Rolled lead alloy foil, electrode for lead acid battery, and lead acid battery

The development of a rolled lead alloy foil with specific compositions and a mixed grain structure addresses the corrosion issues in lead-acid batteries, enhancing corrosion resistance and battery durability through improved manufacturing processes.

WO2024225273A1PCT designated stage expired Publication Date: 2024-10-31FURUKAWA ELECTRIC CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015926
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-23
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Rolled lead alloy foils used in lead-acid batteries suffer from insufficient corrosion resistance, leading to early deterioration and reduced mass, which affects the battery's performance and lifespan.

Method used

A rolled lead alloy foil with specific compositions of calcium, tin, and bismuth, along with a mixed grain state of rolled and recrystallized grains, is developed to enhance corrosion resistance. The foil is manufactured through a combination of rolling and heat treatment processes to achieve a low Kernel Average Misorientation (KAM) value and small crystal grain size, ensuring excellent corrosion resistance and uniform corrosion patterns.

Benefits of technology

The solution significantly improves the corrosion resistance of the lead alloy foil, reducing the likelihood of premature battery deterioration and maintaining battery performance by preventing penetrating corrosion, thus extending the battery's lifespan and reducing internal resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000024_0000
    Figure 00000024_0000
  • Figure 00000024_0001
    Figure 00000024_0001
Patent Text Reader

Abstract

Provided is a rolled lead alloy foil having excellent corrosion resistance. The rolled lead alloy foil is formed of a lead alloy containing 0.005 mass% to 0.1 mass% of calcium, 0.5 mass% to 2.0 mass% of tin, and at most 0.005 mass% of bismuth, with the balance consisting of lead and unavoidable impurities. When a plurality of measurement regions defined in a mesh shape are set on the cross section of the rolled lead alloy foil obtained by cutting the rolled lead alloy foil along a plane which is parallel to the rolling direction of the rolled lead alloy foil and which is perpendicular to the surface of the rolled lead alloy foil, and a local orientation difference of each measurement region is measured, the proportion of a measurement region, in which the local orientation difference is less than 1 degree, among all the measurement regions is at least 50 area%.
Need to check novelty before this filing date? Find Prior Art

Description

Rolled lead alloy foil, lead-acid battery electrode, and lead-acid battery

[0001] The present invention relates to a rolled lead alloy foil, an electrode for a lead-acid battery, and a lead-acid battery.

[0002] An electrode of a lead-acid battery includes an electrode lead layer made of a lead alloy foil and an active material disposed on the surface of the electrode lead layer. As the lead alloy foil, for example, a rolled lead alloy foil manufactured by rolling a lead alloy has been used (see, for example, Patent Documents 1 and 2).

[0003] International Publication No. WO 2016 / 110907 International Publication No. WO 2015 / 145800

[0004] Corrosion resistance has been required for rolled lead alloy foils used in electrodes of lead-acid batteries. If the corrosion resistance of rolled lead alloy foil is insufficient, the rolled lead alloy foil corrodes, reducing the mass of the lead alloy and causing early deterioration of the lead-acid battery. Therefore, further improvement in corrosion resistance has been required for rolled lead alloy foil. An object of the present invention is to provide a rolled lead alloy foil having excellent corrosion resistance. Another object of the present invention is to provide a lead-acid battery electrode and a lead-acid battery that are resistant to deterioration.

[0005] The rolled lead alloy foil according to one embodiment of the present invention is a rolled lead alloy foil formed of a lead alloy containing 0.005% by mass or more and 0.1% by mass or less of calcium, 0.5% by mass or more and 2.0% by mass or less of tin, and 0.005% by mass or less of bismuth, with the remainder being lead and unavoidable impurities, and wherein a plurality of measurement regions defined in a mesh pattern are set on a cross section of the rolled lead alloy foil that appears when the rolled lead alloy foil is cut along a plane that is parallel to the rolling direction of the rolled lead alloy foil and perpendicular to the surface of the rolled lead alloy foil, and when the local misorientation of each measurement region is measured, the proportion of the measurement regions with a local misorientation of less than 1 degree among all the measurement regions is 50% by area or more.

[0006] Another aspect of the present invention provides a rolled lead alloy foil formed of a lead alloy containing 0.005% by mass or more and 0.1% by mass or less of calcium, 0.5% by mass or more and 2.0% by mass or less of tin, 0.005% by mass or less of bismuth, and 0.1% by mass or less of silver, with the remainder being lead and unavoidable impurities, wherein a plurality of measurement areas defined in a mesh pattern are set on a cross section of the rolled lead alloy foil that appears when the rolled lead alloy foil is cut along a plane that is parallel to the rolling direction of the rolled lead alloy foil and perpendicular to the surface of the rolled lead alloy foil, and when the local misorientation of each measurement area is measured, the proportion of the measurement areas in which the local misorientation is less than 1 degree is 50% by area or more of all the measurement areas.

[0007] Furthermore, a lead-acid battery electrode according to yet another aspect of the present invention comprises an electrode lead layer made of the rolled lead alloy foil according to the above-mentioned aspect or the rolled lead alloy foil according to the above-mentioned other aspect, and an active material disposed on the surface of the electrode lead layer. Furthermore, a lead-acid battery according to yet another aspect of the present invention comprises the lead-acid battery electrode according to the above-mentioned other aspect.

[0008] The rolled lead alloy foil according to the present invention has excellent corrosion resistance, and the lead-acid battery electrode and the lead-acid battery according to the present invention are resistant to deterioration.

[0009] Fig. 1 is a cross-sectional view illustrating the structure of a bipolar lead-acid battery which is one embodiment of the lead-acid battery according to the present invention. Fig. 2 is a diagram illustrating a method for evaluating the corrosion resistance of rolled lead alloy foil. Fig. 3 is a graph showing the relationship between the proportion of measurement areas where the KAM value is less than 1 degree and the corrosion rate of rolled lead alloy foil. Fig. 4 is a graph showing the relationship between the proportion of crystal grains with a grain size of less than 20 µm and the uniformity of corrosion. Fig. 5 is a diagram illustrating a method for measuring the KAM value. Fig. 6 is a diagram illustrating a method for calculating the KAM value of a measurement area.

[0010] An embodiment of the present invention will be described. Note that the embodiment described below is merely an example of the present invention. Furthermore, various modifications and improvements can be made to this embodiment, and such modifications and improvements can also be included in the present invention.

[0011] The structure of a lead-acid battery 1 according to one embodiment of the present invention will be described with reference to FIG. 1 . The lead-acid battery 1 shown in FIG. 1 is a bipolar lead-acid battery and includes a first plate unit in which a negative electrode 110 is fixed to a flat first plate 11; a second plate unit in which an electrolytic layer 105 is fixed to the inside of a frame-shaped second plate 12; a third plate unit in which a bipolar electrode 130, formed by a substrate 111 having a positive electrode 120 formed on one side and a negative electrode 110 formed on the other side, is fixed to the inside of a frame-shaped third plate 13; and a fourth plate unit in which the positive electrode 120 is fixed to a flat fourth plate 14. The second plate units and third plate units are alternately stacked between the first plate unit and the fourth plate unit to form the lead-acid battery 1 having a substantially rectangular parallelepiped shape. The number of second plate units and third plate units stacked is set so that the storage capacity of the lead-acid battery 1 is a desired value.

[0012] The first to fourth plates 11, 12, 13, and 14 and the substrate 111 are formed, for example, from a known molding resin. The first to fourth plates 11, 12, 13, and 14 are fixed to each other by an appropriate method so as to seal the interior and prevent leakage of the electrolyte. A negative electrode terminal 107 is fixed to the first plate 11, and the negative electrode 110 fixed to the first plate 11 is electrically connected to the negative electrode terminal 107. A positive electrode terminal 108 is fixed to the fourth plate 14, and the positive electrode 120 fixed to the fourth plate 14 is electrically connected to the positive electrode terminal 108. The electrolytic layer 105 is formed, for example, from a glass fiber mat impregnated with an electrolyte containing sulfuric acid.

[0013] The negative electrode 110 includes a negative electrode lead layer 102 made of, for example, well-known lead foil, and a negative electrode active material layer 104 disposed on the surface of the negative electrode lead layer 102. The positive electrode 120 includes a positive electrode lead layer 101 (corresponding to the "electrode lead layer" which is a constituent element of the present invention) made of rolled lead alloy foil according to the present embodiment described below, and a positive electrode active material layer 103 disposed on the surface of the positive electrode lead layer 101. The positive electrode 120 and the negative electrode 110 are fixed to the front and back surfaces of a substrate 111, respectively, and electrically connected by an appropriate method. Alternatively, the positive electrode 120 and the negative electrode 110 may be fixed to one surface of two substrates 111, and the other surfaces may be electrically connected and fixed together.

[0014] In the lead-acid battery 1 according to this embodiment having such a configuration, the substrate 111, the positive electrode lead layer 101, the positive electrode active material layer 103, the negative electrode lead layer 102, and the negative electrode active material layer 104 constitute a bipolar electrode 130, which is an electrode for a lead-acid battery. A bipolar electrode is an electrode that functions as both a positive electrode and a negative electrode in one sheet. The lead-acid battery 1 according to this embodiment has a battery configuration in which the cell members are connected in series by alternately stacking and assembling a plurality of cell members, each of which includes a positive electrode 120 having a positive electrode active material layer 103 and a negative electrode 110 having a negative electrode active material layer 104, with an electrolytic layer 105 interposed between them. In this embodiment, a bipolar lead-acid battery having a bipolar electrode that functions as both a positive electrode and a negative electrode is shown as an example of a lead-acid battery, but the lead-acid battery according to this embodiment may also be a lead-acid battery that has an electrode that functions as a positive electrode and an electrode that functions as a negative electrode, and in which the separate positive and negative electrodes are arranged alternately.

[0015] <Regarding the Rolled Lead Alloy Foil Constituting the Positive Electrode Lead Layer 101> Next, the rolled lead alloy foil constituting the positive electrode lead layer 101 will be described. The rolled lead alloy foil according to this embodiment is a foil produced by rolling a lead alloy, and the lead alloy contains 0.005% by mass to 0.1% by mass of calcium (Ca), 0.5% by mass to 2.0% by mass of tin (Sn), and 0.005% by mass or less of bismuth, with the balance consisting of lead (Pb) and unavoidable impurities (hereinafter sometimes referred to as a "first lead alloy"). This lead alloy may also be a lead alloy (hereinafter sometimes referred to as a "second lead alloy") containing 0.005% by mass to 0.1% by mass of calcium, 0.5% by mass to 2.0% by mass of tin, 0.005% by mass or less of bismuth, and 0.1% by mass or less of silver, with the balance consisting of lead and unavoidable impurities.

[0016] Furthermore, this rolled lead alloy foil is a foil in which, when a cross section of the rolled lead alloy foil is cut along a plane parallel to the rolling direction of the rolled lead alloy foil and perpendicular to the surface of the rolled lead alloy foil, a plurality of measurement areas defined in a mesh pattern are set and the local misorientation of each measurement area is measured, the proportion of measurement areas in which the local misorientation is less than 1 degree is 50 area % or more of all measurement areas.In this specification, "local misorientation" is sometimes referred to as "KAM value."KAM is an abbreviation for Kernel Average Misorientation.

[0017] In the rolled lead alloy foil according to this embodiment, the proportion of measurement regions with a KAM value of less than 1 degree is 50 area % or more of all measurement regions, i.e., there are many low-strain regions and few high-strain regions in the rolled lead alloy foil, so there is little residual strain in the rolled lead alloy foil. Therefore, this rolled lead alloy foil has excellent corrosion resistance. High-strain regions with a KAM value of 1 degree or more have accumulated lattice strain, so their internal elastic strain energy is high and they are prone to corrosion, while low-strain regions with a KAM value of less than 1 degree have low internal elastic strain energy and are therefore resistant to corrosion. An example of a method for producing the rolled lead alloy foil according to this embodiment will be described in detail later.

[0018] Therefore, if a lead-acid battery electrode is constructed using the rolled lead alloy foil according to this embodiment, which satisfies the above-mentioned conditions for the KAM value, as the electrode lead layer, the lead layer has excellent corrosion resistance, and therefore the lead-acid battery electrode is less likely to deteriorate. Furthermore, lead-acid batteries, such as bipolar lead-acid batteries, equipped with this lead-acid battery electrode are also less likely to deteriorate. The KAM value can be measured by any method, including, for example, crystal orientation measurement using electron backscatter diffraction. That is, the rolled lead alloy foil according to this embodiment is cut to expose a cross section parallel to the rolling direction of the rolled lead alloy foil and perpendicular to the surface of the rolled lead alloy foil. The KAM value can then be obtained by analyzing the cross section using electron backscatter diffraction.

[0019] In this embodiment, a plurality of measurement regions defined in a mesh pattern are set on the cross section, the KAM value of each measurement region is measured, and the proportion of the area of ​​all measurement regions having a KAM value of less than 1 degree is calculated. The shape of the measurement regions is not particularly limited, and examples thereof include triangles such as equilateral triangles, quadrilaterals such as squares, rectangles, parallelograms, and rhombuses, hexagons such as regular hexagons, and circles such as perfect circles and ellipses. The proportion of all measurement regions having a local misorientation of less than 1 degree must be 50 area% or more, preferably 75 area% or more, more preferably 85 area% or more, and most preferably 100 area%. Furthermore, to improve the corrosion resistance of the rolled lead alloy foil, the proportion of all measurement regions having a local misorientation of less than 5 degrees is preferably 94 area% or more, more preferably 98 area% or more.

[0020] The rolled lead alloy foil according to this embodiment has rolled grains, which are crystal grains formed by rolling. Furthermore, in addition to the rolled grains, the foil may also have recrystallized grains, which are crystal grains formed by heat treatment (i.e., a mixed grain state having both rolled grains and recrystallized grains). In the rolled lead alloy foil according to this embodiment, the grain size is preferably sufficiently small to prevent corrosion from penetrating the thickness of the rolled lead alloy foil. Here, the grain size of the rolled grains is less than 1 μm, which is much smaller than the recrystallized grains, which have a grain size of several μm or more. Therefore, in order to ensure that the grain size of the rolled lead alloy foil is sufficiently small, the grain size of the recrystallized grains is preferably sufficiently small. Specifically, when the diameter (grain size) of the crystal grains observed in the cross section is measured, the proportion of the crystal grains having a grain size of less than 20 μm among all the crystal grains is preferably 95 area % or more. This proportion can be calculated by dividing the total area of ​​the crystal grains having a grain size of less than 20 μm in the cross section by the total area of ​​all the crystal grains in the cross section.

[0021] Recrystallization by heat treatment to form recrystallized grains reduces local misorientation, lowering and stabilizing the internal elastic strain energy, thereby improving the corrosion resistance of the rolled lead alloy foil. Furthermore, if there are many recrystallized grains with large grain sizes, intergranular corrosion that progresses along the grain boundaries may cause the corroded portion to penetrate the rolled lead alloy foil in the thickness direction, potentially damaging the lead-acid battery and rendering it unusable. For example, in bipolar lead-acid batteries, the formation of through-holes from the positive electrode side of the lead layer for the electrodes could further promote corrosion in other components, potentially causing a phenomenon known as a liquid junction, in which the electrolytes on the positive and negative electrodes circulate with each other. As a result, the battery performance of the bipolar lead-acid battery could be degraded, and in the worst case, the bipolar lead-acid battery could become unusable.

[0022] However, if there are many recrystallized grains with small grain sizes, corrosion progresses uniformly in the thickness direction, making it less likely that the corroded portion will penetrate the rolled lead alloy foil in the thickness direction, and thus making the lead-acid battery less likely to become unusable. Furthermore, when corrosion progresses uniformly in the thickness direction, the internal resistance increases, so the degree of deterioration due to corrosion can be detected based on the internal resistance. If corrosion progresses uniformly in the thickness direction, the lead-acid battery will be damaged and become unusable, so the degree of deterioration due to corrosion cannot be detected.

[0023] Furthermore, the thickness of the rolled lead alloy foil according to this embodiment is not particularly limited, but is preferably 0.02 mm to 1.5 mm, more preferably 0.02 mm to 1.0 mm, even more preferably 0.04 mm to 0.6 mm, and particularly preferably 0.05 mm to 0.3 mm. When the thickness of the rolled lead alloy foil is within the above range, the effect of reducing the weight of a lead-acid battery including a lead-acid battery electrode constructed using the rolled lead alloy foil as an electrode lead layer is achieved. When the thickness of the rolled lead alloy foil is 0.02 mm or more, the internal resistance of the lead-acid battery is likely to be low, making it easier to obtain a lead-acid battery with better performance. Furthermore, when the thickness of the rolled lead alloy foil is 0.02 mm or more, the rolled lead alloy foil is less likely to wrinkle or fold during the manufacturing process, improving the reliability of the lead-acid battery and facilitating handling, thereby facilitating a reduction in takt time.

[0024] On the other hand, if the thickness of the rolled lead alloy foil is 1.5 mm or less, the lead-acid battery can be made lighter, thereby increasing the weight energy density. Furthermore, if the thickness of the rolled lead alloy foil is 1.5 mm or less, the amount of rolled lead alloy foil used can be reduced, thereby facilitating a reduction in manufacturing costs. Therefore, if a lead-acid battery electrode is constructed using the rolled lead alloy foil according to this embodiment, which satisfies the above-mentioned conditions regarding the grain size, as the electrode lead layer, corrosion that penetrates the rolled lead alloy foil in the thickness direction is unlikely to occur, and therefore the lead-acid battery electrode and the lead-acid battery including the lead-acid battery electrode are unlikely to be damaged and become unusable.

[0025] <Alloy Composition of Lead Alloy> Next, the alloy composition of the lead alloy forming the rolled lead alloy foil according to this embodiment will be described. This lead alloy is a lead alloy (first lead alloy) containing 0.005% by mass or more and 0.1% by mass or less of calcium, 0.5% by mass or more and 2.0% by mass or less of tin, 0.005% by mass or less of bismuth, and the balance consisting of lead and unavoidable impurities. This lead alloy may also be a lead alloy (second lead alloy) containing 0.005% by mass or more and 0.1% by mass or less of calcium, 0.5% by mass or more and 2.0% by mass or less of tin, 0.005% by mass or less of bismuth, and 0.1% by mass or less of silver, and the balance consisting of lead and unavoidable impurities.

[0026] The inclusion of tin in the lead alloy improves adhesion between the positive electrode lead layer 101, which is made of rolled lead alloy foil, and the positive electrode active material layer 103. However, the inclusion of a large amount of tin in the lead alloy increases susceptibility to intergranular corrosion, tending to make the positive electrode lead layer 101 more susceptible to deterioration. Therefore, in both the first lead alloy and the second lead alloy, the tin content must be 0.5% by mass or more and 2.0% by mass or less, preferably 0.5% by mass or more and 1.8% by mass or less, and more preferably 0.5% by mass or more and 1.6% by mass or less.

[0027] Furthermore, adding calcium to a lead alloy inhibits grain boundary migration, resulting in finer crystal grains. Therefore, the inclusion of tin and calcium in a lead alloy increases the strength of the lead alloy and makes it less susceptible to deformation. The calcium content in the lead alloy, both the first lead alloy and the second lead alloy, must be 0.005% by mass or more and 0.1% by mass or less, preferably 0.005% by mass or more and 0.08% by mass or less, and more preferably 0.005% by mass or more and 0.06% by mass or less. Silver (Ag) has the same additive effect as calcium and may be added to the lead alloy. When silver is added to the lead alloy (second lead alloy), the silver content in the lead alloy must be 0.1% by mass or less, preferably 0.001% by mass or more and 0.1% by mass or less. However, even if silver is not actively added, it may be contained as an unavoidable impurity due to contamination from the base metal, etc.

[0028] On the other hand, if a lead alloy contains bismuth (Bi), the formability of the lead alloy during rolling or the like tends to decrease. That is, bismuth is one of the impurities that is preferably not contained as much as possible in the lead alloy forming the rolled lead alloy foil according to this embodiment. Therefore, the bismuth content in the lead alloy must be 0.005% by mass or less in both the first lead alloy and the second lead alloy, preferably 0.001% by mass or more and 0.005% by mass or less, and most preferably 0% by mass. On the other hand, lead alloys may contain elements other than lead, tin, calcium, silver, and bismuth. These elements are impurities inevitably contained in lead alloys, and the total content of elements other than lead, tin, calcium, silver, and bismuth in the lead alloy is preferably 0.01% by mass or less, and most preferably 0% by mass.

[0029] <Regarding the Manufacturing Method of Rolled Lead Alloy Foil> Next, an example of a method for manufacturing the rolled lead alloy foil constituting the positive electrode lead layer 101 from a lead alloy will be described. The rolled lead alloy foil according to this embodiment can be manufactured by combining rolling and heat treatment. By rolling a lead alloy at a high reduction rate to form a rolled lead alloy foil, fine crystals (rolled grains) can be generated inside the foil. The reduction rate when rolling the lead alloy is preferably 60% or more, more preferably 70% or more, and even more preferably 80% or more.

[0030] After the rolling, the rolled lead alloy foil is heat-treated at a temperature below the solution temperature, causing partial recrystallization and the formation of recrystallized grains. As a result, a mixed grain state containing both rolled grains and recrystallized grains can be formed within the foil. Heat treatment at a temperature above the solution temperature causes grain boundary reaction precipitation of coarse crystals due to the solution treatment, making it more likely that corrosion will penetrate the thickness of the rolled lead alloy foil. The heat treatment temperature for forming recrystallized grains is preferably 100°C or higher but not higher than the solution temperature, more preferably 180°C or higher but not higher than the solution temperature, and even more preferably 200°C or higher but not higher than the solution temperature. The heat treatment time is not particularly limited and varies depending on the heat treatment temperature, but is preferably 30 minutes to 24 hours, more preferably 1 hour to 24 hours, and even more preferably 2 hours to 24 hours.

[0031] Three manufacturing examples of the rolled lead alloy foil according to this embodiment are shown below. (Manufacturing Example 1) A 5 mm thick alloy plate made of a lead alloy is rolled at a rolling reduction of 80% to produce a 1 mm thick rolled plate. This rolling produces rolled grains. Next, the resulting rolled plate is subjected to a heat treatment (intermediate heat treatment) at 180°C for 2 hours. This intermediate heat treatment removes internal strain from the rolled plate. The intermediate heat-treated rolled plate is further rolled at a rolling reduction of 60% to produce a 0.4 mm thick rolled lead alloy foil. Finally, the rolled lead alloy foil is heat treated at 100°C for 24 hours. This heat treatment produces recrystallized grains, forming a mixed grain state and removing internal strain from the rolled lead alloy foil.

[0032] (Production Example 2) A 5 mm thick lead alloy slab was produced and left at 200°C for 1 hour (heat treatment) without cooling to room temperature, and then slowly cooled to room temperature. This resulted in a slab with internal strain removed. Next, this slab was rolled at a reduction of 92% to produce a rolled lead alloy foil with a thickness of 0.4 mm. This rolling process produced rolled grains. Finally, the rolled lead alloy foil was heat treated at 100°C for 24 hours. This heat treatment produced recrystallized grains, resulting in a mixed grain state and removing internal strain in the rolled lead alloy foil.

[0033] (Manufacturing Example 3) A 5 mm thick lead alloy slab was manufactured and left at 200°C for 1 hour (heat treatment) without cooling to room temperature, and then slowly cooled to room temperature. This resulted in a slab with internal strain removed. Next, this slab was rolled at a reduction of 80% to form a 1 mm thick rolled plate. This rolling process produced rolled grains. Next, the resulting rolled plate was heat treated at 180°C for 2 hours (intermediate heat treatment). This intermediate heat treatment removed the internal strain of the rolled plate. The intermediate heat-treated rolled plate was then further rolled at a reduction of 60% to form a 0.4 mm thick rolled lead alloy foil. Finally, the rolled lead alloy foil was heat treated at 100°C for 24 hours. This heat treatment produced recrystallized grains, resulting in a mixed grain state and removing the internal strain of the rolled lead alloy foil.

[0034] [Examples] The present invention will be described in more detail below with reference to examples and comparative examples. (Example 1) A 5.0 mm thick alloy plate was prepared, which was made of a lead alloy containing 0.06 mass% calcium, 1.6 mass% tin, 0.002 mass% or less bismuth, and the remainder being lead and unavoidable impurities. Using this alloy plate as a material, a rolled lead alloy foil was produced by the method shown in Production Example 1 above. That is, the 5.0 mm thick alloy plate was rolled at a rolling reduction of 80% to obtain a 1.0 mm thick rolled plate, which was then subjected to an intermediate heat treatment (first-stage heat treatment) at 180°C for 2 hours. The rolled plate subjected to the intermediate heat treatment was then rolled at a rolling reduction of 60% to obtain a 0.4 mm thick rolled lead alloy foil, which was then subjected to a heat treatment (second-stage heat treatment) at 100°C for 24 hours. The obtained rolled lead alloy foil of Example 1 was subjected to the following analyses and performance evaluations.

[0035] <Measurement of KAM Value and Calculation of Area Ratio> First, the rolled lead alloy foil of Example 1 was cut to expose a cross section parallel to the rolling direction of the rolled lead alloy foil and perpendicular to the surface of the rolled lead alloy foil. Then, within this cross section, an arbitrary location in the central portion in the thickness direction, excluding the portion near the surface of the rolled lead alloy foil where processing strain was large, was used as the measurement portion. The measurement portion was divided into a mesh-like pattern to set multiple measurement regions defined in the mesh-like pattern. In Example 1, as shown in FIG. 5, the shape of the measurement portion was a square with sides of 20 μm, and the shape of each measurement region was a regular hexagon with sides of 0.3 μm. Using a scanning electron microscope JSM-7001FA manufactured by JEOL Ltd., the measurement portion was analyzed by electron backscatter diffraction. The analysis results were then analyzed using analysis software OIM Analysis (registered trademark) manufactured by TSL Solutions Co., Ltd., to calculate the KAM value of each measurement region.

[0036] In this analysis, the measurement target was determined to be a region with a CI (Confidence Index) value of 0.1 or greater, which is an index indicating the reliability of indexing to estimate crystal orientation. This confirmed that regions with significant processing strain were excluded from the measurement target. Furthermore, in this analysis, a misorientation of 15° or greater was defined as a grain boundary. Therefore, according to this analysis, the calculated KAM value for each measurement region falls within the range of 0° or greater and less than 15°. The KAM value for a given measurement region is calculated by averaging the misorientations of adjacent measurement regions. However, adjacent measurement regions with misorientations of less than 0° or greater than 15° are excluded from the calculation of the average. Therefore, the KAM value is the average of the misorientations between adjacent measurement regions within the same crystal grain. Using FIG. 6 as an example, the KAM value for measurement region P is calculated using the formula shown in FIG. 6. The values ​​written within the six measurement regions adjacent to measurement region P represent the misorientations of that measurement region relative to measurement region P.

[0037] Next, each measurement area was classified by KAM value. Classification was performed in 1° increments, resulting in 15 types. That is, measurement areas with KAM values ​​of 0° or more and less than 1°, measurement areas with KAM values ​​of 1° or more and less than 2°, ..., measurement areas with KAM values ​​of 14° or more and less than 15°, were classified into 15 types. The total area of ​​each type of measurement area was then calculated and divided by the total area of ​​all measurement areas to calculate the proportion (area ratio) of each type of measurement area. Furthermore, using the results of the proportion of each type of measurement area, the proportion (area ratio) of measurement areas with KAM values ​​of 0° or more and less than 1°, measurement areas with KAM values ​​of 1° or more and less than 5°, and measurement areas with KAM values ​​of 5° or more and less than 15° was calculated. This analysis was performed on five arbitrary measurement target portions, and the average value was calculated. The results are shown in Table 1.

[0038] <Measurement of Crystal Grain Diameter and Calculation of Area Ratio> The cross section was analyzed by electron backscatter diffraction in the same manner as in the measurement of the KAM value. The analysis results were then analyzed using OIM Analysis (registered trademark) analysis software manufactured by TSL Solutions, Inc., to measure the diameters of the crystal grains observed in the cross section. In this analysis, a misorientation of 15° or more was defined as a grain boundary, and the area of ​​the crystal grain was calculated from the number of measurement regions present in the same crystal grain. The diameter of the crystal grain was calculated by regarding the crystal grain as a perfect circle. Next, each crystal grain was classified by diameter. Classification was performed in 0.1 μm increments, resulting in multiple types. That is, crystal grains with diameters greater than 0 μm and less than 0.1 μm, crystal grains of 0.1 μm or greater but less than 0.2 μm, crystal grains of 0.2 μm or greater but less than 0.3 μm, etc. The total area of ​​each type of crystal grain was calculated and divided by the total area of ​​all measurement regions to calculate the proportion (area ratio) of each type of crystal grain. The results are shown in Table 1.

[0039] <Measurement of corrosion rate> A constant potential test was carried out to evaluate the corrosion resistance of the rolled lead alloy foil of Example 1. A positive electrode made using the rolled lead alloy foil of Example 1 and a negative electrode made using lead foil were immersed in an electrolyte. The electrolyte was sulfuric acid with a specific gravity of 1.28 and a temperature of 60°C. A potential difference of 1350 mV was applied between the positive and negative electrodes, and a current was passed through the rolled lead alloy foil to oxidize (corrode). After 7 days of current application, the positive electrode was removed and the corrosion rate of the rolled lead alloy foil was calculated. The corrosion rate was calculated as follows: Oxides were removed from the removed rolled lead alloy foil, and the mass of the removed oxide was taken as the amount of corrosion. The amount of corrosion was divided by the surface area of ​​the rolled lead alloy foil before the constant potential test (amount of corrosion / surface area) to give the corrosion rate (mg / cm 2 The lower the corrosion rate, the higher the corrosion resistance of the rolled lead alloy foil. 2 If the value is less than 100%, the corrosion resistance is judged to be excellent. The results are shown in Table 1.

[0040] <Evaluation of corrosion uniformity> The rolled lead alloy foil after the constant potential test was cut to expose a cross section parallel to the rolling direction of the rolled lead alloy foil and perpendicular to the surface of the rolled lead alloy foil. Next, the cross section was mirror-finished by electrolytic polishing and observed using an optical microscope. Then, a location where the surface of the rolled lead alloy foil was uniformly corroded (to approximately the same depth) was found, and the thickness of the non-corroded portion where the lead alloy remained uncorroded was measured (see Figure 2 (a)). Similar measurements were performed at five locations, and the average value was taken as the residual thickness value. The corrosion depth A (μm) was determined by subtracting the residual thickness value from the thickness of the rolled lead alloy foil before the constant potential test.

[0041] Next, optical microscope observation was performed in the same manner as above to find areas where linear or wedge-shaped corrosion had progressed from the surface toward the interior of the rolled lead alloy foil, and the depth of the linear or wedge-shaped corrosion was measured (see Figure 2(b)). The starting point for measuring the depth of the linear or wedge-shaped corrosion was not the surface of the rolled lead alloy foil before the constant-potential test, but the surface of the rolled lead alloy foil where uniform corrosion had occurred after the constant-potential test. Similar measurements were performed at five locations, and the maximum value was taken as the corrosion depth B (μm). The corrosion uniformity was then evaluated by dividing the corrosion depth B by the corrosion depth A. If the rolled lead alloy foil is composed of fine crystals, corrosion tends to progress uniformly, resulting in a small corrosion uniformity value. If the rolled lead alloy foil contains coarse crystals, corrosion tends to progress linearly or wedge-shaped, resulting in a large corrosion uniformity value. A corrosion uniformity of 2 or less is considered to be uniform corrosion and excellent corrosion resistance. The results are shown in Table 1.

[0042] <Evaluation of the Presence or Absence of Wrinkles or Folds> The rolled lead alloy foil of Example 1 was fixed to a substrate. Then, the rolled lead alloy foil fixed to the substrate was visually observed to determine whether wrinkles or folds occurred in the rolled alloy foil. The results are shown in Table 1.

[0043]

[0044] (Example 2) A rolled lead alloy foil of Example 2 was produced in exactly the same manner as Example 1, except that the conditions of the second stage heat treatment were different as shown in Table 1. Then, analysis and performance evaluation were carried out in exactly the same manner as Example 1. The results of the analysis and performance evaluation are shown in Table 1.

[0045] (Example 3) A rolled lead alloy foil of Example 3 was produced in exactly the same manner as Example 1, except that the conditions of the second stage heat treatment were different as shown in Table 1. Then, analysis and performance evaluation were carried out in exactly the same manner as Example 1. The results of the analysis and performance evaluation are shown in Table 1.

[0046] (Example 4) A rolled lead alloy foil of Example 4 was produced in exactly the same manner as Example 1, except that the contents of tin and calcium in the lead alloy were different as shown in Table 1. Then, analysis and performance evaluation were carried out in exactly the same manner as Example 1. The results of the analysis and performance evaluation are shown in Table 1.

[0047] (Example 5) A rolled lead alloy foil of Example 5 was produced in exactly the same manner as Example 1, except that the conditions of the second stage heat treatment were different as shown in Table 1. Then, analysis and performance evaluation were carried out in exactly the same manner as Example 1. The results of the analysis and performance evaluation are shown in Table 1.

[0048] (Example 6) A rolled lead alloy foil of Example 6 was produced in exactly the same manner as Example 1, except that the tin and calcium contents in the lead alloy were different as shown in Table 1 and the conditions for the second stage heat treatment were different as shown in Table 1. Then, analysis and performance evaluation were carried out in exactly the same manner as Example 1. The results of the analysis and performance evaluation are shown in Table 1.

[0049] (Examples 7 to 15, 18 to 26) Rolled lead alloy foils of Examples 7 to 15 and 18 to 26 were produced in exactly the same manner as in Example 1, except that the contents of tin, calcium, silver, and bismuth in the lead alloy were different as shown in Table 1. Then, analysis and performance evaluation were carried out in exactly the same manner as in Example 1. The results of the analysis and performance evaluation are shown in Table 1.

[0050] Example 16 A lead alloy having the same composition as in Example 1 was prepared, and a rolled lead alloy foil was produced by the method shown in Production Example 2 above. That is, a lead alloy slab having a thickness of 5.0 mm was produced, and left at 200°C for 1 hour without cooling to room temperature (first-stage heat treatment), and then slowly cooled to room temperature. Next, this slab was rolled at a rolling reduction of 92% to produce a rolled lead alloy foil having a thickness of 0.4 mm. Finally, the rolled lead alloy foil was subjected to a heat treatment at 100°C for 24 hours (second-stage heat treatment).

[0051] Example 17 A lead alloy having the same composition as in Example 1 was prepared, and a rolled lead alloy foil was produced by the method shown in Production Example 3 above. Specifically, a 5.0 mm thick lead alloy slab was produced and left at 200°C for 1 hour without cooling to room temperature (first-stage heat treatment), and then slowly cooled to room temperature. This slab was then rolled at a reduction of 80% to produce a 1.0 mm thick rolled sheet. The resulting rolled sheet was then subjected to a heat treatment at 180°C for 2 hours (intermediate heat treatment). The intermediate-heat-treated rolled sheet was then further rolled at a reduction of 60% to produce a 0.4 mm thick rolled lead alloy foil. Finally, the rolled lead alloy foil was subjected to a heat treatment at 100°C for 24 hours (second-stage heat treatment).

[0052] (Comparative Example 1) A rolled lead foil of Comparative Example 1 was produced in exactly the same manner as in Example 1, except that pure lead was used instead of the lead alloy and the second stage heat treatment was not performed. Then, analysis and performance evaluation were carried out in exactly the same manner as in Example 1. The results of the analysis and performance evaluation are shown in Table 1.

[0053] (Comparative Example 2) A rolled lead alloy foil of Comparative Example 2 was produced in exactly the same manner as in Example 1, except that the second heat treatment was not carried out. Then, analysis and performance evaluation were carried out in exactly the same manner as in Example 1. The results of the analysis and performance evaluation are shown in Table 1.

[0054] (Comparative Example 3) A rolled lead alloy foil of Comparative Example 3 was produced in exactly the same manner as in Example 1, except that the conditions of the second stage heat treatment were different as shown in Table 1. Then, analysis and performance evaluation were carried out in exactly the same manner as in Example 1. The results of the analysis and performance evaluation are shown in Table 1.

[0055] Comparative Example 4 A rolled lead alloy foil of Comparative Example 4 was produced in exactly the same manner as in Example 1, except that the tin and calcium contents in the lead alloy were different as shown in Table 1 and that the second-stage heat treatment was not performed. Analysis and performance evaluation were then carried out in exactly the same manner as in Example 1. The results of the analysis and performance evaluation are shown in Table 1.

[0056] As can be seen from the results shown in Table 1, in Examples 1 to 26, the proportion of the measurement area where the KAM value was less than 1° was 50 area % or more, and therefore the corrosion rate was low and the corrosion resistance was excellent. Furthermore, in Examples 1, 2, 4, and 7 to 26, the proportion of crystal grains with a grain size of less than 20 μm was 95 area % or more, and therefore the corrosion uniformity was high and the corrosion resistance was excellent. On the other hand, in Comparative Examples 2 to 4, the proportion of the measurement area where the KAM value was less than 1° was less than 50 area %, and therefore the corrosion rate was high and the corrosion resistance was insufficient. The results of Examples 1 to 6 and Comparative Examples 2 to 4 are shown in the graphs of Figures 3 and 4. From the graph of Figure 3, it can be seen that when the proportion of the measurement area where the KAM value was less than 1° was 50 area % or more, the corrosion rate was 30 mg / cm. 2 4, when the proportion of crystal grains with a grain size of less than 20 μm is 95% by area or more, the corrosion uniformity is 2 or less, which indicates that the corrosion uniformity is high.

[0057] 1... Lead storage battery 101... Lead layer for positive electrode 102... Lead layer for negative electrode 103... Active material layer for positive electrode 104... Active material layer for negative electrode 105... Electrolytic layer 110... Negative electrode 111... Substrate 120... Positive electrode 130... Bipolar electrode

Claims

1. A rolled lead alloy foil formed of a lead alloy containing 0.005% by mass or more and 0.1% by mass or less of calcium, 0.5% by mass or more and 2.0% by mass or less of tin, and 0.005% by mass or less of bismuth, with the remainder being lead and unavoidable impurities, wherein a plurality of measurement areas defined in a mesh pattern are set on a cross section of the rolled lead alloy foil that appears when the rolled lead alloy foil is cut along a plane that is parallel to the rolling direction of the rolled lead alloy foil and perpendicular to the surface of the rolled lead alloy foil, and when the local orientation difference of each of the measurement areas is measured, the proportion of the measurement areas in which the local orientation difference is less than 1 degree is 50 area % or more of all the measurement areas.

2. A rolled lead alloy foil formed of a lead alloy containing 0.005% by mass or more and 0.1% by mass or less of calcium, 0.5% by mass or more and 2.0% by mass or less of tin, 0.005% by mass or less of bismuth, 0.1% by mass or less of silver, with the remainder being lead and unavoidable impurities, wherein a plurality of measurement areas defined in a mesh pattern are set on a cross section of the rolled lead alloy foil that appears when the rolled lead alloy foil is cut along a plane that is parallel to the rolling direction of the rolled lead alloy foil and perpendicular to the surface of the rolled lead alloy foil, and when the local orientation difference of each of the measurement areas is measured, the proportion of the measurement areas in which the local orientation difference is less than 1 degree is 50 area % or more of all the measurement areas.

3. The rolled lead alloy foil according to claim 1 or 2, wherein, when the diameters of the crystal grains observed in the cross section are measured, the proportion of crystal grains having a grain size of less than 20 μm among all the crystal grains is 95 area % or more.

4. The rolled lead alloy foil according to claim 1 or 2, wherein the ratio of the measurement areas in which the local orientation difference is less than 5 degrees to all of the measurement areas is 94 area % or more.

5. The rolled lead alloy foil according to claim 1 or 2, having a thickness of 0.02 mm or more and 1.5 mm or less.

6. A lead-acid battery electrode comprising an electrode lead layer made of the rolled lead alloy foil according to claim 1 or 2, and an active material disposed on the surface of the electrode lead layer.

7. The electrode for a lead-acid battery according to claim 6, which is for a bipolar lead-acid battery.

8. A lead-acid battery comprising the lead-acid battery electrode according to claim 6.

Citation Information

Patent Citations

  • Lead acid battery

    JP1995065822A

  • Lead and lead alloys, especially for lead-acid batteries and their electrodes, with improved creep and / or intergranular corrosion resistance

    JP2003511823A

  • Alloy for battery grids

    JP2004165149A

  • Lead alloy, positive electrode for lead storage batteries, lead storage battery, and power storage system