodiment will be described with reference to FIG.

[0031] As shown in FIG. 1, the method for producing an insulating film in this embodiment includes a surface pretreatment step S01, an electrodeposition film formation step S02, and a baking step S03.

[0032] (Surface pretreatment step S01) First, a substrate on which an electrodeposited film (insulating film) is to be formed is prepared. This substrate is conductive and is made of a metal material such as copper or a copper alloy, aluminum or an aluminum alloy, etc. Then, oils and greases adhering to the surface of the substrate are removed using a surface treatment liquid such as an organic solvent or a surfactant.

[0033] (Electrodeposited Film Formation Step S02) Next, the substrate and counter electrode are immersed in the electrodeposition solution of this embodiment, and a voltage is applied between the anode (substrate) and the cathode (counter electrode) with the substrate as the anode and the counter electrode as the cathode. This reduces the pH of the electrodeposition solution around the substrate, causing a solid component (in this embodiment, a mixture of polyimide resin and fluororesin) to precipitate on the surface of the substrate. This forms an electrodeposited film on the surface of the substrate. At this time, since an organic acid is added to the electrodeposition solution in this embodiment, the organic solvent is appropriately contained in the electrodeposited film due to the pH buffering effect of the organic acid.

[0034] The temperature of the electrodeposition solution in the electrodeposition film forming step S02 (liquid temperature) is preferably adjusted to a range of 5° C. or higher and 35° C. or lower. By setting the liquid temperature to 5° C. or higher, it is possible to prevent water from being mixed into the electrodeposition solution due to condensation. On the other hand, by setting the liquid temperature to 35° C. or lower, the storage stability of the electrodeposition solution is improved, and the electrodeposition film can be stably formed.

[0035] The voltage applied between the substrate (anode) and the counter electrode (cathode) in the electrodeposition film forming step S02 is preferably in the range of 10 V or more and 600 V or less. By setting the applied voltage to 10 V or more, the electrodeposition rate can be ensured and productivity can be improved. On the other hand, by setting the applied voltage to 600 V or less, the generation of many bubbles on the surface of the substrate can be suppressed, and the bursting of the bubbles in the subsequent baking step S03 can be suppressed, thereby suppressing the generation of numerous irregularities in the insulating coating.

[0036] (Baking step S03) In the baking step S03, the substrate on which the electrodeposited film containing the solid components (in this embodiment, a mixture of polyimide-based resin and fluororesin) obtained in the electrodeposited film forming step S02 has been formed is dried, for example, at a temperature range of 200°C or higher and lower than the melting point of the solid components to remove the residual electrodeposition liquid, and then the electrodeposited film is baked onto the substrate to form an insulating coating.

[0037] The baking temperature in the baking step S03 may be within a temperature range in which an electrodeposited film of the solid components (in this embodiment, a mixture of polyimide resin and fluororesin) is formed and an insulating coating is formed on the substrate, and may be, for example, within a range of 200° C. to 400° C. The baking time may be, for example, within a range of 0.5 minutes to 60 minutes.

[0038] Through the above-described steps, an insulating coating containing a solid component (in this embodiment, a mixture of a polyimide resin and a fluororesin) can be formed on a conductive substrate, which suppresses the occurrence of fine cracks during baking and provides an insulating coating with excellent insulating properties.

[0039] The electrodeposition solution of this embodiment configured as described above contains an organic acid. Therefore, by adjusting the amount of organic solvent contained in the electrodeposition film, the occurrence of fine cracks when the electrodeposition film is baked can be suppressed due to the pH buffering effect of the organic acid and the effect of influencing the compatibility between the resin and the organic solvent, and it is possible to form an insulating coating with high insulating properties.

[0040] In the electrodeposition solution of this embodiment, if the organic acid contains any of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid, a rapid decrease in pH near the surface of the anode (substrate) can be reliably suppressed, and the occurrence of cracks during baking of the electrodeposited film can be sufficiently suppressed. Furthermore, if the solution contains two or more selected from formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid, a rapid decrease in pH near the surface of the anode (substrate) can be even more effectively suppressed, and the occurrence of cracks during baking of the electrodeposited film can be sufficiently suppressed. Furthermore, if the organic acid contains a hydroxy acid, a rapid decrease in pH near the surface of the anode (substrate) can be even more effectively suppressed, and the occurrence of cracks during baking of the electrodeposited film can be sufficiently suppressed.

[0041] In the electrodeposition solution of this embodiment, when the concentration of the organic acid is 5 mg / L or more, the pH buffering effect of the organic acid can be ensured and the occurrence of cracks during baking of the electrodeposition film can be sufficiently suppressed. On the other hand, when the concentration of the organic acid is 500 mg / L or less, the pH buffering effect is prevented from acting excessively, and the electrodeposition film can be efficiently formed without causing blistering.

[0042] In the electrodeposition solution of this embodiment, when the ratio A / B of the neutralizing agent concentration A mg / L to the organic acid concentration B mg / L is within the range of 5 to 500, the content of the neutralizing agent is ensured, and the pH buffering effect of the organic acid can suppress the occurrence of fine cracks during baking without inhibiting the action of the neutralizing agent.

[0043] When the electrodeposition solution of the present embodiment contains a fluororesin as well as a polyimide resin as solid components, an electrodeposition film made of a mixed resin of a polyimide resin and a fluororesin can be formed, making it possible to form an insulating film with particularly excellent insulating properties.

[0044] The method for producing an insulating coating of this embodiment includes an electrodeposited film formation step S02 in which a substrate and a counter electrode are immersed in the electrodeposition solution of this embodiment, and a voltage is applied between the substrate as the anode and the counter electrode as the cathode to form an electrodeposited film on the substrate, and a baking step S03 in which the electrodeposited film is baked.Therefore, it is possible to prevent fine cracks from occurring in the electrodeposited film in the baking step S03, and an insulating coating with excellent insulating properties can be stably produced.

[0045] Although the embodiment of the present invention has been described above, the present invention is not limited to this and can be modified as appropriate within the scope of the technical idea of ​​the invention.

[0046] The results of confirmation experiments conducted to confirm the effectiveness of the present invention will be described below.

[0047] As shown in Tables 1 and 2, water, organic solvent, solid components, neutralizer, and organic acid were prepared and mixed in the mass ratios shown in Tables 1 and 2 to obtain an electrodeposition solution. An oxygen-free copper rectangular bar (1.47 mm x 2.94 mm x 25 cm long) was prepared as the conductive substrate, and a cylindrical copper plate was prepared as the counter electrode. The substrate and counter electrode were immersed in the above-described electrodeposition solution, and an electrodeposition film was formed at a temperature of 20°C, an applied voltage of 500 V, and a holding time of 0.5 minutes. The electrodeposition film was then baked using a three-stage heating profile: a work temperature of 140-170°C for 10 minutes, a temperature of 240-260°C for 5 minutes, and a temperature of 340-350°C for 90 seconds, followed by rapid cooling, to form an insulating coating.

[0048] The concentration of organic acids in the electrodeposited film was evaluated as follows. The electrodeposition solution was diluted with ultrapure water, impurities were removed, and the filtrate was passed through a membrane filter to prepare the solution for ion chromatography. Measurements were then performed using a Thermo Fisher Scientific ICS-5000+ ion chromatograph. The stationary phase of the ion chromatograph was an anion exchange column, Dionex IonPac AG15 or Dionex IonPac AS15, the eluent was potassium hydroxide aqueous solution, the suppressor was Dionex ADRS 600, and the detector was electrical conductivity.

[0049] The appearance of the formed insulating coating was also observed, and the presence of cracks and blisters was evaluated. Those with cracks that allowed the Cu in the substrate to be visually confirmed were rated "D," those with cracks that prevented the Cu in the substrate from being visually confirmed were rated "C," those with cracks that were not visible with the naked eye but visible with a microscope were rated "B," and those with no cracks visible with a microscope were rated "A." Furthermore, those with blisters observed in the insulating coating with the naked eye were rated "present," and those without were rated "absent."

[0050] Furthermore, the dielectric constant of the insulating coating was measured as follows: Silver paste was applied to the surface of the insulating coating at two 10 mm positions on the edges and at a 100 mm distance from the center to prepare a measurement sample. The capacitance between the conductor and the silver paste in the center was measured using a Hioki EE LCR meter IM3536, and the dielectric constant was calculated from the measured capacitance and the thickness of the coating.

[0051] The electrodeposition solution was also evaluated for stability. When the electrodeposition solution was kept at 40°C for 5 days, the solution that showed separation or precipitation was rated as "B," and the solution that showed no separation or precipitation was rated as "A."

[0052]

[0053]

[0054] In Comparative Examples 1 to 3, no organic acid was added to the electrodeposition solution, and cracks were observed in the insulating film after baking, revealing the Cu of the substrate.

[0055] In contrast, in Inventive Examples 1 to 24, an organic acid was added to the electrodeposition solution, and no cracks that would reveal Cu in the substrate were observed in the insulating coating after baking. Furthermore, in Inventive Examples 3 to 24, the organic acid included any of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid, and no cracks were observed visually.

[0056] ​​In addition, in Inventive Examples 1 to 5, the organic acid concentration was less than 5 mg / L, and fine cracks were observed, but no cracks that could be seen in the substrate occurred, and there were no problems with insulation. In Inventive Examples 6 to 9, the organic acid concentration exceeded 500 mg / L, causing blistering of the coating. Furthermore, in Inventive Examples 6, 8, 9, 15, and 16, the ratio A / B of the neutralizing agent concentration A mg / L to the organic acid concentration B mg / L was less than 5, and separation and precipitation occurred in the electrodeposition solution when maintained at 40°C for 5 days, resulting in poor stability of the electrodeposition solution. In Inventive Examples 10 to 14, even though the organic acid concentration was 5 mg / L or higher, the ratio A / B of the neutralizing agent concentration A mg / L to the organic acid concentration B mg / L exceeded 500, causing fine cracks. Furthermore, Inventive Examples 21 and 22 contained polyimide resin and fluororesin as solid components, resulting in a sufficiently low dielectric constant and particularly excellent insulation properties.

[0057] From the results of the above confirmatory experiments, it was confirmed that the present invention can provide an electrodeposition liquid that can suppress the occurrence of fine cracks when baking an electrodeposited film and can form an insulating film with excellent insulating properties, as well as a method for manufacturing an insulating film using this electrodeposition liquid.

[0058] It is possible to provide an electrodeposition liquid that can suppress the occurrence of fine cracks when baking an electrodeposited film and can form an insulating film with excellent insulating properties, and a method for producing an insulating film using this electrodeposition liquid.

Claims

1. An electrodeposition solution for electrodepositing an electrodeposition film on a conductive substrate by anionic electrodeposition, comprising water, an organic solvent, a solid component, a neutralizing agent, and an organic acid, wherein the solid component contains at least a polyimide-based resin.

2. The electrodeposition solution according to claim 1, characterized in that the organic acid contains any one of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid.

3. The electrodeposition solution according to claim 1, characterized in that the organic acid is two or more selected from the group consisting of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid.

4. The electrodeposition solution according to claim 1, characterized in that the organic acid includes a hydroxy acid.

5. The electrodeposition solution according to claim 1, characterized in that the concentration of the organic acid is within the range of 5 mg / L to 500 mg / L.

6. The electrodeposition solution according to claim 1, characterized in that the ratio A / B of the concentration A mg / L of the neutralizing agent to the concentration B mg / L of the organic acid is within the range of 5 to 500.

7. The electrodeposition solution according to claim 1, wherein the solid components further contain a fluororesin.

8. A method for manufacturing an insulating film for forming an insulating film on a surface of a substrate, comprising: an electrodeposition film forming step of immersing the substrate and a counter electrode in the electrodeposition liquid according to any one of claims 1 to 7, using the substrate as an anode and the counter electrode as a cathode, applying a voltage between the anode and the cathode to form an electrodeposition film on the substrate; and a baking step of baking the electrodeposition film.

Citation Information

Patent Citations

  • Manufacture of electrodepositable waterrsoluble organic polymer

    JP1981008436A

  • Insulating aluminum alloy conductor and method for manufacturing the same

    JP2023032641A

  • Electrodeposition solution and method for producing conductor with insulating film using same

    WO2018151091A1