Slurry for forming electrode, nonaqueous electrolyte secondary battery and method for manufacturing same, and dispersant
The introduction of a specific dispersant polymer in the electrode forming slurry for non-aqueous electrolyte secondary batteries addresses the fluidity and performance issues of high-content active material slurries, enhancing battery performance and uniformity by maintaining a slurry-like state and improving handling.
Patent Information
- Application Number
- PCT/JP2024/015278
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-17
- Publication Date
- 2024-10-31
AI Technical Summary
High-content electrode active material slurries for non-aqueous electrolyte secondary batteries face challenges with decreased fluidity, leading to poor uniformity and battery performance, such as increased resistance and capacity variations, due to the solid-like properties of the slurry.
Incorporating a dispersant polymer with a specific composition and molecular weight range into the electrode forming slurry, containing 80-99% of a component represented by formula (1) and 1-20% of components represented by formulas (2) or (3), which enhances the fluidity and dispersibility of the electrode active material in the non-aqueous electrolyte.
The dispersant polymer significantly improves the fluidity of the slurry, ensuring better handling and performance of non-aqueous electrolyte secondary batteries by maintaining a slurry-like state even with high active material content, resulting in improved battery performance and uniformity.
Smart Images

Figure JP2024015278_31102024_PF_FP_ABST
Abstract
Description
Electrode-forming slurry, non-aqueous electrolyte secondary battery and method for producing the same, and dispersant
[0001] The present invention relates to a slurry for forming an electrode of a nonaqueous electrolyte secondary battery, a nonaqueous electrolyte secondary battery and a method for producing the same, and a dispersant.
[0002] Non-aqueous electrolyte secondary batteries, typified by lithium-ion secondary batteries, have high energy density and excellent storage performance, low-temperature operation, etc., and are widely used in portable electronic devices such as mobile phones and laptop computers. Furthermore, larger batteries are being used in transportation equipment such as automobiles, and their use as storage devices for nighttime electricity and electricity generated by natural energy sources is also progressing.
[0003] Techniques for increasing the capacity of non-aqueous electrolyte secondary batteries have been studied. For example, Patent Document 1 discloses a technique for making an electrode active material layer function as a secondary battery in the form of a slurry containing a high amount of active material. Specifically, the document describes an electrochemical cell including: a positive electrode made of a non-binding material containing a first active material and an electrolyte solution in a first non-aqueous liquid electrolyte; a negative electrode made of a non-binding material containing a second active material and an electrolyte solution in a second non-aqueous liquid electrolyte; and an ion-permeable membrane disposed between the positive electrode and the negative electrode, wherein the positive electrode and the negative electrode each have a thickness of about 200 μm to about 3000 μm. According to the technology described in Patent Document 1, like the above-mentioned positive and negative electrodes, the electrode active material layers (positive electrode active material layer and negative electrode active material layer) contain an electrolyte and are in a slurry state and in an unbound state, so that the electrode active material layer can be made into a thick film while maintaining its flexibility, and no binder is required to bind the solid particles together, making it possible to significantly increase the overall charge capacity and energy density while maintaining the flexibility of the battery. A nonaqueous electrolytic secondary battery in which the electrode active material layer is formed in a slurry state containing an electrolytic solution (electrolyte), as described in Patent Document 1, may be referred to as a quasi-solid secondary battery in the following description.
[0004] Japanese Patent Application Laid-Open No. 2022-139794
[0005] To further increase the capacity (energy density) of quasi-solid secondary batteries, attempts have been made to increase the content of electrode active material, which stores and releases ions, in the slurry-like electrode active material layer. In this case, the electrode-forming slurry used to form the slurry-like electrode active material layer is increased in content of solid particle electrode active material, which is then applied to a current collector. However, when the electrode active material content in the slurry is increased, the slurry becomes more like a powder, even though it contains an electrolyte solution. As a result, the fluidity of the slurry decreases, making it difficult to apply it uniformly. As a result, the resulting quasi-solid secondary batteries tend to have variable performance and inferior battery performance (e.g., resistance, capacity).
[0006] The present invention relates to a technology that can sufficiently increase the fluidity of an electrode-forming slurry containing an electrode active material, a conductive additive, and a non-aqueous electrolyte solution (a "nonaqueous electrolyte solution" is a liquid composed of an electrolyte and a non-aqueous solvent), even when the electrode active material content is high, thereby improving the handleability (manufacturability) and the performance of the resulting non-aqueous electrolyte secondary battery (quasi-solid secondary battery).
[0007] That is, the present invention provides the following electrode-forming slurry, nonaqueous electrolyte secondary battery and method for producing the same, and dispersant.
[0008] [1] A slurry for forming an electrode, comprising an electrode active material, a conductive additive, a non-aqueous electrolyte, and a dispersant, the dispersant being made of a polymer having a weight average molecular weight of 1,000 to 15,000, which polymer contains 80 to 99% by mass of a component represented by the following formula (1) and 1 to 20% by mass in total of a component represented by the following formula (2) or (3): In the above formula, * indicates a linking site. 1 represents a hydrocarbon group having 1 to 8 carbon atoms. 2 ~R 6 represents a hydrogen atom or methyl. 7 represents a hydrocarbon group having 5 to 18 carbon atoms. 8represents a group having 1 to 12 carbon atoms and having a nitrogen atom. n is a number from 3 to 30. [2] The electrode-forming slurry according to [1], wherein the electrode active material is a positive electrode active material, and the content of the positive electrode active material in the electrode-forming slurry is 60 to 90 mass %. [3] The electrode-forming slurry according to [1], wherein the electrode active material is a negative electrode active material, and the content of the negative electrode active material in the electrode-forming slurry is 50 to 80 mass %. [4] The electrode-forming slurry according to [2] or [3], wherein the content of the dispersant is 0.1 to 5.0 parts by mass per 100 parts by mass of the total of the nonaqueous electrolyte and the dispersant. [5] A nonaqueous electrolyte secondary battery having an electrode active material layer formed from the electrode-forming slurry according to any one of [1] to [4]. [6] A method for producing a nonaqueous electrolyte secondary battery, comprising forming an electrode active material layer from the electrode-forming slurry according to any one of [1] to [4]. [7] A dispersant comprising the following polymer for use in an electrode-forming slurry containing an electrode active material, a conductive additive, and a non-aqueous electrolyte: <Polymer> A polymer containing 80 to 99 mass % of a component represented by the following formula (1) and 1 to 20 mass % in total of a component represented by the following formula (2) or (3), and having a weight-average molecular weight of 1,000 to 15,000: In the above formula, * indicates a linking site. 1 represents a hydrocarbon group having 1 to 8 carbon atoms. 2 ~R 6 represents a hydrogen atom or methyl. 7 represents a hydrocarbon group having 5 to 18 carbon atoms. 8 represents a group having 1 to 12 carbon atoms and a nitrogen atom, and n is a number from 3 to 30.
[0009] In the description of the present invention, a numerical range expressed using "to" means a range including the numerical values written before and after "to" as the lower and upper limits. In the present invention, "nonaqueous electrolyte" means an electrolyte that does not substantially contain water. In other words, the "nonaqueous electrolyte" may contain a small amount of water within a range that does not impair the effects of the present invention. In the present invention, the "nonaqueous electrolyte" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 20 ppm or less. Note that it is practically difficult to make a nonaqueous electrolyte completely anhydrous, and it usually contains 1 ppm or more of water. In the present invention, "nonaqueous solvent" also means a solvent that does not substantially contain water. In other words, the "nonaqueous solvent" may contain a small amount of water within a range that does not impair the effects of the present invention. In the present invention, the "nonaqueous solvent" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 20 ppm or less. In reality, it is difficult to make a non-aqueous solvent completely free of water, and it usually contains 1 ppm or more of water.
[0010] The electrode-forming slurry of the present invention can sufficiently increase fluidity and has excellent handleability even when the electrode active material is contained at a high content, and can improve the performance of a nonaqueous electrolyte secondary battery (quasi-solid secondary battery) having a slurry-like electrode active material layer formed from this slurry. The nonaqueous electrolyte secondary battery of the present invention is a nonaqueous electrolyte secondary battery having a slurry-like electrode active material layer formed from the electrode-forming slurry of the present invention. The nonaqueous electrolyte secondary battery of the present invention can be obtained by the manufacturing method of the nonaqueous electrolyte secondary battery. By incorporating the dispersant of the present invention into an electrode-forming slurry containing an electrode active material, a conductive additive, and a nonaqueous electrolyte, the fluidity of the slurry can be sufficiently increased even when the electrode active material is contained at a high content.
[0011] FIG. 1 is a longitudinal cross-sectional view showing a schematic diagram of a basic layer structure of an embodiment of a nonaqueous electrolyte secondary battery.
[0012] Although preferred embodiments of the present invention will be described, the present invention is not limited to these embodiments except as defined in the present invention.
[0013] [Slurry for Electrode Formation] The slurry for electrode formation of the present invention (also referred to as "slurry of the present invention") is a slurry (suspension, dispersion) containing an electrode active material, a conductive additive, and a non-aqueous electrolyte, and is suitable for forming an electrode active material layer in a non-aqueous electrolyte secondary battery (i.e., a quasi-solid secondary battery) having a slurry-like electrode active material layer. In addition to the above components, the slurry of the present invention contains, as a dispersant, a polymer having a specific structure and a molecular weight within a specific range. Each component constituting the slurry of the present invention will be described.
[0014] <Dispersant> The polymer constituting the dispersant has a structure containing 80 to 99% by mass of a constituent component represented by the following formula (1) and 1 to 20% by mass in total of a constituent component represented by the following formula (2) or (3). Here, "containing 1 to 20% by mass in total of a constituent component represented by the following formula (2) or (3)" means that when the polymer has a constituent component represented by the following formula (2) but does not have a constituent component represented by the following formula (3), the content of the constituent component represented by the following formula (2) in the polymer is 1 to 20% by mass. Also, when the polymer has a constituent component represented by the following formula (3) but does not have a constituent component represented by the following formula (2), the content of the constituent component represented by the following formula (3) in the polymer is 1 to 20% by mass. Also, when the polymer has both a constituent component represented by the following formula (2) and a constituent component represented by the following formula (3), the total content of the constituent component represented by the following formula (2) and the constituent component represented by the following formula (3) in the polymer is 1 to 20% by mass. The polymer constituting the dispersant preferably contains 83 to 97% by mass of a component represented by the following formula (1) and 3 to 17% by mass in total of a component represented by the following formula (2) or (3), more preferably 85 to 95% by mass of a component represented by the following formula (1) and 5 to 15% by mass in total of a component represented by the following formula (2) or (3), even more preferably 87 to 95% by mass of a component represented by the following formula (1) and 5 to 13% by mass in total of a component represented by the following formula (2) or (3), and even more preferably 87 to 93% by mass of a component represented by the following formula (1) and 7 to 13% by mass in total of a component represented by the following formula (2) or (3).
[0015] The weight average molecular weight (Mw) of the polymer is in the range of 1000 to 15000. The Mw of the polymer can be determined by the following method.
[0016] (Measurement of Weight Average Molecular Weight) In the present invention, the Mw of a polymer is measured by gel permeation chromatography (GPC). Mw is the Mw calculated as polyethylene oxide. As a general rule, the Mw is measured by the following method. However, depending on the type of polymer, an appropriate eluent (carrier) is selected and used. Measuring device: HLC-8320GPC (trade name, manufactured by Tosoh Corporation) Column: TOSOH TSKgel guard column Super HZ-L, Super HZM-H, Super HZ4000, Super HZ2000 (trade name, manufactured by Tosoh Corporation) Carrier: Tetrahydrofuran solution Measurement temperature: 40°C Carrier flow rate: 0.35 ml / min Sample concentration: 0.2% by mass Detector: RI (refractive index) detector
[0017] The Mw of the polymer is preferably in the range of 1,500 to 14,000, more preferably in the range of 2,000 to 13,000, even more preferably in the range of 2,500 to 12,000, and even more preferably in the range of 2,500 to 10,000.
[0018] The polymer contains the specific amounts of each of the above-mentioned components and has an Mw controlled within the above range, so that it is liquid at room temperature (25°C) and is compatible with the non-aqueous solvent or electrolyte in the slurry of the present invention (i.e., it can exist uniformly in the slurry without phase separation or precipitation). The polymer may contain components (other components) other than the components represented by each of the following formulas (1) to (3). The content of other components in the polymer is preferably 10% by mass or less, more preferably 8% by mass or less, even more preferably 6% by mass or less, even more preferably 4% by mass or less, even more preferably 2% by mass or less, even more preferably 1% by mass or less, and even more preferably 0.5% by mass or less. In particular, it is preferable that the polymer does not contain other components.
[0019]
[0020] In the above formula, * indicates a linking site for incorporation into the polymer structure. 1 represents a hydrocarbon group having 1 to 8 carbon atoms. 2 ~R 6 represents a hydrogen atom or methyl. 7 represents a hydrocarbon group having 5 to 18 carbon atoms. 8 represents a group having 1 to 12 carbon atoms and a nitrogen atom, and n is a number from 3 to 30.
[0021] The R of formula (1) 1 is preferably a chain (non-cyclic) hydrocarbon group. This chain hydrocarbon group may be linear or branched, and is preferably linear.
[0022] The above R 1 is preferably a hydrocarbon group having 1 to 6 carbon atoms, more preferably 1 to 5 carbon atoms, even more preferably 1 to 4 carbon atoms, and even more preferably 1 to 3 carbon atoms. 1 is more preferably methyl or ethyl, and particularly preferably methyl.
[0023] In formula (1), n is the average number of moles of oxyalkylene groups added, and is preferably 5 to 30, more preferably 6 to 25, even more preferably 7 to 20, and still more preferably 8 to 15.
[0024] The R of formula (2) 7 R may be a chain (non-cyclic) hydrocarbon group or a hydrocarbon group having a cyclic structure, and a hydrocarbon group having a cyclic structure is more preferred. 7 When R is a chain hydrocarbon group, it may be a straight chain or a branched chain, and is preferably a straight chain. 7 When is a hydrocarbon group having a cyclic structure, it is preferably a hydrocarbon group having an aromatic ring, more preferably a hydrocarbon group having a benzene ring or a naphthalene ring.
[0025] The above R 7 is preferably a hydrocarbon group having 6 to 17 carbon atoms, more preferably 6 to 16 carbon atoms, even more preferably 6 to 15 carbon atoms, still more preferably 6 to 14 carbon atoms, still more preferably 7 to 12 carbon atoms, and particularly preferably 7 to 11 carbon atoms.
[0026] The R of formula (3) 8 is this R 8 The carbon atom to which R 6 It is preferable that the component represented by formula (3) is a component derived from a (meth)acrylamide compound (an acrylamide compound or a methacrylamide compound). 8 The number of nitrogen atoms in R is preferably 1 to 3, more preferably 1 or 2, and even more preferably 1. 8 contains carbon atoms and hydrogen atoms as constituent elements other than nitrogen atoms. It is also preferable that it contains an oxygen atom. This oxygen atom is preferably present as a constituent element of a carbonyl group. 8 The number of oxygen atoms in the R is preferably 1 to 3, more preferably 1 or 2, and even more preferably 1. 8 may have a chain structure or a cyclic structure. 8 When R has a chain structure, it may have a branch. 8 The number of carbon atoms is preferably 2 to 12, more preferably 3 to 12, and even more preferably 4 to 12.
[0027] In the polymer, the component represented by formula (1) mainly exhibits affinity for the non-aqueous electrolyte (non-aqueous solvent), and the component represented by formula (2) or (3) mainly exhibits affinity for the electrode active material. This effectively functions as a dispersant that enhances the dispersibility of the electrode active material in the non-aqueous electrolyte and reduces the viscosity of the slurry. The polymer may be a random polymer, a block polymer, or a graft polymer, and is preferably a random polymer.
[0028] Whether the slurry of the present invention is a slurry for forming a positive electrode or a slurry for forming a negative electrode, the content of the dispersant (polymer) in the slurry of the present invention is preferably 0.1 to 5.0 parts by mass, more preferably 0.2 to 4.0 parts by mass, even more preferably 0.4 to 3.0 parts by mass, still more preferably 0.6 to 2.5 parts by mass, even more preferably 0.7 to 2.0 parts by mass, still more preferably 0.8 to 1.8 parts by mass, even more preferably 0.8 to 1.6 parts by mass, also preferably 0.8 to 1.4 parts by mass, and also preferably 0.8 to 1.2 parts by mass, per 100 parts by mass of the total of the non-aqueous electrolyte and the dispersant.
[0029] For each of the constituent components represented by the formulas (1) to (3) above, preferred specific examples of the monomers from which each constituent component is derived are shown below, but the present invention is not limited to these specific examples. In the structural formulas below, "Me" stands for methyl, and each structural formula is given the abbreviation of the monomer, with the official name being described in the Examples section.
[0030] Monomers leading to the constituents of formula (1)
[0031] Monomers leading to the constituents of formula (2)
[0032] Monomers leading to the building blocks of formula (3)
[0033] <Electrode Active Material> When the slurry of the present invention is used to form a positive electrode active material layer, it contains a positive electrode active material as the electrode active material, and when the slurry is used to form a negative electrode active material layer, it contains a negative electrode active material as the electrode active material.
[0034] (Positive electrode active material) The positive electrode active material is preferably one that can reversibly insert and release lithium ions. The material is not particularly limited as long as it exhibits the desired electronic conductivity, and examples thereof include transition metal oxides, organic substances, sulfur, and other substances that can be composited with Li, as well as sulfur-metal composites. Among these, it is preferable to use lithium-containing transition metal oxides as the positive electrode active material, and it is also preferable to use transition metal elements M aIt is more preferable that the lithium-containing transition metal oxide contains at least one element selected from Co, Ni, Fe, Mn, Cu, and V. b (Elements of Group 1 (Ia) of the periodic table other than lithium, elements of Group 2 (IIa), Al, Ga, In, Ge, Sn, Pb, Sb, Bi, Si, P, B, etc.) may be mixed. The amount of the mixed element may be determined by the following formula: a The amount of Li / M is preferably 0 to 30 mol % relative to the amount of Li / M (100 mol %). a More preferably, the lithium-containing transition metal oxide is synthesized by mixing the above-mentioned components so that the molar ratio of the above-mentioned components is 0.3 to 2.2. Specific examples of the lithium-containing transition metal oxide include (MA) a lithium-containing transition metal oxide having a layered rock salt structure, (MB) a lithium-containing transition metal oxide having a spinel structure, (MC) a lithium-containing transition metal phosphate compound, (MD) a lithium-containing transition metal halide phosphate compound, and (ME) a lithium-containing transition metal silicate compound.
[0035] (MA) Specific examples of lithium-containing transition metal oxides having a layered rock salt structure include LiCoO 2 (Lithium cobalt oxide [LCO]), LiNi 2 O 2 (lithium nickel oxide), LiNi 0.85 Co 0.10 Al 0.05 O 2 (nickel cobalt lithium aluminum oxide [NCA]), LiNi 1/3 Co 1/3 Mn 1/3 O 2 (Lithium nickel manganese cobalt oxide [NMC]) and LiNi 0.5 Mn 0.5 O 2 (Lithium manganese nickel oxide). (MB) Specific examples of lithium-containing transition metal oxides having a spinel structure include LiMn 2 O 4 (LMO), LiCoMnO 4 , Li 2 FeMn 3 O 8 , Li 2 CuMn3 O 8 , Li 2 CrMn 3 O 8 and Li 2 NiMn 3 O 8 Examples of the (MC) lithium-containing transition metal phosphate compound include LiFePO 4 and Li 3 Fe 2 (P.O. 4 ) 3 Olivine-type iron phosphate salts such as LiFeP 2 O 7 Iron pyrophosphates such as LiCoPO 4 Cobalt phosphates such as Li 3 V 2 (P.O. 4 ) 3 (MD) Examples of lithium-containing transition metal halide phosphate compounds include, for example, Li 2 FePO 4 Fluorophosphate iron salts such as F, Li 2 MnPO 4 Fluorophosphate manganese salts such as F and Li 2 CoPO 4 Examples of the (ME) lithium-containing transition metal silicate compound include cobalt fluoride phosphates such as Li 2 FeSiO 4 , Li 2 MnSiO 4 and Li 2 CoSiO 4 In the present invention, the positive electrode active material is preferably a lithium-containing transition metal phosphate compound (MC), such as LiFePO 4 is more preferred.
[0036] The shape of the positive electrode active material is not particularly limited, but particulate form is preferred. The average particle size (average particle size in equivalent spheres) of the positive electrode active material is not particularly limited. For example, it can be 0.1 to 50 μm, preferably 0.2 to 30 μm, more preferably 0.5 to 20 μm, and even more preferably 0.8 to 10 μm. A conventional grinder or classifier can be used to adjust the positive electrode active material to a predetermined particle size. The positive electrode active material obtained by the calcination method may be used after washing with water, an acidic aqueous solution, an alkaline aqueous solution, or an organic solvent.
[0037] When a commercially available positive electrode active material is used, the average particle size of the positive electrode active material is the value listed in the manufacturer's catalog. When the manufacturer's average particle size information is unavailable or when a synthesized positive electrode active material is used, the positive electrode active material is dispersed in water and the particle size value (volume-based median diameter D50 in water) obtained by measuring with a laser diffraction / scattering particle size distribution measurement device (e.g., HORIBA Particle LA-960V2) is used. This also applies to the average particle size of solid particles other than the positive electrode active material.
[0038] The chemical formula of the compound obtained by the above calcination method can be measured by inductively coupled plasma (ICP) emission spectroscopy, or simply calculated from the difference in mass of the powder before and after calcination.
[0039] The surface of the positive electrode active material may be coated with an oxide such as another metal oxide, a carbon-based material, or the like. These surface coating layers can function as an interface resistance stabilizing layer. Examples of surface coating agents include metal oxides containing Ti, Nb, Ta, W, Zr, Al, Si, or Li. Specific examples include titanate spinel, tantalum-based oxides, niobium-based oxides, and lithium niobate-based compounds, such as Li 4 Ti 5 O 12 , Li 2 Ti 2 O 5 , LiTaO 3 , LiNbO 3 , LiAlO 2 , Li 2 ZrO 3 , Li 2 WO 4 , Li2 TiO 3 , Li 2 B 4 O 7 , Li 3 P.O. 4 , Li 2 MoO 4 , Li 3 BO 3 , LiBO 2 , Li 2 CO 3 , Li 2 SiO 3 , SiO 2 , TiO 2 , ZrO 2 , Al 2 O 3 , B 2 O 3 , and Li 3 AlF 6 Carbon-based materials such as C, SiC, and SiOC (carbon-doped silicon oxide) can also be used as the surface coating material.
[0040] The positive electrode active material may be surface-coated with a carbon-based material in order to increase the electronic conductivity to a desired level. In this case, the positive electrode active material is preferably surface-coated with carbon (C). The carbon surface coating can be formed by baking the positive electrode active material in the presence of an additive (organic substance) that serves as a carbon source. Examples of the additive that can be used include styrene-maleic anhydride copolymer, polystyrene, and polycarbonate.
[0041] The surface of the positive electrode active material may be treated with sulfur or phosphorus. Furthermore, the particle surfaces of the positive electrode active material may be treated with actinic rays or an active gas (plasma, etc.) before or after the surface coating.
[0042] The positive electrode active materials may be used alone or in combination of two or more.
[0043] When the slurry of the present invention contains a positive electrode active material (in the case of a positive electrode-forming slurry), the content of the positive electrode active material in the slurry solids is preferably 95.00 to 99.95 mass%, more preferably 96.00 to 99.90 mass%, and even more preferably 97.00 to 99.80 mass%, although it depends on the content of the conductive additive.
[0044] When the slurry of the present invention contains a positive electrode active material (in the case of a positive electrode forming slurry), the content of the positive electrode active material in the slurry is preferably as high as possible within a range that allows the desired low viscosity to be achieved. For example, the content of the positive electrode active material in the slurry can be 60 to 90 mass%, more preferably 65 to 88 mass%, even more preferably 70 to 86 mass%, even more preferably 72 to 85 mass%, even preferably 73 to 84 mass%, even preferably 73 to 83 mass%, even preferably 73 to 82 mass%, even preferably 73 to 81 mass%.
[0045] (Negative electrode active material) The negative electrode active material is preferably one that can reversibly absorb and release lithium ions. The material is not particularly limited as long as it has the desired properties, and examples thereof include carbonaceous materials, silicon-based materials, metal oxides, metal composite oxides, lithium alone, lithium alloys, and negative electrode active materials that can form alloys with lithium. Among these, carbonaceous materials or silicon-based materials are preferably used from the viewpoint of reliability.
[0046] The carbonaceous material used as the negative electrode active material is a material essentially composed of carbon. Examples include carbon black such as petroleum pitch, graphite (natural graphite, artificial graphite such as vapor-grown graphite, etc.), and carbonaceous materials obtained by calcining various synthetic resins such as PAN (polyacrylonitrile)-based resins and furfuryl alcohol resins. Further examples include various carbon fibers such as PAN-based carbon fiber, cellulose-based carbon fiber, pitch-based carbon fiber, vapor-grown carbon fiber, dehydrated PVA (polyvinyl alcohol)-based carbon fiber, lignin carbon fiber, glassy carbon fiber, and activated carbon fiber, as well as mesophase microspheres, graphite whiskers, and tabular graphite.
[0047] The metal oxides and metal composite oxides used as the negative electrode active material are not particularly limited as long as they are oxides capable of absorbing and releasing lithium. Amorphous oxides are preferred, and chalcogenides, which are reaction products of metal elements and elements of Group 16 of the periodic table, are also preferred. The term "amorphous" as used herein refers to an X-ray diffraction method using CuKα radiation that has a broad scattering band with a peak in the 2θ value range of 20° to 40°, and may also have crystalline diffraction lines. Among the above amorphous oxides and chalcogenides, amorphous oxides or chalcogenides of metalloid elements are more preferred, and oxides or chalcogenides consisting of one or a combination of two or more of elements from Groups 13 (IIIB) to 15 (VB) of the periodic table, Al, Ga, Si, Sn, Ge, Pb, Sb, and Bi, are particularly preferred. Specific examples of preferred amorphous oxides and chalcogenides include, for example, Ga, 2 O 3 , GeO, PbO, PbO 2 , Pb 2 O 3 , Pb 2 O 4 , Pb 3 O 4 , Sb 2 O 3 , Sb 2 O 4 , Sb 2 O 8 Bi 2 O 3 , Sb 2 O 8 Si 2 O 3 , Sb 2 O 5 , Bi 2 O 3 , Bi 2 O 4 , GeS, PbS, PbS 2 , Sb 2 S 3 and Sb 2 S 5 are preferred.
[0048] The metal (composite) oxide and the chalcogenide preferably contain at least one of titanium and lithium as a constituent component from the viewpoint of charge / discharge characteristics at high current density. Examples of the lithium-containing metal composite oxide (lithium composite metal oxide) include, for example, composite oxides of lithium oxide and the metal (composite) oxide or the chalcogenide, more specifically, Li 2 SnO 2 Examples include:
[0049] The negative electrode active material preferably contains titanium atoms. More specifically, TiNb 2 O 7 (Niobium titanate oxide [NTO]), Li 4 Ti 5 O1 2 Lithium titanate (LTO) is preferred because it has small volume fluctuations during absorption and desorption of lithium ions, has excellent rapid charge and discharge characteristics, suppresses electrode deterioration, and enables an improvement in the life of the lithium ion secondary battery.
[0050] The lithium alloy as the negative electrode active material is not particularly limited as long as it is an alloy that is commonly used as a negative electrode active material for secondary batteries, and an example thereof is a lithium aluminum alloy.
[0051] The negative electrode active material capable of forming an alloy with lithium is not particularly limited as long as it is one commonly used as a negative electrode active material for secondary batteries. Such active materials undergo large expansion and contraction during charging and discharging, resulting in reduced solid particle binding as described above. However, the present invention achieves high binding by using the binder. Examples of such active materials include negative electrode active materials containing silicon or tin atoms, and metals such as Al and In. Negative electrode active materials containing silicon atoms (silicon-containing active materials) that enable higher battery capacity are preferred, and silicon-containing active materials with a silicon atom content of 40 mol% or more of the total constituent atoms are more preferred. Generally, negative electrodes containing these negative electrode active materials (e.g., Si negative electrodes containing silicon-containing active materials, Sn negative electrodes containing tin-containing active materials) can absorb more Li ions than carbon negative electrodes (e.g., graphite and acetylene black). In other words, the amount of Li ions absorbed per unit mass is increased. This increases battery capacity (energy density). As a result, the battery operating time can be extended. Examples of silicon-atom-containing active materials include silicon materials such as Si and SiOx (0<x≦1), and alloys containing titanium, vanadium, chromium, manganese, nickel, copper, or lanthanum (e.g., LaSi 2 , VSi 2 ), or structured active materials (e.g., LaSi2 / Si), as well as SnSiO 3 , SnSiS 3 Examples of the active material containing silicon atoms and tin atoms include SiOx itself as a negative electrode active material (semi-metal oxide), and can also be used as an active material (precursor material) that can be alloyed with lithium because it generates Si during battery operation. Examples of the negative electrode active material containing tin atoms include Sn, SnO, and SnO 2 , SnS, SnS 2 and active materials containing silicon atoms and tin atoms. Also, composite oxides with lithium oxide, for example, Li 2 SnO 2 Also included are:
[0052] The shape of the negative electrode active material is not particularly limited, but a particulate form is preferred. The average particle diameter of the negative electrode active material is preferably 0.1 to 60 μm. To achieve the desired particle diameter, a conventional grinder or classifier is used. For example, a mortar, ball mill, sand mill, vibration ball mill, satellite ball mill, planetary ball mill, swirling airflow jet mill, or sieve is preferably used. Wet grinding in the presence of water or an organic solvent such as methanol can also be performed during grinding. Classification is preferably performed to achieve the desired particle diameter. The classification method is not particularly limited, and a sieve, air classifier, or the like can be used as desired. Classification can be performed using either a dry method or a wet method.
[0053] The above-mentioned negative electrode active materials may be used singly or in combination of two or more. Among them, a combination of a silicon atom-containing active material and a carbonaceous material is preferred, and a combination of SiOx (0<x≦1) and graphite is particularly preferred. When SiOx (0<x≦1) and graphite are combined, the mass ratio (SiOx / graphite) is preferably 2 or less, more preferably 1 or less, and even more preferably 0.5 or less. When forming a negative electrode active material layer, the unit area (cm 2 The mass (mg) (basis weight) of the negative electrode active material per unit area is not particularly limited and can be determined appropriately depending on the designed battery capacity.
[0054] When the slurry of the present invention contains a negative electrode active material (in the case of a negative electrode-forming slurry), the content of the negative electrode active material in the slurry solids is preferably 95.00 to 99.95 mass%, more preferably 96.00 to 99.90 mass%, and even more preferably 97.00 to 99.80 mass%, although it depends on the content of the conductive additive.
[0055] When the slurry of the present invention contains a negative electrode active material (in the case of a negative electrode-forming slurry), the content of the negative electrode active material in the slurry is preferably as high as possible within a range that allows the desired low viscosity to be achieved. For example, the content of the negative electrode active material in the slurry can be 50 to 80 mass%, more preferably 55 to 78 mass%, even more preferably 58 to 76 mass%, even more preferably 60 to 75 mass%, also preferably 62 to 74 mass%, and also preferably 63 to 73 mass%.
[0056] <Conductive Aid> The slurry of the present invention contains a conductive aid. There are no particular limitations on the conductive aid, and any commonly known conductive aid can be used. For example, the conductive aid may be an electron-conductive material such as graphites (e.g., natural graphite, artificial graphite, etc.), carbon blacks (e.g., acetylene black, ketjen black, furnace black, etc.), amorphous carbon (e.g., needle coke), carbon fibers (e.g., vapor-grown carbon fibers or carbon nanotubes), or carbonaceous materials (e.g., graphene or fullerene). Metal powders or metal fibers (e.g., copper, nickel, etc.) may also be used. Conductive polymers (e.g., polyaniline, polypyrrole, polythiophene, polyacetylene, polyphenylene derivatives) may also be used. When an electrode active material and a conductive aid are used in combination, those conductive aids that do not intercalate or deintercalate Li during charging and discharging the battery and do not function as an active material are considered conductive aids. Therefore, among conductive aids, those that can function as an active material in the active material layer during charging and discharging the battery are classified as active materials rather than conductive aids. Whether or not a conductive additive functions as an active material when a battery is charged and discharged is not uniquely determined, but is determined depending on the combination with the active material. One type of conductive additive may be used, or two or more types may be used.
[0057] The shape of the conductive additive is not particularly limited, but is preferably particulate. The average particle size (average particle size in equivalent sphere form) of the conductive additive is not particularly limited. For example, it is preferably 0.01 to 50 μm, more preferably 0.1 to 10 μm, and even more preferably 0.2 to 2.0 μm.
[0058] Whether the slurry of the present invention is a slurry for forming a positive electrode or a slurry for forming a negative electrode, the content of the conductive assistant in the solid content of the slurry of the present invention is preferably 0.05 to 5.00 mass%, more preferably 0.10 to 4.00 mass%, and even more preferably 0.20 to 3.00 mass%.
[0059] Whether the slurry of the present invention is a slurry for forming a positive electrode or a slurry for forming a negative electrode, the content of the conductive auxiliary agent in the slurry of the present invention can be, for example, 0.1 to 10 mass%, preferably 0.1 to 7 mass%, more preferably 0.2 to 5 mass%, even more preferably 0.4 to 3 mass%, and still more preferably 0.6 to 2 mass%.
[0060] <Non-aqueous Electrolyte> The non-aqueous electrolyte contained in the slurry of the present invention is composed of an electrolyte (electrolyte salt) and a non-aqueous solvent that dissolves the electrolyte.
[0061] (Electrolyte) As the electrolyte, any electrolyte that can be used as an electrolytic solution for a quasi-solid secondary battery can be used appropriately. The electrolyte is preferably a metal salt, such as lithium salt, potassium salt, sodium salt, calcium salt, or magnesium salt. As the lithium salt, lithium salts that are commonly used in electrolytes for lithium ion secondary batteries are preferred, such as the following lithium salts:
[0062] (L-1) Inorganic lithium salt: LiPF 6 , LiBF 4 , LiAsF 6 , LiSbF 6 Inorganic fluoride salts such as LiClO 4 , LiBrO 4 , LiIO 4 perhalogenates such as LiAlCl 4 Inorganic chloride salts, etc.
[0063] (L-2) Fluorine-containing organic lithium salt: LiCF 3 SO 3 perfluoroalkanesulfonates such as LiN(CF 3 SO 2 ) 2 , LiN(CF 3 CF 2 SO 2 ) 2 , LiN(FSO 2 ) 2 , LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 perfluoroalkanesulfonylimide salts such as LiC(CF3 SO 2 ) 3 perfluoroalkanesulfonylmethide salts such as Li[PF 5 (CF 2 CF 2 CF 3 ) )], Li[PF 4 (CF 2 CF 2 CF 3 ) 2 ], Li[PF 3 (CF 2 CF 2 CF 3 ) 3 ], Li[PF 5 (CF 2 CF 2 CF 2 CF 3 ) )], Li[PF 4 (CF 2 CF 2 CF 2 CF 3 ) 2 ], Li[PF 3 (CF 2 CF 2 CF 2 CF 3 ) 3 perfluoroalkyl fluorophosphates such as
[0064] (L-3) Oxalatoborate salts: lithium bis(oxalato)borate, lithium difluorooxalatoborate, etc.
[0065] Among these, LiPF 6 , LiBF 4 , LiAsF 6 , LiSbF 6 , LiClO 4 , Li(R f1 SO 3 ), LiN(R f1 SO 2 ) 2 , LiN(FSO 2 ) 2 , or LiN(R f1 SO 2 ) (R f2 SO 2 ) is preferred, and LiPF 6, LiBF 4 , LiN(R f1 SO 2 ) 2 , LiN(FSO 2 ) 2 , or LiN(R f1 SO 2 ) (R f2 SO 2 ) is more preferred, and LiPF 6 is particularly preferred. f1 and R f2 represents a perfluoroalkyl group, preferably having 1 to 6 carbon atoms.
[0066] The non-aqueous electrolyte may contain one electrolyte alone or two or more electrolytes in any combination.
[0067] In the slurry of the present invention, the electrolyte concentration in the nonaqueous electrolyte is not particularly limited as long as it functions as a nonaqueous electrolyte. For example, it can be 10.0 to 50.0 mass %, preferably 15.0 to 30.0 mass %. The molar concentration is preferably 0.5 to 1.5 M.
[0068] (Non-aqueous Solvent) The non-aqueous solvent serving as the medium for the non-aqueous electrolyte solution is preferably an aprotic organic solvent, and more preferably an aprotic organic solvent having 2 to 10 carbon atoms. Examples of such non-aqueous solvents include linear or cyclic carbonate compounds, lactone compounds, linear or cyclic ether compounds, ester compounds, nitrile compounds, amide compounds, oxazolidinone compounds, nitro compounds, linear or cyclic sulfone or sulfoxide compounds, and phosphate ester compounds. Among these, compounds having an ether bond, carbonyl bond, ester bond, or carbonate bond are preferred. These compounds may have a substituent.
[0069] Examples of non-aqueous solvents include ethylene carbonate, fluorinated ethylene carbonate, vinylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, γ-butyrolactone, γ-valerolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dioxane, 1,4-dioxane, and methyl acetate. , ethyl acetate, methyl propionate, ethyl propionate, methyl butyrate, methyl isobutyrate, methyl trimethylacetate, ethyl trimethylacetate, acetonitrile, glutaronitrile, adiponitrile, methoxyacetonitrile, 3-methoxypropionitrile, N,N-dimethylformamide, N-methylpyrrolidone (NMP), N-methyloxazolidinone, N,N'-dimethylimidazolidinone, nitromethane, nitroethane, sulfolane, trimethyl phosphate, dimethyl sulfoxide, dimethyl sulfoxide phosphate, etc. These may be used alone or in combination of two or more. Among these, at least one selected from the group consisting of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and γ-butyrolactone is preferred, and a combination of a high-viscosity (high-dielectric constant) solvent (e.g., relative dielectric constant ε≧30) such as ethylene carbonate or propylene carbonate with a low-viscosity solvent (e.g., viscosity≦1 mPa s) such as dimethyl carbonate, ethyl methyl carbonate, or diethyl carbonate is more preferred. Using a mixed solvent with such a combination improves the dissociation properties of the electrolyte and the mobility of ions. A particularly preferred nonaqueous solvent is a combination of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate.
[0070] The content of the nonaqueous electrolyte in the slurry of the present invention is preferably 8 to 38% by mass, more preferably 10 to 33% by mass, even more preferably 12 to 28% by mass, and even more preferably 13 to 26% by mass, preferably 14 to 25% by mass, even more preferably 16 to 25% by mass, even more preferably 18 to 25% by mass, and even more preferably 20 to 25% by mass. In the case of a slurry for forming a negative electrode, the content is preferably 18 to 48% by mass, more preferably 20 to 43% by mass, even more preferably 22 to 40% by mass, even more preferably 23 to 38% by mass, even more preferably 24 to 36% by mass, and even more preferably 25 to 35% by mass.
[0071] <Other Components> The slurry of the present invention may optionally contain an ionic liquid, a thickener, an antifoaming agent, a leveling agent, a dehydrating agent, an antioxidant, etc. These may be those typically used in non-aqueous electrolyte secondary batteries. When the slurry of the present invention contains other components, the amount of the other components is preferably 0.05 to 1.5 parts by mass, more preferably 0.1 to 1.0 parts by mass, per 100 parts by mass of the total content of the electrode active material and the conductive aid.
[0072] The slurry of the present invention can be obtained by uniformly mixing the components constituting the slurry. For example, a non-aqueous solvent, an electrolyte, and a polymer are mixed to obtain a solution in which the non-aqueous electrolyte and the polymer are compatible, and this solution is then mixed with an electrode active material and a conductive additive to obtain a slurry in which the electrode active material and the conductive additive are dispersed in the solution. The mixing method is not particularly limited, and any method commonly used in this technical field can be appropriately adopted.
[0073] [Non-aqueous electrolyte secondary battery] The non-aqueous electrolyte secondary battery of the present invention (hereinafter also referred to as "secondary battery of the present invention") is a non-aqueous electrolyte secondary battery having an electrode active material layer composed of the slurry of the present invention. That is, it is a so-called quasi-solid secondary battery in which at least one of the positive electrode active material layer and the negative electrode active material layer is composed of the slurry of the present invention. The secondary battery of the present invention usually has a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector in this order, and at least one of the positive electrode active material layer and the negative electrode active material layer is composed of the slurry of the present invention. In the non-aqueous electrolyte secondary battery of the present invention, it is preferable that both the positive electrode active material layer and the negative electrode active material layer are composed of the slurry of the present invention.
[0074] Prior to describing the secondary battery of the present invention, the structure of a general nonaqueous electrolyte secondary battery will be described. FIG. 1 is a cross-sectional view showing a schematic representation of the laminated structure of a general nonaqueous electrolyte secondary battery 10, including the working electrode when the battery is operated. The nonaqueous electrolyte secondary battery 10 has a laminated structure (hereinafter also referred to as an electrode laminate) including, as viewed from the negative electrode side, a negative electrode current collector 1, a negative electrode active material layer 2, a separator 3, a positive electrode active material layer 4, and a positive electrode current collector 5, in this order. The negative electrode active material layer 2 and the positive electrode active material layer 4 are filled with a nonaqueous electrolyte (not shown) and separated by the separator 3. The separator 3 has pores, and during normal battery use, functions as a separator between the positive and negative electrodes, insulating them by allowing the electrolyte and ions to pass through the pores. With this structure, for example, in the case of a lithium-ion secondary battery, electrons (e - ) is supplied, and at the same time, lithium ions (Li + ) moves and accumulates in the negative electrode. On the other hand, during discharge, the lithium ions (Li + ) is returned to the positive electrode side through the electrolyte, and electrons are supplied to the operating part 6. In the illustrated example, a light bulb is used as the operating part 6, and it is lit by discharge.
[0075] Next, the basic structure characteristic of quasi-solid secondary batteries will be described. As described above, in quasi-solid secondary batteries, the electrode active material layer is formed in a slurry state containing an electrode active material and an electrolyte. Therefore, the electrode active material layer is a layer using a slurry (suspension, dispersion) in which the electrode active material is dispersed in a non-aqueous electrolyte, which distinguishes the structure from a typical non-aqueous electrolyte secondary battery. That is, in a typical non-aqueous electrolyte secondary battery, a coating solution is prepared by dispersing the electrode active material in a medium that does not contain an electrolyte, and the coating solution is applied to a current collector to form a coating film. The coating film is then dried to form a thin-film electrode active material layer. This coating solution usually contains a binder, which firmly binds the electrode active material particles together to form a hard electrode active material layer. Since the non-aqueous electrolyte is present on the electrode active material layer thus formed (between the negative electrode active material layer and the positive electrode active material layer), even if there are portions in the electrode active material layer that can be penetrated by the non-aqueous electrolyte, the electrode active material layer is in the form of a hard solid particle layer overall, not a slurry layer. In contrast, in a quasi-solid secondary battery, the electrode active material layer is an electrode slurry layer formed by dispersing solid particles containing an electrode active material and a conductive additive in a non-aqueous electrolyte solution obtained by dissolving an electrolyte such as a lithium salt in a non-aqueous solvent. For this electrode slurry layer to function as an electrode active material layer, strong binding between the electrode active material particles is not required, and therefore the electrode slurry layer usually does not contain a binder. Except for the fact that the electrode active material layer is an electrode slurry layer and that the electrode slurry layer is in contact with the separator, the basic layer configuration of a quasi-solid secondary battery is the same as the layer configuration shown in FIG.
[0076] In the secondary battery of the present invention, at least one of the positive electrode active material layer and the negative electrode active material layer is a slurry layer formed from the slurry of the present invention. In the secondary battery of the present invention, it is preferable that both the positive electrode active material layer and the negative electrode active material layer are slurry layers formed from the slurry of the present invention.
[0077] In the secondary battery of the present invention, the materials and components such as the positive electrode current collector, the negative electrode current collector, and the separator are not particularly limited, except that the slurry of the present invention is used to form at least one of the electrode active material layers of the positive electrode active material layer and the negative electrode active material layer. These materials and components can be appropriately applied from those used in ordinary secondary batteries. For the components and manufacturing methods typically used in these secondary batteries, reference can be made to, for example, JP 2016-201308 A, JP 2005-108835 A, JP 2012-185938 A, WO 2018 / 135395, and the like.
[0078] In the secondary battery of the present invention, the thickness of the electrode active material layer (slurry layer) is not particularly limited and can be, for example, 5 to 500 μm, preferably 20 to 400 μm, more preferably 40 to 400 μm, and even more preferably 80 to 350 μm.
[0079] [Method for Manufacturing a Non-Aqueous Electrolyte Secondary Battery] The method for manufacturing a non-aqueous electrolyte secondary battery of the present invention includes forming an electrode active material layer using the slurry of the present invention. Typically, the method involves applying the slurry of the present invention to an electrode current collector to form a slurry-like electrode active material layer. If the electrode is a positive electrode, a positive electrode-forming slurry containing a positive electrode active material as the slurry of the present invention is applied to the positive electrode current collector. If the electrode is a negative electrode, a negative electrode-forming slurry containing a negative electrode active material as the slurry of the present invention is applied to the negative electrode current collector. The method for applying the slurry is not particularly limited, and can be, for example, application using a roll coater, drop coating, applying the slurry evenly on the current collector and then pressing (roll press or flat press), or applying the slurry by placing it within a frame of a specified thickness and spreading it. Conventional methods can also be used for manufacturing a non-aqueous electrolyte secondary battery of the present invention, except that the electrode active material layer is formed using the slurry of the present invention. For example, Japanese Patent Application Laid-Open No. 2016-201308, Japanese Patent Application Laid-Open No. 2005-108835, Japanese Patent Application Laid-Open No. 2012-185938, Japanese Patent Application Laid-Open No. 2017-147222, etc. can be referenced as appropriate.
[0080] The nonaqueous electrolyte secondary battery of the present invention can be installed in electronic devices such as notebook computers, pen-input personal computers, mobile personal computers, electronic book players, mobile phones, cordless phone handsets, pagers, handheld terminals, portable fax machines, portable copiers, portable printers, headphone stereos, video camcorders, LCD televisions, handheld vacuum cleaners, portable CD players, mini-discs, electric shavers, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power supplies, and memory cards. It can also be installed in consumer electronic devices such as automobiles, electric vehicles, motors, lighting fixtures, toys, game devices, road conditioners, clocks, flash devices, cameras, and medical devices (pacemakers, hearing aids, shoulder massagers, etc.). It can also be used for various military and space applications. It can also be combined with solar cells.
[0081] The present invention will be described in more detail below with reference to examples, but the present invention should not be construed as being limited thereto.
[0082] [Preparation of Dispersant] <Preparation of Polymer 1> Polymer 1 was prepared using the monomer blend amounts (parts by mass) shown in Table 1 below. Details are described below. 18 g of methoxypolyethylene glycol monomethacrylate (MPEGM), 2 g of butyl methacrylate (MBu), 3.5 g of azobisisobutyronitrile, and 40 g of methyl ethyl ketone were mixed at room temperature to prepare Solution A. 100 g of methyl ethyl ketone was added to a three-neck flask equipped with a stirrer, thermometer, reflux condenser, thermostat, and dropping pump while purging with nitrogen, and the temperature was raised to 85°C with stirring. Solution A was added dropwise to this three-neck flask at a constant rate over 1 hour using the dropping pump. After the dropwise addition was completed, the mixture was stirred at the same temperature, and the reaction was terminated after 5 hours. After the reaction was completed, the solution was concentrated to remove the methyl ethyl ketone, thereby obtaining Polymer 1. The Mw of the obtained Polymer 1 was approximately 4000. Polymer 1 corresponds to n=10 in the constituent component represented by general formula (1) (constituent component derived from MPEGM).
[0083] <Preparation of Polymers 2 to 4, 5a, 5e, 5f, 5h, and 6 to 17> Polymers 2 to 4, 5a, 5e, 5f, 5h, and 6 to 17 were prepared in the same manner as for polymer 1, except that in the preparation of polymer 1, the types and amounts of monomers used were as shown in Table 1 below. Polymers 5e, 5f, and 5h were prepared by changing n in the constituent component represented by general formula (1) (constituent component derived from MPEGM) in polymer 5a to 3, 30, and 50, respectively, as shown in Table 2 below.
[0084] <Preparation of Polymers 5b, 5c, 5d, and 5g> Polymers 5b, 5c, 5d, and 5g were prepared in the same manner as in the preparation of Polymer 5a, except that the amount of azobisisobutyronitrile added was changed so that the resulting polymers had Mw values shown in Table 2 below.
[0085] <Preparation of Polymer 18> Polyvinylpyrrolidone (referred to as PVP, manufactured by Sigma-Aldrich, trade name: PVP10) was used as polymer 18.
[0086] <Preparation of Polymer 19> Polyvinyl alcohol (referred to as PVA, manufactured by Sigma-Aldrich, saponification degree 80%) was used as polymer 19.
[0087]
[0088] The names and structures of the monomers abbreviated in Table 1 above are shown below: MPEGM: methoxypolyethylene glycol monomethacrylate MPPGM: methoxypolypropylene glycol monomethacrylate MPEGA: methoxypolyethylene glycol monoacrylate MBu: butyl methacrylate MPe: pentyl methacrylate MSt: stearyl methacrylate MDc: docosyl methacrylate MBn: benzyl methacrylate MNpM: (2-naphthyl)methyl methacrylate ABn: benzyl acrylate NVF: N-vinylformamide NVP: N-vinylpyrrolidone TBMA: N-t-butylmethacrylamide NVC: N-vinylcarbazole
[0089]
[0090] [Preparation of Slurry for Electrode Formation] <Preparation of Non-Aqueous Electrolyte> Ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 3:4:3 to prepare a non-aqueous solvent. 6 and each of the polymers prepared above to obtain a non-aqueous electrolyte corresponding to each polymer type. 6 The concentration of the solvent was 1 M (mol / liter), and the polymer concentration was 1% by mass.
[0091] <Preparation of Slurry for Positive Electrode Formation> LiFePO was used as the positive electrode active material. 4 The polymers were uniformly mixed using a centrifugal planetary mixer (manufactured by Thinky Corporation, product name: Awatori Rentaro) so that the polymer content was 74% by mass of the polymer (manufactured by Gelon), 1.5% by mass of acetylene black (manufactured by Denka Company, Ltd.) as a conductive additive, and 24.5% by mass of the nonaqueous electrolyte solution, thereby obtaining a slurry for forming a positive electrode corresponding to each polymer type.
[0092] <Preparation of Slurry for Forming Negative Electrode> 64 mass % of artificial graphite (UF-G30 manufactured by Showa Denko K.K.) as the negative electrode active material, 1 mass % of acetylene black (Denka Black manufactured by Denka Co., Ltd.) as the conductive additive, and 35 mass % of the above nonaqueous electrolyte were uniformly mixed using a centrifugal planetary mixer (manufactured by Thinky Corporation, product name: Awatori Rentaro) to obtain a slurry for forming a negative electrode corresponding to each polymer type.
[0093] [Fabrication of Nonaqueous Electrolyte Secondary Battery (Quasi-Solid Secondary Battery)] The positive electrode-forming slurry was applied to an 8 cm long, 5 cm wide aluminum current collector, and the negative electrode-forming slurry was applied to an 8 cm long, 5 cm wide copper current collector, each to a thickness of 300 μm. In this way, a positive electrode having a positive electrode active material layer (slurry layer) on the positive electrode current collector and a negative electrode having a negative electrode active material layer (slurry layer) on the negative electrode current collector were fabricated. A separator was then placed on the negative electrode active material layer of the negative electrode, and the positive electrode was placed on the separator so that the positive electrode active material layer was in contact with the separator. An aluminum tab was attached to the end of the aluminum current collector, and a nickel tab was attached to the end of the copper current collector by ultrasonic welding to form an electrode assembly. This electrode assembly was sandwiched between two aluminum laminate films, and three sides were heat-sealed and the remaining side was vacuum-sealed to fabricate a laminated battery. In this way, quasi-solid secondary batteries corresponding to each polymer type were obtained.
[0094] [Battery Performance Evaluation] This laminated battery was initialized by charging under the following charging conditions and then discharging under the following discharging conditions. Next, the battery was charged to 50% SOC (State of charge) under the following charging conditions, and the DC resistance value was measured. The obtained value was taken as the battery resistance. (Charging conditions) CC-CV charging: current value 10 mA, upper limit voltage 3.6 V, end current value 0.5 mA (Discharging conditions) CC discharging: current value 10 mA, upper limit voltage 2.0 V The obtained resistance value was applied to the following evaluation criteria to evaluate the battery performance. The lower the resistance, the better the battery performance can be evaluated. The results are shown in Table 2 below. - Evaluation criteria - A: 30 Ω cm 2 Less than B: 30 Ω cm 2 More than 40 Ωcm 2 Less than C: 40 Ω cm 2 End
[0095] [Flowability Test of Electrode-Forming Slurry] As described in the above section [Fabrication of Non-Aqueous Electrolyte Secondary Battery (Quasi-Solid Secondary Battery)], a positive electrode having a positive electrode active material layer (slurry layer, 300 μm) on a positive electrode current collector was obtained. This positive electrode was sandwiched between stainless steel (SUS) plates and subjected to a flow rate of 0.4 ton / cm. 2The film thickness change rate when pressed for 30 seconds at a pressure of 100 psi was calculated according to the following formula: Film Thickness Change Rate (%) = 100 - {(Film Thickness After Pressing) / (Film Thickness Before Pressing)} × 100 The obtained film thickness change rate was applied to the following evaluation criteria to evaluate the fluidity of the positive electrode-forming slurry. A higher film thickness change rate indicates higher fluidity. Higher fluidity improves the uniformity and reproducibility of the coated film. The results are shown in Table 2 below. A: 50% or more B: 30% or more but less than 50% C: 15% or more but less than 30% D: Less than 15% As described in the above section [Fabrication of Nonaqueous Electrolyte Secondary Battery (Quasi-Solid State Secondary Battery)], a negative electrode having a negative electrode active material layer (slurry layer, 300 μm) on a negative electrode current collector was obtained. This negative electrode was sandwiched between stainless steel (SUS) plates and pressed at a pressure of 0.4 ton (ton) / cm. 2 The film thickness change rate when the negative electrode slurry was pressed for 30 seconds at a pressure of 1000 kJ / cm2 was calculated in the same manner as above. The obtained film thickness change rate was applied to the above evaluation criteria to evaluate the fluidity of the negative electrode-forming slurry. The results are shown in Table 2 below.
[0096]
[0097] As shown in the table above, Comparative Example 1, in which no dispersant was added, resulted in poor slurry fluidity. Furthermore, the battery of Comparative Example 1 had a resistance of 30 Ωcm even without the addition of a polymer (insulating material). 2 The results were as above. Comparative Examples 2, 3, and 5, in which the polymer constituting the dispersant contained the constituent component represented by formula (1) but did not contain any of the constituent components represented by formulas (2) and (3), resulted in poor slurry fluidity. Furthermore, the battery resistance of these comparative examples was 40 Ω cm 2 The same result was obtained for Comparative Example 7, in which the polymer constituting the dispersant did not contain the component represented by formula (1). Even though the structure of the components contained in the polymer constituting the dispersant satisfied the requirements of the present invention, Comparative Example 4, in which the content ratio of the components did not satisfy the requirements of the present invention, resulted in poor slurry fluidity. Furthermore, the battery resistance of these Comparative Examples was 40 Ω cm 2The structure and content ratio of the constituent components of the polymer constituting the dispersant satisfied the requirements of the present invention, but Comparative Example 6, in which the Mw did not satisfy the requirements of the present invention, resulted in poor slurry fluidity. Furthermore, the battery resistance of these Comparative Examples was 40 Ω cm 2 The resistance increased to above 100%. In Comparative Example 8, in which the polymer constituting the dispersant was PVP containing none of the components represented by formulas (1), (2), and (3), the polymer did not dissolve in the electrolyte solution and did not function as a dispersant in the electrode-forming slurry envisioned by the present invention. In Comparative Example 9, in which the polymer constituting the dispersant was PVA, the polymer dissolved in the electrolyte solution, but the fluidity of the slurry was poor. In addition, the battery resistance of this comparative example was 40 Ω cm 2 In contrast, Examples 1 to 18, in which the polymer constituting the dispersant satisfied the requirements of the present invention, all had excellent slurry fluidity and, despite containing a polymer (insulating material), had battery resistance values equivalent to or lower than that of Comparative Example 1, which did not contain such a polymer. The above results demonstrate that the dispersant specified in the present invention has excellent properties as a dispersant for electrode-forming slurries in quasi-solid secondary batteries.
[0098] While the present invention has been described in connection with embodiments thereof, we do not intend to limit our invention to any of the details of the description unless otherwise specified, and believe that the claims should be construed broadly without departing from the spirit and scope of the invention as set forth in the appended claims.
[0099] This application claims priority based on Japanese Patent Application No. 2023-074129, filed in Japan on April 28, 2023, the contents of which are incorporated herein by reference as part of the present specification.
[0100] REFERENCE SIGNS LIST 10 Non-aqueous electrolyte secondary battery 1 Negative electrode current collector 2 Negative electrode active material layer 3 Separator 4 Positive electrode active material layer 5 Positive electrode current collector 6 Operating part (light bulb)
Claims
1. A slurry for forming an electrode, comprising an electrode active material, a conductive assistant, a non-aqueous electrolyte, and a dispersant, the dispersant being made of a polymer having a weight average molecular weight of 1,000 to 15,000, containing 80 to 99% by mass of a component represented by the following formula (1) and 1 to 20% by mass in total of a component represented by the following formula (2) or (3): In the above formula, * indicates a linking site. 1 R represents a hydrocarbon group having 1 to 8 carbon atoms. 2 ~R 6 represents a hydrogen atom or methyl. 7 R represents a hydrocarbon group having 5 to 18 carbon atoms. 8 represents a group having 1 to 12 carbon atoms and a nitrogen atom, and n is a number from 3 to 30.
2. The electrode-forming slurry according to claim 1, wherein the electrode active material is a positive electrode active material, and the content of the positive electrode active material in the electrode-forming slurry is 60 to 90 mass %.
3. The electrode-forming slurry according to claim 1, wherein the electrode active material is a negative electrode active material, and the content of the negative electrode active material in the electrode-forming slurry is 50 to 80 mass %.
4. The electrode-forming slurry according to claim 2 or 3, wherein the content of the dispersant is 0.1 to 5.0 parts by mass per 100 parts by mass of the total of the nonaqueous electrolyte and the dispersant.
5. A non-aqueous electrolyte secondary battery having an electrode active material layer formed from the electrode forming slurry according to claim 4.
6. A method for producing a non-aqueous electrolyte secondary battery, comprising forming an electrode active material layer from the electrode forming slurry according to claim 4.
7. A dispersant comprising the following polymer for use in an electrode-forming slurry containing an electrode active material, a conductive assistant, and a non-aqueous electrolyte: <Polymer> A polymer containing 80 to 99 mass % of a component represented by the following formula (1) and 1 to 20 mass % in total of a component represented by the following formula (2) or (3), and having a weight average molecular weight of 1,000 to 15,000. In the above formula, * indicates a linking site. 1 R represents a hydrocarbon group having 1 to 8 carbon atoms. 2 ~R 6 represents a hydrogen atom or methyl. 7 R represents a hydrocarbon group having 5 to 18 carbon atoms. 8 represents a group having 1 to 12 carbon atoms and a nitrogen atom, and n is a number from 3 to 30.
Citation Information
Patent Citations
Rechargeable lithium-ion secondary battery
JP2005108835A
Nonaqueous secondary battery
JP2012185938A
Nonaqueous electrolyte and nonaqueous secondary battery
JP2016201308A
Lithium-ion battery
JP2017147222A
Nonaqueous electrolyte power storage element
JP2022139794A