Nonaqueous electrolyte secondary battery and battery pack
The non-aqueous electrolyte secondary battery with a lithium-containing transition metal composite oxide and a sulfonic acid compound under high pressure addresses the inefficiencies in initial charge/discharge and cycle characteristics, achieving enhanced performance by reducing reaction resistance and preventing cracking.
Patent Information
- Application Number
- PCT/JP2024/013929
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-04
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional non-aqueous electrolyte secondary batteries face challenges in achieving both high initial charge/discharge efficiency and excellent cycle characteristics, with existing techniques failing to sufficiently address these issues.
A non-aqueous electrolyte secondary battery with a structure featuring a positive electrode and negative electrode stacked with a separator, where the positive electrode contains a lithium-containing transition metal composite oxide with a layered rock salt structure and a sulfonic acid compound on its surface, and is subjected to a pressure of 8.00×10^−2 MPa or more, suppressing cracking and side reactions.
This configuration enhances both initial charge/discharge efficiency and cycle characteristics by reducing reaction resistance and preventing cracking of the positive electrode active material particles, leading to improved battery performance.
Smart Images

Figure JP2024013929_31102024_PF_FP_ABST
Abstract
Description
Nonaqueous electrolyte secondary battery and battery pack
[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery and a battery pack in which a plurality of non-aqueous electrolyte secondary batteries are connected together.
[0002] In recent years, the use of non-aqueous electrolyte secondary batteries has expanded to include power sources for electric vehicles and energy storage devices for utilizing natural energy. Because the positive electrode significantly affects battery characteristics, including battery capacity, output characteristics, and cycle characteristics, much research has been conducted on the positive electrode. Patent Document 1 discloses a non-aqueous electrolyte secondary battery having a flat electrode assembly in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween, and which uses, as the positive electrode active material, a lithium-containing transition metal composite oxide in which a compound containing elements such as Al, Mg, Ti, Zr, and W is attached to the particle surface. Patent Document 1 also discloses that applying a predetermined external pressure to the flat portion of the non-aqueous electrolyte secondary battery suppresses expansion of the positive electrode active material, thereby improving the cycle characteristics of the battery.
[0003] Patent No. 6509989
[0004] In non-aqueous electrolyte secondary batteries, achieving both high initial charge-discharge efficiency and excellent cycle characteristics is an important issue. Conventional techniques including those described in Patent Document 1 have not been able to adequately address this issue, and there is still much room for improvement.
[0005] A non-aqueous electrolyte secondary battery according to one aspect of the present disclosure is a non-aqueous electrolyte secondary battery including an electrode assembly having a structure in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween, and an exterior body that houses the electrode assembly, wherein the positive electrode has a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core and containing a positive electrode active material, the positive electrode active material containing a lithium-containing transition metal composite oxide having a layered structure, and the lithium-containing transition metal composite oxide is represented by the general formula Li x Ni a Co b Mn c M d O 2-y(wherein 0.80<x<1.20, 0.75<a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr), and the secondary particles are formed by aggregation of primary particles, and the sulfonic acid compound represented by formula (I) is present on the surface of the secondary particles, and when pressure is applied from the outside of the exterior body in the stacking direction of the positive electrode, negative electrode, and separator, the electrode body is formed of 8.00×10 ―2 It is characterized in that a pressure of 100 MPa or more is applied. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)
[0006] A battery pack according to one aspect of the present disclosure is a battery pack including a plurality of the nonaqueous electrolyte secondary batteries described above, characterized in that the plurality of nonaqueous electrolyte secondary batteries are arranged in a stacking direction of the positive electrode, the negative electrode, and the separator, and are constrained to one another in the arrangement direction.
[0007] According to a nonaqueous electrolyte secondary battery according to one aspect of the present disclosure, it is possible to improve the initial charge-discharge efficiency and cycle characteristics.
[0008] BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1 is a perspective view showing the appearance of a non-aqueous electrolyte secondary battery according to an embodiment. Fig. 2 is a cross-sectional view taken along line AA in Fig. 1. Fig. 3 is a perspective view showing a battery pack according to an embodiment.
[0009] The layered rock salt structure of a lithium-containing transition metal composite oxide has a transition metal layer such as Ni, a Li layer, and an oxygen layer, and the charge / discharge reaction of the battery progresses as Li ions present in the Li layer reversibly enter and exit. Generally, lithium nickel oxide-based lithium-containing transition metal composite oxides containing Ni as a main component are known as high-capacity positive electrode active materials. From the viewpoint of increasing the capacity of the battery, the Ni content in the lithium-containing transition metal composite oxide is preferably more than 75 mol% with respect to the total number of moles of metal elements excluding Li.
[0010] As a result of the inventors' investigations, it has been found that the presence of a sulfonic acid compound represented by the above formula (I) on the surface of secondary particles of a lithium-containing transition metal composite oxide used as a positive electrode active material can realize a nonaqueous electrolyte secondary battery with improved initial charge-discharge efficiency. This is believed to be because the function of the sulfonic acid compound reduces the reaction resistance at the positive electrode, making it possible to deepen the charge-discharge depth. However, a new problem has arisen: deterioration in cycle performance, accompanied by the deepening charge-discharge depth due to the reduced reaction resistance. This is presumably because the deepening charge-discharge depth causes a large volume change in the crystal lattice of the positive electrode active material, leading to cracking of the positive electrode active material particles and the resulting side reaction between the positive electrode active material particles and the nonaqueous electrolyte.
[0011] Therefore, the present inventors have conducted further studies and have discovered that in a non-aqueous electrolyte secondary battery having an electrode body in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween, a lithium-containing transition metal composite oxide in which a sulfonic acid compound is attached to the surface of secondary particles is used as a positive electrode active material, and a 8.00 × 10 ―2 It has been found that by applying a pressure of 8.00 × 10 MPa or more, a nonaqueous electrolyte secondary battery can be realized that ensures high capacity while improving the initial charge-discharge efficiency and cycle characteristics. ―2 It is presumed that the application of a pressure of 100 MPa or more suppresses cracking of the positive electrode active material particles during charge and discharge, even when a sulfonic acid compound is present on the surface of the secondary particles.
[0012] Hereinafter, an example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail with reference to the drawings. Note that configurations formed by selectively combining the components of the multiple embodiments and variations described below are included within the scope of the present disclosure. Note that the drawings referred to in the description of the embodiments are schematic, and the dimensional ratios of the components depicted in the drawings may differ from the actual products. In addition, in this specification, "to" means a range that includes the upper and lower limits before and after "to."
[0013] In the following, a prismatic battery in which the electrode assembly 11 is housed in a prismatic battery case 14 as an exterior body will be exemplified as the nonaqueous electrolyte secondary battery, but the battery exterior body is not limited to a prismatic battery case. The nonaqueous electrolyte secondary battery according to the present disclosure may be, for example, a laminate battery having an exterior body made of a laminate sheet including a metal layer and a resin layer.
[0014] Fig. 1 is a perspective view showing a nonaqueous electrolyte secondary battery 10 according to an embodiment, and Fig. 2 is a cross-sectional view taken along line AA in Fig. 1. As illustrated in Fig. 1 and Fig. 2, the nonaqueous electrolyte secondary battery 10 includes an electrode assembly 11 and a nonaqueous electrolyte (not shown).
[0015] The electrode body 11 has a long positive electrode 20, a long negative electrode 21, and a separator 22 interposed between the positive electrode 20 and the negative electrode 21. The electrode body 11 has a wound structure in which the positive electrode 20 and the negative electrode 21 are spirally wound with the separator 22 interposed therebetween. Note that the structure of the electrode body 11 is not limited to the wound type, and may be a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked one by one with separators interposed therebetween.
[0016] The non-aqueous electrolyte secondary battery 10 includes a rectangular battery case 14 as an exterior body that houses an electrode assembly 11 and a non-aqueous electrolyte. The battery case 14 is externally charged with 8.00 × 10 sieves from both sides in a stacking direction α of the positive electrode 20, the negative electrode 21, and the separator 22 (hereinafter, sometimes simply referred to as the “stacking direction α”). ―2 Therefore, the electrode body 11 is pressed with a pressure of 8.00 × 10 ―2 The positive electrode 20 is pressed with a pressure of 100 MPa or more. This suppresses cracking of the positive electrode active material particles constituting the positive electrode 20 and the side reaction between the positive electrode active material and the non-aqueous electrolyte that accompanies the cracking. As a result, even when a sulfonic acid compound is present on the surface of the particles, the cycle characteristics can be improved.
[0017] In this embodiment, the nonaqueous electrolyte secondary battery 10 is modularized, so that the electrode body 11 is pressed from both sides in the stacking direction α (see FIG. 3 described later). Note that expansion of the electrode body 11 during charging generates stress that tends to push the battery case 14 outward, and a reaction force that counters this stress is generated.
[0018] The battery case 14 is a rectangular metal case composed of a substantially box-shaped case body 15 and a sealing body 16 that closes the opening of the case body 15. A positive electrode terminal 12 electrically connected to the positive electrode 20 and a negative electrode terminal 13 electrically connected to the negative electrode 21 are provided on the sealing body 16. A lead portion of the positive electrode is connected to the positive electrode terminal 12 directly or via another conductive member. A lead portion of the negative electrode is connected to the negative electrode terminal 13 directly or via another conductive member. For ease of explanation, the direction in which the positive electrode terminal 12 and the negative electrode terminal 13 are aligned will be referred to as the "horizontal direction" of the battery case 14, etc., and the direction perpendicular to the stacking direction α and the horizontal direction will be referred to as the "vertical direction."
[0019] The case body 15 has a flat shape that is longer in the horizontal and vertical directions than the stacking direction α. The case body 15 and the sealing body 16 are made of a metal material, for example, primarily aluminum, and an electrode holder may be attached to the inner surface to ensure insulation. The electrode holder is a plate molded from a resin such as polypropylene and has a thickness of 0.05 mm to 0.5 mm. The sealing body 16 has, for example, a generally rectangular shape that is longer in the horizontal direction, and its peripheral edge is welded to the peripheral edge of the opening of the case body 15.
[0020] Through holes (not shown) are formed on both lateral sides of the sealing body 16, and the positive electrode terminal 12 and the negative electrode terminal 13 are inserted into the battery case 14 through the respective through holes. The positive electrode terminal 12 and the negative electrode terminal 13 are each fixed to the sealing body 16 via, for example, insulating members 17 disposed in the through holes. Note that the sealing body 16 is generally provided with a gas exhaust mechanism (not shown).
[0021] 3 is a perspective view of a battery pack 30 configured using a plurality of nonaqueous electrolyte secondary batteries 10. As illustrated in FIG. 3, the battery pack 30 includes a battery group 31 configured by arranging a plurality of nonaqueous electrolyte secondary batteries 10 in the stacking direction α, a plurality of spacers 32, and a pair of end plates 33. The spacers 32 are insulating members interposed between adjacent nonaqueous electrolyte secondary batteries 10. The end plates 33 are members that press the battery group 31 from both sides in the stacking direction α with a predetermined force. The pressing force of the end plates 33 is 8.00×10 ―2 MPa or more.
[0022] The battery pack 30 is fixed to a pair of end plates 33 that sandwich the battery group 31 from both sides in the stacking direction α (the direction in which the multiple nonaqueous electrolyte secondary batteries 10 are lined up), and includes bind bars 35, 36 for binding the batteries that make up the battery group 31. The bind bars 35, 36, together with the end plates 33, maintain the bound state of the batteries and hold the batteries in place. The bind bar 35 is attached to one lateral side of the battery group 31 along the stacking direction α, and the bind bar 36 is attached to the other lateral side of the battery group 31 along the stacking direction α.
[0023] In this embodiment, the same nonaqueous electrolyte secondary batteries 10 are arranged with their orientations reversed, and adjacent batteries are arranged so that the lateral positions of their positive and negative terminals are reversed. In this case, the positive electrode terminals 12 and negative electrode terminals 13 are alternately arranged along the stacking direction α. The battery pack 30 includes bus bars 34 that electrically connect adjacent nonaqueous electrolyte secondary batteries 10. In the example shown in FIG. 1 , the nonaqueous electrolyte secondary batteries 10 are connected in series by the bus bars 34, but the connection of the batteries is not limited to this.
[0024] In the battery pack 30, bind bars 35, 36 are fixed to a pair of end plates 33 and the end plates 33 are pressed against the battery group 31, thereby binding and pressing the nonaqueous electrolyte secondary batteries 10 that make up the battery group 31. The end plates 33 are, for example, resin plates that are slightly larger than the nonaqueous electrolyte secondary batteries 10. The end plates 33 have, for example, bolt holes formed therein for fastening the bind bars 35, 36.
[0025] The positive electrode 20, negative electrode 21, separator 22, and nonaqueous electrolyte that constitute the nonaqueous electrolyte secondary battery 10, and in particular the positive electrode active material that constitutes the positive electrode 20, will be described in detail below.
[0026] [Positive Electrode] The positive electrode 20 has a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core. The positive electrode mixture layer is preferably formed on both sides of the positive electrode core. The positive electrode core can be made of a foil of a metal, such as aluminum or an aluminum alloy, that is stable within the potential range of the positive electrode 20, or a film with such a metal disposed on the surface. The positive electrode mixture layer may contain a positive electrode active material, a conductive agent, and a binder. The thickness of the positive electrode mixture layer is, for example, 10 μm to 150 μm on one side of the positive electrode core. The positive electrode 20 can be produced, for example, by applying a positive electrode slurry containing a positive electrode active material, a conductive agent, a binder, etc. to the surface of the positive electrode core, drying the coating, and then rolling it to form a positive electrode mixture layer on both sides of the positive electrode core.
[0027] Examples of the conductive agent contained in the positive electrode mixture layer include carbon black (CB) such as acetylene black (AB) and ketjen black, carbon nanotubes (CNT), graphene, graphite, and other carbon-based materials. These may be used alone or in combination of two or more.
[0028] Examples of the binder contained in the positive electrode mixture layer include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide-based resins, acrylic-based resins, polyolefin-based resins, etc. These may be used alone or in combination of two or more.
[0029] The positive electrode active material contained in the positive electrode mixture layer includes a lithium-containing transition metal composite oxide and a sulfonic acid compound present on the surface of the lithium-containing transition metal composite oxide. The lithium-containing transition metal composite oxide includes, for example, secondary particles formed by aggregation of primary particles. Here, the surface of the lithium-containing transition metal composite oxide refers to the surface of the secondary particles of the lithium-containing transition metal composite oxide or the interface where the primary particles contact each other. In other words, the sulfonic acid compound is present on the surface of the secondary particles of the lithium-containing transition metal composite oxide or the interface where the primary particles contact each other.
[0030] The particle size of the primary particles constituting the secondary particles of the lithium-containing transition metal composite oxide is, for example, 0.02 μm to 2 μm. The particle size of the primary particles is measured as the diameter of the circumscribed circle in a particle image observed with a scanning electron microscope (SEM). The volume-based median diameter (D50) of the secondary particles of the lithium-containing transition metal composite oxide is, for example, 2 μm to 30 μm. D50 refers to the particle size at which the cumulative frequency in the volume-based particle size distribution is 50% from the smallest particle size, and is also called the median diameter. The particle size distribution of the secondary particles of the lithium-containing transition metal composite oxide can be measured using a laser diffraction particle size distribution analyzer (e.g., MT3000II, manufactured by Microtrac-Bell Corporation) using water as a dispersion medium.
[0031] The lithium-containing transition metal composite oxide has a layered rock salt structure. Examples of the layered rock salt structure of the lithium-containing transition metal composite oxide include a layered rock salt structure belonging to the space group R-3m and a layered rock salt structure belonging to the space group C2 / m. From the viewpoints of increasing capacity and stability of the crystal structure, the lithium-containing transition metal composite oxide preferably has a layered rock salt structure belonging to the space group R-3m. The layered rock salt structure of the lithium-containing transition metal composite oxide may include a transition metal layer, a Li layer, and an oxygen layer.
[0032] The lithium-containing transition metal composite oxide has the general formula Li x Ni a Co b Mn c M d O 2-y(wherein 0.80<x<1.20, 0.75<a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr.) The content of the elements constituting the lithium-containing transition metal composite oxide can be measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), or the like.
[0033] By setting the Ni content in the lithium-containing transition metal composite oxide to more than 75 mol % and not more than 95 mol %, a battery with a high capacity can be obtained. The higher the Ni content, the higher the capacity of the battery that can be obtained.
[0034] The content of Co in the lithium-containing transition metal composite oxide is 0 mol % to 15 mol %, and Co is an optional component. In other words, the lithium-containing transition metal composite oxide does not need to contain Co. By containing Co, the lithium-containing transition metal composite oxide can improve the heat resistance of the battery.
[0035] The content of Mn in the lithium-containing transition metal composite oxide is 0 mol % to 25 mol %, and Mn is an optional component. In other words, the lithium-containing transition metal composite oxide does not necessarily contain Mn. By containing Mn, the lithium-containing transition metal composite oxide can stabilize its crystal structure.
[0036] The content of M (M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr) in the lithium-containing transition metal composite oxide is 0 mol % to 10 mol %, and M is an optional component. In other words, the lithium-containing transition metal composite oxide does not necessarily contain M.
[0037] The sulfonic acid compound represented by formula (I) is present on the surface of the secondary particles of the lithium-containing transition metal composite oxide. In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2. A is preferably a Group 1 element. Among these, A is more preferably Li or Na, and particularly preferably Li. The sulfonic acid compound may be present in the form of dots so as to cover at least a portion of the surface of the secondary particles of the lithium-containing transition metal composite oxide, or may be present so as to cover the entire surface of the secondary particles. Furthermore, the sulfonic acid compound may be present on the surface of the primary particles of the lithium-containing transition metal composite oxide.
[0038] In formula (I), R is preferably an alkyl group. The number of carbon atoms in the alkyl group is preferably 5 or less, more preferably 3 or less. From the viewpoint of reducing reaction resistance, a suitable example of R is an alkyl group having 3 or less carbon atoms, and among these, a methyl group is preferred. In R, some of the hydrogen atoms bonded to the carbon may be substituted with fluorine. In formula (I), n is preferably 1.
[0039] Specific examples of the sulfonic acid compound include lithium methanesulfonate, lithium ethanesulfonate, lithium propanesulfonate, sodium methanesulfonate, sodium ethanesulfonate, magnesium methanesulfonate, lithium fluoromethanesulfonate, etc. Among these, at least one selected from the group consisting of lithium methanesulfonate, lithium ethanesulfonate, and sodium methanesulfonate is preferred, with lithium methanesulfonate being particularly preferred.
[0040] The sulfonic acid compound reduces the reaction resistance in the positive electrode 20. Furthermore, as the resistance decreases, it becomes possible to deepen the charge / discharge depth, thereby improving the initial charge / discharge efficiency. Even a very small amount of sulfonic acid compound can exert this effect, but the amount of sulfonic acid compound present on the secondary particle surface of the lithium-containing transition metal composite oxide is preferably 0.1% by mass or more, and more preferably 0.3% by mass or more, relative to the mass of the lithium-containing transition metal composite oxide. Furthermore, from the viewpoint of cycle characteristics, the amount of sulfonic acid compound present on the secondary particle surface of the lithium-containing transition metal composite oxide is preferably 1.0% by mass or less, and more preferably 0.8% by mass or less, relative to the mass of the lithium-containing transition metal composite oxide. Therefore, the amount of sulfonic acid compound is preferably 0.1% by mass to 1.0% by mass, and more preferably 0.3% by mass to 0.8% by mass, relative to the mass of the lithium-containing transition metal composite oxide.
[0041] The presence of the sulfonic acid compound on the surface of the secondary particles of the lithium-containing transition metal composite oxide can be confirmed by Fourier transform infrared spectroscopy (FT-IR). In the infrared absorption spectrum obtained by FT-IR, the positive electrode active material containing lithium methanesulfonate exhibits, for example, a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It has an absorption peak around 1238 cm -1 , 1175 cm -1 , 1065 cm -1 The peak around 785 cm is due to the SO stretching vibration of lithium methanesulfonate. -1 The peak around 1000 nm is a peak due to the C-S stretching vibration derived from lithium methanesulfonate. Note that the presence of a positive electrode active material containing a sulfonic acid compound other than lithium methanesulfonate can also be confirmed from the absorption peak derived from the sulfonic acid compound in the infrared absorption spectrum.
[0042] The presence of the sulfonic acid compound can also be confirmed by X-ray photoelectron spectroscopy (XPS). In the spectrum obtained by XPS, a peak with a binding energy of approximately 165 to 170 eV and an intensity (c / s) of 200 to 1000 is observed for the positive electrode active material containing lithium methanesulfonate. The presence of the sulfonic acid compound on the secondary particle surface of the lithium-containing transition metal composite oxide can also be confirmed by ICP, atomic absorption spectroscopy, synchrotron XRD measurement, time-of-flight secondary ion mass spectrometry (TOF-SIMS), and the like.
[0043] A surface modification layer containing at least one of Ca and Sr (hereinafter referred to as "M1") may be present on the surface of the primary particles of the lithium-containing transition metal composite oxide. This effectively suppresses erosion and deterioration of the lithium-containing transition metal composite oxide due to side reactions with the non-aqueous electrolyte, improving the charge-discharge cycle characteristics of the non-aqueous electrolyte secondary battery 10. Here, the surface of the primary particles includes the surface of the secondary particles, and specifically refers to the surfaces of the secondary particles and the interfaces between the primary particles. The surface modification layer may be present in a dotted pattern so as to cover at least a portion of the surface of the primary particles, or may be present so as to cover the entire surface of the primary particles.
[0044] The total amount of M1 contained in the surface modification layer is preferably 1 mol % or less, more preferably 0.5 mol % or less, based on the total molar amount of metal elements excluding Li in the lithium-containing transition metal composite oxide. The lower limit of the total amount of M1 is, for example, 0.01 mol %.
[0045] Furthermore, the surface modification layer may contain, in addition to M1, at least one element selected from the group consisting of W, Mo, Ti, Si, Nb, and Zr (hereinafter referred to as "M2"). In this case, erosion and deterioration of the lithium-containing transition metal composite oxide due to side reactions with the non-aqueous electrolyte are more effectively suppressed. The total amount of M2 contained in the surface modification layer is 2 mol% or less, more preferably 1 mol% or less, and even more preferably 0.5 mol% or less, based on the total molar amount of metal elements excluding Li in the lithium-containing transition metal composite oxide. The lower limit of the total amount of M2 is, for example, 0.01 mol%.
[0046] The presence of the surface modification layer on the surface of the primary particles of the lithium-containing transition metal composite oxide, the presence of M1 contained in the surface modification layer, and the presence of M2 contained in the surface modification layer can be confirmed by measuring the cross section of the secondary particles of the lithium-containing transition metal composite oxide using TEM-EDX (transmission electron microscope-energy dispersive X-ray spectroscopy). The total amount of M1 and the total amount of M2 can each be measured by, for example, inductively coupled plasma (ICP) atomic emission spectroscopy.
[0047] A compound containing M1 (hereinafter referred to as "M1 compound") and a compound containing M2 (hereinafter referred to as "M2 compound") may be fixed to the surface of the primary particles of the lithium-containing transition metal composite oxide. Examples of the M1 compound include oxides, hydroxides, carbonates, etc. containing M1. Examples of the M2 compound include oxides, hydroxides, carbonates, sulfates, etc. containing M2.
[0048] The surface of the primary particle of the lithium-containing transition metal composite oxide is provided with a compound of the general formula M1 α M2 β O γ (wherein 1≦α≦2, 1≦β≦5, 4≦γ≦9, M1 is at least one element selected from Ca and Sr, and M2 is at least one element selected from W, Mo, Ti, Si, Nb, and Zr) (hereinafter referred to as “M1 α M2 β O γ The M1 compound, the M2 compound, and the M1 compound may be fixed to the surface of the primary particle of the lithium-containing transition metal composite oxide. α M2 β O γ The compounds may coexist.
[0049] M1 α M2 β O γ The presence of the compound can be confirmed using synchrotron radiation X-ray diffraction measurement. α M2 β O γThe compound may be, for example, scattered on the surfaces of the primary particles and secondary particles of the lithium-containing transition metal composite oxide, or may be present in the form of a layer so as to widely cover the surfaces of the primary particles and secondary particles. α M2 β O γ The compound is widely present on the surface of the primary particles as well as inside and on the surface of the secondary particles. The secondary particles of the lithium-containing transition metal composite oxide are formed by agglomerating, for example, five or more primary particles, and the surface area of the primary particles is larger inside than on the surface of the secondary particles. α M2 β O γ For example, the compound is contained in a larger amount inside the secondary particles than on the surface thereof.
[0050] M1 α M2 β O γ Specific examples of the compound include CaWO 4 , CaMoO 3 , CaMoO 4 , CaTiO 3 , Ca 2 TiO 4 , CaSiO 3 , Ca 2 SiO 4 , CaNbO 3 , CaNb 2 O 6 , CaZrO 3 , CaZr 4 O 9 , SrWO 4 , SrMoO 3 , SrMoO 4 , SrTiO 3 , Sr 2 TiO 4 , SrSiO 3 , Sr 2 SiO 4 , SrNbO 3 , SrNb 2 O 6 , SrZrO 3 , SrZr 4 O 9 Examples include:
[0051] A nonmetallic compound may be present on the surface of the primary particles of the lithium-containing transition metal composite oxide. The nonmetallic compound contains, for example, one or more nonmetallic elements selected from the group consisting of P and B. Examples of the P-containing compound include Li, 3-x H x P.O. 4 (0≦x≦3) can be exemplified. 3 BO 3 , Li 3 BO 3 , Li 2 B 4 O 7 Examples include:
[0052] The positive electrode mixture layer may contain, in addition to the positive electrode active material of the present embodiment, other positive electrode active materials, such as lithium-containing transition metal composite oxides having a Ni content of 0 mol % or more and 75 mol % or less.
[0053] The positive electrode active material, which is one example of the embodiment, can be produced by the following method: Note that the production method described here is only an example, and the method for producing the positive electrode active material is not limited to this method.
[0054] The manufacturing process of the positive electrode active material includes a synthesis step of mixing a metal oxide with a Li compound or the like to obtain a mixture and calcining the mixture to obtain a lithium-containing transition metal composite oxide; a washing step of washing the calcined product with water and dehydrating it to obtain a cake-like composition; a drying step of drying the cake-like composition to obtain a powder-like composition; and an addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition or the powder-like composition.
[0055] In the synthesis step, for example, a metal oxide containing more than 75 mol % and not more than 95 mol % of Ni, 0 mol % to 15 mol % of Co, 0 mol % to 25 mol % of Mn, and 0 mol % to 10 mol % of M (M is at least one element selected from W, Mg, Mo, Nb, Ti, Si, Al, and Zr) is mixed with a Li compound to obtain a mixture.
[0056] The metal oxide can be obtained, for example, by adding an alkaline solution such as sodium hydroxide dropwise to a stirred solution of a metal salt containing Ni and an arbitrary metal element (Co, Mn, M, etc.) to adjust the pH to the alkaline side (e.g., 8.5 to 12.5) to precipitate (co-precipitate) a composite hydroxide containing Ni and the arbitrary metal element, and then heat-treating the composite hydroxide. The heat-treatment temperature is not particularly limited, but is, for example, in the range of 250°C to 600°C.
[0057] Examples of Li compounds include Li 2 CO 3 , LiOH, Li 2 O 2 , Li 2 O, LiNO 3 , LiNO 2 , Li 2 SO 4 , LiOH·H 2 Examples of the metal oxide include O, LiH, and LiF. In order to facilitate adjustment of the above-mentioned parameters to the ranges specified above, the mixing ratio of the metal oxide and the Li compound is preferably such that the molar ratio of the total amount of metal elements in the metal oxide to Li falls within a range of 1:0.80 to 1:1.20, and more preferably falls within a range of 1:1.00 to 1:1.10.
[0058] Next, the synthesis step includes a calcination step in which the resulting mixture is calcined. The calcination step is a multi-stage calcination step that includes at least a first calcination step in which the mixture is calcined at 300°C to 680°C under an oxygen stream, and a second calcination step in which the calcined product obtained by the first calcination step is calcined at a temperature exceeding 680°C under an oxygen stream. In the first calcination step, the temperature is increased to a first set temperature of 680°C or less at a first temperature increase rate of 0.2°C / min to 4.5°C / min. In the second calcination step, the temperature is increased to a second set temperature of 900°C or less at a first temperature increase rate of 0.5°C / min to 3.5°C / min. Note that multiple first and second temperature increase rates may be set for each temperature range as long as they are within the above-specified range.
[0059] The holding time of the first set temperature in the first firing step is preferably 5 hours or less, more preferably 3 hours or less. The holding time of the first set temperature is the time during which the first set temperature is maintained after reaching the first set temperature, and the holding time may be zero. The holding time of the second set temperature in the second firing step is preferably 1 hour to 10 hours, more preferably 1 hour to 5 hours. The holding time of the second set temperature is the time during which the second set temperature is maintained after reaching the second set temperature. The firing of the mixture is carried out, for example, in an oxygen stream with an oxygen concentration of 60% or more, and the flow rate of the oxygen stream is set to 10 cm / min. 3 The flow rate is 0.2 mL / min to 4 mL / min per kg of the mixture and 0.3 L / min or more per kg of the mixture.
[0060] In the washing step, the lithium-containing transition metal composite oxide obtained in the synthesis step is washed with water and dehydrated to obtain a cake-like composition. The washing and dehydration can be performed by a known method and under known conditions. The washing and dehydration can be performed within a range that does not cause lithium to leach out from the lithium-containing transition metal composite oxide and deteriorate the battery characteristics.
[0061] In the drying step, the cake-like composition obtained in the washing step is dried to obtain a powdery composition. The drying step may be performed in a vacuum atmosphere. The drying conditions are, for example, 150°C to 400°C and 0.5 hours to 15 hours.
[0062] In the adding step, at least one of a sulfonic acid compound and a sulfonic acid solution is added to the cake-like composition obtained in the washing step or the powder-like composition obtained in the drying step. This allows the sulfonic acid compound to adhere to the surface of the lithium-containing transition metal composite oxide. It is preferable to add at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition. The sulfonic acid compound to be added may be in the form of either a powder or a solution. The sulfonic acid solution is, for example, a methanesulfonic acid solution obtained by dissolving methanesulfonic acid in water. Li compounds remain in the cake-like composition, and these remaining Li compounds are dissolved in the water contained in the cake-like composition. Therefore, even when a sulfonic acid solution is added, a sulfonic acid compound containing Li is formed. To more easily achieve the effects of the present application, a Li compound or a Li compound solution may be added to the cake-like composition or the powder-like composition together with the sulfonic acid solution, or a mixed solution prepared by premixing the sulfonic acid solution with the Li compound or the Li compound solution may be added to the cake-like composition or the powder-like composition. The Li compound is, for example, LiOH, and the Li compound solution is, for example, a LiOH solution prepared by dissolving LiOH in water. The amounts of the Li compound and the sulfonic acid solution added to the cake-like composition preferably satisfy the relationship of 0≦Li compound / sulfonic acid≦1.3 in molar ratio. The amount of the sulfonic acid compound or sulfonic acid added is preferably 0.1% by mass to 1% by mass, more preferably 0.3% by mass to 0.8% by mass, relative to the mass of the lithium-containing transition metal composite oxide. The concentrations of the sulfonic acid solution and the sulfonic acid compound solution are, for example, 0.5% by mass to 40% by mass. The addition step may be carried out during the washing step, after the washing step, during the drying step, or after the drying step, and the timing of the addition step can be changed as appropriate.
[0063] A metal compound containing one or more metal elements selected from the group consisting of Sr, Ca, W, Mo, Ti, Si, Nb, and Zr can be attached to the surface of the lithium-containing transition metal composite oxide by adding a raw material of the metal compound or non-metal compound, for example, during the synthesis process, after the synthesis process, during the washing process, after the washing process, during the drying process, after the drying process, or during the addition process. 2 , Sr(OH) 2 ・8H 2 O, SrO, SrCo 3 , SrSO 4 , Sr(NO 3 ) 2、 SrCl 2 , SrAlO 4 Examples of Ca raw materials include Ca(OH) 2 , CaO, CaCO 3 , CaSO 4 , Ca(NO 3 ) 2、 CaCl 2 , CaAlO 4 Examples of W raw materials include tungsten oxide (WO 3 ), lithium tungstate (Li 2 WO 4 , Li 4 WO 5 , Li 6 W 2 O 9 ) and the like. Examples of Mo raw materials include MoO 3 , Li 2 MoO 4 Examples of Ti raw materials include TiO 2 , Ti(OH) 4 Examples of the Si raw material include SiO 2 , SiO, etc. Examples of Nb raw materials include Nb 2 O 5 , Nb 2 O 5 ・nH 2 O, etc. Zr raw materials include Zr(OH) 4 , ZrO 2 , Zr(CO 3 ) 2 , Zr(SO 4 )2 ・4H 2 These raw materials may be used after being subjected to pulverization, drying, or the like to appropriately adjust the water content (including hydrates) and particle size.
[0064] [Negative Electrode] The negative electrode 21 has a negative electrode core and a negative electrode mixture layer formed on the surface of the negative electrode core. The negative electrode mixture layer is preferably formed on both sides of the negative electrode core. The negative electrode core can be made of a foil of a metal, such as copper or a copper alloy, that is stable within the potential range of the negative electrode 21, or a film with such a metal disposed on the surface. The negative electrode mixture layer may contain a negative electrode active material and a binder. The thickness of the negative electrode mixture layer is, for example, 10 μm to 150 μm on one side of the negative electrode core. The negative electrode 21 can be produced, for example, by applying a negative electrode slurry containing a negative electrode active material, a binder, etc. to the surface of the negative electrode core, drying the coating, and then rolling it to form a negative electrode mixture layer on both sides of the negative electrode core.
[0065] The negative electrode active material contained in the negative electrode mixture layer is not particularly limited as long as it can reversibly absorb and release lithium ions, and generally, carbon materials such as graphite are used. Graphite may be any of natural graphite such as flake graphite, lump graphite, and amorphous graphite, or artificial graphite such as lump artificial graphite and graphitized mesophase carbon microbeads. Furthermore, metals that alloy with Li, such as Si and Sn, metal compounds containing Si, Sn, and lithium-titanium composite oxides may also be used as the negative electrode active material. Furthermore, those provided with a carbon coating may also be used. For example, SiO x (0.5≦x≦1.6) or Li 2y SiO (2+y) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0<y<2) may be used in combination with graphite.
[0066] Examples of binders contained in the negative electrode mixture layer include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.
[0067] [Separator] The separator 22 may be, for example, a porous sheet having ion permeability and insulating properties. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 22 may have a single-layer structure or a laminated structure. Furthermore, the surface of the separator 22 may be provided with a highly heat-resistant resin layer such as an aramid resin, or a filler layer containing an inorganic compound filler.
[0068] [Non-aqueous electrolyte] The non-aqueous electrolyte has ion conductivity (for example, lithium ion conductivity). The non-aqueous electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.
[0069] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent that can be used include esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen atoms in these solvents are substituted with halogen atoms such as fluorine. Examples of the halogen-substituted compound include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylic acid esters such as methyl fluoropropionate (FMP).
[0070] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylic acid esters such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).
[0071] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, and methyl phenyl ether. and chain ethers such as ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
[0072] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiClO 4 , LiBF 4 , LiPF 6 , LiAlCl 4 , LiSbF 6 , LiSCN, LiCF3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiB 10 Cl 10 , lower aliphatic lithium carboxylates, LiCl, LiBr, LiI, phosphates, borates, and imide salts. Examples of phosphates include lithium difluorophosphate (LiPO 2 F 2 Examples of the borate salt include lithium bis(oxalato)borate (LiBOB) and lithium difluoro(oxalato)borate (LiDFFOB). Examples of the imide salt include lithium bisfluorosulfonylimide (LiN(FSO 2 ) 2 ), lithium bistrifluoromethanesulfonyl imide (LiN(CF 3 SO 2 ) 2 ), lithium trifluoromethanesulfonate nonafluorobutanesulfonate imide (LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 )), lithium bispentafluoroethanesulfonyl imide (LiN(C 2 F 5 SO 2 ) 2 Among these, LiPF is preferred from the viewpoint of ionic conductivity, electrochemical stability, etc. 6 The concentration of the lithium salt may be, for example, 4 mol or less, or 3 mol or less, preferably 1.8 mol or less, and more preferably 0.8 to 1.8 mol per liter of the non-aqueous solvent.
[0073] The non-aqueous electrolyte may contain an additive such as an unsaturated carbonate ester, an acid anhydride, a phenol compound, a benzene compound, a nitrile compound, an isocyanate compound, a sultone compound, a sulfate compound, a borate ester compound, a phosphate ester compound, or a phosphite ester compound.
[0074] Examples of unsaturated cyclic carbonates include vinylene carbonate, 4-methylvinylene carbonate, 4,5-dimethylvinylene carbonate, 4-ethylvinylene carbonate, 4,5-diethylvinylene carbonate, 4-propylvinylene carbonate, 4,5-dipropylvinylene carbonate, 4-phenylvinylene carbonate, 4,5-diphenylvinylene carbonate, vinylethylene carbonate, and divinylethylene carbonate. One type of unsaturated cyclic carbonate may be used alone, or two or more types may be used in combination. Some of the hydrogen atoms in the unsaturated cyclic carbonate may be substituted with fluorine atoms. The acid anhydride may be an anhydride formed by intermolecular condensation of multiple carboxylic acid molecules, but is preferably an acid anhydride of a polycarboxylic acid. Examples of polycarboxylic acid anhydrides include succinic anhydride, maleic anhydride, and phthalic anhydride.
[0075] Examples of phenolic compounds include phenol, hydroxytoluene, etc. Examples of benzene compounds include fluorobenzene, hexafluorobenzene, cyclohexylbenzene (CHB), etc.
[0076] Examples of nitrile compounds include adiponitrile, pimelonitrile, propionitrile, and succinonitrile. Examples of isocyanate compounds include methyl isocyanate (MIC), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), and bisisocyanatomethylcyclohexane (BIMCH). Examples of sultone compounds include propane sultone and propene sultone. Examples of sulfate compounds include ethylene sulfate, ethylene sulfite, dimethyl sulfate, and lithium fluorosulfate. Examples of borate ester compounds include trimethyl borate and tris(trimethylsilyl)borate. Examples of phosphate ester compounds include trimethyl phosphate and tris(trimethylsilyl)phosphate. Examples of phosphite ester compounds include trimethyl phosphite and tris(trimethylsilyl)phosphite.
[0077] As the solid electrolyte, for example, a solid or gel-like polymer electrolyte, an inorganic solid electrolyte, etc. can be used. As the inorganic solid electrolyte, a material known in all-solid-state lithium ion secondary batteries, etc. (for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a halogen-based solid electrolyte, etc.) can be used. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs the non-aqueous solvent and gels is used. As the polymer material, for example, a fluororesin, an acrylic resin, a polyether resin, etc. can be used.
[0078] Hereinafter, the present disclosure will be further described with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0079] Example 1 Preparation of Positive Electrode Active Material [Ni 0.90 Co 0.05 Mn 0.05 ](OH) 2The composite hydroxide represented by the formula (1) was calcined at 500°C for 8 hours to obtain a metal oxide containing Ni, Co, and Mn. Next, LiOH and the metal oxide were mixed so that the molar ratio of Li to the total amount of Ni, Co, and Mn was 1.03:1 to obtain a mixture. This mixture was then heated under an oxygen flow (10 cm) with an oxygen concentration of 95%. 2 The mixture was heated from room temperature to 650°C at a rate of 2.0°C / min under a flow rate of 2 mL / min per kg of mixture and 5 L / min per kg of mixture, and then heated from 650°C to 780°C at a rate of 0.5°C / min. The mixture was then maintained at this temperature for 4 hours to obtain a lithium-containing transition metal composite oxide (synthesis step). Water was added to the lithium-containing transition metal composite oxide to a slurry concentration of 1500 g / L, and the mixture was stirred for 15 minutes and filtered to obtain a cake-like composition (washing step). Powdered lithium methanesulfonate was added to the cake-like composition (addition step). The amount of lithium methanesulfonate added was 0.1% by mass relative to the total mass of the lithium-containing transition metal composite oxide. After the addition step, a drying step was performed under vacuum at 180°C for 2 hours to obtain the positive electrode active material of Example 1. The presence of lithium methanesulfonate on the surface of the positive electrode active material was confirmed by Fourier transform infrared spectroscopy (FT-IR).
[0080] [Preparation of Positive Electrode] 95 parts by mass of the above positive electrode active material, 3 parts by mass of acetylene black (AB), and 2 parts by mass of polyvinylidene fluoride (PVDF) were mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode mixture slurry. Next, the positive electrode mixture slurry was applied to both sides of a positive electrode core made of aluminum foil, and after drying the coating, the coating was rolled with a rolling roller and cut to a predetermined electrode size to prepare a positive electrode. In addition, an exposed portion in which the surface of the positive electrode core was exposed was provided in a part of the positive electrode.
[0081] [Preparation of Negative Electrode] 98 parts by mass of artificial graphite, 1 part by mass of sodium carboxymethyl cellulose (CMC-Na), and 1 part by mass of styrene butadiene rubber (SBR) were mixed, and an appropriate amount of water was added to prepare a negative electrode mixture slurry. Next, the negative electrode mixture slurry was applied to both sides of a negative electrode core made of copper foil, and after drying the coating, the coating was rolled with a rolling roller and cut to a predetermined electrode size to prepare a negative electrode. Note that an exposed portion was provided in part of the negative electrode, exposing the surface of the negative electrode core.
[0082] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF 6 ) was dissolved in the solution to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0083] [Preparation of Test Cell] A positive electrode lead was attached to the exposed portion of the positive electrode, and a negative electrode lead was attached to the exposed portion of the negative electrode. The positive and negative electrodes were spirally wound with a polyolefin separator interposed therebetween, and then pressed radially to prepare a flat wound electrode assembly. This electrode assembly was housed in an exterior body made of an aluminum laminate sheet, and the nonaqueous electrolyte was poured into it. The opening of the exterior body was then sealed to obtain a test cell.
[0084] [Evaluation of Initial Charge-Discharge Efficiency] The test cell was charged at a constant current of 0.2 It in a temperature environment of 25°C until the cell voltage reached 4.3 V, and then charged at a constant voltage of 4.3 V until the current value reached 0.01 It. After 1 hour, the cell was discharged at a constant current of 0.2 It until the cell voltage reached 2.5 V. The charge capacity and discharge capacity at this time were measured, and the initial charge-discharge efficiency of the test cell was calculated using the following formula. Note that in the test cell of Example 1, the test cell was pressed from the outside from both sides in the stacking direction α in FIG. 2, and a pressure of 8.00 × 10 was applied to the electrode body. -2 The above evaluation was carried out under a pressure (constitutive pressure) of 100 MPa. Initial charge / discharge efficiency = discharge capacity / charge capacity
[0085] [Evaluation of cycle characteristics] The test cell was charged to 4.3 V at a constant current of 0.2 It in a temperature environment of 25°C, and then charged to 0.02 It at a constant voltage of 4.3 V. Thereafter, the test cell was discharged to 2.5 V at a constant current of 0.2 It. This charge / discharge cycle constituted one cycle, and this cycle was repeated 100 times, and the capacity retention rate was calculated using the following formula. Note that in the test cell of Example 1, the test cell was pressed from the outside from both sides in the stacking direction α in FIG. 2, and a pressure of 8.00 × 10 was applied to the electrode body. -2 The above evaluation was performed under a pressure of 100 MPa. Capacity retention rate = (discharge capacity at 100th cycle / discharge capacity at 1st cycle) x 100
[0086] Example 2 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing the positive electrode active material, the amount of lithium methanesulfonate added was 0.3 mass % relative to the total mass of the lithium-containing transition metal composite oxide.
[0087] Example 3 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing the positive electrode active material, the amount of lithium methanesulfonate added was 0.5 mass % relative to the total mass of the lithium-containing transition metal composite oxide.
[0088] Example 4 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing the positive electrode active material, the amount of lithium methanesulfonate added was 0.8 mass % relative to the total mass of the lithium-containing transition metal composite oxide.
[0089] Example 5 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing the positive electrode active material, the amount of lithium methanesulfonate added was 1 mass % relative to the total mass of the lithium-containing transition metal composite oxide.
[0090] Example 6 In the addition step of preparing the positive electrode active material, the amount of lithium methanesulfonate added was 0.5% by mass relative to the total mass of the lithium-containing transition metal composite oxide. The test cell was pressed from both sides in the stacking direction α in FIG. 2 , and a 1.30×10 -1Test cells were fabricated and evaluated in the same manner as in Example 1, except that the initial charge-discharge efficiency and cycle characteristics were evaluated under a pressure of 100 MPa.
[0091] Example 7 In the addition step of preparing the positive electrode active material, the amount of lithium methanesulfonate added was 0.5% by mass relative to the total mass of the lithium-containing transition metal composite oxide. The test cell was pressed from both sides in the stacking direction α in FIG. 2 , and a 5.70×10 -1 Test cells were fabricated and evaluated in the same manner as in Example 1, except that the initial charge-discharge efficiency and cycle characteristics were evaluated under a pressure of 100 MPa.
[0092] Example 8 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing a positive electrode active material, the amount of lithium methanesulfonate added was 0.5% by mass relative to the total mass of the lithium-containing transition metal composite oxide, and the test cell was pressed from both sides in the stacking direction α in FIG. 2 so that a structural pressure of 1.30 MPa was applied to the electrode body, and the initial charge-discharge efficiency and the cycle characteristics were evaluated.
[0093] Example 9 A test cell was prepared and evaluated in the same manner as in Example 1, except that in the addition step of preparing the positive electrode active material, a lithium methanesulfonate solution prepared by dissolving lithium methanesulfonate in pure water was added instead of powdered lithium methanesulfonate, and the amount of lithium methanesulfonate added was 0.5% by mass relative to the total mass of the lithium-containing transition metal composite oxide. The concentration of the added lithium methanesulfonate solution was 10% by mass, and the lithium methanesulfonate solution was added so that the amount of lithium methanesulfonate added was as described above.
[0094] Example 10 A test cell was prepared and evaluated in the same manner as in Example 1, except that in the addition step of preparing the positive electrode active material, a methanesulfonic acid solution prepared by dissolving methanesulfonic acid in pure water was added instead of powdered lithium methanesulfonate, and the amount of methanesulfonic acid added relative to the total mass of the lithium-containing transition metal composite oxide was 0.5% by mass. The concentration of the added methanesulfonic acid solution was 10% by mass, and the methanesulfonic acid solution was added so that the amount of lithium methanesulfonate added was as described above. The presence of lithium methanesulfonate on the surface of the positive electrode active material was confirmed by Fourier transform infrared spectroscopy (FT-IR).
[0095] Example 11 A test cell was prepared and evaluated in the same manner as in Example 1, except that in the addition step of preparing the positive electrode active material, a solution containing methanesulfonic acid and LiOH (hereinafter, methanesulfonic acid + LiOH solution) prepared by dissolving methanesulfonic acid and LiOH in pure water at a molar ratio of 1:0.5 was added instead of powdered lithium methanesulfonate, and the amount of lithium methanesulfonate added was 0.5 mass% relative to the total mass of the lithium-containing transition metal composite oxide. The concentration of the added methanesulfonic acid + LiOH solution was 10 mass%, and the methanesulfonic acid + LiOH solution was added so that the amount of lithium methanesulfonate added was as described above.
[0096] Example 12 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing a positive electrode active material, a methanesulfonic acid + LiOH solution was added in place of powdered lithium methanesulfonate so that the molar ratio of methanesulfonic acid to LiOH was 1:1, and the amount of lithium methanesulfonate added was 0.5 mass% relative to the total mass of the lithium-containing transition metal composite oxide. The concentration of the added methanesulfonic acid + LiOH solution was 10 mass%, and the methanesulfonic acid + LiOH solution was added so that the amount of lithium methanesulfonate added was as described above.
[0097] Example 13 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing a positive electrode active material, powdery sodium methanesulfonate was added instead of powdery lithium methanesulfonate, and the amount of sodium methanesulfonate added was 0.5 mass % relative to the total mass of the lithium-containing transition metal composite oxide.
[0098] Example 14 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing a positive electrode active material, powdered lithium ethanesulfonate was added instead of powdered lithium methanesulfonate, and the amount of lithium ethanesulfonate added was 0.5 mass % relative to the total mass of the lithium-containing transition metal composite oxide.
[0099] <Comparative Example 1> A test cell was prepared and evaluated in the same manner as in Example 1, except that in the preparation of the positive electrode active material, the addition step was not performed and the initial charge-discharge efficiency and the cycle characteristics were evaluated without applying pressure to the test cell.
[0100] Comparative Example 2 A test cell was produced and evaluated in the same manner as in Example 1, except that the addition step was not carried out in the production of the positive electrode active material.
[0101] <Comparative Example 3> A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing a positive electrode active material, the amount of lithium methanesulfonate added was 0.5 mass % relative to the total mass of the lithium-containing transition metal composite oxide, and the initial charge-discharge efficiency and the cycle characteristics were evaluated without applying any pressure to the test cell.
[0102] Comparative Example 4 In the addition step of preparing the positive electrode active material, the amount of lithium methanesulfonate added was 0.5% by mass relative to the total mass of the lithium-containing transition metal composite oxide. The test cell was pressed from both sides in the stacking direction α in FIG. 2 , and 4.00×10 -2 Test cells were fabricated and evaluated in the same manner as in Example 1, except that the initial charge-discharge efficiency and cycle characteristics were evaluated under a pressure of 100 MPa.
[0103] <Comparative Example 5> A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing a positive electrode active material, a 10 mass % lithium succinate solution was added instead of powdered lithium methanesulfonate, and the amount of lithium succinate added was 0.5 mass % with respect to the total mass of the lithium-containing transition metal composite oxide.
[0104] <Comparative Example 6> A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing a positive electrode active material, a 10 mass % lithium oxalate solution was added instead of powdered lithium methanesulfonate, and the amount of lithium oxalate added was 0.5 mass % relative to the total mass of the lithium-containing transition metal composite oxide.
[0105] The initial charge-discharge efficiencies and capacity retention rates of the test cells of Examples 1 to 14 and Comparative Examples 1 to 6 are shown in Table 1. Table 1 also shows the composition of the lithium-containing transition metal composite oxide, the added compounds, the addition method, the added amounts, and the external pressure applied to the structure. The initial charge-discharge efficiencies and capacity retention rates of the test cells of Examples 1 to 14 and Comparative Examples 1 to 6 shown in Table 1 are expressed relative to the initial charge-discharge efficiency and capacity retention rate of the test cell of Comparative Example 1, which are set to 100. A larger value for the initial charge-discharge efficiency indicates better initial charge-discharge efficiency, and a larger value for the capacity retention rate indicates better cycle characteristics.
[0106]
[0107] As shown in Table 1, the test cells of the examples have improved initial charge-discharge efficiency and capacity retention rate compared to the test cells of the comparative examples. ―2 The test cell of Comparative Example 2, in which a construction pressure of 100 MPa or more was applied but no sulfonic acid compound was present on the surface of the secondary particles, showed a slightly improved capacity retention rate compared to the test cell of Comparative Example 1, but did not show an improved initial charge-discharge efficiency.
[0108] In addition, while a sulfonic acid compound is present on the surface, the electrode body is ―2The test cells of Comparative Examples 3 and 4, to which no structural pressure of 8.00 × 10 MPa or more was applied, exhibited a worse capacity retention rate than the test cell of Comparative Example 1. This is presumably because the presence of the sulfonic acid compound on the surface of the secondary particles increases the volume change of the crystal lattice of the positive electrode active material, causing cracking of the positive electrode active material particles and a side reaction between the cracking and the positive electrode active material particles and the non-aqueous electrolyte. On the other hand, when the test cell of the Example and the test cell of Comparative Example 2 are compared, the test cell of the Example exhibits improved initial charge / discharge efficiency as well as improved capacity retention. In other words, when the electrode body is subjected to a pressure of 8.00 × 10 ―2 By applying a pressure of 8.00 × 10 MPa or more and allowing the sulfonic acid compound to be present on the surfaces of the secondary particles, the capacity retention rate is also improved. This is presumably because cracking of the positive electrode active material particles is suppressed by the external pressure, and the sulfonic acid compound coats the surfaces of the positive electrode active material particles, thereby suppressing side reactions between the positive electrode active material particles and the non-aqueous electrolyte. In other words, when the external pressure is 8.00 × 10 ―2 If the thickness is less than 8.00 × 10, the positive electrode active material particles are likely to crack, making it difficult to obtain the effect of coating the surfaces of the positive electrode active material particles with the sulfonic acid compound. ―2 It can be said that by applying a pressure of 100 MPa or more, it is possible to provide a nonaqueous electrolyte secondary battery that is excellent in cycle characteristics while improving the initial charge-discharge efficiency.
[0109] Example 15 In the synthesis process for producing a positive electrode active material, the composition of the composite hydroxide was changed to [Ni 0.80 Co 0.10 Mn 0.10 ] (OH 2 ) and in the addition step, the amount of lithium methanesulfonate added with respect to the total mass of the lithium-containing transition metal composite oxide was set to 0.5 mass %, and a test cell was produced and evaluated in the same manner as in Example 1.
[0110] Example 16 In the synthesis process for producing a positive electrode active material, the composition of the composite hydroxide was changed to [Ni 0.90 Mn 0.05 Al 0.05 ] (OH 2) and in the addition step, the amount of lithium methanesulfonate added with respect to the total mass of the lithium-containing transition metal composite oxide was set to 0.5 mass %, and a test cell was produced and evaluated in the same manner as in Example 1.
[0111] Example 17 In the synthesis process for producing a positive electrode active material, the composition of the composite hydroxide was changed to [Ni 0.82 Co 0.02 Mn 0.10 Al 0.06 ](OH) 2 A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step, the amount of lithium methanesulfonate added was changed to 0.5 mass % relative to the total mass of the lithium-containing transition metal composite oxide.
[0112] Comparative Example 7 In the synthesis step of producing the positive electrode active material, the composition of the composite hydroxide was changed to [Ni 0.80 Co 0.10 Mn 0.10 ](OH) 2 A test cell was produced and evaluated in the same manner as in Example 1, except that the addition step was not performed.
[0113] Comparative Example 8 In the synthesis step of producing the positive electrode active material, the composition of the composite hydroxide was changed to [Ni 0.90 Co 0.05 Mn 0.05 ](OH) 2 A test cell was produced and evaluated in the same manner as in Example 1, except that the addition step was not performed.
[0114] Comparative Example 9 In the synthesis step of producing the positive electrode active material, the composition of the composite hydroxide was changed to [Ni 0.82 Co 0.02 Mn 0.10 Al 0.06 ](OH) 2 A test cell was produced and evaluated in the same manner as in Example 1, except that the addition step was not performed.
[0115] The initial charge-discharge efficiencies and capacity retention rates of the test cells of Examples 15 to 17 and Comparative Examples 7 to 9 are shown in Tables 2 to 4. Tables 2 to 4 also show the composition of the lithium-containing transition metal composite oxide, the added compounds, the addition method, the added amount, and the external pressure. The initial charge-discharge efficiencies and capacity retention rates of the test cell of Example 15 shown in Table 2 are expressed relative to the initial charge-discharge efficiencies and capacity retention rates of the test cell of Comparative Example 7, which are set to 100. The initial charge-discharge efficiencies and capacity retention rates of the test cell of Example 16 shown in Table 3 are expressed relative to the initial charge-discharge efficiencies and capacity retention rates of the test cell of Comparative Example 8, which are set to 100. The initial charge-discharge efficiencies and capacity retention rates of the test cell of Example 17 shown in Table 4 are expressed relative to the initial charge-discharge efficiencies and capacity retention rates of the test cell of Comparative Example 9, which are set to 100. As with Table 1, a larger value for the initial charge-discharge efficiency indicates better initial charge-discharge efficiency, and a larger value for the capacity retention rate indicates better cycle characteristics.
[0116]
[0117]
[0118]
[0119] As shown in Tables 2 to 4, the test cells of the examples have improved initial charge-discharge efficiency and capacity retention rate compared to the test cells of the comparative examples. In other words, the effects of the present disclosure are exhibited even when the composition of the metal oxide is changed.
[0120] Example 18 A test cell was produced in the same manner as in Example 1, except for the following changes in the preparation of the positive electrode active material: (1) In the synthesis step, the composition of the composite hydroxide was changed to [Ni 0.90 Co 0.05 Mn 0.05 ](OH) 2 After obtaining a metal oxide as above, Ca(OH) was added to the metal oxide so that the molar ratio of Ca was 0.25 mol % and the molar ratio of W was 0.5 mol % relative to the total amount of Ni, Co, and Mn. 2 and W.O. 3Furthermore, lithium hydroxide monohydrate (LiOH·H) was added so that the molar ratio of Li to the total amount of Ni, Co, Mn, Ca, and W was 1.03:1. 2 (2) In the addition step, the amount of lithium methanesulfonate added was 0.5% by mass relative to the total mass of the lithium-containing transition metal composite oxide.
[0121] The surfaces of the secondary particles and the interfaces between the primary particles inside the secondary particles were observed by TEM-EDX for the prepared positive electrode active material, and it was confirmed that a surface modification layer containing Ca and W was present. Furthermore, the compounds present in the positive electrode active material were identified by synchrotron X-ray diffraction measurement, and it was found that CaWO 4 The existence of was confirmed.
[0122] Comparative Example 10 A test cell was produced and evaluated in the same manner as in Example 17, except that the addition step was not carried out in the production of the positive electrode active material.
[0123] Table 5 shows the initial charge-discharge efficiencies and capacity retention rates of the test cells of Example 18 and Comparative Example 10. Table 5 also shows the composition of the lithium-containing transition metal composite oxide, the added compounds, the addition method, the added amount, and the external pressure. The initial charge-discharge efficiencies and capacity retention rates of the test cell of Example 18 shown in Table 5 are expressed relative to the initial charge-discharge efficiency and capacity retention rate of the test cell of Comparative Example 10, which are set to 100. As with Table 1, a larger value for the initial charge-discharge efficiency indicates better initial charge-discharge efficiency, and a larger value for the capacity retention rate indicates better cycle characteristics.
[0124]
[0125] As shown in Table 5, the test cell of Example 18 had improved initial charge-discharge efficiency and capacity retention rate compared to the test cell of Comparative Example 10. In other words, the effects of the present disclosure are exhibited even when a surface modification layer containing Ca and W is present on the surface of the primary particles.
[0126] Comparative Example 11 A test cell was produced in the same manner as in Example 1, except that the positive electrode active material was produced as follows.
[0127] [Ni] obtained by coprecipitation method 0.90 Co 0.05 Mn 0.05 ](OH) 2 The composite hydroxide represented by the formula (I) was calcined at 500°C for 8 hours to obtain a metal oxide. Next, LiOH and the metal oxide were mixed so that the molar ratio of Li to the total amount of Ni, Co, and Mn was 1.03:1 to obtain a mixture. This mixture was then heated under an oxygen flow (10 cm) with an oxygen concentration of 95%. 2 The mixture was heated from room temperature to 650°C at a temperature increase rate of 2.0°C / min under a temperature increase condition of 2 mL / min per 1 kg of the mixture and 5 L / min per 1 kg of the mixture, and then heated from 650°C to 780°C at a temperature increase rate of 0.5°C / min, and then maintained at this temperature for 4 hours to obtain a lithium-containing transition metal composite oxide.
[0128] Next, 1000 g of the lithium-containing transition metal composite oxide was prepared and added to 3.0 L of pure water and stirred to prepare a suspension. Next, erbium nitrate pentahydrate [Er(NO 3 ) 3 ・5H 2 875 mL of a solution prepared by dissolving 3.15 g of [C10] in 200 mL of pure water was added to the suspension, and a 10% by mass aqueous solution of nitric acid or a 10% by mass aqueous solution of sodium hydroxide was added appropriately to adjust the pH of the suspension to 9.0.
[0129] Next, after the addition of the erbium nitrate pentahydrate solution was completed, the mixture was subjected to suction filtration and further washed with water. The resulting powder was then dried at 120°C to obtain a powder in which erbium hydroxide was attached to a portion of the surface of the lithium-containing transition metal composite oxide as a surface-attached compound. Measurement of the resulting powder using an ICP atomic emission spectrometer revealed that the amount of erbium compound attached, in terms of elemental erbium, was 0.50% by mass relative to the lithium-containing transition metal composite oxide. The resulting powder was then heat-treated in air at 300°C for 5 hours to produce a positive electrode active material. Most of the erbium compound after the heat treatment was erbium oxyhydroxide.
[0130] Comparative Example 12 A test cell was prepared and evaluated in the same manner as in Comparative Example 11, except that in the preparation of the positive electrode, aluminum hydroxide was used as the compound to be adhered instead of erbium hydroxide, and heat treatment was performed at 400°C. Most of the adhered aluminum hydroxide was converted to oxide after heat treatment. The result of measuring the obtained powder using an ICP atomic emission spectrometer showed that the amount of adhered aluminum compound was 0.50 mass% in terms of aluminum element relative to the lithium-containing transition metal composite oxide.
[0131] <Comparative Example 13> A test cell was prepared and evaluated in the same manner as in Comparative Example 11, except that in the preparation of the positive electrode, magnesium hydroxide was used as the compound to be adhered instead of erbium hydroxide, and heat treatment was performed at 400°C. Most of the adhered magnesium hydroxide was converted to oxide after heat treatment. Note that, as a result of measuring the obtained powder using an ICP atomic emission spectrometer, the amount of adhered magnesium compound was 0.50 mass% in terms of magnesium element relative to the lithium-containing transition metal composite oxide.
[0132] Comparative Example 14 A test cell was prepared and evaluated in the same manner as in Comparative Example 11, except that in the preparation of the positive electrode, zirconium hydroxide was used as the compound to be adhered instead of erbium hydroxide, and heat treatment was performed at 400°C. Most of the adhered zirconium hydroxide was converted to oxide after heat treatment. Note that, as a result of measuring the obtained powder using an ICP atomic emission spectrometer, the amount of adhered zirconium compound was 0.50 mass% in terms of elemental zirconia relative to the lithium-containing transition metal composite oxide.
[0133] Comparative Example 15 A test cell was produced in the same manner as in Example 1, except that tungsten oxide was added instead of lithium methanesulfonate in the step of adding the positive electrode active material. The result of measuring the obtained powder using an ICP optical emission spectrometer showed that the amount of the tungsten compound attached was 0.50 mass% in terms of elemental tungsten relative to the lithium-containing transition metal composite oxide.
[0134] Table 6 shows the initial charge-discharge efficiencies and capacity retention rates of the test cells of Example 3 and Comparative Examples 11 to 15. Table 6 also shows the composition of the lithium-containing transition metal composite oxide, the added compounds, the addition method, the added amount, and the external pressure. The initial charge-discharge efficiencies and capacity retention rates of the test cells shown in Table 6 are expressed relative to the initial charge-discharge efficiency and capacity retention rate of the test cell of Comparative Example 1, which are set to 100. As in Table 1, a larger value for the initial charge-discharge efficiency indicates better initial charge-discharge efficiency, and a larger value for the capacity retention rate indicates better cycle characteristics.
[0135]
[0136] As shown in Table 6, the test cell of Example 3 has improved initial charge-discharge efficiency and capacity retention rate compared to the test cell of Comparative Example 1. In other words, when a sulfonic acid compound is present on the surface of the secondary particles, the initial charge-discharge efficiency and capacity retention rate are significantly improved compared to when an Er-containing compound, an Al-containing compound, an Mg-containing compound, a Zr-containing compound, or a W-containing compound is present on the surface of the particles.
[0137] The present disclosure will be further described by the following embodiments. Configuration 1: A non-aqueous electrolyte secondary battery including an electrode assembly having a structure in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween, and an exterior housing that houses the electrode assembly, wherein the positive electrode has a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core and containing a positive electrode active material, the positive electrode active material containing a lithium-containing transition metal composite oxide having a layered structure, and the lithium-containing transition metal composite oxide is represented by the general formula Li x Ni a Co b Mn c M d O 2-y(wherein 0.80<x<1.20, 0.75<a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr), and the secondary particles are formed by aggregation of primary particles, and the sulfonic acid compound represented by formula (I) is present on the surface of the secondary particles, and when pressure is applied from the outside of the outer package in the stacking direction of the positive electrode, the negative electrode, and the separator, the electrode body is formed of a 8.00×10 ―2 A non-aqueous electrolyte secondary battery to which a pressure of 100 MPa or more is applied. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) Configuration 2: The nonaqueous electrolyte secondary battery according to Configuration 1, wherein A is a Group 1 element. Configuration 3: The nonaqueous electrolyte secondary battery according to Configuration 1 or 2, wherein A is Li. Configuration 4: The nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 3, wherein R is an alkyl group. Configuration 5: The nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein R is a methyl group. Configuration 6: The nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 5, wherein, in the positive electrode active material, the amount of the sulfonic acid compound present on the surface of the lithium-containing transition metal composite oxide is 0.1 mass % or more and 1 mass % or less, relative to the mass of the lithium-containing transition metal composite oxide. Configuration 7: The nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 6, wherein a surface modification layer containing at least one of Ca and Sr is present on the surfaces of the primary particles. Configuration 8: A battery pack including a plurality of the nonaqueous electrolyte secondary batteries according to any one of Configurations 1 to 7, wherein the plurality of nonaqueous electrolyte secondary batteries are arranged in a stacking direction of the positive electrode, the negative electrode, and the separator, and are constrained to each other in the arrangement direction.
[0138] REFERENCE SIGNS LIST 10 Non-aqueous electrolyte secondary battery, 11 Electrode body, 12 Positive electrode terminal, 13 Negative electrode terminal, 14 Battery case (exterior body), 15 Case body, 16 Sealing body, 17 Insulating member, 20 Positive electrode, 21 Negative electrode, 22 Separator, 30 Battery pack, 31 Battery group, 32 Spacer, 33 End plate, 34 Bus bar, 35, 36 Bind bar
Claims
1. A non-aqueous electrolyte secondary battery comprising an electrode assembly having a structure in which a positive electrode and a negative electrode are laminated with a separator interposed therebetween, and an exterior housing for housing the electrode assembly, wherein the positive electrode has a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core and containing a positive electrode active material, the positive electrode active material contains a lithium-containing transition metal composite oxide having a layered structure, and the lithium-containing transition metal composite oxide is represented by the general formula Li x Ni a Co b Mn c M d O 2-y (wherein 0.80<x<1.20, 0.75<a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr), and the secondary particles are formed by aggregation of primary particles, and a sulfonic acid compound represented by formula (I) is present on the surface of the secondary particles, and a pressure is applied from the outside of the exterior body in the stacking direction of the positive electrode, the negative electrode, and the separator, whereby the electrode body is compressed to a pressure of 8.00×10 ―2 A non-aqueous electrolyte secondary battery to which a pressure of MPa or more is applied. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein A is a Group 1 element.
3. The nonaqueous electrolyte secondary battery according to claim 1, wherein A is Li.
4. The nonaqueous electrolyte secondary battery according to claim 1, wherein R is an alkyl group.
5. The nonaqueous electrolyte secondary battery according to claim 1, wherein R is a methyl group.
6. The nonaqueous electrolyte secondary battery according to claim 1, wherein in the positive electrode active material, the amount of the sulfonic acid compound present on the surface of the lithium-containing transition metal composite oxide is 0.1 mass % or more and 1 mass % or less with respect to the mass of the lithium-containing transition metal composite oxide.
7. The nonaqueous electrolyte secondary battery according to claim 1, wherein a surface modification layer containing at least one of the elements Ca and Sr is present on the surfaces of the primary particles.
8. An assembled battery comprising a plurality of the nonaqueous electrolyte secondary batteries according to any one of claims 1 to 7, wherein the plurality of nonaqueous electrolyte secondary batteries are arranged in a stacking direction of the positive electrode, negative electrode and separator and are mutually constrained in the arrangement direction.
Citation Information
Patent Citations
Flat non-aqueous electrolyte secondary battery and battery pack using the same
JP6509989B2
Lithium ion secondary battery and anode plate of lithium ion secondary battery
CN102610790A
Composite high-nickel ternary positive electrode material and preparation method thereof
CN112164774A
Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery
JP2019169286A
Flat nonaqueous electrolyte secondary battery and battery pack using same
WO2014119275A1