Blank, method for manufacturing structural member, and structural member

The described blank for hot stamping, with a thin steel plate having higher emissivity and a thicker plate, addresses the issue of non-uniformity in hot-stamped structural members by ensuring uniform hardenability and improved shock absorption, thus enhancing the performance and accuracy of large annular components.

WO2024225327A1PCT designated stage expired Publication Date: 2024-10-31NIPPON STEEL CORPORATION

Patent Information

Application Number
PCT/JP2024/016110
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

In hot stamping processes for manufacturing structural members, such as automobile body components, the integration of steel plates with different thicknesses can lead to non-uniform hardness and stress distribution, resulting in reduced shock absorption performance and dimensional accuracy, especially in large annular structural members.

Method used

A blank for hot stamping is designed with a plurality of steel plates arranged to form an annular shape, where the first steel plate has the smallest thickness and a higher emissivity than the second steel plate, allowing for quicker temperature rise and longer high-temperature retention, thereby improving hardenability and uniformity, and reducing the thickness ratio between the minimum and maximum plates to maintain corrosion resistance and weldability.

Benefits of technology

This approach enhances the hardness uniformity and impact absorption performance of the structural member, reduces twisting and dimensional inaccuracies, and secures a process window for manufacturing, even with large annular members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016110_31102024_PF_FP_ABST
    Figure JP2024016110_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A blank (20, 20A) for hot stamping is provided with a plurality of steel sheets. The plurality of steel sheets are arranged and joined with one another so as to form a ring shape when seen in a plan view of the blank (20, 20A). The plurality of steel sheets include a first steel sheet (21) and a second steel sheet (22). The first steel sheet (21) has the lowest sheet thickness (tmin) among the plurality of steel sheets. The second steel sheet (22) has a sheet thickness which is greater than the sheet thickness (tmin) of the first steel sheet (21). The first steel sheet (21) is configured in a manner such that the emissivity of at least one surface of the two surfaces thereof is greater than the emissivity of the two surfaces of the second steel sheet (22).
Need to check novelty before this filing date? Find Prior Art

Description

Blank, manufacturing method of structural member, and structural member

[0001] The present disclosure relates to a blank for hot stamping, a method for manufacturing a structural member using the blank, and the structural member.

[0002] Structures such as automobile bodies are formed from multiple structural members. Structural members are manufactured, for example, by press-forming a blank. To ensure high strength and good dimensional accuracy, structural members are sometimes manufactured by a press-forming method called hot stamping. Hot stamping is a technique in which a blank, which is a steel plate, is heated to a temperature in the austenite range, and then press-formed using a die. The blank is then held in the die and quenched by removing heat (rapid cooling).

[0003] Patent Document 1 discloses a steel sheet (blank) for hot stamping. The steel sheet of Patent Document 1 has a surface treatment film on the entire surface of at least one surface, the surface treatment film having an emissivity of 60% or more at a wavelength of 8.0 μm at 25° C. According to Patent Document 1, the surface of the steel sheet to which the surface treatment film is applied has an increased emissivity, and the heat transfer effect by radiation is large. Therefore, when the steel sheet is heated during hot stamping, the steel sheet undergoes a transformation into an austenite phase, where the metal structure of the steel sheet is transformed into an austenite phase. c3 Patent Document 1 describes that this makes it possible to shorten the heating time and improve the productivity of hot stamped members.

[0004] Patent Document 2 discloses a method for manufacturing an automobile body side structural frame from a plurality of blanks. In Patent Document 2, the plurality of blanks are joined to form a composite blank, and the composite blank is press-formed to manufacture the body side structural frame. Patent Document 2 also describes hot forming (hot stamping) the composite blank.

[0005] International Publication No. 2022 / 215229 Special Publication No. 2021-528248

[0006] In recent years, integrating two or more components from the blank stage has been considered to simplify the manufacturing process of structures. Patent Document 2, for example, discloses a method of hot stamping a composite blank having an annular shape in a plan view to form an annular body side structural frame integrated with pillars, rockers, and the like. However, if the composite blank contains steel sheets of different thicknesses, the performance of the resulting structural component may be degraded. Specifically, during hot stamping, the blank is heated, for example, in a heating furnace until its microstructure is austenitized, and then formed using a die. However, because thinner steel sheets are more easily cooled than thicker steel sheets, the portions of the blank where the thinner steel sheets are located may begin to transform to ferrite before the blank is removed from the heating furnace and forming begins, potentially resulting in poor hardenability. Partially degraded hardenability of the blank may result in non-uniform hardness in the structural component formed from the blank, potentially reducing its impact absorption performance. Furthermore, partial degraded hardenability may result in non-uniform stress in the structural component. This can lead to twisting, particularly in the case of annular structural members, and can lead to a deterioration in dimensional accuracy. The deterioration in impact absorption performance (crash resistance performance) due to deterioration in hardenability or dimensional accuracy becomes more pronounced as the annular structural member becomes larger.

[0007] An object of the present disclosure is to provide a hot stamping blank that can improve the performance of an annular structural component, particularly a large annular structural component, when the component is formed from a steel plate having a thickness smaller than that of other steel plates.

[0008] A hot stamping blank according to the present disclosure includes a plurality of steel plates. The plurality of steel plates are arranged and joined to form an annular shape in a plan view of the blank. The plurality of steel plates include a first steel plate and a second steel plate. The first steel plate has the smallest thickness among the plurality of steel plates. The second steel plate has a thickness greater than that of the first steel plate. The first steel plate is configured so that the emissivity of at least one of both surfaces of the first steel plate is greater than the emissivity of both surfaces of the second steel plate.

[0009] According to the hot stamping blank of the present disclosure, when an annular structural component, particularly a large annular structural component, is formed using a steel plate having a smaller plate thickness than other steel plates, the performance of the component can be improved.

[0010] FIG. 1 is a plan view of a structural member according to the first embodiment. FIG. 2 is a cross-sectional view taken along line II-II of FIG. 1. FIG. 3A is a schematic view illustrating a manufacturing method for a structural member according to the first embodiment, showing a blank according to the first embodiment. FIG. 3B is a schematic view illustrating a manufacturing method for a structural member according to the first embodiment, showing a blank according to the first embodiment. FIG. 3C is a schematic view illustrating a manufacturing method for a structural member according to the first embodiment, showing a blank according to the first embodiment. FIG. 3D is a schematic view illustrating a manufacturing method for a structural member according to the first embodiment, showing a blank according to the first embodiment. FIG. 3E is a schematic view illustrating a manufacturing method for a structural member according to the first embodiment. FIG. 3F is a schematic view illustrating a manufacturing method for a structural member according to the first embodiment. FIG. 3G is a schematic view illustrating a manufacturing method for a structural member according to the first embodiment. FIG. 4 is a cross-sectional view of a structural member manufactured by the manufacturing method according to the first embodiment. FIG. 5 is a plan view of a blank according to a second embodiment. FIG. 6 is a cross-sectional view taken along line VI-VI of FIG. 5. FIG. 7 is a plan view of a structural member according to the second embodiment. FIG. 8 is a plan view of a structural member according to a modification of each embodiment. FIG. 9A is a diagram showing a division pattern of a structural member in the first embodiment. FIG. 9B is a diagram showing another division pattern of a structural member in the first embodiment. FIG. 9C is a diagram showing yet another division pattern of a structural member in the first embodiment. FIG. 9D is a diagram showing yet another division pattern of a structural member in the first embodiment. FIG. 9E is a diagram showing yet another division pattern of a structural member in the first embodiment. FIG. 9F is a diagram showing yet another division pattern of a structural member in the first embodiment. FIG. 9G is a diagram showing yet another division pattern of a structural member in the first embodiment. FIG. 10A is a diagram showing a division pattern of a structural member in the second embodiment. FIG. 10B is a diagram showing another division pattern of a structural member in the second embodiment. FIG. 10C is a diagram showing yet another division pattern of a structural member in the second embodiment. FIG. 10D is a diagram showing yet another division pattern of a structural member in the second embodiment.

[0011] A hot stamping blank according to an embodiment includes a plurality of steel plates. The plurality of steel plates are arranged and joined to form an annular shape in a plan view of the blank. The plurality of steel plates include a first steel plate and a second steel plate. The first steel plate has the smallest thickness among the plurality of steel plates. The second steel plate has a thickness greater than that of the first steel plate. The first steel plate is configured so that the emissivity of at least one of both surfaces of the first steel plate is greater than the emissivity of both surfaces of the second steel plate (first configuration).

[0012] The blank according to the first configuration includes a first steel plate having a minimum thickness and a second steel plate having a thickness greater than that of the first steel plate. The emissivity of at least one surface of the first steel plate is greater than the emissivity of both surfaces of the second steel plate. This allows for an increased heating rate of the thin-walled portion of the first steel plate when the blank is heated during hot stamping. Therefore, the first steel plate can be heated to the austenite temperature more quickly, ensuring a longer holding time for the first steel plate at that temperature. This allows for coarsening of austenite grains in the first steel plate. As a result, the ferrite transformation region (ferrite nose) in the CCT diagram shifts to the long-time side, delaying the onset of ferrite transformation in the first steel plate after heating of the blank is completed. This allows blank forming to begin while maintaining the microstructure of the first steel plate in the austenite phase. In other words, the hardenability of the thin-walled first steel plate can be improved.

[0013] In the blank according to the first configuration, the hardenability of the first steel plate having a smaller thickness is improved, and therefore the first steel plate can be well hardened when a structural component is formed from the blank by hot stamping. This facilitates uniform hardness in the structural component, thereby preventing partial reductions in the structural component's strength. Furthermore, because uneven stress is less likely to occur in the structural component, twisting is less likely to occur even when the formed structural component is annular, ensuring good dimensional accuracy in the structural component. Therefore, when an annular structural component, particularly a large annular structural component, including a first steel plate having a smaller thickness than the second steel plate is formed from the blank, poor strength and dimensional accuracy of the structural component can be reduced, and the impact absorption performance (crash resistance) of the structural component can be improved.

[0014] In the blank according to the first configuration, the emissivity of the first steel sheet with the minimum thickness is higher than that of the second steel sheet with a relatively large thickness. In this case, the first steel sheet heats up faster than the second steel sheet, and the high-temperature holding time of the first steel sheet, i.e., the time from when the first steel sheet reaches the austenite temperature range until the second steel sheet and the entire blank reach the austenite temperature range, is longer than when the first steel sheet has the same emissivity as the second steel sheet. This reduces non-uniformity in phase transformation due to differences in cooling rates between the steel sheets after the blank is heated. Specifically, the initiation of the austenite-to-ferrite phase transformation in the first steel sheet with the minimum thickness can be delayed, thereby reducing the difference in the phase transformation initiation time between the first steel sheet with the minimum thickness and the other steel sheets. As a result, the hardenability can be made uniform between the first steel sheet with the minimum thickness and the other steel sheets.

[0015] In the first configuration, the first steel plate may have a plate thickness of less than 1.4 mm (second configuration).

[0016] When the thickness of the first steel plate is less than 1.4 mm as in the second configuration, the first steel plate is particularly susceptible to heat dissipation after the heating of the blank is completed, making the hardenability of the first steel plate more likely to deteriorate. However, even when the thickness of the first steel plate is less than 1.4 mm, by increasing the emissivity of at least one surface of the first steel plate compared to the relatively thick second steel plate, it is possible to promote the temperature rise of the first steel plate when the blank is heated during hot stamping, thereby ensuring a long high-temperature holding time for the first steel plate. Therefore, the hardenability of the first steel plate can be improved.

[0017] In the first or second configuration, the first steel sheet may be a plated steel sheet. In this case, the first steel sheet may have a base steel sheet and an aluminum-based plating layer provided on the base steel sheet (third configuration).

[0018] When the first steel sheet is a plated steel sheet having an aluminum-based plating layer, as in the third configuration, the temperature rise rate of the first steel sheet tends to be slow when the blank is heated during hot stamping. Because the aluminum-based plating layer is nearly white, it tends to reflect heat energy and inhibit the temperature rise of the first steel sheet. However, even when the first steel sheet is a plated steel sheet having an aluminum-based plating layer, by increasing the emissivity of at least one surface of the first steel sheet compared to that of a relatively thick second steel sheet, the temperature rise of the first steel sheet can be promoted when the blank is heated during hot stamping. This allows the first steel sheet to be held at a high temperature for a long time, thereby improving the hardenability of the first steel sheet.

[0019] In any of the first to third configurations, at least one surface of the first steel plate may be coated with a coating having an emissivity of 60% or more at a wavelength of 8.0 μm at 25°C (fourth configuration).

[0020] In any one of the first to third configurations, at least one surface of the first steel plate may be coated with a coating, which comprises carbon black, one or more oxides selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide, and a 0 to 0.30 g / m 2The content of carbon black in the coating can be X CB (g / m 2 ), the oxide content is X Oxide (g / m 2 ) and then X CB and X Oxide It is preferable that the following formula (1) (see Patent Document 1) is satisfied (fifth configuration): 118.9≦24280 / {6700 / (100+76×X CB ) + 18000 / (130 + 65 x X Oxide )≦332.0 (1)

[0021] In any one of the first to fifth configurations, the first steel sheet may be a plated steel sheet having a base steel sheet and a plating layer provided on the base steel sheet. In this case, the plate thickness of the first steel sheet may be t min The thickness of the steel plate having the largest thickness among the plurality of steel plates is t max When 1.0<t max / t min It is preferable that the ratio is ≦3.2 (sixth configuration).

[0022] Among the multiple steel plates included in the blank, the smallest plate thickness t min The first steel plate having a maximum plate thickness t max When the difference in thickness between the steel plate and other steel plates having the minimum thickness t is large, it becomes difficult to ensure the process window in the manufacture of structural members. min and maximum plate thickness t max If the difference is large, when the blank is heated during hot stamping, the maximum plate thickness t max While waiting for the steel sheet having the minimum sheet thickness t to reach the austenite temperature range, alloying of the coating layer of the first steel sheet, which has been heated to the austenite temperature range in advance, progresses, and the diffusion layer becomes thick, which may make it impossible to ensure the corrosion resistance or weldability of the first steel sheet due to the coating layer. min Maximum plate thickness t max The ratio is set to 3.2 or less. max The temperature rise rate and minimum plate thickness t of the steel plate minSince the heating rate of the first steel sheet does not deviate too much from the heating rate of the other steel sheet, heating of the other steel sheet can be completed before excessive alloying of the coating layer of the first steel sheet progresses. Therefore, a structural component can be manufactured while maintaining the corrosion resistance or weldability of the first steel sheet, and a process window can be secured in the manufacture of the structural component.

[0023] In any one of the first to sixth configurations, the first steel sheet may be a plated steel sheet having a base steel sheet and a plating layer provided on the base steel sheet. The blank may further include an overlap portion. The overlap portion is formed by overlapping the ends of two adjacent steel sheets among the plurality of steel sheets, the steel sheets being other than the second steel sheet. The overlap portion may have a total thickness of greater than 2.5 mm and not greater than 4.0 mm. In this case, it is preferable that the emissivity of each of the two steel sheets at the surface located outside the overlap portion is greater than the emissivity of both surfaces of the second steel sheet (seventh configuration).

[0024] When a blank has an overlap portion formed by overlapping the ends of two steel sheets, it may be impossible to ensure a process window for manufacturing a structural component. Specifically, if the steel sheets included in the blank have different thicknesses and the total thickness of the overlap portion exceeds 2.5 mm, when the blank is heated during hot stamping, alloying of the coating layer of the first steel sheet with the smallest thickness may progress while waiting for the overlap portion to reach the austenite temperature range, resulting in a thick diffusion layer, making it impossible to ensure the corrosion resistance or weldability of the first steel sheet. Therefore, in the seventh configuration, the emissivity of the outer surface of the overlap portion is increased on each of the two steel sheets forming the overlap portion. This accelerates the temperature rise of the overlap portion, allowing heating of the overlap portion to be completed before excessive alloying of the coating layer of the first steel sheet progresses, thereby enabling the structural component to be manufactured while maintaining the corrosion resistance or weldability of the first steel sheet. In other words, it is easier to ensure a process window for manufacturing a structural component. However, even if the emissivity of the overlapping portion is increased, if the total thickness of the overlapping portion becomes excessively large, it becomes difficult to ensure a process window, so it is preferable that the total thickness of the overlapping portion be 4.0 mm or less.

[0025] A method for manufacturing a structural component according to an embodiment includes the steps of preparing a blank according to any one of the first to seventh configurations, heating a plurality of steel plates included in the blank to a temperature equal to or higher than the austenite transformation completion temperature, and using a mold to form the heated blank into a structural component that is annular in plan view and quenching it (eighth configuration).

[0026] A structural member according to an embodiment includes a member body and a coating. The member body is formed by a plurality of steel plates joined together and has an annular shape in plan view. The plurality of steel plates include a first steel plate having a minimum plate thickness and a second steel plate having a plate thickness greater than that of the first steel plate. The coating is provided on the first steel plate. The coating contains one or more oxides selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide at a concentration of 0.001 g / m 2 or more (ninth configuration).

[0027] A structural member according to an embodiment includes a member body and a coating. The member body is formed by a plurality of steel plates joined together and has an annular shape in plan view. The plurality of steel plates includes a first steel plate having a minimum plate thickness and a second steel plate having a plate thickness greater than that of the first steel plate. The coating is provided on the first steel plate. The coating contains carbon black at a concentration of 0.500 g / m. 2 The following is contained (tenth configuration).

[0028] In the ninth or tenth configuration, the structural member may be a door ring part of an automobile. In this case, the member body may include a front pillar, a center pillar, and a rocker connecting the front pillar and the center pillar (eleventh configuration).

[0029] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In each drawing, the same or equivalent components are designated by the same reference numerals, and the same description will not be repeated.

[0030] <First embodiment> [Structural member] Fig. 1 is a diagram (plan view) of a structural member 10 according to this embodiment, viewed from above in a state where it is placed on a horizontal surface. The structural member 10 is used, for example, in the body of an automobile. The structural member 10 is typically a door ring component of the automobile. In this embodiment, an example in which the structural member 10 is a door ring component will be described.

[0031] The structural member 10 is a hot-stamped member. That is, the structural member 10 is formed by hot stamping (hot press processing) a blank made of multiple steel plates. The structural member 10 includes a member main body 11. The member main body 11 has an annular shape in a plan view of the structural member 10. The member main body 11 includes a front pillar 111, a center pillar 112, and a rocker 113. When the structural member 10 is assembled to the body of an automobile, the center pillar 112 is disposed rearward of the front pillar 111. The center pillar 112 extends generally in the vertical direction of the vehicle body. The front pillar 111 extends toward the center pillar 112. When the structural member 10 is assembled to the body of an automobile, the rocker 113 is disposed below the front pillar 111 and the center pillar 112. The rocker 113 connects the front pillar 111 and the center pillar 112.

[0032] In this embodiment, the member body 11 is formed of a plurality of steel plates 21, 22, and 23 joined together. In the example of FIG. 1 , the front pillar 111 is mainly formed of the steel plates 21 and 22. The center pillar 112 is mainly formed of the steel plate 23. The rocker 113 is also formed of the steel plates 21 and 23.

[0033] FIG. 2 is a cross-sectional view taken along line II-II of FIG. 1 . FIG. 2 shows a cross-section of the structural member 10 cut in the thickness direction at the position of the steel plate 21. As shown in FIG. 2 , the steel plate 21 has an open cross-section. In a cross-sectional view of the structural member 10, the steel plate 21 has, for example, a generally hat-shaped shape. More specifically, the steel plate 21 includes a top plate 211, vertical walls 212 and 213, and flanges 214 and 215. The vertical wall 212 is disposed on the opposite side of the vertical wall 213 with respect to the top plate 211. In a cross-sectional view of the structural member 10, one end of the vertical walls 212 and 213 is connected by the top plate 211. In a cross-sectional view of the structural member 10, the other end of the vertical walls 212 and 213 is connected to flanges 214 and 215, respectively. The flanges 214 and 215 protrude from the vertical walls 212 and 213, respectively, to the outside of the structural member 10.

[0034] In the structural member 10, the width W of the steel plate 21 may be 30 mm or more and 750 mm or less. The height H of the steel plate 21 may be 25 mm or more and 150 mm or less. The width W is the distance from the end of the R on the vertical wall 212 side of the corner portion between the top plate 211 and the vertical wall 212 to the end of the R on the vertical wall 213 side of the corner portion between the top plate 211 and the vertical wall 213 in the cross section of the structural member 10. The height H is the distance from the top plate 211 to the flanges 214, 215 in the plate thickness direction of the top plate 211.

[0035] Although not shown, the other steel plates 22, 23 also have an open cross section similar to the steel plate 21. The steel plates 22, 23 may also have, for example, a generally hat shape in a cross section of the structural member 10. The width of the steel plates 22, 23 may be 15 mm or more and 300 mm or less. The height of the steel plates 22, 23 may be 10 mm or more and 150 mm or less.

[0036] The size of the annular structural member 10 in a plan view is, for example, 1.0 m or more. The size of the structural member 10 may be, for example, 4.0 m or less. The size of the structural member 10 is the length of a line segment connecting any two points on the outer periphery of the structural member 10 that are farthest apart when the structural member 10 is placed on a horizontal surface and viewed vertically.

[0037] 3A to 3G, a method for manufacturing the structural member 10 will be described. The method for manufacturing the structural member 10 according to this embodiment includes the steps of preparing a blank 20, heating the blank 20, and forming the heated blank 20 into the structural member 10.

[0038] 3A , in the preparation step, a blank 20 having a shape obtained by unfolding the structural member 10 is prepared. The blank 20 includes a plurality of steel plates 21, 22, and 23. The steel plates 21, 22, and 23 are arranged and joined together so as to have an annular shape when the blank 20 is viewed from above.

[0039] 3B, 3C, and 3D are cross-sectional views of the blank 20 showing the joints between the steel plates 21, 22, and 23. FIGS. 3B, 3C, and 3D are cross-sectional views taken along lines IIIB-IIIB, IIIC-IIIC, and IIID-IIID in FIG. 3A, respectively. Referring to FIGS. 3B and 3C, the steel plate 21 is butt-joined to each of the steel plates 22 and 23. That is, the end face of the steel plate 21 is joined to the end face of the steel plate 22 while abutting against the end face of the steel plate 22, and the other end face of the steel plate 21 is joined to the end face of the steel plate 23 while abutting against the end face of the steel plate 23. Referring to FIG. 3D, the steel plate 22 is butt-joined to the steel plate 21 as well as the steel plate 23. The end face of the steel plate 22 is joined to the end face of the steel plate 23 while abutting against the end face. The steel plates 21, 22, and 23 are joined by, for example, laser welding. In this embodiment, the blank 20 is a so-called tailor weld blank.

[0040] 3B and 3C, among the steel plates 21, 22, and 23, the steel plate 21 has a minimum plate thickness t min The steel plate 22 has a thickness t min The steel plate 23 has a thickness t min In the present embodiment, the thickness of each of the steel plates 22 and 23 is equal to or greater than the thickness t min In this embodiment, the steel plate 23 has the largest plate thickness t max The steel plate 22 has a thickness t min is larger than the thickness t of the steel plate 23 max Plate thickness t smaller than mid However, the steel plate 22 may have a thickness equal to or greater than that of the steel plate 23. That is, among the steel plates 21, 22, and 23, the steel plate 22 has the maximum thickness t max It can also have:

[0041] Plate thickness t of steel plate 21 min is typically less than 1.4 mm. min The thickness t of the steel plate 21 may be, for example, 0.8 mm or more. min and the thickness t of the steel plate 23 max is 1.0<t max / tmin ≦3.2, and 1.3≦t max / t min It is more preferable that the ratio ≦3.2 is satisfied.

[0042] The minimum thickness t of the blank 20 min The steel plate 21 having the minimum thickness t is configured so that the emissivity of at least one of its two surfaces is greater than the emissivity of both surfaces of the steel plate 22. For example, the emissivity at a wavelength of 8.0 μm at 25° C. is 60% or more on one or both surfaces of the steel plate 21, and less than 60% on both surfaces of the steel plate 22. The emissivity at a wavelength of 8.0 μm at 25° C. on one or both surfaces of the steel plate 21 is more preferably 70% or more, and even more preferably 80% or more. min The difference in emissivity at a wavelength of 8.0 μm at 25°C between the steel sheet 21 having the above-mentioned characteristic and the other steel sheet 22 is preferably greater than 5%, more preferably greater than 10%, and even more preferably greater than 20%. The emissivity can be measured in accordance with JIS R 1801 (2002). In this case, a sample taken from the steel sheet to be measured is placed in a Fourier transform infrared spectrophotometer, and the radiation intensity at a wavelength of 8.0 μm at 25°C is measured to calculate the emissivity. Alternatively, it is also possible to measure the radiation intensity of a target portion at 25°C using a radiation thermometer set to a measurement wavelength of 8.0 μm, and calculate the emissivity from the ratio to the radiation intensity of a blackbody.

[0043] In this embodiment, one surface of the steel plate 21 is covered with a coating 26. On the other hand, the steel plate 22 is not provided with a coating 26. As a result, the emissivity of the one surface of the steel plate 21 is higher than the emissivity of both surfaces of the steel plate 22.

[0044] The coating 26 is, for example, a black coating. For example, the lightness L * Value (CIE 1976 lightness index L defined in JIS Z8781-4 (2013) *If the emissivity at a wavelength of 8.0 μm at 25°C is 60% or more, preferably 70% or more, and more preferably 80% or more, the coating 26 can be determined to be black. The coating 26 may be a carbon-based surface treatment coating (a coating containing carbon (C)). The emissivity at a wavelength of 8.0 μm at 25°C of the coating 26 is 60% or more, preferably 70% or more, and more preferably 80% or more. That is, the emissivity at a wavelength of 8.0 μm at 25°C of the surface of the steel sheet 21 to which the coating 26 is applied is 60% or more, preferably 70% or more, and more preferably 80% or more. The coating 26 may have an emissivity at a wavelength of 8.0 μm at 700°C of 60% or more. For example, the surface treatment coating described in Patent Document 1 can be used as the coating 26. Specifically, the coating 26 can contain carbon black and one or more oxides selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide. The coating 26 may or may not contain silica. That is, the silica content of the coating 26 is 0 g / m 2 The silica content of the coating 26 is 0.30 g / m 2 The silica content may be more preferably 0.10 g / m or less. 2 More preferably, it is 0.05 g / m or less. 2 The following is the result.

[0045] The carbon black and oxides can be dispersed throughout the entire surface of the coating 26 that is perpendicular to the thickness direction of the steel sheet 21. CB (g / m 2 ), the content of one or more oxides (metal oxides) selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide is X Oxide (g / m 2 ) and then X CB and X Oxide It is preferable that the following formula (1) is satisfied: 118.9≦24280 / {6700 / (100+76×X CB ) + 18000 / (130 + 65 x X Oxide )≦332.0 (1)

[0046] In formula (1), the central formula: 24280 / {6700 / (100+76×X CB) + 18000 / (130 + 65 x X Oxide )) is preferably 119.0 or more, more preferably 170.0 or more, and even more preferably 220.0 or more. The value calculated by the middle formula is preferably 330.0 or less, more preferably 310.0 or less, and even more preferably 300.0 or less.

[0047] The dispersion state of the carbon black and metal oxide in the coating 26 can be confirmed by performing an area analysis of the coating 26 with an electron probe micro analyzer (EPMA) for elements derived from the carbon black (e.g., C) and elements derived from the oxide (Zr, Zn, and Ti). CB can be measured by cross-sectional analysis of the coating 26 using a transmission electron microscope (TEM). That is, a cross-sectional analysis of the coating 26 is performed by TEM-EDS analysis on an area of ​​a predetermined size (thickness of the coating 26 × 5 μm), and the thickness of the coating 26 and the area ratio of particles with a carbon content of 70 mass % or more in that area are measured. The density of carbon black is defined as ρ (ton / m 3 ), the film thickness is d (μm), and the area ratio is a (%), the value expressed by ρ×d×a is the carbon black content X CB (g / m 2 ) The oxide content X Oxide can be determined by performing elemental analysis on the surface of the coating 26 using an X-ray fluorescence analyzer (ZSX Primus, manufactured by RIGAKU Corporation) and quantifying the amounts of metal Zr, metal Zn, and metal Ti.

[0048] Carbon black content X in the coating 26 CB is 0.030 g / m 2 It is preferable that the content is 0.100 g / m or more. 2 It is more preferable that the content X is equal to or greater than this. CB is set within a range that satisfies the formula (1), but is preferably 0.800 g / m 2 or less, more preferably 0.600 g / m2 The following is the result.

[0049] Coating 26 may contain 5.0% or more, preferably 8.0% or more, by volume, of carbon black. Coating 26 may contain 40.0% or less, preferably 30.0% or less, by volume, of carbon black.

[0050] Metal oxide content X in the coating 26 Oxide is 0.030 g / m 2 It is preferable that the content is 0.060 g / m or more. 2 It is more preferable that the content X is equal to or greater than this. Oxide is set within a range that satisfies the formula (1), but is preferably 0.500 g / m 2 More preferably, it is 0.300 g / m or less. 2 The following is the result.

[0051] The coating 26 may contain 1.0% or more metal oxide by volume. The coating 26 may also contain 30.0% or less metal oxide by volume, and preferably contains 25.0% or less metal oxide by volume.

[0052] Carbon black content X CB (g / m 2 ) and the metal oxide content X Oxide (g / m 2 ) ratio: X Oxide / X CB is preferably 0.20 or more and 200.00 or less. Oxide / X CB is more preferably 0.40 or more and 10.00 or less, and further preferably 0.60 or more and 5.00 or less.

[0053] The coating 26 may contain various binder components and additives in addition to the carbon black and metal oxides described above.

[0054] The binder component is preferably a water-dispersible or water-soluble resin. The content of the binder component is preferably 40% by volume or more relative to the total volume of the coating 26. As the binder component selected from water-dispersible or water-soluble resins, various known resins exhibiting water dispersibility or water solubility can be used. Examples of such water-dispersible or water-soluble resins include polyurethane resins, polyester resins, acrylic resins, epoxy resins, fluororesins, polyamide resins, polyolefin resins, and polymer compounds obtained by hydrolysis and condensation polymerization of silane coupling agents. The binder component is more preferably one or more selected from the group consisting of polyester resins, polyurethane resins, polyolefin resins, acrylic resins, epoxy resins, fluororesins, and polyamide resins. When a polyurethane resin is used as the binder component, the polyurethane resin is preferably a polyether-based polyurethane resin.

[0055] Examples of additives include leveling agents, water-soluble solvents, metal stabilizers, and etching inhibitors. The leveling agent is, for example, a nonionic or cationic surfactant. Examples of nonionic or cationic surfactants include polyethylene oxide or polypropylene oxide adducts, acetylene glycol compounds, and the like. Examples of water-soluble solvents include alcohols such as ethanol, isopropyl alcohol, t-butyl alcohol, and propylene glycol; cellosolves such as ethylene glycol monobutyl ether and ethylene glycol monoethyl ether; esters such as ethyl acetate and butyl acetate; and ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone. Examples of metal stabilizers include chelate compounds such as EDTA (ethylenediaminetetraacetic acid) and DTPA (diethylenetriaminepentaacetic acid). Examples of etching inhibitors include amine compounds such as ethylenediamine, triethylenepentamine, guanidine, and pyrimidine.

[0056] The coating 26 can be formed by applying an organic or inorganic treatment liquid containing, for example, carbon black and a metal oxide to the entire surface of the steel sheet 21, and then drying the volatile components in the treatment liquid. The treatment liquid can be applied to the surface of the steel sheet 21 by, for example, a roll coater, a curtain coater, or an inkjet. In the case of inkjet coating, the thickness of the coating 26 can also be changed continuously. The thickness of the coating 26 is, for example, 0.5 μm or more and 5.0 μm or less. The thickness of the coating 26 is preferably 1.0 μm or more and 3.0 μm or less. The thickness of the coating 26 is determined by the thickness t of the steel sheet 21. min Therefore, the thickness of the steel plate 21 measured including the coating 26 is set to the thickness t min can be treated as

[0057] The steel sheet 21 may be a plated steel sheet. In this case, the steel sheet 21 has a base steel sheet 216 and a plating layer 217. The type of the base steel sheet 216 is not particularly limited. The plating layer 217 is provided on the base steel sheet 216. The plating layer 217 covers the entire or almost the entire surface of both sides of the base steel sheet 216. The plating layer 217 is a metal plating layer. The plating layer 217 may be, for example, hot-dip aluminum plating, hot-dip galvanneal plating, or electrogalvanization. As the steel sheet 21, a known aluminum-plated steel sheet, zinc-plated steel sheet, etc. can be used.

[0058] The plating layer 217 is typically a plating layer containing aluminum as a main component (aluminum-based plating layer). The configuration of the aluminum-based plating layer is not particularly limited. A known aluminum-based plating layer can be adopted as the plating layer 217. When the steel sheet 21 is a plated steel sheet, the thickness t min is the combined thickness of the base steel sheet 216 and the plating layer 217.

[0059] The steel sheets 22, 23 may be known plated steel sheets, similar to the steel sheet 21. The steel sheets 22, 23 may be aluminum plated steel sheets or zinc plated steel sheets. The steel sheets 22, 23 may be plated steel sheets of the same type as the steel sheet 21, or may be plated steel sheets of a different type from the steel sheet 21. Furthermore, the steel sheet 22 may be plated steel sheets of the same type as the steel sheet 23, or may be plated steel sheets of a different type from the steel sheet 23. When the steel sheet 22 is a plated steel sheet, the thickness t mid Similarly, when the steel sheet 23 is a plated steel sheet, the thickness t max is the combined thickness of the base steel sheet and the plating layer. When two or more of the steel sheets 21, 22, and 23 are plated steel sheets, the coating weight of each steel sheet may be the same as or different from that of the other steel sheets.

[0060] (Heating Step) The prepared blank 20 is formed into the structural member 10 (FIGS. 1 and 2) by hot stamping (hot press working). During the hot stamping, the blank 20 is subjected to a heating step. Referring to FIG. 3E, in the heating step, the blank 20 is heated, for example, by a heating furnace 30. The plurality of steel plates 21, 22, and 23 included in the blank 20 are heated to an austenite transformation completion temperature (A c3 The steel plates 21, 22, and 23 are heated to, for example, 900° C. or higher, so that the microstructures of the steel plates 21, 22, and 23 are transformed, for example, entirely or almost entirely into an austenite phase.

[0061] (Forming Process) Referring to Fig. 3F, in the forming process, a die 40 is used to form the heated blank 20 into a structural member 10 (Figs. 1 and 2) that is annular in plan view and quench it. The blank 20 heated in the heating process is removed from the heating furnace 30 (Fig. 3E) and transported to the die 40. The die 40 is attached to a known press device. The die 40 includes, for example, a punch 41 and a die 42. The blank 20 is placed between the punch 41 and the die 42.

[0062] 3G , after the blank 20 is placed between the punch 41 and the die 42, the die 42 moves relatively close to the punch 41. The blank 20 is clamped (pressed) between the punch 41 and the die 42 and formed into a shape that conforms to the forming surfaces of the punch 41 and the die 42. The blank 20 remains clamped between the punch 41 and the die 42. The blank 20 is cooled (quenched) by the die 40, and its microstructure is transformed into martensite. This allows the structural member 10 to be manufactured from the blank 20.

[0063] FIG. 4 is a cross-sectional view of the structural member 10 after hot stamping. FIG. 4 shows a cross-section of the structural member 10 at the position of the steel plate 21 ( FIGS. 3B and 3C ) to which the black coating 26 was applied at the blank 20 stage. This structural member 10 includes a member body 11 and a coating 12. The coating 12 is provided on the steel plate 21. The black coating 26 ( FIGS. 3B and 3C ) applied to the steel plate 21 in the blank 20 becomes the coating 12 through hot stamping. If the coating 26 contains carbon black, this carbon black is almost completely eliminated by the high-temperature heating during hot stamping, but may remain on the member body 11. If the coating 26 before hot stamping satisfies the above formula (1), the coating 12 after hot stamping may not contain carbon black, or may contain 0.500 g / m 2 In some cases, the coating 12 after hot stamping contains carbon black. When the coating 12 contains carbon black, the carbon black content in the coating 12 is 0 g / m 2 Furthermore, when the coating 26 before hot stamping satisfies the above formula (1), the coating 12 after hot stamping satisfies the central formula: 24280 / {6700 / (100+76×X CB ) + 18000 / (130 + 65 x X Oxide )} is, for example, 120.0 or more and 150.0 or less.

[0064] When the coating 26 (FIGS. 3B and 3C) before hot stamping satisfies the above formula (1), the coating 12 after hot stamping contains one or more oxides (metal oxides) selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide at a concentration of, for example, 0 g / m 2 More preferably, 0.001 g / m 2 The metal oxide content of the coating 12 is, for example, 0.500 g / m 2 In this way, when the metal oxide remains on the structural member 10, that is, when the coating 12 is 0 g / m or less, 2 When the coating 26 before hot stamping satisfies the above formula (1), the coating 12 after hot stamping has a metal oxide content of 0 to 0.30 g / m or more, which is more desirable because it improves the corrosion resistance of the structural member 10. 2 Contains silica.

[0065] The carbon black content, metal oxide content, and silica content in the coating 12 can be measured in the same manner as for the coating 26 at the blank 20 stage. Specifically, a vehicle body part is disassembled to obtain an annular structural member 10, and an analytical sample is obtained from this structural member 10, for example, by laser cutting. For example, an analytical sample is obtained from each of the multiple steel plates included in the structural member 10. The analytical sample is obtained from the center or its vicinity of the top plate of each steel plate having an open cross section. The cross section of the obtained analytical sample is adjusted, for example, by polishing the cross section to outside the heat-affected zone caused by laser cutting, to prepare a sample for coating analysis. The surface analysis of the coating 12 for elements derived from carbon black (e.g., C) and elements derived from oxides (Zr, Zn, and Ti) can be performed using EPMA to confirm the dispersion state of the carbon black and metal oxide in the coating 12.

[0066] In many cases, the outermost surface layer of the structural member 10 is, for example, an electrodeposition coating film. In such cases, the coating layer that is below the electrodeposition coating film layer and above the alloyed metal plating layer is analyzed. The carbon black content X in the coating 12 is CBcan be measured by cross-sectional analysis of the coating 26 using a TEM. That is, a cross-sectional analysis of the coating 12 is performed by TEM-EDS analysis in an area of ​​a predetermined size (thickness of the coating 12 × 5 μm), and the thickness of the coating 12 and the area ratio of particles with a carbon content of 70 mass % or more in that area are measured. The density of carbon black is defined as ρ (ton / m 3 ), the film thickness is d (μm), and the area ratio is a (%), the value expressed by ρ×d×a is the carbon black content X CB (g / m 2 ) The oxide content X Oxide can be determined by performing elemental analysis of the coating layer that is present below the electrodeposition coating layer and above the alloyed metal plating layer using the above-mentioned X-ray fluorescence analyzer, and quantifying the amounts of metal Zr, metal Zn, and metal Ti.

[0067] Minimum plate thickness t min In the cross section of the structural member 10 at the position of the steel plate 21 having the minimum martensite fraction (%), the martensite fraction variation is, for example, 20% or less, when the difference is the maximum martensite fraction (%) minus the minimum martensite fraction (%). The martensite fraction variation is preferably 15% or less, and more preferably 10% or less. The martensite fraction variation can be measured as follows. That is, min Ten or more analysis samples (for example, a length of about 10 mm) are cut out from positions at least 20 mm away from the end of the cross section of the structural member 10 at the position of the steel plate 21 having the above structure, and each sample is at least 10 mm away from the end. Then, each sample is mirror-polished so that the thickness direction of the steel plate serves as the observation surface, and etched with LePeller's reagent. Then, an optical microscope is used to observe the area from the surface of the steel plate to a depth of 1 / 4 of the plate thickness (a region from the surface of the steel plate to a depth of 1 / 8 of the plate thickness to a depth of 3 / 8 of the plate thickness) at a magnification of 1000x, with one field of view of 2,400 μm. 2 The above structural photographs are taken from 30 fields of view, and the obtained structural photographs are subjected to image analysis.

[0068] The image analysis method involves obtaining the maximum brightness value Lmax and minimum brightness value Lmin from the image, designating the area with pixels whose brightness ranges from Lmax-0.3 (Lmax-Lmin) to Lmax as a white area, and calculating the ratio of the number of pixels in the white area to the total number of pixels to measure the martensite fraction. This type of image analysis is performed on a total of 30 observation fields of each analysis sample to determine the martensite fraction, and the average value is used as the martensite fraction for each analysis sample. Furthermore, the difference between the maximum and minimum martensite fractions in 10 or more analysis samples is calculated based on the minimum plate thickness t min The variation in martensite fraction in the cross section of the structural member 10 at the position of the steel plate 21 having the minimum plate thickness t min If there are multiple steel plates having the above structure, such analysis is performed on each steel plate to determine the martensite fraction, and the maximum variation in martensite fraction among these steel plates is taken as the variation in martensite fraction in the structural member 10.

[0069] In some steel sheets, the area fraction of martensite obtained by image analysis, i.e., the area fraction of the white region, may contain a few percent of the area fraction of retained austenite. However, since the variation in the martensite fraction is calculated as a difference, the impact is minor.

[0070] After the forming process (hot stamping), the steel sheet 21 can have a tensile strength of, for example, 0.5 GPa or more, and preferably has a tensile strength of 1.0 GPa or more. Similarly, after the forming process (hot stamping), the steel sheets 22 and 23 ( FIG. 1 ) can have a tensile strength of, for example, 0.5 GPa or more, and preferably has a tensile strength of 1.0 GPa or more. At least one of the steel sheets 21, 22, and 23 may have a tensile strength of 1.5 GPa or more after the forming process. The tensile strength of each of the steel sheets 21, 22, and 23 may be the same as or different from the tensile strength of the other steel sheets.

[0071] [Effect] In the blank 20 according to this embodiment, the minimum plate thickness t minThe emissivity of one surface of the steel sheet 21 having a thickness of 1 / 2 mm is higher than the emissivity of both surfaces of the steel sheet 22 having a thickness of 1 / 2 mm. That is, the surface of the steel sheet 21 is treated to increase the emissivity. As a result, when the blank 20 is heated during hot stamping, the temperature rise rate of the steel sheet 21 is significantly higher than that of the steel sheet 22. Therefore, in the heating process, the steel sheet 21 can be quickly heated to a temperature in the austenite range, ensuring a long high-temperature holding time for the steel sheet 21. As a result, the austenite grains in the microstructure of the steel sheet 21 coarsen, and the ferrite transformation region (ferrite nose) in the CCT diagram shifts to the long-time side. Therefore, it is possible to prevent the transformation of austenite to ferrite in the steel sheet 21 after removal from the heating furnace 30 and before the start of forming with the die 40. Therefore, it is possible to start forming the blank 20 with the die 40 while maintaining the microstructure of the steel sheet 21 in the austenite phase, and it is possible to prevent the transformation of austenite to ferrite in the steel sheet 21. min The hardenability of the steel plate 21 having this can be improved.

[0072] In this embodiment, the hardenability of the relatively thin steel plate 21 is improved, so that the hardness of the structural member 10 formed from the blank 20 can be made uniform. More specifically, the minimum plate thickness t min Since the steel plate 21 having a thickness of 1000 .0 mm or less can be quenched well, the variation in the martensite fraction in the steel plate 21 can be kept to 20% or less. This makes it less likely for deformation concentration to occur when a collision load is input to the structural member 10, making it easier for the structural member 10 to exhibit high impact absorption performance. Therefore, even when an annular structural member 10 including a thin steel plate 21, particularly a large annular structural member 10, is formed from the blank 20, it is possible to reduce strength defects in the structural member 10 and improve the impact absorption performance of the structural member 10.

[0073] The smaller the variation in the martensite fraction, the less non-uniformity there is in the mechanical properties within the structural member 10, which is preferable from the viewpoint of the functionality of the structural member 10. On the other hand, a large variation in the martensite fraction indicates that parts with insufficient hardenability, i.e., parts with insufficient hardness, are unevenly distributed within the structural member 10, and when the structural member 10 is deformed by a collision, deformation tends to concentrate in the parts with insufficient hardness, thereby reducing the functionality of the structural member 10.

[0074] In this embodiment, the hardenability of the relatively thin steel plate 21 is improved, which makes it less likely that uneven stress will occur in the structural member 10. Therefore, even when the annular structural member 10 is formed from an annular blank 20, twisting is less likely to occur in the structural member 10. Therefore, even when an annular structural member 10 including a thin steel plate 21, particularly a large annular structural member 10, is formed from the blank 20, it is possible to reduce poor dimensional accuracy of the structural member 10 and improve the impact absorption performance of the structural member 10.

[0075] In the blank 20 according to this embodiment, the minimum plate thickness t min The surface of the steel plate 21 is substantially covered with a black coating 26, while the steel plate 22, which is thicker than the steel plate 21, is not provided with the coating 26. Therefore, the emissivity of the surface of the steel plate 21 is higher than the emissivity of both surfaces of the steel plate 22. In this case, the steel plate 21 heats up faster than the steel plate 22, so the high-temperature retention time of the steel plate 21 is longer compared to when the steel plate 21 has the same emissivity as the steel plate 22. This makes it possible to reduce non-uniformity in phase transformation caused by differences in cooling rate between the steel plates 21, 22, and 23 after heating of the blank 20 is completed. Specifically, min Since the start of the phase transformation from austenite to ferrite can be delayed for the steel plate 21, the difference in the phase transformation start time between the steel plate 21 and the other steel plates 22 and 23 is reduced. As a result, the hardenability of the steel plates 21, 22, and 23 included in the blank 20 can be made uniform.

[0076] For example, if the plating layer 217 of the steel sheet 21 is an aluminum-based plating layer, the temperature rise rate of the steel sheet 21 is likely to be slow during the heating process. Because the aluminum-based plating layer is white, it tends to reflect heat energy and inhibit the temperature rise of the steel sheet 21. However, in the blank 20 according to this embodiment, the surface of the steel sheet 21 is treated to increase the emissivity. Therefore, even if the steel sheet 21 is a plated steel sheet having an aluminum-based plating layer, the temperature rise of the steel sheet 21 during the heating process can be promoted and the high-temperature holding time of the steel sheet 21 can be ensured to be long. Therefore, the hardenability of the thin-walled steel sheet 21 can be ensured.

[0077] In this embodiment, in the heating process, first, the minimum plate thickness t min The steel plate 21 having the intermediate thickness t mid and a steel plate 22 having a maximum plate thickness t max The steel plate 23 having the minimum plate thickness t min and maximum plate thickness t max Ratio to: t max / t min It is preferable that the thickness t min The alloying of the plating layer 217 of the steel sheet 21 having the thickness t max Therefore, the steel plate 23 having the above-mentioned structure can be heated sufficiently until the phase transformation to austenite is completed. Therefore, the process window can be secured in the manufacturing of the structural member 10.

[0078] In this embodiment, a coating 26 can be applied to the steel sheet 21 in order to increase the emissivity of the steel sheet 21. The emissivity of the coating 26 (at a temperature of 25°C and a wavelength of 8.0 μm) is, for example, 60% or more. This allows the steel sheet 21 to be efficiently radiantly heated, and the temperature rise rate of the steel sheet 21 in the heating process is more likely to be increased.

[0079] In this embodiment, the coating 26 is made of a material containing carbon black, one or more oxides selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide, and a carbon black content of 0 to 0.30 g / m 2The carbon black content X may be the following: CB (g / m 2 ), and the oxide content X Oxide (g / m 2 ) preferably satisfies the above formula (1). As described in Patent Document 1, formula (1) is a function of the ratio (%) of the increase in the temperature rise rate (°C / s) and the carbon black content X CB and oxide content X Oxide Formula (1) defines the relationship between the carbon black and oxides. Formula (1) indicates that carbon black primarily functions as a heat absorbing material in the temperature range up to 700°C, and oxides primarily function as heat absorbing materials in the temperature range of 700°C or higher. When coating 26 satisfies formula (1), the surface of steel sheet 21 to which coating 26 is applied tends to have an emissivity of 60% or more at a wavelength of 8.0 μm at 25°C.

[0080] The carbon black and oxides can be dispersed throughout the entire surface of the coating 26 that is perpendicular to the thickness direction of the steel sheet 21. This makes it easier to make the emissivity of the surface of the steel sheet 21 uniform. Therefore, in the heating process, min The steel plate 21 having the above structure can be heated quickly and uniformly.

[0081] However, the configuration of the coating 26 is not limited to this. The coating 26 may be a substantially black coating in order to increase the emissivity of the steel sheet 21 compared to an untreated steel sheet. For example, the coating 26 may contain graphite, soot, or the like instead of or in addition to carbon black. Alternatively, the coating 26 may contain, for example, an acicular compound having an aspect ratio of 4 to 50 and a hexagonal crystal structure in order to increase the emissivity of the steel sheet 21. The compound having a hexagonal crystal structure is typically graphite (C), but may also be lanthanum silicate, magnesium diboride, beryllium oxide (beryllia), zinc oxide, β-quartz, goethite (NiS), wurtzite (ZnS), or the like.

[0082] <Second embodiment> Fig. 5 is a plan view of a blank 20A according to a second embodiment. The blank 20 according to the first embodiment is a tailored blank in which steel plates 21, 22, and 23 are butt-joined to one another. The blank 20A according to this embodiment differs from the first embodiment mainly in the form of the joint between the steel plates.

[0083] 5, the blank 20A includes a plurality of steel plates 21, 22, 23, 24, and 25. The steel plates 21, 22, 23, 24, and 25 are arranged and joined to form an annular shape in a plan view of the blank 20. As in the first embodiment, the steel plate 21 has a minimum plate thickness t min and the emissivity of at least one surface thereof is configured to be greater than the emissivity of both surfaces of the steel plate 22. Therefore, the blank 20A according to this embodiment can also achieve the same effects as those of the first embodiment.

[0084] The blank 20A has an overlap portion 27. Fig. 6 is a cross-sectional view taken along line VI-VI in Fig. 5, showing a cross section of the overlap portion 27. In this embodiment, the overlap portion 27 is formed by overlapping the ends of two adjacent steel plates 23, 24. The end of the steel plate 23 is joined to the end of the steel plate 24 in an overlapping state. The steel plates 23, 24 are joined to each other by, for example, spot welding or laser welding.

[0085] The overlap portion 27 has a total thickness t. The total thickness t is the sum of the thicknesses of the steel sheets 23 and 24. If at least one of the steel sheets 23 and 24 is a plated steel sheet, the total thickness t also includes the thickness of the plating layer. The total thickness t of the overlap portion 27 is, for example, greater than 2.5 mm and less than 4.0 mm. In this case, the steel sheet 23 is configured so that the emissivity of the surface located outside the overlap portion 27, i.e., the surface opposite the steel sheet 24, is higher than the emissivity of both surfaces of the steel sheet 22 ( FIG. 5 ). The steel sheet 24 is configured so that the emissivity of the surface located outside the overlap portion 27, i.e., the surface opposite the steel sheet 23, is higher than the emissivity of both surfaces of the steel sheet 22. That is, in each of the steel sheets 23 and 24, the surface located outside the overlap portion 27 is entirely treated to increase the emissivity. For example, the emissivity at 25°C at a wavelength of 8.0 μm is 60% or more, preferably 70% or more, and more preferably 80% or more, on the surfaces of the steel plates 23, 24 located outside the overlap portion 27. The difference in emissivity at a wavelength of 8.0 μm at 25°C between the surfaces of the steel plates 23, 24 located outside the overlap portion 27 and both surfaces of the other steel plate 22 is preferably greater than 5%, more preferably greater than 10%, and even more preferably greater than 20%. The emissivity of the surfaces of the steel plates 23, 24 located inside the overlap portion 27 may be greater than the emissivity of both surfaces of the steel plate 22, or may be less than or equal to the emissivity of both surfaces of the steel plate 22.

[0086] In the steel plates 23 and 24, the surfaces located outside the overlap portion 27 may be covered with the coating 26, so that the emissivity of the surfaces may be higher than that of the steel plate 22 ( FIG. 5 ). The coating 26 used on the steel plates 23 and 24 may have a configuration similar to that of the coating 26 used on the steel plate 21. As described above, the thickness of the coating 26 is very small, and therefore the total plate thickness t of the overlap portion 27 can be the plate thickness measured including the coating 26.

[0087] If the total thickness t of the overlap portion 27 exceeds, for example, 2.5 mm, the overlap portion 27 is difficult to heat up. Therefore, when the blank 20A is heated during hot stamping, the overlap portion 27 may reach the minimum thickness t by the time it reaches the temperature in the austenite region. min In some cases, the plating layer 217 (FIGS. 3B and 3C) of the steel sheet 21 having the above-mentioned structure is alloyed, causing a diffusion layer to grow, which can result in the corrosion resistance or weldability of the steel sheet 21 being impaired. However, in this embodiment, the emissivity of the overlap portion 27 is increased to promote temperature rise. Therefore, even if the total thickness t of the overlap portion 27 is greater than 2.5 mm, the overlap portion 27 can be sufficiently heated until the phase transformation to austenite is completed before the alloying of the plating layer 217 of the steel sheet 21 progresses and the diffusion layer becomes thick enough to cause a loss of corrosion resistance or weldability. This ensures a process window in the manufacture of structural members.

[0088] In the blank 20A according to this embodiment, the steel plate 21 may be butt-joined to the steel plates 22 and 23, or may form an overlap portion 27 with one or both of the steel plates 22 and 23. The steel plate 25 may be butt-joined to the steel plates 22 and 24, or may form an overlap portion 27 with one or both of the steel plates 22 and 24. When the steel plates 21 and 23 form the overlap portion 27 and the total thickness t of the overlap portion 27 exceeds 2.5 mm, the steel plates 21 and 23 may be configured so that the emissivity of the surfaces located outside the overlap portion 27 is higher than the emissivity of both surfaces of the steel plate 22. Similarly, when the steel plates 24 and 25 form the overlap portion 27 and the total thickness t of the overlap portion 27 exceeds 2.5 mm, the steel plates 24 and 25 may be configured so that the emissivity of the surfaces located outside the overlap portion 27 is higher than the emissivity of both surfaces of the steel plate 22.

[0089] 7 is a plan view of a structural member 10A manufactured from a blank 20A. The structural member 10A has substantially the same configuration as the structural member 10 of the first embodiment (FIGS. 1 and 2). However, in the structural member 10A, the member body 11 is formed from five steel plates 21, 22, 23, 24, and 25. The method for manufacturing the structural member 10A from the blank 20A is the same as that of the first embodiment.

[0090] The structural member 10A can have a size similar to that of the structural member 10 according to the first embodiment. That is, the size of the structural member 10A, which is annular in plan view, is, for example, 1.0 m or more and 4.0 mm or less. In the structural member 10A, each of the steel plates 21, 22, 23, 24, and 25 has an open cross section similar to that of the first embodiment. Each of the steel plates 21, 22, 23, 24, and 25 can have, for example, a generally hat shape in a cross-sectional view of the structural member 10A.

[0091] Although not shown, in the structural member 10A, the width of the steel plate 21 arranged on the upper part of the front pillar 111 is, for example, 15 mm or more and 300 mm or less. The height of the steel plate 21 may be, for example, 10 mm or more and 150 mm or less. In the structural member 10A, the width of the steel plate 22 arranged on the lower part of the front pillar 111 is, for example, 30 mm or more and 750 mm or less. The height of the steel plate 22 may be, for example, 25 mm or more and 150 mm or less. In the structural member 10A, the width of the steel plates 23, 24 arranged at the position of the center pillar 112 is, for example, 15 mm or more and 300 mm or less. The height of the steel plates 23, 24 may be, for example, 10 mm or more and 150 mm or less. In the structural member 10A, the width of the steel plate 25 arranged at the position of the rocker 113 is, for example, 30 mm or more and 300 mm or less. The height of the steel plate 25 may be, for example, 25 mm or more and 150 mm or less.

[0092] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments, and various modifications are possible without departing from the spirit of the present disclosure.

[0093] In each of the above embodiments, the minimum plate thickness t minIn order to increase the emissivity of the surface of the steel plate 21 having the above-mentioned roughness more than that of the steel plate 22, the surface of the steel plate 21 is coated with a coating 26. However, the method for increasing the emissivity of the surface of the steel plate 21 is not limited to the coating 26. For example, the emissivity of the surface of the steel plate 21 can also be increased more than that of the steel plate 22 by making the surface roughness of the steel plate 21 greater than that of the steel plate 22. Similarly, the method for increasing the emissivity of the outer surface of the overlap portion 27 is not limited to the coating 26.

[0094] In each of the above embodiments, the minimum plate thickness t min In the above example, the emissivity of only one of the two surfaces of the steel plate 21 having the same thickness is made higher than the emissivity of the steel plate 22. However, the emissivity of both surfaces of the steel plate 21 may be made higher than the emissivity of the steel plate 22. For example, both surfaces of the steel plate 21 may be coated with the coating 26. Alternatively, the surface roughness of both surfaces of the steel plate 21 may be made higher than the surface roughness of the steel plate 22.

[0095] In the first embodiment, the steel plates 21, 22, and 23 included in the blank 20 may each be single-layered or multi-layered. That is, the steel plates 21, 22, and 23 may each be a single steel plate or a plate material formed by stacking multiple steel plates. Similarly, in the second embodiment, the steel plates 21, 22, 23, 24, and 25 may each be single-layered or multi-layered.

[0096] In the first embodiment, the blank 20 includes three steel plates 21, 22, and 23. In the second embodiment, the blank 20A includes five steel plates 21, 22, 23, 24, and 25. However, the number of steel plates included in the blanks 20 and 20A is not limited to this. The blanks 20 and 20A have at least a minimum plate thickness t min and a steel plate 21 having a plate thickness t minThe blank 20, 20A may include a steel plate 22 having a thickness greater than t. The emissivity of one or both sides of the steel plate 21 is greater than the emissivity of both sides of the steel plate 22. The steel plate 21 is joined directly or indirectly to the steel plate 22. The blank 20, 20A, which is annular in plan view, may typically include three or more steel plates. In the blank 20, 20A, the steel plates other than the steel plates 21, 22 may or may not be treated to increase the emissivity. In either of the blanks 20, 20A, the minimum plate thickness t min When there are a plurality of steel plates 21 having the same emissivity, it is preferable that the emissivity of one or both sides of all of the steel plates 21 is higher than the emissivity of both sides of the other steel plates 22. In the annular blanks 20, 20A, the arrangement of the plurality of steel plates including the steel plates 21, 22 is not particularly limited.

[0097] In each of the above embodiments, the minimum plate thickness t min In the above example, the steel sheet 21 having the above-described characteristics is a plated steel sheet. However, the steel sheet 21 does not necessarily have to be a plated steel sheet. The steel sheet 21 may be a steel sheet (bare material) that does not have a plating layer on its surface. Similarly, steel sheets other than the steel sheet 21 may also be plated steel sheets or bare materials.

[0098] In the first embodiment, the mold 40 used for hot stamping the blank 20 includes a punch 41 and a die 42. However, the configuration of the mold 40 is not limited to the example described in the first embodiment. The mold 40 may further include, for example, a pad and a blank holder.

[0099] In the above-described embodiments, the main body 11 of the structural member 10, 10A includes a front pillar 111, a center pillar 112, and a rocker 113. However, the member main body 11 may further include other components. For example, as shown in FIG. 8 , the member main body 11 may further include a rear pillar 114. The structural members 10, 10A according to the above-described embodiments are door ring components having a single ring shape (single door ring components). On the other hand, the structural member shown in FIG. 8 is a door ring component having a double ring shape (double door ring component). When manufacturing double door ring components, the blank used as the raw material also has a double ring shape.

[0100] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to the following examples.

[0101] [First Example] In order to confirm the effects of the present disclosure, a CAE analysis was performed on a press-formed (hot stamped) structural member that is a single door ring part, using commercially available software (AUTOFORM R.10, manufactured by AUTOFORM) while changing the type (material type) and thickness of the steel plate included in the structural member, as well as the division pattern of the structural member.

[0102] The steel plates used in this analysis are shown in Table 1.

[0103]

[0104] In Table 1, the material type is listed in the order of plating type, tensile strength, and application (hot stamping). Regarding the coating specifications, the black coating is a black coating containing carbon black and metal oxide. "Black coating - one side" means that one entire side of the steel sheet is coated with a black coating. "Black coating - both sides" means that both entire sides of the steel sheet are coated with a black coating.

[0105] The division patterns of the structural members are shown in Figures 9A to 9G. Figures 9A to 9G show the number of steel plates (materials) included in the structural member, which is a single door ring component, and the positions of the joints between the steel plates in the structural member. In Figures 9A to 9G, each steel plate is given a number in parentheses.

[0106] The analysis conditions and results for division patterns 1 and 2 shown in Figures 9A and 9B are shown in Table 2. In Figures 9A and 9B, the structural member is formed from three pieces of material (1) to (3).

[0107]

[0108] Referring to Table 2, in Example 1, the minimum thickness t min In Example 2, the material (3) having the smallest thickness t of the materials (1) to (3) is provided with a black coating on both sides. min In Example 3, a black coating is applied to one side of the material (1) having a thickness of 1.2 mm. min : A black coating is applied to both sides of the material (2) having a thickness of 1.2 mm. On the other hand, in Comparative Examples 1 and 2, a black coating is not applied to any of the materials (1) to (3). In Comparative Examples 1 and 2, min : No black coating was applied to the material having a thickness of 1.2 mm.

[0109] In Table 2, the "time to reach 910°C" indicates the time to reach 910°C (A) the fastest among the materials contained in the blank. c3 The "phase transformation start time" is the time required for a blank heated to 910°C from the start of heating to reach 910°C for a material heated to a furnace temperature of 920°C for 5 minutes and 30 seconds and then removed from the heating furnace. Table 2 shows that in Examples 1 to 3, in which the emissivity of the thinnest material was increased by a black coating, the time to reach 910°C was 20 seconds or more shorter than in Comparative Examples 1 and 2, and the heating rate of the thinnest material in the heating process was higher. Furthermore, in Examples 1 to 3, the phase transformation start time exceeded 20 seconds, which was slower than in Comparative Examples 1 and 2. This makes it easier to start forming the blank before the onset of ferrite transformation, enabling the blank to be uniformly quenched during the forming process.

[0110] The analysis conditions and results for division patterns 3 and 4 shown in Figures 9C and 9D are shown in Table 3. In Figures 9C and 9D, the structural member is formed from four pieces of material (1) to (4).

[0111]

[0112] Referring to Table 3, in Examples 4 to 10, the minimum plate thickness t min In Examples 4 to 10, a black coating is applied to a material having a minimum plate thickness t min The material is covered with a black coating on one or both sides. min In the case where there are multiple blanks having the same thickness, all of these blanks are provided with a black coating. On the other hand, in Comparative Examples 3 to 7, none of the blanks (1) to (4) are provided with a black coating. In Comparative Examples 3 to 7, min No black coating is applied to the material having the above.

[0113] From Table 3, it can be seen that in Examples 4 to 10, the time to reach 910°C was 20 seconds or more shorter than in Comparative Examples 3 to 7, and the temperature rise rate of the thinnest material in the heating process was higher. Furthermore, in Examples 4 to 10, the phase transformation start time exceeded 20 seconds, which was later than in Comparative Examples 3 to 7. This made it easier to start forming the blank before the onset of ferrite transformation, and made it possible to uniformly quench the blank in the forming process.

[0114] The analysis conditions and results for division patterns 5 to 7 shown in Figures 9E to 9G are shown in Table 4. In Figures 9E to 9G, the structural member is formed from five pieces of material (1) to (5).

[0115]

[0116] Referring to Table 4, in Examples 11 to 15, the minimum plate thickness t min In Examples 11 to 15, a black coating is applied to a material having a minimum plate thickness t min The material is covered with a black coating on one or both sides. minIn the case where there are multiple blanks having the same thickness, all of these blanks are provided with a black coating. On the other hand, in Comparative Examples 8 to 11, none of the blanks (1) to (5) are provided with a black coating. In Comparative Examples 8 to 11, min No black coating is applied to the material having the above.

[0117] Table 4 shows that in Examples 11 to 15, the time to reach 910°C was 20 seconds or more shorter than in Comparative Examples 8 to 11, and the temperature rise rate of the thinnest material in the heating process was higher. Furthermore, in Examples 11 to 15, the phase transformation start time exceeded 20 seconds, which was later than in Comparative Examples 8 to 11. This made it easier to start forming the blank before the onset of ferrite transformation, and enabled the blank to be uniformly quenched in the forming process.

[0118] In each of the examples and comparative examples shown in Tables 2 to 4, the materials are butted together and then laser-joined (butt-jointed). On the other hand, in each of the examples and comparative examples shown in Table 5 below, some of the materials are joined by, for example, spot welding to form overlapping portions.

[0119]

[0120] Referring to Table 5 and Fig. 9F, in Example 16 and Comparative Example 12, material (2) and material (5), material (3) and material (4), and material (4) and material (5) form overlapping portions at their joints. Referring to Table 5 and Fig. 9E, in Example 17 and Comparative Example 13, material (2) and material (5), and material (3) and material (4) form overlapping portions at their joints.

[0121] As shown in Table 5, in Examples 16 and 17, the minimum plate thickness t min On the other hand, in Comparative Examples 12 and 13, no black coating was applied to any of the materials (1) to (5). min No black coating is applied to the material having the above.

[0122] As can be seen from Table 5, in Examples 16 and 17, the time to reach 910°C was 20 seconds or more shorter and the time to start phase transformation was also delayed compared to Comparative Examples 12 and 13. Therefore, it was confirmed that even when an overlapping portion exists in the blank, an effect similar to that of butt welding can be obtained by increasing the emissivity of the thinnest material.

[0123] Second Example Regarding the press forming (hot stamping) of a structural member that is a double door ring part, an analysis similar to that of the first example was carried out while changing the material type and plate thickness of the structural member, as well as the division pattern of the structural member.

[0124] As with the first embodiment, the steel plates used as raw materials were selected from those shown in Table 1. The division pattern of the structural members is as shown in Figures 10A to 10D. Figures 10A to 10D show the number of steel plates (raw materials) included in the structural members that are double door ring components, and the positions of the joints between the steel plates in the structural members. In Figures 10A to 10D, each steel plate used as raw material is given a number in parentheses.

[0125] The analysis conditions and results for division patterns 8 and 9 shown in Figures 10A and 10B are shown in Table 6. In Figures 10A and 10B, the structural member is formed from six materials (1) to (6).

[0126]

[0127] Referring to Table 6, in Examples 18 to 20, the minimum plate thickness t min In Examples 18 to 20, a black coating is applied to a material having a minimum plate thickness t min On the other hand, in Comparative Examples 14 and 15, no black coating was applied to any of the materials (1) to (6). min No black coating is applied to the material having the above.

[0128] From Table 6, it can be seen that in Examples 18 to 20, the time to reach 910°C was about 20 seconds shorter than in Comparative Examples 14 and 15, and the temperature rise rate of the thinnest material in the heating process was higher. Furthermore, in Examples 18 to 20, the phase transformation start time was slower than in Comparative Examples 14 and 15. Therefore, it can be said that by increasing the emissivity of the thinnest material, it becomes easier to start forming the blank before the onset of ferrite transformation, and it becomes possible to uniformly harden the blank in the forming process.

[0129] The analysis conditions and results for division patterns 10 and 11 shown in Figures 10C and 10D are shown in Table 7. In Figures 10C and 10D, the structural member is formed from seven pieces of material (1) to (7).

[0130]

[0131] Referring to Table 7, in Examples 21 to 23, the minimum plate thickness t min In Examples 21 to 23, a black coating is applied to a material having a minimum plate thickness t min On the other hand, in Comparative Examples 16 and 17, no black coating was applied to any of the materials (1) to (7). min No black coating is applied to the material having the above.

[0132] From Table 7, it can be seen that in Examples 21 to 23, the time to reach 910°C was shorter and the temperature rise rate of the thinnest material in the heating process was higher compared to Comparative Examples 16 and 17. Furthermore, in Examples 21 to 23, the phase transformation start time was slower than in Comparative Examples 16 and 17. Therefore, it becomes easier to start forming the blank before the start of ferrite transformation, and it becomes possible to uniformly quench the blank in the forming process.

[0133] [Example 3] To confirm the influence of plate thickness on the press forming (hot stamping) of a structural member that is a single door ring part, an analysis similar to that of Example 1 was carried out while changing the combination of materials and the joining mode. The analysis conditions and results are shown in Table 8.

[0134]

[0135] The division pattern of Test Examples 1 and 5 is division pattern 7 shown in FIG. 9G. The division pattern of Test Example 4 is division pattern 5 shown in FIG. 9E. In Test Examples 1, 4, and 5, some of the materials form overlapping portions at the joints. More specifically, in Test Examples 1 and 5, material (1) and material (2), material (1) and material (3), material (2) and material (5), and material (4) and material (5) each form overlapping portions at the joints. In Test Example 4, material (1) and material (2), material (1) and material (3), material (3) and material (4), and material (2) and material (5) each form overlapping portions at the joints. In all of these test examples, the minimum plate thickness t min In addition, in all of these test examples, black coatings were applied to both outer sides of the overlap portion having the maximum total plate thickness t.

[0136] The division pattern of Test Examples 2, 3, and 6 is division pattern 7 shown in FIG. 9G. In Test Examples 2, 3, and 6, the materials are joined by butt welding. In all of these test examples, the minimum plate thickness t min A black coating is applied to the material having the above structure.

[0137] The "process window (PW)" in Table 8 is the value obtained by subtracting the time required for the entire blank to reach 910°C after the earliest temperature reached 910°C from the heating time that can be tolerated for the material contained in the blank that reached 910°C first. If the process window is 5 seconds or less, alloying of the plating layer of the material that reached 910°C first in the heating process will progress, making it impossible to ensure the corrosion resistance of the plating layer and making it difficult to manufacture a structural component with good quality.

[0138] As shown in Table 8, the minimum plate thickness t min Maximum plate thickness t max Ratio of: t max / t min In Test Examples 5 and 6, where t exceeded 3.2, the process window was negative, and it was not possible to ensure the process window necessary for satisfactory manufacturing of structural members.max / t min In Test Examples 1 to 4 where the value was 3.2 or less, the process window could be secured.

[0139] As shown in Table 8, in Test Example 5, where the maximum total plate thickness t of the overlap portion exceeded 4.0 mm, the process window was negative and it was not possible to ensure the process window necessary for satisfactory manufacturing of structural members. On the other hand, in Test Examples 1 and 4, where the maximum total plate thickness t of the overlap portion was greater than 2.5 mm and equal to or less than 4.0 mm, a process window of 5 seconds or more was ensured.

[0140] Reference Example 1 is an example of division pattern 5 similar to Test Example 4, but no black coating is applied to any of the materials, including the overlapping portions. However, in Reference Example 1, there is no difference in plate thickness between the materials, and the problem of alloying progression in the coating layer of the thinnest material does not occur, so a process window of 5 seconds or more could be secured.

[0141] For Test Examples 1 to 4 and Comparative Examples 10 and 13A, the blanks were heated at a furnace temperature of 920°C until the entire blank reached 910°C. Then, the blanks were transferred to a press in 17 seconds, hot stamped at a forming speed of 40 mm / s, and held at bottom dead center for 20 seconds while applying a pressure of 3000 kN to obtain hot-stamped structural components. Analysis samples were taken from the thinnest portions of these structural components using the method described in the above embodiment, and the martensite fraction variation was measured. Furthermore, shape accuracy and impact absorption performance measurements were also conducted on these structural components. The evaluation results are shown in Table 9.

[0142]

[0143] In Table 9, the variation in martensite fraction is, as explained in the above embodiment, the variation in the minimum plate thickness t min The martensite fraction (%) is the maximum martensite fraction (%) minus the minimum martensite fraction (%) in the cross section of the structural member at the location of the material having the martensite fraction (%).

[0144] The shape accuracy was evaluated by measuring the distance between the structural member and the mating member at the overlapping portion when the structural member, which is approximately hat-shaped in cross section, is attached to another member. In Table 9, a value of ○ indicates that the distance from the surface of the mating member is within ±2.0 mm, a value of △ indicates that the distance is between ±2.0 mm and ±3.0 mm, and a value of × indicates that the distance is greater than ±3.0 mm.

[0145] Regarding the impact absorption performance, a small overlap (SOL) collision and a side collision were assumed with the structural member assembled to a vehicle, and an impactor simulating a vehicle was collided with the structural member to evaluate the maximum intrusion amount during the SOL collision and the maximum intrusion amount during the side collision. The impact absorption performance was evaluated based on the impact absorption performance of a door ring component formed by hot stamping each material and then joining them, and compared with the impact absorption performance of the base. In Table 9, impact absorption performance equivalent to the impact absorption performance of the base is represented by "good," impact absorption performance superior to the impact absorption performance of the base is represented by "better," impact absorption performance slightly lower than the impact absorption performance of the base is represented by "marginal," and impact absorption performance even lower than the impact absorption performance is represented by "poor."

[0146] Comparative Example 10 is a comparative example of the first embodiment, and similar to Test Example 2, the materials were butt-joined by laser welding. Comparative Example 13A is the same plate assembly as Comparative Example 13 of the first embodiment, but similar to Test Example 4, the materials were partially overlap-joined. Unlike the other test examples, Comparative Example 10 and Comparative Example 13A do not have a black coating applied to any of the materials, including the thinnest material. As shown in Table 9, the martensite fraction variation was 20% or less in all of Test Examples 1 to 4, and the martensite fraction variation was significantly reduced compared to Comparative Examples 10 and 13A. Test Examples 1 to 4 also had better shape accuracy than Comparative Examples 10 and 13A.

[0147] Test Examples 1 to 4, which had small variations in the martensite fraction, also showed improved impact absorption performance compared to Comparative Examples 10 and 13A. In particular, Test Examples 1 to 3, which had a martensite fraction variation of 15% or less, were able to ensure impact absorption performance equal to or greater than that of the base. That is, even though multiple materials were integrated at the blank stage to form an annular structural member, impact absorption performance equal to or greater than that of a structural member formed by press-molding and then joining the materials individually was ensured. In Test Examples 2 and 3, the strength against axial force was improved by butt-joining the materials, resulting in better impact absorption performance than Test Example 1. Test Examples 2 and 3 demonstrated high impact absorption performance, particularly in SOL collisions.

[0148] 10, 10A: Structural member 11: Member body 111: Front pillar 112: Center pillar 113: Rocker 12: Coating 20, 20A: Blank 21: Steel plate (first steel plate) 216: Base steel plate 217: Plating layer 22: Steel plate (second steel plate) 23, 24, 25: Steel plate 26: Coating 27: Overlap portion 40: Mold

Claims

1. A blank for hot stamping, comprising a plurality of steel plates joined and arranged to have a ring shape when viewed in a plane of the blank, the plurality of steel plates including: a first steel plate having the smallest thickness among the plurality of steel plates; and a second steel plate having a thickness greater than that of the first steel plate, the first steel plate being configured such that the emissivity of at least one of both surfaces of the first steel plate is greater than the emissivity of both surfaces of the second steel plate.

2. A blank according to claim 1, wherein the first steel plate has a plate thickness of less than 1.4 mm.

3. A blank according to claim 1, wherein the first steel sheet is a plated steel sheet having a base steel sheet and an aluminum-based plating layer provided on the base steel sheet.

4. A blank according to claim 1, wherein said at least one surface of said first steel plate is covered with a coating having an emissivity of 60% or more at a wavelength of 8.0 μm at 25° C.

5. A blank according to claim 1, wherein at least one surface of the first steel plate is coated with a coating, and the coating is a composite material including carbon black, one or more oxides selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide, and a 0 to 0.30 g / m 2 and silica, and the content of the carbon black in the coating is X CB (g / m 2 ), the content of the oxide is X Oxide (g / m 2 ) and then X CB and X Oxide A blank that satisfies the following formula (1). 118.9≦24280 / {6700 / (100+76×X CB ) + 18000 / (130 + 65 x X Oxide ))≦332.0 (1) 6. A blank according to claim 1, wherein the first steel sheet is a plated steel sheet having a base steel sheet and a plated layer provided on the base steel sheet, and the thickness of the first steel sheet is t minThe thickness of the steel plate having the largest thickness among the plurality of steel plates is t max When 1.0<t max / t min ≦3.2, blank.

7. A blank as described in claim 1, wherein the first steel plate is a plated steel plate having a base steel plate and a plating layer provided on the base steel plate, and the blank further comprises an overlap portion formed by overlapping ends of two adjacent steel plates among the plurality of steel plates other than the second steel plate, the overlap portion having a total plate thickness of greater than 2.5 mm and not greater than 4.0 mm, and the two steel plates are each configured so that the emissivity of the surface located outside the overlap portion is greater than the emissivity of both surfaces of the second steel plate.

8. A method for manufacturing a structural component, comprising the steps of: preparing a blank as described in any one of claims 1 to 7; heating the plurality of steel plates contained in the blank to a temperature equal to or higher than the austenite transformation completion temperature; and using a die to form the heated blank into a structural component that is annular in plan view and quenching the blank.

9. A structural member, comprising: a first steel plate having a minimum plate thickness; and a second steel plate having a plate thickness greater than that of the first steel plate, the first steel plate being formed by a plurality of steel plates joined together, the main body being annular in plan view; and a second steel plate having a thickness greater than that of the first steel plate, the second steel plate being formed on the first steel plate, and containing at least one oxide selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide at a concentration of 0.001 g / m. 2 A structural member comprising:

10. A structural member comprising: a first steel plate having a minimum plate thickness; and a second steel plate having a plate thickness greater than that of the first steel plate, the first steel plate being joined to the second steel plate; a member body having an annular shape in a plan view; and a carbon black layer provided on the first steel plate and containing 0.500 g / m 2 A structural member comprising:

11. A structural member as claimed in claim 9 or 10, which is a door ring part of an automobile, and the member body includes a front pillar, a center pillar, and a rocker connecting the front pillar and the center pillar.

Citation Information

Patent Citations

  • Vehicle body side structural frame

    JP2021528248A

  • Overlapped blank and method for manufacturing hot stamp molding using the same

    JP2021154370A

  • Method of manufacturing blank for hot-press, and blank for hot-press

    JP2023180687A

  • mold

    JP7101730B2

  • Manufacturing method of hot press-formed product and steel plate

    JP7260765B2

Cited By

  • Cut steel plates, tailored blanks, methods for manufacturing tailored blanks, hot-pressed products, and methods for manufacturing hot-pressed products.

    JP2026115966A

  • Method for manufacturing welded steel sheets, method for manufacturing tailored blanks, method for manufacturing hot press-formed products, welded steel sheets, tailored blanks, and hot press-formed products

    JP2026166184A

  • Cut steel plates, tailored blanks, methods for manufacturing tailored blanks, hot-pressed products, and methods for manufacturing hot-pressed products.