Positive electrode and secondary battery
The combination of first and second positive electrode active material particles with a phosphorus compound coating on the first particles in a controlled mass ratio addresses the issue of increased internal resistance and side reactions in secondary batteries, enhancing battery capacity and efficiency.
Patent Information
- Application Number
- PCT/JP2024/015948
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-23
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional secondary batteries face issues with increased internal resistance due to side reactions such as reduction and elution of transition metals and electrolyte decomposition, which accelerate battery deterioration.
A positive electrode configuration using a combination of first and second positive electrode active material particles, with a phosphorus compound coating on the surface of the first particles, where the mass ratio of phosphorus on the second particles to the first particles is controlled to suppress side reactions and reduce internal resistance.
This configuration effectively reduces internal resistance and gas generation while improving battery capacity and charging efficiency, effectively addressing the challenges of side reactions and capacity enhancement.
Smart Images

Figure JP2024015948_31102024_PF_FP_ABST
Abstract
Description
Positive electrodes and secondary batteries
[0001] The present disclosure relates to a positive electrode and a secondary battery.
[0002] It is known that conventional secondary batteries are subject to side reactions, such as reduction and elution of transition metals contained in the active material, which in turn cause decomposition of the electrolyte. These side reactions accelerate the deterioration of the secondary battery.
[0003] Known techniques for addressing the issue of electrolyte decomposition reactions include, for example, the technique disclosed in Patent Document 1. Patent Document 1 describes a coated positive electrode active material having a coating containing at least one selected from a specific phosphonic acid and a specific phosphite triester.
[0004] International Publication No. 2017 / 126276
[0005] However, coating the positive electrode active material as described above increases the internal resistance. In other words, reducing the increase in internal resistance due to the configuration for suppressing side reactions is also an important issue. The present disclosure provides a positive electrode that can reduce the increase in internal resistance while suppressing side reactions in the positive electrode of a battery.
[0006] The positive electrode of the present disclosure includes: first positive electrode active material particles; second positive electrode active material particles; and a phosphorus compound attached to at least a portion of the surface of the first positive electrode active material particles; the first positive electrode active material particles are particles formed by aggregating 51 or more and 20,000 or less first primary particles; the second positive electrode active material particles are particles formed by aggregating one second primary particle or 2 or more and 50 or less second primary particles; and a mass ratio of P contained in the phosphorus compound attached to the surface of the second positive electrode active material particles to P contained in the phosphorus compound attached to the surface of the first positive electrode active material particles is 0 or more and 0.5 or less.
[0007] According to the technology of the present disclosure, it is possible to reduce an increase in internal resistance while suppressing side reactions in the positive electrode of a battery.
[0008] Fig. 1 is a cross-sectional view showing a schematic configuration of an example of a positive electrode according to Embodiment 1. Fig. 2 is a schematic cross-sectional view showing an example of a nonaqueous electrolyte secondary battery according to Embodiment 2.
[0009] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. The present disclosure is not limited to the following embodiments.
[0010] (Embodiment 1) A positive electrode according to Embodiment 1 includes first positive electrode active material particles, second positive electrode active material particles, and a phosphorus compound attached to at least a portion of the surface of the first positive electrode active material particles. The first positive electrode active material particles are particles formed by agglomeration of 51 or more and 20,000 or less first primary particles. The second positive electrode active material particles are particles formed by agglomeration of one second primary particle or two or more and 50 or less second primary particles. The mass ratio of P contained in the phosphorus compound attached to the surface of the second positive electrode active material particles to P contained in the phosphorus compound attached to the surface of the first positive electrode active material particles is 0 or more and 0.5 or less.
[0011] Conventionally, first positive electrode active material particles, which are particles formed by the aggregation of many primary particles, have been used in positive electrodes. However, to further improve battery capacity, the use of a positive electrode active material with a smaller particle size to fill the gaps in the positive electrode has been considered. However, as the particle size of the first positive electrode active material particles decreases, the surface area increases, accelerating side reactions and further increasing the amount of gas generated at the positive electrode. The use of a positive electrode active material with a simple particle size change is undesirable because it generates a large amount of gas relative to the increase in capacity. Therefore, the use of second positive electrode active material particles has been considered as a positive electrode active material with a particle size sufficient to fill the gaps in the positive electrode. The second positive electrode active material particles are particles consisting of single primary particles or particles formed by a small number of such primary particles. Although such second positive electrode active material particles can suppress gas generation even when their particle size is smaller than that of the first positive electrode active material particles, there is a concern that the internal resistance of the battery may increase due to the small number of grain boundaries between the primary particles. Just to be clear, by filling the gaps in the positive electrode, i.e., the spaces between the first positive electrode active material particles, with the second positive electrode active material particles, the battery capacity is improved compared to when the second positive electrode active material particles are not included in the positive electrode.
[0012] Therefore, the researchers investigated the possibility of suppressing the amount of gas generated at the positive electrode and improving battery capacity by using second positive electrode active material particles having a particle size that fills the gaps between the first positive electrode active material particles while suppressing side reactions of the first positive electrode active material particles. To suppress side reactions such as gas generation at the positive electrode, they investigated coating the positive electrode with a phosphorus compound.
[0013] The inventors investigated the relationship between battery characteristics and first positive electrode active material particles, second positive electrode active material particles, and first positive electrode active material particles with a phosphorus compound attached to their surfaces. The first positive electrode active material particles were lithium nickel manganese oxide particles (average particle diameter 17 μm) formed by agglomeration of approximately 4,000 primary particles with an average particle diameter of 1 μm. The second positive electrode active material particles were lithium nickel manganese oxide particles (average particle diameter 5 μm) formed by agglomeration of four primary particles with an average particle diameter of 3 μm. Tristrimethylsilyl phosphate (TMSP) was used as the phosphorus compound. The surfaces of the first positive electrode active material particles were coated with TMSP using a procedure similar to that described later in the examples of the present disclosure. Evaluation cells were fabricated using the above first positive electrode active material particles, second positive electrode active material particles, and first positive electrode active material particles with a phosphorus compound attached to their surfaces as the positive electrode active materials, and the internal resistance and gas generation rate were measured. The procedure for fabricating the evaluation cells was similar to that described later in the examples of this disclosure.
[0014] As a result of the above verification, the battery using only the second positive electrode active material particles had an internal resistance value more than twice that of the battery using only the first positive electrode active material particles, but the amount of gas generated after the trickle test was 17%.The battery using the first positive electrode active material particles coated with TMSP had an internal resistance value 1.13 times that of the battery using only the first positive electrode active material particles, and the amount of gas generated after the trickle test was reduced to 56%.
[0015] The positive electrode of the present disclosure is a positive electrode that uses both first and second positive electrode active material particles, and the mass ratio of the phosphorus compound attached to the surface of the second positive electrode active material particles to the phosphorus compound attached to the surface of the first positive electrode active material particles is appropriately adjusted. As a result, it is possible to achieve an improvement in battery capacity while suppressing side reactions in the positive electrode of the battery and an increase in internal resistance.
[0016] FIG. 1 is a cross-sectional view showing a schematic configuration of an example of a positive electrode according to Embodiment 1. The positive electrode 10 includes a positive electrode current collector 1 and a positive electrode active material layer 2, in this order. The positive electrode active material layer 2 is a layer containing first positive electrode active material particles 3, second positive electrode active material particles 4, and a phosphorus compound, and is supported on the positive electrode current collector 1. At least a portion of the surface of the first positive electrode active material particles 3 is coated with a coating material 5 containing a phosphorus compound. The surface of the second positive electrode active material particles 4 may or may not be coated with the coating material 5. The mass ratio (mass ratio P2 / P1) of the P contained in the phosphorus compound in the coating material 5 coating the surface of the second positive electrode active material particles 4 to the P contained in the phosphorus compound in the coating material 5 coating the surface of the first positive electrode active material particles 3 is 0 or more and 0.5 or less.
[0017] The first positive electrode active material particle 3 is a secondary particle formed by aggregating 51 to 20,000 first primary particles. The second positive electrode active material particle 4 is a particle formed by aggregating one second primary particle or two to 50 second primary particles.
[0018] In the positive electrode 10 according to the first embodiment, a phosphorus compound is attached to at least a portion of the surface of the first positive electrode active material particles 3, thereby suppressing side reactions. Examples of side reactions that can be suppressed include gas generation. The phosphorus compound need only be attached to the surface of the first positive electrode active material particles 3, i.e., the surface of the secondary particles. It is not necessary for the phosphorus compound to be attached to the surface of the first primary particles located inside the first positive electrode active material particles 3. Furthermore, in the positive electrode 10, the positive electrode active material layer 2 contains the first positive electrode active material particles 3 and the second positive electrode active material particles 4, and satisfies the above-described mass ratio of the phosphorus compounds. This configuration can suppress side reactions in the positive electrode while reducing an increase in the internal resistance of the battery. In particular, side reactions and an increase in internal resistance during long-term charging of the battery can be suppressed.
[0019] The mass ratio P2 / P1 is a value calculated by the formula: (mass of P contained in the phosphorus compound contained in the coating material 5 that coats the surfaces of the second positive electrode active material particles 4 in the positive electrode 10) / (mass of P contained in the phosphorus compound contained in the coating material 5 that coats the surfaces of all of the first positive electrode active material particles 3 in the positive electrode 10). The mass ratio P1 / P2 can be calculated, for example, using energy dispersive X-ray spectroscopy (STEM-EDX) using a scanning transmission electron microscope and inductively coupled plasma (ICP) analysis. Specifically, the mass ratio P1 / P2 can be calculated by calculating the ratio of P coating the surfaces of the first positive electrode active material particles 3 and the second positive electrode active material particles 4 using STEM-EDX of a cross section of the positive electrode 10, and then determining the mass of P using ICP analysis.
[0020] The mass ratio P2 / P1 may be 0 or more and 0.3 or less, 0 or more and 0.2 or less, 0 or more and 0.1 or less, 0 or more and 0.05 or less, or 0 or more and 0.025 or less.
[0021] The first positive electrode active material particles 3 are preferably particles formed by agglomeration of 1,000 or more and 10,000 or less first primary particles, and more preferably particles formed by agglomeration of 2,000 or more and 5,000 or less first primary particles.
[0022] The first primary particles may have an average particle size of 50 nm or more and 5 μm or less, and the second primary particles may have an average particle size of 0.5 μm or more and 7 μm or less.
[0023] The average particle size of the first primary particles may be 100 nm or more and 3 μm or less, or 100 nm or more and less than 2 μm. The average particle size of the second primary particles may be 0.5 μm or more and 5 μm or less, or 2 μm or more and 5 μm or less.
[0024] The average particle size of the first primary particles may be smaller than the average particle size of the second primary particles. With the above configuration, the internal resistance of the battery can be reduced.
[0025] The second positive electrode active material particle 4 is preferably a particle formed by aggregating one second primary particle or two or more and five or less second primary particles.
[0026] The second primary particles may have higher crystallinity than the first primary particles. The second primary particles may be single crystal. The second positive electrode active material particles 4 may be single crystal particles.
[0027] The average particle diameters of the first primary particles and the second primary particles are determined by the following method. A cross section of the positive electrode 10 is observed with a scanning electron microscope (SEM). In the obtained SEM image, the first positive electrode active material particles 3 and the second positive electrode active material particles 4 are distinguished from each other based on the number of primary particles. The particle diameters of 50 randomly selected first primary particles from the group of first primary particles constituting the first positive electrode active material particles 3 are calculated, and the average value is regarded as the average particle diameter of the first primary particles. Similarly, the particle diameters of 50 randomly selected second primary particles from the group of second primary particles constituting the second positive electrode active material particles 4 are calculated, and the average value is regarded as the average particle diameter of the second primary particles.
[0028] The first positive electrode active material particles 3 have an average particle diameter of, for example, 3 μm or more and 20 μm or less, and preferably 6 μm or more and 17 μm or less. The second positive electrode active material particles 4 have an average particle diameter of, for example, 0.5 μm or more and 7 μm or less, and preferably 2 μm or more and 5 μm or less. With the above configuration, it is possible to suppress side reactions in the positive electrode while reducing an increase in the internal resistance of the battery.
[0029] The average particle diameters of the first positive electrode active material particles 3 and the second positive electrode active material particles 4 can be determined by a laser diffraction scattering method using a commercially available laser diffraction measurement device. For example, the laser diffraction scattering method can be performed on the first positive electrode active material particles 3 used as a raw material for producing the positive electrode active material layer 2, and the average particle diameter of the first positive electrode active material particles 3 can be determined based on the obtained particle size distribution. Here, the average particle diameter is defined as the particle diameter at which the cumulative volume in the volume-based particle size distribution is equal to 50%. Similarly, the laser diffraction scattering method can be performed on the second positive electrode active material particles 4 used as a raw material for producing the positive electrode active material layer 2, and the average particle diameter of the second positive electrode active material particles 4 can be determined based on the obtained particle size distribution.
[0030] The average particle diameters of the first positive electrode active material particles 3 and the second positive electrode active material particles 4 may be determined by the following method: In a cross-sectional SEM image of the positive electrode 10, the particle diameters (circle-equivalent diameters) of 50 randomly selected first positive electrode active material particles 3 and the particle diameters (circle-equivalent diameters) of 50 randomly selected second positive electrode active material particles 4 are calculated, and the average values are regarded as the average particle diameters of the first positive electrode active material particles 3 and the second positive electrode active material particles 4, respectively.
[0031] The average particle size of the first positive electrode active material particles 3 may be larger than the average particle size of the second positive electrode active material particles 4. The average particle size of the first positive electrode active material particles 3 may be larger than the average particle size of the second positive electrode active material particles 4, and the average particle size of the first primary particles may be smaller than the average particle size of the second primary particles.
[0032] The average particle diameter of the first positive electrode active material particles 3 may be greater than 5 μm and less than 20 μm, or may be 10 μm or greater and less than 20 μm. The average particle diameter of the second positive electrode active material particles 4 may be 0.5 μm or greater and less than 5 μm.
[0033] The mass ratio of the first positive electrode active material particles 3 to the second positive electrode active material particles 4 (mass ratio A1 / A2) may be 0.67 or more and 4.0 or less.
[0034] The mass ratio A1 / A2 is a value calculated by the formula: (total mass of the first positive electrode active material particles 3 in the positive electrode 10) / (total mass of the second positive electrode active material particles 4 in the positive electrode 10). The mass ratio A1 / A2 may be 1.5 or more and 4.0 or less, 2.0 or more and 3.8 or less, or 2.5 or more and 3.5 or less. This configuration can further reduce an increase in the internal resistance of the battery while suppressing side reactions in the positive electrode. Furthermore, the battery capacity and charge / discharge efficiency can also be improved.
[0035] The mass ratio A1 / A2 can be determined using, for example, SEM and STEM-EDX. The total mass of the first positive electrode active material particles 3 is calculated by multiplying the particle volume of the first positive electrode active material particles 3 by the average particle number per positive electrode volume, the mass density of the first positive electrode active material particles 3, and the positive electrode volume. The same applies to the total mass of the second positive electrode active material particles 4. The particle volume is calculated from the average particle diameter of the first positive electrode active material particles 3 or the second positive electrode active material particles 4. The average particle number per positive electrode volume is calculated from the average particle number within a predetermined area in an SEM image. For example, when an oxide containing Ni and Mn is used as the positive electrode active material particles, the mass density of the positive electrode active material particles is calculated from the Ni atomic mass ratio, Mn atomic mass ratio, and O atomic mass ratio measured by STEM-EDX. The mass ratio A1 / A2 can be determined from the total mass of the first positive electrode active material particles 3 and the total mass of the second positive electrode active material particles 4 calculated as above.
[0036] The first positive electrode active material particles 3 and the second positive electrode active material particles 4 are particles of a positive electrode active material. The positive electrode active material is not particularly limited. Examples of the positive electrode active material include lithium-containing transition metal oxides, lithium-containing transition metal phosphates, transition metal fluorides, polyanionic materials, fluorinated polyanionic materials, transition metal sulfides, transition metal oxysulfides, and transition metal oxynitrides. In particular, using a lithium-containing transition metal oxide or a lithium-containing transition metal phosphate as the positive electrode active material can reduce the manufacturing cost of the battery and increase the average discharge voltage. Examples of lithium-containing transition metal oxides include lithium cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide, and lithium nickel manganese oxide. Examples of lithium-containing transition metal phosphates include lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, and lithium nickel phosphate. At least one selected from these positive electrode active materials can be used.
[0037] The first positive electrode active material particles 3 and the second positive electrode active material particles 4 may be made of materials having the same composition, or may be made of materials having different compositions.
[0038] The coating material 5 contains a phosphorus compound. The coating material 5 may contain a material other than a phosphorus compound. The coating material 5 may contain only a phosphorus compound, excluding inevitable impurities. The coating material 5 is in contact with and coats the surfaces of the first positive electrode active material particles 3. The coating material 5 may form a coating layer that coats the surfaces of the first positive electrode active material particles 3.
[0039] The phosphorus compound may contain a P=O bond. Examples of the phosphorus compound include phosphoric acid, phosphonic acid, phosphinic acid, pyrophosphoric acid, phosphate esters, phosphonate esters, phosphinate esters, derivatives thereof, and condensates thereof. The phosphorus compound may be an organic phosphorus compound. In this specification, an organic phosphorus compound means a compound containing carbon and phosphorus. The phosphorus compound may be an organic phosphorus compound having a carbon-phosphorus bond.
[0040] The phosphorus compound may contain a P-O-P bond. The phosphorus compound may be polyphosphoric acid, a polyphosphate ester, or a derivative thereof. With the above configuration, side reactions at the positive electrode can be further suppressed.
[0041] The phosphorus compound may include a structure represented by chemical formula (1).
[0042]
[0043] In chemical formula (1), n1 and n2 are each independently an integer of 0 or greater. 1 , R 2 , R 4 , and R 5 are each independently -OR or -(CH2) m1 represents X1. 3 and R each independently represent a direct bond to the first positive electrode active material particle 3, a hydrogen atom, or —(CH) m2 X2 represents a trimethylsilyl group or a triethylsilyl group. m1 is an integer of 0 to 15. m2 is a natural number of 1 to 3. X1 and X2 each independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxy group, a cyano group, or a fluorine atom. R 2 If there are multiple R 2 are independent of each other. 4 If there are multiple R 4 are independent of each other.
[0044] Because the phosphorus compound has such a structure, it is relatively stable even under high voltage environments, and therefore side reactions such as gas generation can be sufficiently suppressed even when the upper limit voltage of the secondary battery is high, for example, even when it exceeds 4.3 V. In addition, the effect of suppressing side reactions can be maintained for a longer period of time.
[0045] In chemical formula (1), n1 and n2 may be, independently of each other, 1 or greater. At least one selected from the group consisting of n1 and n2 may be 1 or greater. n1 and n2 may be, independently of each other, 500 or less. X1 may be a hydrogen atom. X2 may be a hydrogen atom.
[0046] In chemical formula (1), m1 may be an integer of 0 to 11, or an integer of 0 to 6. When m1 is an integer of 0 to 6, side reactions can be further suppressed.
[0047] In the chemical formula (1), m2 may be 1 or 2. 3 may be a direct bond to the first positive electrode active material particle 3 .
[0048] The phosphorus compound may be, for example, silyl phosphite, phosphonic acid, phosphoric acid, pyrophosphate, or a condensate thereof. The phosphorus compound may be silyl phosphite, tristrimethylsilyl phosphate (TMSP), or a compound derived from TMSP, such as a condensate of TMSP. In the chemical formula (1), R 1 , R 2 , R 4 , and R 5 are each independently -OR, and R 3 and R may each independently represent a direct bond to the first positive electrode active material particle 3, a hydrogen atom, or a trimethylsilyl group. This configuration can further suppress side reactions in the positive electrode of the battery. In addition, an increase in internal resistance can be further reduced.
[0049] The phosphorus compound may be phosphoric acid or a condensate of phosphoric acid. 1 , R 2 , R 4 , and R 5 are each independently -OR, and R 3 and R may each independently represent a direct bond to the first positive electrode active material particle 3 or a hydrogen atom.
[0050] The positive electrode active material layer 2 may contain one or more types of phosphorus compounds. That is, the positive electrode 10 may contain one or more types of phosphorus compounds.
[0051] The phosphorus compound may or may not form a chemical bond with the first positive electrode active material particles 3. The phosphorus compound may be physically attached to the first positive electrode active material particles 3.
[0052] The mass ratio of P contained in the coating material 5 coating the first positive electrode active material particles 3 relative to the first positive electrode active material particles 3 is, for example, 0.1% or more, or may be 0.14% to 0.3% or less, or 0.14% to 0.24% by mass or less. When TMSP is added to the electrolyte, there is a limit to the TMSP content that can be dissolved in the electrolyte, so a sufficient amount of TMSP cannot be used to improve characteristics. When TMSP is added to the electrolyte, a TMSP self-coating film may be formed on the positive electrode. In this case, the mass ratio of P in the coating relative to the total amount of the positive electrode active material is approximately 0.006% by mass. Furthermore, adding TMSP to the electrolyte is undesirable because a TMSP self-coating film is also formed on the surface of the second positive electrode active material particles 4, increasing the mass ratio P2 / P1 and potentially becoming a resistance component.
[0053] At least a portion of the surface of the second positive electrode active material particles 4 may be coated with the coating material 5, but is preferably not coated. When at least a portion of the surface of the second positive electrode active material particles 4 is coated with the coating material 5, the mass ratio of P contained in the coating material 5 that coats the second positive electrode active material particles 4 relative to the second positive electrode active material particles 4 is, for example, 0.01% or less, and may also be 0.006% or less. The phosphorus compound attached to the surface of the first positive electrode active material particles 3 and the phosphorus compound attached to the second positive electrode active material particles 4 may have the same composition or different compositions.
[0054] The positive electrode active material layer 2 may contain other materials such as a conductive additive, an ion conductor, and a binder.
[0055] Conductive additives and ion conductors are used to reduce the resistance of the electrodes. Examples of conductive additives include carbon materials and conductive polymer compounds. Examples of carbon materials include carbon black, graphite, acetylene black, carbon nanotubes, carbon nanofibers, graphene, fullerene, and graphite oxide. Examples of conductive polymer compounds include polyaniline, polypyrrole, and polythiophene. At least one selected from these conductive additives can be used.
[0056] Examples of ionic conductors include gel electrolytes such as polymethyl methacrylate and polymethyl methacrylate, organic solid electrolytes such as polyethylene oxide, and Li7La3Zr2O 12 At least one selected from these ion conductors can be used.
[0057] Binders are used to improve the binding properties of the materials that make up the electrode. Examples of binders include polymeric materials such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, polytetrafluoroethylene, carboxymethyl cellulose, polyacrylic acid, styrene-butadiene copolymer rubber, polypropylene, polyethylene, and polyimide. At least one selected from these binders can be used.
[0058] The positive electrode current collector 1 is a sheet or film made of a metal material such as aluminum, an aluminum alloy, stainless steel, titanium, or a titanium alloy. The sheet or film may be porous or non-porous. Examples of the sheet or film include metal foil and metal mesh. A carbon material may be applied to the surface of the positive electrode current collector 1 as a conductive auxiliary material.
[0059] The positive electrode 10 according to the first embodiment can be produced, for example, by the following method.
[0060] First positive electrode active material particles 3 and second positive electrode active material particles 4 are prepared. The surfaces of first positive electrode active material particles 3 are coated with coating material 5 containing a phosphorus compound. The coating method is not particularly limited, but may be performed, for example, by the following procedure.
[0061] Next, a solution containing a phosphorus compound and a solvent is prepared.
[0062] As described above, the phosphorus compound includes a structure represented by chemical formula (1). The phosphorus compounds in the raw material stage are in a state before they can condense with each other and / or bond with the positive electrode active material, and can be distinguished from the phosphorus compounds contained in the positive electrode active material layer 2. The phosphorus compounds in the raw material stage include, for example, a structure represented by chemical formula (2).
[0063]
[0064] In chemical formula (2), R 7 is a hydrogen atom, -(CH2) k1 Y1 represents a trimethylsilyl group or a triethylsilyl group. 6 and R 8 are each independently -OR or -(CH2) k2 Y2 represents a hydrogen atom, -(CH2) k3 Y3 represents a trimethylsilyl group or a triethylsilyl group. k1 and k3 are each independently a natural number from 1 to 3. k2 is an integer from 0 to 15. Y1, Y2, and Y3 are each independently a hydrogen atom, a hydroxyl group, an amino group, a carboxy group, a cyano group, or a fluorine atom.
[0065] The phosphorus compound in the raw material stage may include at least one selected from the group consisting of silyl phosphite and phosphoric acid. The silyl phosphite may be TMSP.
[0066] As the solvent, cyclic carbonate esters, chain carbonate esters, cyclic carboxylic acid esters, etc. are used. Examples of cyclic carbonate esters include propylene carbonate (PC). Examples of chain carbonate esters include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Examples of cyclic carboxylic acid esters include γ-butyrolactone (GBL), γ-valerolactone (GVL), etc. One type of solvent may be used alone, or two or more types may be used in combination.
[0067] The concentration of the phosphorus compound in the solution may be from 0.1% to 20% by weight.
[0068] Next, the prepared solution is brought into contact with the first positive electrode active material particles 3. This contact may be performed by immersing the particles in the solution. Alternatively, the solution may be applied to the particles, for example, by spraying. For example, the positive electrode active material containing the particles may be formed into a layer, and the solution may be applied onto the layer or impregnated into the solution, thereby bringing the positive electrode active material particles into contact with the solution. The contact time with the solution is, for example, 15 minutes or more and 120 minutes or less, and the temperature is, for example, 20°C or more and 60°C or less.
[0069] The positive electrode active material particles that have been brought into contact with the solution are vacuum-dried. The vacuum drying time may be, for example, 5 minutes to 48 hours. In this manner, first positive electrode active material particles 3 are obtained, at least a portion of whose surface is coated with coating material 5 containing a phosphorus compound. Vacuum drying refers to drying at a pressure lower than atmospheric pressure.
[0070] After contact with the solution, the first positive electrode active material particles 3 may be washed before vacuum drying. For example, washing is performed using a solvent. The solvent used for washing may be the solvent used in the solution containing the phosphorus compound and the solvent, such as DMC. This makes it possible to remove by-products such as decomposition products of the phosphorus compound. This makes it possible to suppress gas generation in the positive electrode due to a reaction between the by-products and the electrolyte.
[0071] Next, a positive electrode slurry is prepared containing first positive electrode active material particles 3 at least partly coated with the above-obtained coating material 5 containing a phosphorus compound, and second positive electrode active material particles 4. For example, the positive electrode slurry is prepared by dispersing the positive electrode active material particles, a binder, and a conductive additive in a dispersion medium.
[0072] The positive electrode active material layer 2 is formed by applying the positive electrode slurry to the positive electrode current collector 1. Specifically, the positive electrode slurry is applied to the positive electrode current collector 1 to form a coating film. The positive electrode active material layer 2 is obtained by removing the dispersion medium from the coating film. One method for removing the dispersion medium is to heat the coating film. As the dispersion medium, for example, N-methyl-2-pyrrolidone (NMP) or the like is used.
[0073] In this manner, the positive electrode 10 according to the first embodiment is obtained.
[0074] (Embodiment 2) A nonaqueous electrolyte secondary battery according to embodiment 2 includes the positive electrode, negative electrode, and electrolyte according to embodiment 1. By using the positive electrode according to embodiment 1, the characteristics of the nonaqueous electrolyte secondary battery can be improved.
[0075] FIG. 2 is a schematic cross-sectional view showing an example of a nonaqueous electrolyte secondary battery according to Embodiment 2. The secondary battery 100 includes a container 11 and an electrode group 14. The electrode group 14 has a wound structure. The electrode group 14 is housed in the container 11. The electrode group 14 includes a positive electrode 15, a negative electrode 16, and a pair of separators 17. The electrode group 14 is impregnated with an electrolyte. The opening of the container 11 is closed by a sealing plate 12. The positive electrode 15 includes a positive electrode current collector 15a and a positive electrode active material layer 15b. One end of a positive electrode lead 15c is connected to the positive electrode 15. The other end of the positive electrode lead 15c is connected to the back surface of the sealing plate 12. An insulating packing 13 is disposed around the sealing plate 12. The negative electrode 16 includes a negative electrode current collector 16a and a negative electrode active material layer 16b. One end of a negative electrode lead 16c is connected to the negative electrode 16. The other end of the negative electrode lead 16c is connected to the bottom surface of the container 11. An insulating ring 18 is disposed on each of the upper and lower surfaces of the electrode group 14.
[0076] Each component of the secondary battery 100 will be specifically described below.
[0077] The positive electrode 15 is the positive electrode according to the first embodiment.
[0078] The negative electrode current collector 16a may be a sheet or film made of a metal material such as stainless steel, nickel, copper, or an alloy thereof. The sheet or film may be porous or non-porous. Examples of the sheet or film include metal foil and metal mesh. A carbon material such as carbon may be applied to the surface of the negative electrode current collector 16a as a conductive auxiliary material.
[0079] The negative electrode active material layer 16b includes a negative electrode active material. The negative electrode active material can be a material capable of absorbing and releasing lithium ions. The negative electrode active material includes, for example, at least one selected from the group consisting of carbon materials and materials capable of forming an alloy with lithium. Examples of carbon materials include graphite. Examples of materials capable of forming an alloy with lithium include silicon, silicon-containing oxides, tin, zinc alloys, bismuth, and germanium. One type selected from these negative electrode active materials may be used, or two or more types may be used in combination.
[0080] The negative electrode active material layer 16b may contain at least one selected from the group consisting of graphite and silicon as the negative electrode active material. The negative electrode active material layer 16b may contain only graphite as the negative electrode active material. Graphite is recommended because it is resistant to deterioration even when repeatedly charged and discharged at a deep depth. Carbon materials other than graphite may also be used as the negative electrode active material. Silicon exhibits a larger capacity than graphite and is therefore advantageous for increasing the capacity of the secondary battery 100.
[0081] The negative electrode active material layer 16b may contain other materials such as a conductive additive, an ion conductor, a binder, etc. Materials that can be used as the conductive additive, the ion conductor, and the binder in the positive electrode active material layer 15b can also be used in the negative electrode active material layer 16b.
[0082] The electrolyte is a non-aqueous electrolyte impregnated into the positive electrode 15, the negative electrode 16, and the separator 17. The electrolyte may fill the internal space of the container 11. The electrolyte allows lithium ions to move between the positive electrode 15 and the negative electrode 16.
[0083] The electrolyte may contain a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. The concentration of the lithium salt in the electrolyte may be, for example, 0.5 mol / L or more and 2 mol / L or less. By controlling the lithium salt concentration within the above range, an electrolyte having excellent ionic conductivity and appropriate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.
[0084] Examples of non-aqueous solvents that can be used include cyclic carbonates, chain carbonates, cyclic ethers, chain ethers, cyclic esters, chain esters, fluorine-containing solvents, and nitriles. Examples of cyclic carbonates include ethylene carbonate, propylene carbonate, and butylene carbonate. Examples of chain carbonates include dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate. Examples of cyclic ethers include tetrahydrofuran, 1,4-dioxane, and 1,3-dioxolane. Examples of chain ethers include 1,2-dimethoxyethane and 1,2-diethoxyethane. Examples of cyclic esters include γ-butyrolactone. Examples of chain esters include methyl acetate. Examples of fluorine-containing solvents include fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, fluoroethyl methyl carbonate, and fluorodimethylene carbonate. Examples of nitriles include acetonitrile. At least one selected from these non-aqueous solvents can be used.
[0085] Examples of lithium salts that can be used include lithium hexafluorophosphate (LiPF), lithium tetrafluoroborate (LiBF), lithium perchlorate (LiClO), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bisperfluoroethylsulfonylimide (LiN(SO2C2F5)2), LiAsF6, LiCF3SO3, and lithium difluoro(oxalato)borate. One selected from these electrolyte salts may be used, or two or more may be used in combination.
[0086] The separator 17 has lithium ion conductivity. The material of the separator 17 is not particularly limited as long as it allows lithium ions to pass through. The material of the separator 17 can be at least one selected from the group consisting of a gel electrolyte, an ion exchange resin membrane, a semipermeable membrane, and a porous membrane. Making the separator 17 from these materials can adequately ensure the safety of the secondary battery 100. Examples of gel electrolytes include gel electrolytes containing fluororesins such as PVdF. Examples of ion exchange resin membranes include cation exchange membranes and anion exchange membranes. Examples of porous membranes include porous membranes made of polyolefin resins and porous membranes containing glass paper obtained by weaving glass fibers into nonwoven fabric.
[0087] The container 11 is made of a metal such as aluminum or stainless steel, and may have a cylindrical shape or a rectangular tube shape.
[0088] The electrode group 14 may be wound into a cylindrical shape or an oval shape.
[0089] The shape of the secondary battery 100 is not particularly limited. In the present disclosure, as an example of the structure of the nonaqueous electrolyte secondary battery according to embodiment 2, the configuration example shown in FIG. 2 is described, i.e., a secondary battery in which an electrode group formed by winding a positive electrode and a negative electrode with a separator interposed therebetween and an electrolyte solution are housed in an exterior body. However, the secondary battery according to the present disclosure is not limited to this configuration example. The secondary battery according to the present disclosure may have any shape, such as a cylindrical shape, a prismatic shape, a coin shape, a button shape, or a laminate shape. Furthermore, as the electrode group in the secondary battery according to the present disclosure, instead of a wound-type electrode group, an electrode group of another shape, such as a stacked-type electrode group formed by stacking a positive electrode and a negative electrode with a separator interposed therebetween, may be used.
[0090] The application of the positive electrode of the present disclosure is not limited to the secondary battery 100. In addition to lithium secondary batteries, the positive electrode of the present disclosure can be applied to various secondary batteries such as sodium secondary batteries and magnesium secondary batteries.
[0091] (Other Embodiments) (Additional Notes) The above description of the embodiments discloses the following techniques.
[0092] (Technology 1) A positive electrode comprising: first positive electrode active material particles; second positive electrode active material particles; and a phosphorus compound attached to at least a portion of a surface of the first positive electrode active material particles; wherein the first positive electrode active material particles are particles formed by aggregating 51 or more and 20,000 or less first primary particles; and the second positive electrode active material particles are particles formed by aggregating one second primary particle or 2 or more and 50 or less second primary particles; and wherein a mass ratio of P contained in the phosphorus compound attached to a surface of the second positive electrode active material particles to P contained in the phosphorus compound attached to a surface of the first positive electrode active material particles is 0 or more and 0.5 or less.
[0093] This configuration can suppress side reactions at the positive electrode while reducing an increase in the internal resistance of the battery.
[0094] (Technology 2) The positive electrode according to Technology 1, wherein the first primary particles have an average particle size of 50 nm or more and 5 μm or less, and the second primary particles have an average particle size of 0.5 μm or more and 7 μm or less. With this configuration, it is possible to reduce an increase in the internal resistance of the battery while suppressing side reactions in the positive electrode.
[0095] (Technology 3) The positive electrode according to Technology 1 or 2, wherein the first positive electrode active material particles have an average particle diameter of 3 μm or more and 20 μm or less, and the second positive electrode active material particles have an average particle diameter of 0.5 μm or more and 7 μm or less. With this configuration, it is possible to reduce an increase in the internal resistance of the battery while suppressing side reactions in the positive electrode.
[0096] (Technology 4) The positive electrode according to any one of Technologies 1 to 3, wherein the average particle size of the first primary particles is smaller than the average particle size of the second primary particles. With this configuration, it is possible to suppress side reactions in the positive electrode and reduce an increase in the internal resistance of the battery.
[0097] (Technology 5) The positive electrode according to any one of Technologies 1 to 4, wherein the second positive electrode active material particle is a single single crystal particle. With this configuration, it is possible to suppress side reactions in the positive electrode and reduce an increase in the internal resistance of the battery.
[0098] (Technology 6) The positive electrode according to any one of Technologies 1 to 5, wherein the average particle diameter of the first positive electrode active material particles is larger than the average particle diameter of the second positive electrode active material particles. This configuration can suppress side reactions in the positive electrode while reducing an increase in the internal resistance of the battery. Furthermore, the second positive electrode active material particles can be arranged to fill gaps between the first positive electrode active material particles, thereby improving battery capacity.
[0099] (Technology 7) The positive electrode according to any one of Techniques 1 to 6, wherein the average particle diameter of the first positive electrode active material particles is larger than the average particle diameter of the second positive electrode active material particles, and the average particle diameter of the first primary particles is smaller than the average particle diameter of the second primary particles. This configuration can further reduce an increase in the internal resistance of the battery while suppressing side reactions in the positive electrode. Furthermore, the second positive electrode active material particles can be arranged to fill the gaps between the first positive electrode active material particles, thereby improving battery capacity.
[0100] (Technology 8) The positive electrode according to any one of Technologies 1 to 7, wherein the mass ratio of the first positive electrode active material particles to the second positive electrode active material particles is 0.67 or more and 4.0 or less. With this configuration, it is possible to further reduce an increase in the internal resistance of the battery while suppressing side reactions in the positive electrode. In addition, it is possible to improve the battery capacity and charge / discharge efficiency.
[0101] (Technology 9) The positive electrode according to any one of Technologies 1 to 8, wherein the phosphorus compound contains a P—O—P bond. With this configuration, side reactions at the positive electrode can be further suppressed.
[0102] (Technology 10) The positive electrode according to any one of Technologies 1 to 9, wherein the phosphorus compound includes a structure represented by chemical formula (1). According to this configuration, since the phosphorus compound has such a structure, it is relatively stable even under a high-voltage environment, and therefore, even when the upper limit voltage of the battery is high, side reactions in the positive electrode can be sufficiently suppressed. In addition, the effect of suppressing side reactions can be maintained for a longer period of time. In the chemical formula (1), n1 and n2 are each independently an integer of 0 or more, and R 1 , R 2 , R 4 , and R5 are each independently -OR or -(CH2) m1 represents X1, and R 3 and R each independently represent a direct bond to the first positive electrode active material particle, a hydrogen atom, or —(CH) m2 X2 represents a trimethylsilyl group or a triethylsilyl group, m1 represents an integer of 0 to 15, m2 represents a natural number of 1 to 3, X1 and X2 each independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxy group, a cyano group, or a fluorine atom, R 2 If there are multiple R 2 are independent of each other, and R 4 If there are multiple R 4 are independent of each other.
[0103] (Technology 11) In the chemical formula (1), R 1 , R 2 , R 4 , and R 5 are each independently -OR, and R 3 and R each independently represent a direct bond to the first positive electrode active material particle, a hydrogen atom, or a trimethylsilyl group. This configuration can further suppress side reactions in the positive electrode of the battery. Furthermore, it can further reduce an increase in internal resistance.
[0104] (Technology 12) A nonaqueous electrolyte secondary battery comprising: the positive electrode according to any one of claims 1 to 11; a negative electrode; and an electrolyte.
[0105] This configuration can improve the characteristics of the nonaqueous electrolyte secondary battery.
[0106] The present disclosure will be described in more detail below using examples. The following examples are merely examples of embodiments, and are not intended to limit the scope of the present disclosure.
[0107] Example 1 Tristrimethylsilyl phosphate (TMSP) was added to a solvent containing dimethyl carbonate (DMC) as the main component to obtain a TMSP solution having a TMSP concentration of 2% by mass.
[0108] Lithium nickel manganese oxide particles (average particle diameter 17 μm) were prepared as first positive electrode active material particles. These particles were formed by agglomeration of approximately 4,000 primary particles with an average particle diameter of 1 μm. The lithium nickel manganese oxide was a layered Li-containing oxide with an atomic ratio of Ni:Mn = 8:2. 4 g of the first positive electrode active material particles were immersed in a TMSP solution and stirred at room temperature for 1 hour. After stirring, the first positive electrode active material particles were recovered by filtration. The recovered first positive electrode active material particles were introduced into the above-mentioned DMC-based solvent and stirred for 5 minutes, and the solvent was removed by filtration to wash the first positive electrode active material particles. After repeating the washing twice, the first positive electrode active material particles were vacuum-dried at 60°C for 10 hours. In this way, the surfaces of the first positive electrode active material particles were coated with a phosphorus compound.
[0109] Lithium nickel manganese oxide particles (average particle diameter 5 μm) were prepared as the second positive electrode active material particles. These particles were formed by agglomerating four primary particles with an average particle diameter of 3 μm. The lithium nickel manganese oxide had the same composition as the first positive electrode active material particles. The surface-coated first positive electrode active material particles, second positive electrode active material particles, acetylene black (AB), and polyvinylidene fluoride (PVDF) were mixed with N-methyl-2-pyrrolidone (NMP) and stirred to prepare a positive electrode slurry. The mass ratio of the first positive electrode active material particles to the second positive electrode active material particles was 2.5:1. The mass ratio of these materials in the positive electrode active material layer was positive electrode active material:AB:PVDF=96:2:2.
[0110] The positive electrode slurry was applied to the surface of an aluminum foil (1.45 cm × 1.45 cm), the coating was dried, and then rolled to form a positive electrode active material layer. In this way, the positive electrode of Example 1 was obtained. The mass ratio of the phosphorus compound coating the surfaces of the second positive electrode active material particles to the phosphorus compound coating the surfaces of the first positive electrode active material particles was 0.
[0111] An evaluation cell for Example 1 was fabricated using the positive electrode, Li metal foil as a counter electrode, a separator, and an electrolyte solution from Example 1. A PP / PE / PP three-layer resin separator was used as the separator. The concentration of LiPF in the electrolyte solution was 1.3 mol / L. The solvent for the electrolyte solution was a mixed solvent of fluoroethylene carbonate (FEC), ethylene carbonate (EC), and DMC in a volume ratio of FEC:EC:DMC = 5:20:75.
[0112] Reference Example 1 A positive electrode of Reference Example 1 was produced in the same manner as in Example 1, except that the surfaces of the first positive electrode active material particles were not coated with a phosphorus compound. An evaluation cell of Reference Example 1 was produced in the same manner as in Example 1 using the positive electrode of Reference Example 1.
[0113] Reference Example 2 The surfaces of second positive electrode active material particles were coated with a phosphorus compound in the same manner as the first positive electrode active material particles in Example 1. A positive electrode of Reference Example 2 was produced in the same manner as Example 1, except that the surface-coated second positive electrode active material particles were used. An evaluation cell of Reference Example 2 was produced in the same manner as Example 1, using the positive electrode of Reference Example 2.
[0114] Reference Example 3 The surfaces of the first positive electrode active material particles were not coated with a phosphorus compound. The surfaces of the second positive electrode active material particles were coated with a phosphorus compound in the same manner as the first positive electrode active material particles of Example 1. A positive electrode of Reference Example 3 was produced in the same manner as Example 1, except that first positive electrode active material particles not coated with a phosphorus compound and second positive electrode active material particles coated with a phosphorus compound were used. An evaluation cell of Reference Example 3 was produced in the same manner as Example 1, using the positive electrode of Reference Example 3.
[0115] [Battery Evaluation] The evaluation cells of Example 1 and Reference Examples 1 to 3 were charged at a constant current of 0.1 C at an ambient temperature of 25°C until the voltage reached 4.5 V, and then discharged at a constant current of 0.1 C until the voltage reached 2.5 V. This charge-discharge cycle was repeated twice. Here, the current value at which the time required to reach the lower limit voltage from the upper limit voltage during constant current discharge is defined as 1 C. Then, a trickle test was performed according to the following procedure. The cells were charged at a constant current of 0.2 C until the voltage reached 4.5 V, and then trickle charged at an ambient temperature of 55°C, maintaining a voltage of 4.5 V for three days. Then, the cells were discharged at a current of 0.1 C at an ambient temperature of 25°C.
[0116] The evaluation results are shown in Table 1. The internal resistance is a relative value when the internal resistance of Reference Example 1 is set to 100%, and was calculated from the discharge curve during the initial charge and discharge. The amount of gas generated is the amount of gas generated in the battery during the trickle test, and was calculated by {(volume of battery after trickle test) - (volume of battery before trickle test)} / (mass of positive electrode active material). The relative values when the amount of gas generated in Example 1 is set to 100% are shown in Table 1. The mass of the positive electrode active material is the sum of the masses of the first positive electrode active material particles and the second positive electrode active material particles.
[0117]
[0118] (Discussion) From Table 1, it can be seen that the amount of gas generated in Example 1 was reduced to less than half that of Reference Example 1. In Reference Example 2, the amount of gas generated was reduced compared to Reference Example 1, but the internal resistance was significantly increased compared to Example 1. In Example 1, the amount of gas generated was reduced to the same extent as in Reference Example 2, while the increase in internal resistance was reduced by about 30% compared to Reference Example 2. In Example 1, the amount of gas generated was reduced compared to Reference Example 3, and the increase in internal resistance was also suppressed. From the above, it can be seen that the positive electrode of the present disclosure was able to significantly suppress side reactions in the positive electrode without significantly increasing the internal resistance.
[0119] The technology of the present disclosure is useful for, for example, lithium ion secondary batteries.
Claims
1. A positive electrode comprising: first positive electrode active material particles; second positive electrode active material particles; and a phosphorus compound attached to at least a portion of a surface of the first positive electrode active material particles; the first positive electrode active material particles are particles formed by agglomeration of 51 or more and 20,000 or less first primary particles; the second positive electrode active material particles are one second primary particle or particles formed by agglomeration of 2 or more and 50 or less second primary particles; and a mass ratio of P contained in the phosphorus compound attached to a surface of the second positive electrode active material particles to P contained in the phosphorus compound attached to a surface of the first positive electrode active material particles is 0 or more and 0.5 or less.
2. The positive electrode according to claim 1, wherein the first primary particles have an average particle size of 50 nm or more and 5 μm or less, and the second primary particles have an average particle size of 0.5 μm or more and 7 μm or less.
3. The positive electrode according to claim 1, wherein the first positive electrode active material particles have an average particle diameter of 3 μm or more and 20 μm or less, and the second positive electrode active material particles have an average particle diameter of 0.5 μm or more and 7 μm or less.
4. The positive electrode according to claim 1, wherein the average particle size of the first primary particles is smaller than the average particle size of the second primary particles.
5. The positive electrode according to claim 1, wherein the second positive electrode active material particle is a single single crystal particle.
6. The positive electrode according to claim 1, wherein the average particle size of the first positive electrode active material particles is larger than the average particle size of the second positive electrode active material particles.
7. The positive electrode according to claim 1, wherein an average particle diameter of the first positive electrode active material particles is larger than an average particle diameter of the second positive electrode active material particles, and an average particle diameter of the first primary particles is smaller than an average particle diameter of the second primary particles.
8. The positive electrode according to claim 1, wherein a mass ratio of the first positive electrode active material particles to the second positive electrode active material particles is 0.67 or more and 4.0 or less.
9. The positive electrode according to claim 1, wherein the phosphorus compound includes a P-O-P bond.
10. The positive electrode according to claim 1, wherein the phosphorus compound includes a structure represented by chemical formula (1). n1 and n2 are each independently an integer of 0 or more; R 1 , R 2 , R 4 , and R 5 are each independently -OR or -(CH2) m1 represents X1, 3 and R each independently represent a direct bond to the first positive electrode active material particle, a hydrogen atom, -(CH) m2 X2 represents a trimethylsilyl group or a triethylsilyl group, m1 represents an integer of 0 to 15, m2 represents a natural number of 1 to 3, X1 and X2 each independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxy group, a cyano group, or a fluorine atom, R 2 If there are multiple R 2 are independent of each other, R 4 If there are multiple R 4 are independent of each other.
11. In the above chemical formula (1), R 1 , R 2 , R 4 , and R 5 each independently represents -OR; 3 and R each independently represent a direct bond to the first positive electrode active material particle, a hydrogen atom, or a trimethylsilyl group.
12. A non-aqueous electrolyte secondary battery comprising: the positive electrode according to any one of claims 1 to 11; a negative electrode; and an electrolyte.
Citation Information
Patent Citations
Positive electrode active material for lithium secondary cell, positive electrode for lithium secondary cell, lithium secondary cell, and methods for manufacturing same
WO2017126276A1
Nonaqueous secondary battery
JP2002216768A
Electrode for battery, manufacturing method thereof, and battery
JP2009283353A
Nonaqueous electrolyte battery and battery pack
JP2012199145A
Lithium ion secondary battery
JP2018097945A