Gas barrier coating agent, multilayer body, and method for producing same
A gas barrier coating agent using a water-soluble polysaccharide and metal salt, cured with active energy rays, addresses the limitations of existing materials by providing effective oxygen barrier and water resistance under high humidity, enhancing the performance and cost-effectiveness of packaging materials.
Patent Information
- Application Number
- PCT/JP2024/016297
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-21
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Current gas barrier packaging materials face challenges in maintaining oxygen barrier properties under high humidity conditions, water resistance, and transparency, particularly when using environmentally friendly biomass raw materials, which are costly and have low productivity due to viscosity and storage stability issues.
A gas barrier coating agent comprising a water-soluble polysaccharide and a compound with an amino group and hydroxyl group, combined with a metal salt, which is cured using active energy rays like ultraviolet rays or electron beams to form a laminate with excellent gas barrier properties, transparency, and substrate adhesion.
The solution achieves high oxygen barrier properties, water resistance, and transparency even under high humidity conditions, making it suitable for use as a top coat in packaging materials without the need for heat treatment or crosslinking agents, thereby improving productivity and reducing costs.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Gas barrier coating agent, laminate, and method for producing the same
[0001] FIELD OF THE INVENTION The present invention relates to a gas barrier coating agent, a laminate, and a method for producing the same.
[0002] Packaging materials used for packaging foods, pharmaceuticals, and the like are required to prevent deterioration of the contents. The deterioration of the contents is mainly caused by oxygen that permeates the packaging material or other gases that react with the contents. Therefore, packaging materials used for packaging foods, pharmaceuticals, and the like are required to have properties that prevent the permeation of gases such as oxygen, i.e., gas barrier properties. In particular, in the case of food packaging, extending the expiration date or best-before date is expected to lead to a reduction in the large amount of waste generated from ordinary households and commercial facilities such as supermarkets and convenience stores (Non-Patent Document 1).
[0003] To impart barrier properties to packaging materials, it is effective to use metals such as aluminum or inorganic materials including alumina, silica, etc. as a barrier layer. Specifically, high gas barrier properties are ensured by forming a laminate with an aluminum foil laminated structure or by using a method of forming an inorganic layer on a plastic film substrate by a vacuum process such as CVD or vapor deposition. However, it is desirable to eliminate the process of laminating aluminum foil from the viewpoint of energy saving and recyclability, while structures including inorganic layers have problems such as resistance due to defects such as cracks.
[0004] Molding and Processing Vol. 34 No. 4 2022
[0005] Japanese Patent Application Laid-Open No. 60-157830 Japanese Patent No. 3203287 Japanese Patent Application Laid-Open No. 2019-178130 Japanese Patent Application Laid-Open No. 2003-171419 Japanese Patent Application Laid-Open No. 2016-159576 Japanese Patent Application Laid-Open No. 2021-113244 Japanese Patent Application Laid-Open No. 2017-202665 Japanese Patent No. 7179976
[0006] To address these challenges, gas barrier films composed of flexible gas barrier polymers with relatively high gas barrier properties and laminates using such films as base films have been proposed. Conventionally, polymers containing hydrogen-bonding groups within the molecule, such as poly(meth)acrylic acid, ethylene-vinyl alcohol copolymers, vinylamine-vinyl alcohol copolymers, or mixtures thereof, have been used as oxygen barrier polymers (see Patent Documents 1, 2, 7, and 8). However, while gas barrier materials composed of these polymers have excellent oxygen barrier properties under dry conditions, they suffer from problems such as a significant decrease in oxygen barrier properties under high-humidity conditions due to their hydrophilicity, and the films also suffer from poor water-friction resistance and resistance to hot water. Naturally, it is practically difficult to use such films with poor water resistance as the outermost layer (top coat) of a packaging material.
[0007] To solve these problems, it is known to incorporate a polyvalent metal compound into the substrate itself, or to laminate a polycarboxylic acid polymer layer and a polyvalent metal compound-containing layer adjacent to each other on the substrate, and then convert the polyvalent metal salt of the polycarboxylic acid polymer into a polyvalent metal salt by an interlayer reaction (Patent Documents 3 and 4). It has been shown that the gas barrier packaging material obtained in this manner has high oxygen gas barrier properties even under high humidity conditions. However, the gas barrier packaging materials described in Patent Documents 3 and 4 require heat treatment at 150°C or higher, immersion treatment in a crosslinking agent, or retort treatment, which reduces productivity. Furthermore, to achieve high barrier properties, it is necessary to form a layer containing a high concentration of polyvalent metal salt in an insoluble state, which poses the problem of reduced transparency.
[0008] In recent years, growing interest in environmental issues has led to active product development that actively utilizes biomass feedstocks and biodegradable materials. It can be said that there is a great social need for similar materials in the packaging field. As a gas barrier material with high hydrogen bonding properties derived from natural materials and an alternative to petroleum-derived poly(meth)acrylic acid and polyvinyl alcohol, polysaccharides have been reported that possess numerous hydrogen-bonding groups and anionic hydrophilic groups within the molecule by subjecting naturally occurring cellulose raw materials, which are abundant in nature, to TEMPO oxidation treatment or sulfuric acid treatment (Patent Documents 5 and 6). Patent Document 6 achieves relatively high oxygen barrier properties under high humidity conditions by forming a water-soluble nanocellulose coating film in combination with a crosslinking agent or a layered inorganic compound on an undercoat layer containing a metal salt. However, the barrier properties are insufficient and transparency is low. Furthermore, modified cellulose is relatively expensive, and it is difficult to increase the solids content during water solubilization due to issues with viscosity and storage stability, resulting in low productivity during printing and coating. As described above, no oxygen barrier coating agent has yet been reported that uses environmentally friendly raw materials, has gas barrier properties and transparency under high humidity, has substrate adhesion, and also has sufficient water resistance, and can be used as a top coat.
[0009] Therefore, some embodiments of the present invention solve any of the above problems and provide a gas barrier coating agent that can be applied to a substrate, even when a general-purpose substrate such as a polyethylene terephthalate (PET) film, a polypropylene (OPP, CPP) film, or paper is used, and then cured by irradiation with active energy rays such as ultraviolet rays or electron beams, thereby producing a laminate that exhibits excellent gas barrier properties even under high humidity conditions and that further has transparency, water friction resistance, and substrate adhesion.
[0010] As a result of extensive research into solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by a gas barrier coating agent for packaging materials comprising a water-soluble polysaccharide (A1) and / or a compound (A2) having an amino group and a hydroxyl group, a compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond and having a molecular weight of 50 or more and less than 300, and a metal salt (C) having, as a ligand, a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and having a molecular weight of 50 or more and less than 300, and have arrived at the present invention.
[0011] That is, one embodiment of the present invention relates to a gas barrier coating agent comprising a water-soluble polysaccharide (A1), a compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more but less than 300, and a metal salt (C) having, as a ligand, a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more but less than 300.
[0012] Another embodiment of the present invention relates to a gas barrier coating agent comprising: a compound (A2) having an amino group and a hydroxyl group; a compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond, and having a molecular weight of 50 or more and less than 300; and a metal salt (C) having, as a ligand, a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond, and having a molecular weight of 50 or more and less than 300, wherein the compound (A2) has an amine value of 30 to 600 mgKOH / g and a hydroxyl value of 400 to 1300 mgKOH / g.
[0013] Yet another embodiment of the present invention relates to a laminate having a gas barrier layer formed on a substrate using the gas barrier coating agent of any of the above embodiments.
[0014] Yet another embodiment of the present invention relates to a method for producing a laminate, comprising the steps of: applying the gas barrier coating agent of any of the above embodiments to a substrate to obtain a coated product; and irradiating the coated product with ultraviolet light or electron beams to form a gas barrier layer on the substrate.
[0015] According to some embodiments of the present invention, it is possible to provide a gas barrier coating agent that, even when using a general-purpose substrate such as a polyethylene terephthalate (PET) film, a polypropylene (OPP, CPP) film, or paper, can be applied to the substrate and cured by irradiation with active energy rays such as ultraviolet light or electron beams, and that exhibits excellent gas barrier properties even under high humidity conditions, and that can also produce a laminate that has transparency, water abrasion resistance, and substrate adhesion.
[0016] The following examples are provided to explain the embodiments of the present invention in detail, but the matters described below are examples or representative examples of the embodiments of the present invention, and the present invention is not limited to these contents as long as they do not deviate from the gist of the invention.
[0017] <Gas Barrier Coating Agent> In some embodiments of the present invention, the gas barrier coating agent comprises a water-soluble polysaccharide (A1), a compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more and less than 300, and a metal salt (C) having, as a ligand, a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more and less than 300.
[0018] In some embodiments of the present invention, the gas barrier coating agent comprises a compound (A2) having an amino group and a hydroxyl group, a compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond and having a molecular weight of 50 or more and less than 300, and a metal salt (C) having, as a ligand, a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and having a molecular weight of 50 or more and less than 300.
[0019] The gas barrier coating agent can be suitably used for packaging material applications. In this specification, the water-soluble polysaccharide (A1) and the compound (A2) having an amino group and a hydroxyl group may be collectively referred to as "compound (A)." The compound (A) may be a compound that functions as a binder resin, and includes at least one selected from the group consisting of the water-soluble polysaccharide (A1) and the compound (A2) having an amino group and a hydroxyl group. The compound (A) may be, for example, a compound consisting only of the water-soluble polysaccharide (A1); a compound consisting only of the compound (A2) having an amino group and a hydroxyl group; or a compound containing the water-soluble polysaccharide (A1) and the compound (A2) having an amino group and a hydroxyl group.
[0020] [Water-soluble polysaccharide (A1)] Polysaccharide is a general term for a substance in which a large number of monosaccharide molecules are polymerized in a chain form through glycosidic bonds. The water-soluble polysaccharide (A1) used in the embodiment of the present invention refers to a compound that dissolves when mixed with water or hot water in any ratio, or that stably exhibits a colloidal or suspended state in water. The chain polysaccharide may be a linear or branched polysaccharide, but linear polysaccharides are preferred from the viewpoints of water solubility and viscosity when made into an aqueous solution. Examples of linear water-soluble polysaccharides include anionic water-soluble polysaccharides such as amylose, chitin, chitosan, agarose, agar, dextran, hyaluronic acid, chondroitin sulfate, starch, inulin, cellulose, tuberose polysaccharide, quince seed extract, gellan gum, sodium alginate, pectin, carboxymethylcellulose, sodium chondroitin sulfate, hyaluronic acid, and carrageenan; and hydroxyethyl cellulose, hydroxypropyl cellulose, guar gum, agarose, pullulan, locust bean gum, galactan, gum arabic, tara gum, tamarind seed gum, and agar. These may be used alone or in combination of two or more. Among these, chitosan, guar gum, and xanthan gum are preferred, with chitosan being more preferred from the viewpoints of coatability and barrier properties.
[0021] Chitosan is obtained by treating chitin, which is found in large quantities in the shells of crustaceans such as shrimp and crab, with a strong base to deacetylate the acetamide groups in the chitin's molecular structure and convert them to amino groups. Because this deacetylation process requires a lot of energy and cost to complete, most commercially available chitosan generally contains undeacetylated acetamide groups, and quality specifications state that the deacetylation rate is 70 mol% or more, 80 mol% or more, etc. While the present invention also contemplates the use of chitosan with a similar deacetylation rate, this is not limited to the specific formulation, provided that a sufficient cured coating film is obtained.
[0022] The deacetylation rate can be measured by the following method. Chitosan is dissolved in a 0.05% by mass dilute acetic acid solution to prepare a 0.05% by mass chitosan aqueous solution. 50 mL of ion-exchanged water and approximately 0.2 mL of toluidine blue solution are added to prepare a sample solution, which is then titrated with a potassium polyvinyl sulfate solution (N / 400PVSK, Fujifilm Wako Pure Chemical Industries, Ltd.). As a blank test, a similar titration test is performed using ion-exchanged water instead of the 0.05% by mass chitosan / 0.05% by mass acetic acid aqueous solution used in the above titration test. The deacetylation rate is then calculated using the following formula: X = 1 / 400 × 161 × f × (V−B) / 1000 = 0.4025 × f × (V−B) / 1000 Y = 0.5 / 100 − X X: mass of free amino groups in chitosan (equivalent to the mass of glucosamine residues) Y: mass of bound amino groups in chitosan (equivalent to the mass of N-acetylglucosamine residues) f: titer of N / 400PVSK V: titer of sample solution (mL) B: titer of blank test (mL) Deacetylation rate (%) = (free amino groups) / {(free amino groups)+(bound amino groups)}×100 = (X / 161) / (X / 161+Y / 203)×100 Note that "161" is the molecular weight of the glucosamine residue, and "203" is the molecular weight of the N-acetylglucosamine residue.
[0023] The water-soluble polysaccharide (A1) is likely to exhibit excellent oxygen barrier properties because it has multiple hydrogen-bonding functional groups in the molecule, such as hydroxyl groups, carboxyl groups, amino groups, sulfo groups, etc. Furthermore, because it has a high molecular weight, it is suitable as a binder resin in that it can impart coating suitability, wettability to substrates, adhesion, and flexibility that prevents cracking even when bent.
[0024] [Compound (A2) Having an Amino Group and a Hydroxyl Group] The compound (A2) having an amino group and a hydroxyl group has a plurality of hydrogen-bonding functional groups in the molecule, and therefore tends to exhibit excellent oxygen barrier properties. Furthermore, if it is a high molecular weight compound, it is suitable as a binder resin in that it can impart coatability, wettability to a substrate, adhesiveness, and flexibility that prevents cracking even when bent.
[0025] Generally, the term "amino group" refers to a primary amine, but in the embodiment of the present invention, the amino group possessed by the compound (A2) may be in the form of a secondary or tertiary amine in which the hydrogen atom bonded to the nitrogen atom is substituted with an alkyl group, an aryl group, or the like, or may be in the form of a quaternary ammonium salt if part of the amino group is present. On the other hand, it is known that the more substituents there are, the higher the ability to trap and stabilize radicals generated by electron beam or UV irradiation, and curing inhibition is more likely to occur, so the use of a primary amine compound is desirable.
[0026] For the compound (A2) having an amino group and a hydroxyl group, the functional group values for exhibiting excellent curability and oxygen barrier properties are preferably an amine value of 30 to 600 mgKOH / g and a hydroxyl value of 400 to 1300 mgKOH / g, more preferably an amine value of 30 to 550 mgKOH / g and a hydroxyl value of 500 to 1300 mgKOH / g, and even more preferably an amine value of 30 to 500 mgKOH / g and a hydroxyl value of 600 to 1300 mgKOH / g.
[0027] The amine value can be measured by the following method. The amine value is measured by a known titration method in accordance with JIS K0070:1992. That is, 0.5 to 2 g of a sample (compound (A2)) is precisely weighed out (sample amount: S g, solid content: Z %), and 30 mL of neutral ethanol is added to the precisely weighed sample to dissolve it. If the sample has low solubility, ion-exchanged water may be added appropriately. The resulting solution is titrated with a 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The point at which the color of the solution changes from green to yellow is set as the endpoint, and the titration amount (A mL) at this point is used to calculate the amine value according to the following (Equation 1): (Equation 1) Amine value = (A x f x 0.2 x 56.106) / (S x Z / 100)
[0028] The hydroxyl value can be calculated based on the structure of the polymer (compound (A2)) using the following formula (2): (Formula 2) Hydroxyl value = 56106 x A / M A: number of hydroxyl groups in the polymer structural unit M: molecular weight of the polymer structural unit
[0029] As the compound (A2) having an amino group and a hydroxyl group, a vinylamine-vinyl alcohol copolymer is preferred because it has a molecular structure that achieves both a relatively high amine value and a sufficiently high hydroxyl value, and the composition ratio can be controlled in the synthesis process.
[0030] Vinylamine-vinyl alcohol copolymers can be obtained by hydrolyzing copolymers of N-vinylformamide or N-vinylacetamide with vinyl carboxylates, and the like. From the viewpoints of availability of raw materials and ease of hydrolysis, it is preferable to hydrolyze copolymers of N-vinylformamide and vinyl acetate. The copolymerization can be carried out by known methods such as bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization. Considering ease of reaction control, solution polymerization, suspension polymerization, and emulsion polymerization are preferred. Alternatively, emulsion polymerization or suspension polymerization can be carried out by forming a water-in-oil emulsion (see, for example, JP 2004-315792 A and JP 2002-069124 A).
[0031] From the viewpoint of achieving appropriate solids content and viscosity of the coating liquid and satisfying the cured physical properties of the coating film, the vinylamine-vinyl alcohol copolymer preferably has a number average molecular weight of 1,000 to 200,000, more preferably 5,000 to 100,000, and even more preferably 10,000 to 70,000. Furthermore, from the viewpoint of the above-mentioned curing inhibition and aqueous solution stability, there is a preferred range for the amine value, and the molar fraction of amino groups to hydroxyl groups (amino groups:hydroxyl groups) in the vinylamine-vinyl alcohol copolymer is preferably 5:95 to 40:60, more preferably 10:90 to 30:70.
[0032] The number average molecular weight can be measured by the following method. The number average molecular weight is calculated by aqueous GPC (gel permeation chromatography). The measurement is carried out, for example, under the following conditions: Measurement device: Agilent 1260 Infinity II GPC / SEC system Column: OHpak SB-800 HQ Solvent: water / methanol = 5 / 5 vol% + lithium chloride 50 mM Standard substance: polyethylene oxide / polyethylene glycol
[0033] [Compound (B) Having an Anionic Hydrophilic Group and an Ethylenically Unsaturated Double Bond] In an embodiment of the present invention, the compound having an anionic hydrophilic group and an ethylenically unsaturated double bond includes compound (B) having a molecular weight of 50 or more but less than 300. The anionic hydrophilic group refers to a functional group from which more than half of the hydrogen ions dissociate in water at pH 7, and examples thereof include a carboxyl group, a sulfonic acid group, a phosphonic acid group, a phosphinic acid group, and a phosphate group. Each of these groups possesses hydrogen bonding properties, thereby complementing the oxygen barrier properties of the water-soluble polysaccharide (A1) or the compound (A2) having an amino group and a hydroxyl group. Furthermore, since compound (B) contains an ethylenically unsaturated double bond, it can improve coating film strength and water resistance by crosslinking using thermal polymerization, photopolymerization, electron beams, or the like, and suppress deterioration of oxygen barrier properties under high humidity. When the water-soluble polysaccharide (A1) has a cationic hydrophilic group, chitosan, for example, is preferred because it is modified by forming an ionic bond with compound (B) (anionic monomer) to become a reactive binder. Examples of the compound (A2) having an amino group and a hydroxyl group include vinylamine-vinyl alcohol copolymers, which are preferred because they are modified by forming an ionic bond with compound (B) (anionic monomer) to become a reactive binder.
[0034] The compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond has a molecular weight of 50 or more and less than 300, and from the viewpoints of molecular mobility and reactivity derived from steric hindrance, the molecular weight is preferably 50 or more and less than 200, and more preferably 50 or more and less than 120. Furthermore, from the viewpoint of radical polymerization reactivity, the compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond is preferably (meth)acrylic acid or a (meth)acrylate compound, and more preferably (meth)acrylic acid.
[0035] Specific examples of compound (B) include acrylic acid, methacrylic acid, cinnamic acid, crotonic acid, senecioic acid, tiglic acid, sorbic acid, itaconic acid, maleic acid, angelic acid, aconitic acid, citraconic acid, mesaconic acid, 3-cyclopentene-1-carboxylic acid, 2-methyl-4-pentenoic acid, 2-amino-4-pentenoic acid, 2-hydroxy-3-butenoic acid, trans-2-pentenoic acid, trans-3-hexenedioic acid, sulfoalkyl (meth)acrylate, 2-acrylamido-2-methylpropanesulfonic acid, 2-methacryloyloxyethyl acid phosphate, vinylsulfonic acid, styrenesulfonic acid, vinylphosphonic acid, and cinnamylphosphonic acid. Acrylic acid and methacrylic acid are more preferred, and acrylic acid is particularly preferred in terms of gas barrier properties and cost. The above compounds can be used alone or in combination of two or more.
[0036] [Metal Salt (C)] In an embodiment of the present invention, the metal salt includes a metal salt (C) having, as a ligand, a compound having a molecular weight of 50 to 300 and containing an anionic hydrophilic group and an ethylenically unsaturated double bond. Examples of the central metal of the metal salt (C) include divalent or higher polyvalent metals such as magnesium (Mg), calcium (Ca), barium (Ba), zinc (Zn), copper (Cu), cobalt (Co), nickel (Ni), aluminum (Al), and iron (Fe). Among these, zinc, calcium, magnesium, and aluminum are preferred. When used simultaneously with the water-soluble polysaccharide (A1) and / or the compound (A2) as the binder resin and the compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond, the metal salt containing a divalent or higher metal increases the density of crosslinking by thermal polymerization, photopolymerization, electron beam, or the like, thereby improving curability. This inhibits the penetration of water and water vapor into the cured coating film, improving water resistance and gas barrier properties under high humidity. The metal salt (C) may be used alone or in combination of two or more. The compound having an anionic hydrophilic group and an ethylenically unsaturated double bond as a ligand and a molecular weight of 50 or more but less than 300 is synonymous with the aforementioned compound (B). The compound as a ligand of the metal salt (C) and the aforementioned compound (B) may be the same or different.
[0037] Examples of the metal salt (C) include calcium acrylate, magnesium acrylate, zinc acrylate, aluminum acrylate, and zinc 2-acrylamido-2-methylpropanesulfonate.
[0038] By forming a cured coating film (gas barrier layer) using a gas barrier coating agent containing the water-soluble polysaccharide (A1), compound (B), and metal salt (C), high levels of oxygen barrier property, substrate adhesion, and water resistance can be achieved. Regarding the content of each component, the content (mass%) of the water-soluble polysaccharide (A1) is preferably 20 to 70% by mass, more preferably 30 to 60% by mass, based on 100% by mass of the solids content of the gas barrier coating agent. The content (mass%) of the compound (B) is preferably 10 to 60% by mass, more preferably 15 to 60% by mass, and even more preferably 20 to 50% by mass. The content (mass%) of the metal salt (C) is preferably 10 to 70% by mass, more preferably 15 to 60% by mass, and even more preferably 20 to 50% by mass.
[0039] By forming a cured coating film (gas barrier layer) using the gas barrier coating agent containing the above-mentioned compound (A2) having an amino group and a hydroxyl group, compound (B), and metal salt (C), high levels of oxygen barrier property, substrate adhesion, and water resistance can be achieved. Regarding the content of each component, the content (mass%) of compound (A2) having an amino group and a hydroxyl group, based on 100% by mass of the solids content of the gas barrier coating agent, is preferably 20 to 70% by mass, more preferably 30 to 60% by mass. The content (mass%) of compound (B) is preferably 3 to 60% by mass, more preferably 4 to 60% by mass, and even more preferably 5 to 50% by mass. The content (mass%) of compound (B) may be 10 to 60% by mass, 15 to 60% by mass, or 20 to 50% by mass. The content (mass %) of the metal salt (C) is preferably from 10 to 70 mass %, more preferably from 15 to 60 mass %, and even more preferably from 20 to 50 mass %.
[0040] The gas barrier coating agent may contain components other than the water-soluble polysaccharide (A1), the compound (A2) having an amino group and a hydroxyl group, the compound (B), and the metal salt (C) as needed. The gas barrier coating agent may contain optional components such as a solvent, an initiator, a sensitizer, a resin, a crosslinking agent, and other additives as needed. Examples of other additives include a surface conditioner, an ultraviolet absorber, an antioxidant, a polymerization inhibitor, a wax, and an inorganic compound.
[0041] [Solvent] The gas barrier coating agent preferably contains a solvent. It is preferable to use water as the solvent to form an aqueous composition. In order to improve wettability to the substrate or to achieve uniform dissolution or dispersion of each component, a small amount of organic solvent (e.g., alcohols) may be added within a range that does not inhibit the polymerization reaction.
[0042] [Initiator] Because the gas barrier coating agent contains an ethylenically unsaturated double bond as a polymerizable group, a crosslinking reaction can be carried out by irradiation with ultraviolet light or electron beams to obtain a cured coating film. Electron beam irradiation is preferred because it allows the crosslinking reaction to occur without the use of a polymerization initiator, but if necessary, a polymerization initiator can also be contained in the gas barrier coating agent. Typical polymerization initiators are photopolymerization initiators and thermal polymerization initiators. Photopolymerization initiators and thermal polymerization initiators may also be used in combination. The thermal polymerization initiator may be an azo compound or peroxide that is activated by irradiation with ionizing radiation. The initiators can be used alone or in combination of two or more.
[0043] The polymerization reaction after applying the gas barrier coating agent to the substrate may be carried out after the solvent has been thoroughly evaporated in an oven, or may be carried out in a wet state before drying. When irradiating a wet coating film with ultraviolet light, it is preferable to include a photopolymerization initiator in the gas barrier coating agent. Photopolymerization initiators are sometimes simply called photoinitiators or sensitizers. Examples of photopolymerization initiators include acetophenones, benzophenones, Michler's ketones, benzils, benzoins, benzoin ethers, benzil dimethyl ketals, thioxanthones, and mixtures of two or more of these.
[0044] Specific preferred examples of the photopolymerization initiator include acetophenones such as acetophenone, 2,2-diethoxyacetophenone, m-chloroacetophenone, p-tert-butyltrichloroacetophenone, 4-dialkylacetophenone, and 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methylpropan-1-one; benzophenones such as benzophenone; Michler's ketones such as Michler's ketone; benzils such as benzil methyl ether and benzyl methyl ether; benzoins such as benzoin and 2-methylbenzoin; benzoin ethers such as benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin butyl ether; benzil dimethyl ketals such as benzil dimethyl ketal; thioxanthone and other thioxanthone; and carbonyl compounds such as propiophenone, anthraquinone, acetoin, butyroin, toluoin, benzoyl benzoate, and α-acyloxime ester.
[0045] In addition to the above carbonyl compounds, examples of the photopolymerization initiator include sulfur compounds such as tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetramethylthiuram monosulfide, thioxanthone, and 2-chlorothioxanthone; azo compounds such as azobisisobutyronitrile and azobis-2,4-dimethylvaleronitrile; and peroxides such as benzoyl peroxide and di-tert-butyl peroxide.
[0046] When these photopolymerization initiators are added to the gas barrier coating agent, they are typically added in a proportion of 0.001 to 10% by mass, preferably 0.01 to 5% by mass, relative to the polymerizable compound containing compound (B). Although the addition of a photopolymerization initiator is not essential, when polymerization is performed by irradiation with ultraviolet light, adding a photopolymerization initiator is preferable to improve polymerization efficiency. When a hydrogen abstraction photopolymerization initiator such as benzophenone is used, a portion of the α,β-unsaturated carboxylic acid monomer is grafted to the plastic film used as the substrate, thereby improving interlayer adhesion between the substrate and the ionically crosslinked polycarboxylic acid polymer film layer. Other general-purpose additives, such as sensitizers and light stabilizers, may also be added together with the photopolymerization initiator.
[0047] When the coating film in a wet state is heated to carry out thermal polymerization, it is preferable to use a thermal polymerization initiator that thermally dissociates to function as an initiator. Examples of the thermal polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate; azo polymerization initiators such as 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis[2-methyl-N-[1,1-bis(hydroxymethyl)ethyl]propionamide], 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(methyl isobutyrate), 1,2'-azobis(N,N'-dimethyleneisobutylamidine)dihydrochloride, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide, 1,1'-azobis(cyclohexane-1-carbonitrile); and tert-alkylhydrocarbonyl compounds. peroxides such as di-tert-butyl peroxide, dicumyl peroxide, lauroyl peroxide, benzoyl peroxide, tert-butylperoxy-2-ethylhexanoate, tert-hexylperoxy-2-ethylhexanoate, tert-butyl peroxypivalate, di-isopropyl peroxydicarbonate, di-tert-butylperoxyisophthalate, 1,1',3,3'-tetramethylbutylperoxy-2-ethylhexanoate, and tert-butyl peroxybutyrate. When a thermal polymerization initiator is used, it is added in an amount of typically 0.001 to 10% by mass, and preferably 0.01 to 5% by mass, based on the solid content of the gas barrier coating agent.
[0048] [Sensitizer] In the gas barrier coating agent, a sensitizer can be used in combination with the photopolymerization initiator. Examples of the sensitizer include amine-based sensitizers, anthracene-based sensitizers, and thioxanthone-based sensitizers. The sensitizers can be used alone or in combination of two or more types.
[0049] Examples of the amine sensitizer include trimethylamine, methyldimethanolamine, triethanolamine, p-diethylaminoacetophenone, ethyl p-dimethylaminobenzoate, isoamyl p-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, N,N-dimethylbenzylamine, and 4'-bis(diethylamino)benzophenone.
[0050] Examples of the anthracene-based sensitizer include 9,10-dibutoxyanthracene, 9,10-diethoxyanthracene, 9,10-dipropoxyanthracene, and 9,10-bis(2-ethylhexyloxy)anthracene.
[0051] Examples of thioxanthone sensitizers include 2,4-diethylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, etc. Representative examples of commercially available products include amine sensitizers such as EPA (manufactured by Nippon Kayaku Co., Ltd.), anthracene sensitizers such as DBA and DEA (manufactured by Kawasaki Kasei Chemicals Ltd.), and thioxanthone sensitizers such as DETX and ITX (manufactured by Lambson). The sensitizer is preferably a thioxanthone sensitizer.
[0052] [Resin] The gas barrier coating agent can contain a non-polymerizable resin to the extent that it does not impair performance such as gas barrier properties and water resistance, and an aqueous resin is preferred. The inclusion of a non-polymerizable resin in the gas barrier coating agent can improve the flexibility of the coating, wettability to the substrate, and reduce the cure shrinkage of the coating film that occurs during curing, thereby suppressing curling of the substrate and possibly improving adhesion to the substrate. Examples of resins include acrylic resins, epoxy resins, polyurethane resins, polyurethane-urea resins, (modified) styrene-maleic anhydride copolymers, (modified) vinyl chloride-vinyl acetate copolymers, (modified) vinyl chloride-vinyl acetate-maleic anhydride copolymers, ketone aldehyde resins, polyester resins, polypropylene resins, polylactic acid resins, cellulose acetate resins, cellulose acetate butyrate resins, esterified cellulose resins, and butyral resins. These resins can be used alone or in combination of two or more.
[0053] [Crosslinking Agent] The gas barrier coating agent may use a water-soluble or water-dispersible crosslinking agent for the purpose of improving gas barrier properties and water resistance under high humidity conditions, and a crosslinking agent capable of reacting with functional groups such as hydroxyl groups, carboxyl groups, and amino groups in the molecules of compounds contained in the gas barrier coating agent is preferred. Typical examples of crosslinking agents capable of reacting with the above functional groups include compounds having an isocyanate group, epoxy group, carbodiimide group, oxazoline group, etc., and metal chelates such as titanium and zirconium may also be used. These may be used alone or in combination of two or more.
[0054] Specific examples of the crosslinking agent include water-dispersible isocyanates Duranate WB40-100 and Duranate WT20-100 manufactured by Asahi Kasei Corporation, water-soluble polyfunctional epoxy compounds Denacol EX-313 and Denacol EX-321 manufactured by Nagase ChemteX Corporation, carbodiimide compounds Carbodilite E-02 and Carbodilite E-05 manufactured by Nisshinbo Co., Ltd., oxazoline compounds WS-500 and K2020E manufactured by Nippon Shokubai Co., Ltd., titanium chelates Orgatix TC-300 and TC-310 manufactured by Matsumoto Fine Chemical Co., Ltd., and zirconium chelates ZC-126 and ZC-300 manufactured by Matsumoto Fine Chemical Co., Ltd.
[0055] [Surface Conditioner] The surface conditioner is a material having a surface conditioning function such as leveling or cissing prevention. Suitable surface conditioners include silicone-based surface conditioners such as polyether-modified polydimethylsiloxanes having acrylic groups, polyether-modified dimethylsiloxanes, polyester-modified dimethylsiloxanes having acrylic groups, polyether-modified polydimethylsiloxanes, polyester-modified polydimethylsiloxanes, and aralkyl-modified polymethylalkylsiloxanes. Other examples include acrylic-based surface conditioners, fluorine-based surface conditioners, and acetylene glycol-based surface conditioners. These can be used alone or in combination of two or more types, and are preferably present in an amount of 0.001% by mass or more and 2.0% by mass or less, and more preferably 0.01% by mass or more and 1.0% by mass or less, relative to 100% by mass of the total of components (A) to (C).
[0056] [UV absorber] UV absorbers are used to prevent deterioration of the laminate due to UV rays emitted from sunlight or lighting. Examples include benzophenone-based, benzotriazole-based, and triazine-based UV absorbers, and many water-dispersible products for aqueous applications are commercially available. These can be used alone or in combination of two or more types, and are preferably present in an amount of 0.001% by mass or more and 1.0% by mass or less, relative to 100% by mass of the total of components (A) to (C).
[0057] [Antioxidant] The antioxidant is used for the purpose of preventing deterioration, similar to the ultraviolet absorber, and examples thereof include hindered phenol-based antioxidants, hindered amine-based antioxidants, etc. These can be used alone or in combination of two or more, and are preferably used in an amount of 0.001% by mass or more and 0.5% by mass or less, relative to 100% by mass of the total of components (A) to (C).
[0058] [Polymerization Inhibitor] A polymerization inhibitor may be used in the gas barrier coating agent to improve storage stability. The polymerization inhibitor can be appropriately selected from known ones. Examples of polymerization inhibitors include hindered phenols, hindered amines, quinones, nitrosamines, phenothiazines, and piperidine-1-oxyls. When a polymerization inhibitor is used, the content is preferably 0.001% by mass or more and 0.2% by mass or less relative to 100% by mass of the total of components (A) to (C), in order to achieve both storage stability and photocurability.
[0059] [Wax] When the gas barrier coating agent is aqueous, the wax is preferably in the form of an aqueous dispersion, i.e., an emulsion. Examples of wax emulsions include wax emulsions containing polyolefin wax, paraffin wax, sazol wax, etc. Polyolefin wax is a polymer or copolymer primarily composed of an olefin monomer. Paraffin wax is a petroleum-based wax consisting of a mixture of linear saturated hydrocarbons having 20 to 30 carbon atoms. Sazol wax is a synthetic wax consisting of nearly saturated linear hydrocarbons produced by the Fischer-Tropsch process using carbon monoxide and hydrogen as raw materials. Wax emulsions containing one or more waxes selected from polyolefin wax and paraffin wax are preferred, and wax emulsions containing polyolefin wax are more preferred. Wax emulsions containing the above waxes can be used alone or in combination of two or more types.
[0060] [Inorganic Compound] The gas barrier coating agent may further contain an inorganic compound for the purpose of imparting higher gas barrier properties. The inorganic compound is preferably in a plate-like form, which is likely to exhibit a labyrinth effect, but this is not necessarily optimal from the standpoint of coatability and stability over time, and it may be in a spherical or amorphous form. Examples of plate-like inorganic compounds suitable for use in the present invention include hydrous silicates (such as phyllosilicate minerals), kaolinite-serpentine clay minerals (such as halloysite, kaolinite, endelite, dickite, nacrite, antigorite, chrysotile, etc.), pyrophyllite-talc (such as pyrophyllite, talc, keroli), smectite clay minerals (such as montmorillonite, beidellite, nontronite, saponite, hectorite, sauconite, stevensite, etc.), vermiculite clay minerals (such as vermiculite), mica or mica clay minerals (muscovite, phlogopite, margarite, tetrasilylic mica, taeniolite, etc.), chlorite (such as cucaite, sudoite, clinochlore, chamosite, nimite, etc.), hydrotalcite, plate-like barium sulfate, boehmite, and aluminum polyphosphate. These minerals may be natural or synthetic clay minerals.
[0061] <Method for Producing a Gas Barrier Coating Agent> The gas barrier coating agent is not particularly limited as long as it contains the above-mentioned compound (A), compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 to less than 300, and metal salt (C) having a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 to less than 300 as a ligand. Specific production methods include mixing the raw materials with water and dissolving them over time using a roller stirrer or roller mixer, or stirring them with a stirrer such as a homodisper to prepare the coating agent. Any method may be used as long as it produces a uniform solution without lumps. However, from the above perspective, it is preferable to prepare compound (A) and metal salt (C) in a water-soluble or dispersed state in water at a desired ratio before mixing them. Furthermore, when compound (B) having an anionic hydrophilic group (e.g., chitosan) is used to water-solubilize compound (A), it is preferable to first mix and dissolve the compound (B) and then mix it with an aqueous solution of metal salt (C). When additives are added, it is desirable to dilute them with water or alcohol before use in order to prevent shock at the time of addition.
[0062] <Gas Barrier Laminate> In an embodiment of the present invention, a laminate comprises a substrate and a gas barrier layer formed on the substrate using the gas barrier coating agent described above. For example, the gas barrier laminate has a gas barrier layer formed by applying the gas barrier coating agent according to an embodiment of the present invention to one or both sides of the substrate and optionally curing it, and is suitable for use in packaging applications. [Substrate] The substrate or film substrate is selected from the group consisting of resin sheets, paper, and aluminum sheets (aluminum foil). Examples of resin sheets include resin sheets formed from resins such as polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polycarbonate resins, polyarylate resins, acrylic resins, polyphenylene sulfide resins, polystyrene resins, vinyl resins, vinyl chloride resins, polyimide resins, epoxy resins, polyethylene, polypropylene, and polyolefin resins such as polynorbornene. Furthermore, the laminate may comprise a metal laminated on these sheets, for example, a laminate comprising a metal laminated on a polyethylene terephthalate (PET) sheet. Among the above substrates, polypropylene, polyethylene terephthalate, polyethylene, etc. are preferred because they can produce laminate sheets with good stretchability, light transmittance, and rigidity. The substrate may contain one or more optional components as long as the effects of the present invention are not impaired. The substrate may contain an ultraviolet absorber, an antioxidant, an antistatic agent, a surfactant, a pigment, a fluorescent whitening agent, etc. The substrate may contain inorganic particles containing silica, calcium carbonate, titanium oxide, etc., or organic particles containing acrylic resin, styrene resin, etc.
[0063] [Method of Coating Gas Barrier Coating Agent] The method of coating the gas barrier coating agent includes a printing method and is not particularly limited, and any known coating method can be used. Examples of coating methods include wire bar coating, die coating, cast coating, slot coating, omega coating, spiral coating, controlled seam coating, slot coating, dot coating, hot melt applicator coating, hot melt coater coating, blade coating, dip coating, gravure coating, microgravure coating, curtain spray coating, bead coating, hot melt roll coater coating, and spin coating. Examples of printing methods include inkjet printing, spray printing, roll coating, doctor roll printing, doctor blade printing, curtain coating, slit coating, screen printing, reverse printing, push coating, and slit coater printing. After the oxygen barrier laminate is applied to the substrate by these methods, it may be heated and dried or dried under reduced pressure as needed to remove the solvent or promote crosslinking. The drying conditions are not particularly limited as long as they do not deteriorate the substrate, and depend on the film thickness, substrate, and selected organic solvent, but hot air heating at about 40 to 200°C is preferably used.
[0064] The thickness of the gas barrier coating agent layer (coated product) is not particularly limited, but is preferably a thin film for the purpose of preventing cracking and the like when folded, and is preferably 0.1 to 200 μm in a dry state, more preferably 0.5 to 20 μm, and even more preferably 1.0 to 10.0 μm. Furthermore, the gas barrier coating agent layer formed here may be laminated in one or more layers on one or both sides of the substrate. When multiple gas barrier coating layers are provided, the compositions of the layers may be the same or different. For example, after coating one side of the substrate with the gas barrier coating agent, a drying process may be performed, and then the same water vapor barrier layer may be formed in a similar process to form two layers, or different gas barrier coating agents may be formed to form three layers.
[0065] [Method for curing the gas barrier coating layer] The gas barrier coating agent according to an embodiment of the present invention is most preferably applied by various coating methods and then passed through an electron beam irradiator to obtain a cured coating film (gas barrier layer). In the case of electron beam irradiation, the irradiation dose varies depending on the film thickness and the desired degree of curing, but for a film thickness of 10 μm or less, it is desirable to irradiate at an acceleration voltage of 80 to 150 kV and a dose of 10 to 100 kGy, preferably at an acceleration voltage of 100 to 120 kV and a dose of 30 to 80 kGy. After electron beam irradiation, heating can be carried out as necessary to promote curing.
[0066] In addition to electron beam curing, the gas barrier coating agent can also be suitably cured by ultraviolet irradiation to obtain a cured coating film. When using ultraviolet irradiation, it is preferable to add the above-mentioned photopolymerization initiator, photosensitizer, etc. to the gas barrier coating agent. Examples of ultraviolet irradiation means that can be used include high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, excimer laser lamps, xenon lamps, and ultraviolet light-emitting diodes (UV-LEDs).
[0067] Among ultraviolet irradiation means, UV-LEDs have the advantage of emitting ultraviolet light with a narrow wavelength range and being easily miniaturized. Therefore, the irradiation wavelength and usage method of the UV-LED can be adjusted to some extent to suit the characteristics of the photopolymerization initiator in the gas barrier coating agent. The peak wavelength of the UV-LED used is preferably 280 to 420 nm, and particularly preferably 320 to 400 nm.
[0068] When using an ultraviolet irradiation means (ultraviolet lamp) other than a UV-LED as the ultraviolet irradiation means, a metal halide lamp is preferably used from the viewpoint that it can efficiently emit ultraviolet rays in the UV-A region and allow the irradiation light to reach the inside of the ink coating sufficiently. Note that a metal halide lamp can also be used in combination with the above-mentioned UV-LED.
[0069] The maximum UV intensity is 80mW / cm 2 It is preferable that the power is 120 mW / cm or more. 2The integrated light amount during irradiation varies depending on the type and content of the polymerizable monomer and the photopolymerization initiator, but is preferably 100 mJ / cm or more. 2 It is preferable to set the dose to 150 mJ / cm or more. 2 More preferably, it is 200 mJ / cm or more. 2 It is more preferable that the above
[0070] When a gas barrier coating agent is cured by electron beam or ultraviolet light, the usual process is to apply the coating, dry the solvent, and then irradiate the solvent with electron beams or ultraviolet light to obtain a cured coating film. However, if the binder resin used has a high molecular weight, molecular mobility is restricted, and the degree of crosslinking can sometimes be improved by prioritizing the polymerization reaction in a wet state. In other words, by limiting the solvent drying process to pre-drying to a level where a certain amount of solvent remains, irradiating the solvent with electron beams or ultraviolet light, and then completely drying the resulting coating, a more highly crosslinked coating film can be obtained, potentially improving its barrier properties and water resistance.
[0071] [Optional Layers] In addition to the substrate and gas barrier layer, the gas barrier laminate may include an optional organic or inorganic layer. Examples of optional layers include an anchor coat layer, a printing ink layer, an adhesive layer, a top coat layer, or an overcoat layer. One or more of these layers may be included. The optional layer is not particularly limited, but may be formed directly on the substrate layer or via a gas barrier layer. For example, a protective layer and an adhesive layer may be provided on the gas barrier layer as needed to protect the oxygen barrier composition layer or improve its abrasion resistance. The anchor coat layer is preferably formed between the gas barrier layer and the substrate layer, and the top coat layer is preferably formed on the gas barrier layer formed via the substrate. The thickness of the laminate when the optional layer is provided is not particularly limited, but is preferably 0.1 to 200 μm in a dry state, more preferably 0.5 to 20 μm, and even more preferably 1.0 to 10.0 μm.
[0072] The method for laminating the organic or inorganic layer is not particularly limited. For example, the layers may be laminated by a wet process such as coating, or by overlaying layers using film, extrusion, or lamination. Alternatively, the laminate may include layers formed by a vacuum process such as vapor deposition or CVD. Examples of materials for the organic layer include polyvinyl alcohol, polyolefins (polyethylene, polypropylene, poly-4-methyl-1-pentene, polybutene, etc.), cyclic olefin polymers, polyesters (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyamides (nylon-6, nylon-66, polymetaxylene adipamide, etc.), polyphenylene sulfide, polyethyleneimine, and polyimides. These may be used alone or in combination of two or more. Examples of materials for the inorganic layer include metals and semimetals such as chromium, zinc, cobalt, aluminum, tin, and silicon, as well as oxides, nitrides, nitrides, sulfides, and phosphides of the aforementioned metals and semimetals, such as silica, alumina, titanium oxide, zinc oxide, and silicon nitride. These may be used alone or in combination of two or more. When one or more oxygen barrier composition layers and one or more organic or inorganic layers are provided on one or both sides of the substrate, the order of lamination of these layers is arbitrary.
[0073] The laminate may further have a heat-sealable heat-fusible layer as needed. The heat-fusible layer of the laminate makes it heat-sealable and suitable for use as a packaging material.
[0074] [Applications] The laminate can be used as a multilayer packaging material for the purpose of protecting food, medicines, etc. When used as a multilayer packaging material, the layer structure can be changed depending on the contents, the environment of use, and the form of use. There are no particular restrictions on the application, but the laminate can be suitably used for food, daily necessities, electronic materials, medical use, etc., which require high barrier properties.
[0075] <Examples of Embodiments> The present invention includes, for example, the following embodiments. The embodiments of the present invention are not limited to the following. [1] A gas barrier coating agent comprising a water-soluble polysaccharide (A1), a compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more but less than 300, and a metal salt (C) having, as a ligand, a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more but less than 300. [2] The gas barrier coating agent according to [1] above, wherein the water-soluble polysaccharide (A1) comprises chitosan. [3] The gas barrier coating agent according to [1] above or [2] above, wherein, based on 100% by mass of the solids content of the gas barrier coating agent, the content of the water-soluble polysaccharide (A1) is 20 to 70% by mass, the content of the compound (B) is 10 to 60% by mass, and the content of the metal salt (C) is 10 to 70% by mass. [4] A gas barrier coating agent comprising: a compound (A2) having an amino group and a hydroxyl group; a compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond, and having a molecular weight of 50 or more and less than 300; and a metal salt (C) having as a ligand the compound having an anionic hydrophilic group and an ethylenically unsaturated double bond, and having a molecular weight of 50 or more and less than 300, wherein the compound (A2) has an amine value of 30 to 600 mg KOH / g and a hydroxyl value of 400 to 1,300 mg KOH / g. [5] The gas barrier coating agent according to [4] above, wherein the compound (A2) having an amino group and a hydroxyl group comprises a vinylamine-vinyl alcohol copolymer. [6] The gas barrier coating agent according to [4] or [5] above, wherein, based on 100% by mass of the solid content of the gas barrier coating agent, the content of compound (A2) is 20 to 70% by mass, the content of compound (B) is 3 to 60% by mass, and the content of metal salt (C) is 10 to 70% by mass. [7] The gas barrier coating agent according to any of [1] to [6] above, wherein the central metal of metal salt (C) comprises at least one selected from the group consisting of zinc, calcium, magnesium, and aluminum. [8] The gas barrier coating agent according to any of [1] to [7] above, which is used for packaging. [9] A laminate comprising a substrate and a gas barrier layer formed on the substrate using the gas barrier coating agent according to any of [1] to [8] above.
[10] A method for producing a laminate, comprising the steps of: applying the gas barrier coating agent according to any one of [1] to [8] above to a substrate to obtain a coated product; and irradiating the coated product with ultraviolet light or electron beams to form a gas barrier layer on the substrate.
[0076] The disclosure of this application is related to the subject matter described in Japanese Patent Application No. 2023-72411 filed on April 26, 2023, Japanese Patent Application No. 2023-200448 filed on November 28, 2023, and Japanese Patent Application No. 2023-215371 filed on December 21, 2023, the entire disclosures of which are incorporated herein by reference.
[0077] Specific examples of the present invention will be described below together with comparative examples, but the present invention is not limited to the following examples. In the following examples and comparative examples, "parts" and "%" represent "parts by mass" and "% by mass", respectively, unless otherwise specified.
[0078] Example I: Gas Barrier Coating Agent and Laminate Containing Water-Soluble Polysaccharide (A1) Preparation of Metal Salt (C) Aqueous Solution [Calcium Acrylate Aqueous Solution] 10 parts of calcium hydroxide powder (FUJIFILM Wako Pure Chemical Industries, Ltd., special grade, 0.135 mol) and 64 parts of ion-exchanged water were placed in a 225 ml mayonnaise bottle (glass bottle) and gently mixed using a homodisper to prevent lumps from forming. While stirring, 20 parts (0.278 mol) of acrylic acid was gradually added dropwise, ensuring that the temperature in the system did not exceed 50°C due to an exothermic reaction. The addition of acrylic acid changed the cloudy dispersion to a transparent liquid, and stirring was continued for approximately 10 minutes to terminate the reaction. After filtration through a #200 filter cloth, ion-exchanged water was added to a solids content of 30.0%, yielding a calcium acrylate aqueous solution. The molecular weight of acrylic acid was 72.1 g / mol.
[0079] [Magnesium acrylate aqueous solution] 10 parts of magnesium hydroxide powder (FUJIFILM Wako Pure Chemical Industries, Ltd., special grade, 0.171 mol) and 74 parts of ion-exchanged water were placed in a 225 ml mayonnaise bottle and gently mixed using a homodisper to prevent lumps from forming. While stirring, 25 parts (0.347 mol) of acrylic acid was gradually added dropwise, so as not to allow the temperature in the system to exceed 50°C due to an exothermic reaction. The addition of acrylic acid caused the mixture to change from a cloudy white dispersion to a transparent liquid, and stirring was continued for approximately 10 minutes to terminate the reaction. After filtration through a #200 mesh filter cloth, the solids content was adjusted to 30.0%, yielding an aqueous magnesium acrylate solution.
[0080] [Zinc acrylate aqueous solution] 10 parts of zinc oxide powder (FUJIFILM Wako Pure Chemical Industries, Ltd., special grade, 0.123 mol) and 60 parts of ion-exchanged water were placed in a 225 ml mayonnaise bottle and gently mixed using a homodisper to prevent lumps from forming. While stirring, 18.2 parts (0.253 mol) of acrylic acid was gradually added dropwise, so as not to allow the temperature in the system to exceed 50°C due to an exothermic reaction. The addition of acrylic acid caused the dispersion to change from a cloudy white state to a transparent liquid, and stirring was continued for approximately 10 minutes to terminate the reaction. After filtration through a #200 mesh filter cloth, the solids content was adjusted to 30.0%, yielding an aqueous zinc acrylate solution.
[0081] [Aqueous Solution of Zinc 2-Acrylamido-2-methylpropanesulfonate] 5.0 parts of zinc oxide powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade, 0.061 mol) and 60 parts of ion-exchanged water were placed in a 225 ml mayonnaise bottle and gently mixed using a homodisper to prevent lumps from forming. While stirring, 25.7 parts (0.124 mol) of 2-acrylamido-2-methylpropanesulfonic acid was gradually added dropwise, ensuring that the temperature in the system did not exceed 50°C due to an exothermic reaction. The dropwise addition of 2-acrylamido-2-methylpropanesulfonic acid changed the cloudy dispersion state to a transparent liquid, and stirring was continued for approximately 10 minutes to terminate the reaction. The mixture was filtered through a #200 mesh filter cloth and adjusted to a solids content of 30.0%, yielding an aqueous solution of zinc 2-acrylamido-2-methylpropanesulfonate. The molecular weight of 2-acrylamido-2-methylpropanesulfonic acid is 207.3 g / mol.
[0082] [Aqueous Polyurethane Solution] A four-necked 2000 ml flask equipped with a reflux condenser, a dropping funnel, a gas inlet tube, a stirrer, and a thermometer was charged with 240 parts of PTG-2000SN (manufactured by Hodogaya Chemical Co., Ltd., polytetramethylene glycol having a number average molecular weight of 2000), 24 parts of PEG2000 (polyethylene glycol having a number average molecular weight of 2000), 35 parts of dimethylolbutanoic acid (manufactured by HighChem Co., Ltd.), 75 parts of isophorone diisocyanate (manufactured by Evonik Degussa Japan Co., Ltd.), and 94 parts of MEK (methyl ethyl ketone), and the mixture was purged with dry nitrogen. The temperature was gradually raised to 85°C under stirring, and the mixture was allowed to react for 5 hours. Next, while cooling, a mixed solution of 8.9 parts of 28% aqueous ammonia, 900 parts of ion-exchanged water, and 119 parts of isopropyl alcohol was gradually added dropwise to the obtained solvent-based polyurethane resin to neutralize it and make it water-soluble. The solvent was then removed by distillation under reduced pressure, and the residue was replaced with ion-exchanged water to obtain an aqueous polyurethane resin solution (PU-1) with a solids content of 24%. PU-1 had 6.4% polyethylene glycol-derived structural units, a weight-average molecular weight of 30,000, a glass transition temperature of −80° C., and an acid value of 35 mg KOH / g.
[0083] <Preparation of Gas Barrier Coating Agent> [Example I-1] 10 parts of chitosan powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Chitosan 10), 110 parts of ion-exchanged water, and 10 parts of acrylic acid were placed in a 225 ml mayonnaise bottle, and the bottle was closed and stirred with a roller stirrer for 2 hours to dissolve the chitosan. After removing any remaining insoluble matter using a filter cloth, 66.7 parts of an aqueous calcium acrylate solution was added, and the bottle was stirred again with the roller stirrer for 30 minutes to obtain a transparent, viscous gas barrier coating agent.
[0084] Examples I-2 to 15, 17, and 18 Gas barrier coating agents were obtained in the same manner as in Example I-1, except that the compounds and the amounts thereof were changed to those shown in Table I-1.
[0085] Example I-16: A 450 ml mayonnaise bottle was charged with 10 parts of high molecular weight chitosan powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Chitosan 100), 250 parts of ion-exchanged water, 5 parts of methacrylic acid, and 5 parts of Light Ester P-1M (manufactured by Kyoeisha Chemical Co., Ltd.), and the bottle was capped and stirred for 2 hours with a roller stirrer to dissolve the chitosan. After removing any remaining insoluble matter using a filter cloth, 10 parts of an aqueous zinc acrylate solution was added, and the mixture was stirred again with the roller stirrer for 30 minutes. Two parts of aluminum acrylate powder (manufactured by Asada Chemical Industry Co., Ltd.) and 80 parts of glass beads (5 μm) were added, and the mixture was shaken and stirred for 1 hour using a Scandex wet media disperser to complete the dispersion. The glass beads were removed using a filter cloth, and a gas barrier coating agent was obtained.
[0086] Comparative Examples I-1 to I-4 Coating agents were obtained in the same manner as in Example I-1, except that the compounds and the amounts thereof were changed to those shown in Table I-2.
[0087] [Comparative Example I-5] A 450 ml mayonnaise bottle was charged with 10 parts of ethylene-vinyl alcohol copolymer (EVOH) powder (AQ-4104, manufactured by Kuraray Co., Ltd.) and 200 parts of ion-exchanged water, and the bottle was then capped and placed in a 95°C oven for 1 hour. After returning to room temperature, 10 parts of acrylic acid was added, and the mixture was stirred with a roller stirrer and filtered using a filter cloth. 33.3 parts of a 30% aqueous zinc acrylate solution was added, and the mixture was stirred again with the roller stirrer for 30 minutes to obtain a coating agent.
[0088] Comparative Example I-6 41.7 parts of aqueous polyurethane (PU-1), 20 parts of ion-exchanged water, and 12.5 parts of Carbodilite E-02 (manufactured by Nisshinbo Co., Ltd.) were placed in a 225 ml mayonnaise bottle, and the mixture was stirred and mixed using a homodisper to obtain a coating agent.
[0089] [Comparative Example I-7] A 225 ml mayonnaise bottle was charged with 10 parts of polyacrylic acid (manufactured by Wako Pure Chemical Industries, Ltd., average molecular weight 25,000), 40 parts of ion-exchanged water, and 5 parts of Denacol EX-313 (manufactured by Nagase ChemteX Corporation), and the mixture was stirred and mixed using a Homodisper to obtain a coating agent.
[0090]
[0091]
[0092] The abbreviations and properties of the raw materials listed in Tables I-1 and I-2 are as follows: The compound amounts listed in the tables represent the solid amounts.
[0093] (Water-soluble polysaccharides (A1)) Chitosan 10: Manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., low molecular weight product, deacetylation rate of 80.0 mol% or more Chitosan 100: Manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., high molecular weight product, deacetylation rate of 80.0 mol% or more Guar gum: white powder, product name Guapak PF-20 MP Gokyo Food & Chemical Co., Ltd. Xanthan gum: white powder, product name Labolgum GS-C MP Gokyo Food & Chemical Co., Ltd.
[0094] (Compounds having an anionic hydrophilic group and an ethylenically unsaturated double bond) Acrylic acid: manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., molecular weight 72.1 g / mol Methacrylic acid: manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., molecular weight 86.1 g / mol AAmSA (2-acrylamido-2-methylpropanesulfonic acid): manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., molecular weight 207.3 g / mol Light Ester P-1M: 2-methacryloxyethyl acid phosphate, manufactured by Kyoeisha Chemical Co., Ltd., molecular weight 210 g / mol Light Ester P-2M: 2-methacryloxyethyl acid phosphate, manufactured by Kyoeisha Chemical Co., Ltd., molecular weight 322 g / mol *The molecular weights of Light Ester P-1M and Light Ester P-2M were calculated from the chemical structures of the main components.
[0095] (Metal Salt (C)) Calcium acrylate: 30% aqueous calcium acrylate solution prepared above Magnesium acrylate: 30% aqueous magnesium acrylate solution prepared above Zinc acrylate: 30% aqueous zinc acrylate solution prepared above Zinc AAmSA: 30% aqueous zinc 2-acrylamido-2-methylpropanesulfonate solution prepared above Aluminum acrylate: white powder, manufactured by Wako Pure Chemical Industries, Ltd.
[0096] (Resin (D)) EVOH: ethylene-vinyl alcohol copolymer AQ-4104 (manufactured by Kuraray Co., Ltd.) Aqueous polyurethane (PU-1): the aqueous polyether polyurethane resin prepared above, solid content 24%, average molecular weight 30,000, acid value 35 mgKOH / g Polyacrylic acid: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., average molecular weight 25,000
[0097] (Crosslinking Agent (E)) Carbodilite E-02: carbodiimide crosslinking agent, manufactured by Nisshinbo, Inc., carbodiimide equivalent 445 g / eq., solid content 40% Denacol EX-313: glycerol polyglycidyl ether (epoxy crosslinking agent), manufactured by Nagase ChemteX Corporation, epoxy equivalent 141 g / eq.
[0098] [Preparation of Laminates] In Examples I-1 to I-18 and Comparative Examples I-1 to I-7, the prepared coating agents were applied to a PET substrate (E-5102, manufactured by Toyobo Co., Ltd., film thickness 25 μm) using a Mayer bar. The number of the Mayer bar was selected so that the coating film thickness would fall within 3 to 5 μm when measured at multiple locations. After coating, the coated material was evaporated in a drying oven at 75°C for 3 minutes to remove the solvent, and then cured using an electron beam irradiator EC250 / 15 / 180L manufactured by Iwasaki Electric Co., Ltd. at an acceleration voltage of 110 kV and an electron beam dose of 70 kGy. Laminates were prepared as shown in Tables I-1 and I-2, and used as samples to evaluate the physical properties of the cured coating film.
[0099] [Evaluation of physical properties of cured coating film] <Oxygen permeability measurement> The oxygen permeability of the laminates obtained in Examples I-1 to I-18 and Comparative Examples I-1 to I-7 was measured under conditions of a temperature of 23°C and 65% RH and a temperature of 23°C and 90% RH. RH indicates relative humidity. The oxygen permeability was measured by the isobaric method using an oxygen permeability measuring device OX-TRAN2 / 22 manufactured by MOCON Corporation in accordance with JIS K 7126. The measurement area of the laminate set in the measurement cell was 50 cm. 2 The oxygen barrier properties required for general packaging materials are an oxygen permeability of 1 cc / m under conditions of a temperature of 23°C and a relative humidity of 65% RH. 2 If the permeability is less than 20 cc / m under the above conditions, the performance is sufficient, and in addition, the permeability is so excellent that the deterioration of the barrier properties under high humidity conditions can be suppressed. 2Barrier films with oxygen permeability of 1.0 cc / m or more are marked as OVER because the reproducibility of oxygen permeability is low. The oxygen permeability measured under normal humidity and high humidity was evaluated according to the following criteria, and the results are shown in Tables I-1 and I-2. (Oxygen permeability under normal humidity) A: Excellent 1.0 cc / m 2 ・Less than day・atm B: Good 1.0cc / m 2 ・day・atm or more 5.0cc / m 2 ・day・atm or less C: Practical level 5.0cc / m 2 ・day・atm or more 20.0cc / m 2 ・day・atm Less than D: Poor 20.0cc / m 2 ・day・atm or more (oxygen permeability under high humidity) A: Excellent 3.0cc / m 2 ・Less than day・atm B: Good 3.0cc / m 2 ・day・atm or more 10.0cc / m 2 ・day・atm or less C: Practical level 10.0cc / m 2 ・day・atm or more 20.0cc / m 2 ・day・atm Less than D: Poor 20.0cc / m 2 ・day・atm or more
[0100] <Water-Rubbing Resistance> Water-rubbing resistance was evaluated using the laminates obtained in Examples I-1 to I-18 and Comparative Examples I-1 to I-7. A cotton swab thoroughly wetted with water was rubbed from one side from the uncoated substrate portion to the coated portion a certain number of times, and the degree of dissolution of the edge of the coated portion, the degree of swelling of the rubbed portion, and the degree of abrasion of the cured coating surface were visually evaluated. The ratings were determined according to the following criteria and are shown in Tables I-1 and I-2. (Evaluation criteria) A: Excellent - No change in appearance even after rubbing 200 times or more B: Good - Changes in appearance such as swelling and abrasion of the cured coating surface occurred after 200 rubs C: Practical level - Edge dissolution occurred after 100 to less than 200 rubs D: Poor - Dissolution occurred at the edge or the entire rubbed area after less than 100 rubs, and exposure of the substrate
[0101] <Adhesion to Substrate> The laminates obtained in Examples I-1 to I-18 and Comparative Examples I-1 to I-7 were used to evaluate adhesion to substrates. Measurements were performed using adhesive tape (cellophane tape (width: 12 mm) manufactured by Nichiban Co., Ltd.) attached to the coated surface and peeled off at an angle of 180 degrees. The area percentage of the cured coating film remaining on the substrate side was measured according to the following criteria, and the evaluation results are shown in Tables I-1 and I-2. (Evaluation criteria) A: Excellent, no peeling B: Good, peeling occurred (less than 40%) C: Practical level, peeling occurred (40% or more but less than 90%) D: Poor, peeling occurred (90% or more)
[0102] <HAZE> The transparency of the laminates obtained in Examples I-1 to I-18 and Comparative Examples I-1 to I-7 was evaluated using a spectroscopic haze meter SH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) to measure the turbidity (haze value) according to the following criteria, and the evaluation results are shown in Tables I-1 and I-2. (Evaluation criteria) A: Excellent Haze value less than 3.0% B: Good Haze value 3.0% or more and less than 6.0% C: Practical level Haze value 6.0% or more and less than 10.0% D: Poor Haze value 10.0% or more
[0103] As shown in Table I-1, the gas barrier coating material (cured coating film) of Example I not only exhibits excellent oxygen barrier properties under mild humidity conditions of 23°C and 65% RH, but also shows the ability to inhibit a decrease in barrier properties under high humidity conditions of 23°C and 90% RH. It also achieves high levels of substrate adhesion, transparency, and water resistance, demonstrating its suitability for use as a top coating for packaging materials.
[0104] Example II: Gas Barrier Coating Agent and Laminate Containing Compound (A2) Having an Amino Group and a Hydroxyl Group Preparation of Compound (A2) Having an Amino Group and a Hydroxyl Group (Preparation of Vinylamine-Vinyl Alcohol Copolymer) Referring to the production example in JP 2004-315792 A, the following vinylamine-vinyl alcohol copolymer resin powder was obtained through polymerization, hydrolysis, and purification processes. The amine value, hydroxyl value, and number-average molecular weight of the vinylamine-vinyl alcohol copolymer were determined using the methods described above. The specific method for calculating the hydroxyl value is as follows: Copolymer 1 is a copolymer containing 10.2 mol% vinylamine units and 89.8 mol% vinyl alcohol units. The content ratio (mol%) of the monomer units was calculated using the masses and molecular weights of N-vinylformamide and vinyl acetate used in the polymerization. The molecular weight (M) of the polymer structural unit contained in copolymer 1 can be calculated as the weighted average of vinylamine units (molecular weight 43.07) and vinyl alcohol units (molecular weight 44.05), and is 43.95. The number of hydroxyl groups (A) in the polymer structural unit is 0.898, since the content of vinyl alcohol units having one hydroxyl group is 89.8 mol%. Therefore, the hydroxyl value of copolymer 1 is 1146 mg KOH / g, calculated from (Equation 2) hydroxyl value = 56106 × 0.898 (A) / 43.95 (M). Copolymers 2 and 3 were also calculated in the same way. Copolymer 1: amine value 130 mg KOH / g, hydroxyl value 1146 mg KOH / g, number average molecular weight 22000 Copolymer 2: amine value 213 mg KOH / g, hydroxyl value 1065 mg KOH / g, number average molecular weight 32000 Copolymer 3: amine value 300 mg KOH / g, hydroxyl value 980 mg KOH / g, number average molecular weight 27000
[0105] <Preparation of Aqueous Solution of Metal Salt (C)> In the same manner as in Example I, a metal salt (C) having as a ligand a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more but less than 300 was obtained.
[0106] <Preparation of Gas Barrier Coating Agent> [Example II-1] 10 parts of copolymer 1 powder and 50 parts of ion-exchanged water were placed in a 225 ml mayonnaise bottle, and after the lid was placed, the bottle was stirred and mixed for 20 minutes using a roller mixer. The bottle was heated in an oven at 95°C for 1 hour to fully dissolve the crystals, and then insoluble matter was removed using a filter cloth. 10 parts of acrylic acid and 66.7 parts of a 30% aqueous calcium acrylate solution (solids amount: 20 parts) were added to the filtered aqueous solution, and the mixture was stirred and mixed for 20 minutes using a roller mixer to obtain a transparent, viscous gas barrier coating agent.
[0107] Examples II-2 to 13, 15 to 19 Gas barrier coating agents were obtained in the same manner as in Example II-1, except that the compounds and the amounts thereof were changed to those shown in Table II-1.
[0108] Example II-14: 10 parts of Copolymer 3, 60 parts of ion-exchanged water, and 10 parts of acrylic acid were placed in a 225 ml mayonnaise bottle, the jar was capped, and the mixture was stirred and mixed for 20 minutes using a roller mixer. The mixture was heated in an oven at 95°C for 1 hour to fully dissolve the crystals, and then the remaining insoluble matter was removed using a filter cloth. To the filtered aqueous solution, 10 parts of a zinc acrylate aqueous solution (3 parts solids), 2 parts of aluminum acrylate powder (manufactured by Asada Chemical Industry Co., Ltd.), and 30 parts of glass beads (5 μm) were added, and the mixture was shaken and stirred using a Scandex wet media disperser for 1 hour to complete the dispersion. The glass beads were removed using a filter cloth, yielding a gas barrier coating agent.
[0109] Comparative Examples II-1 to II-4 Coating agents were obtained in the same manner as in Example II-1, except that the compounds and the amounts thereof were changed to those shown in Table II-2.
[0110] Comparative Example II-5: 33.3 parts of polyethyleneimine (P-1000, manufactured by Nippon Shokubai Co., Ltd., solids content 30%, amine value 18 mmol / g), 5 parts of ion-exchanged water, and 15 parts of acrylic acid were placed in a 225 ml mayonnaise bottle and stirred using a roller mixer. 66.7 parts of a 30% aqueous zinc acrylate solution was added, and the mixture was stirred again using the roller mixer for 30 minutes to obtain a coating agent.
[0111] Comparative Example II-6 41.7 parts of aqueous polyurethane (PU-1, solid content 24%), 20 parts of ion-exchanged water, and 12.5 parts of Carbodilite E-02 (manufactured by Nisshinbo Industries, Inc., solid content 40%) were placed in a 225 ml mayonnaise bottle, and the mixture was stirred and mixed using a homodisper to obtain a coating agent.
[0112] [Comparative Example II-7] A 225 ml mayonnaise bottle was charged with 10 parts of polyacrylic acid (manufactured by Wako Pure Chemical Industries, Ltd., average molecular weight 25,000), 40 parts of ion-exchanged water, and 5 parts of Denacol EX-313 (manufactured by Nagase ChemteX Corporation), and the mixture was stirred and mixed using a Homodisper to obtain a coating agent.
[0113]
[0114]
[0115] The abbreviations and properties of the raw materials listed in Tables II-1 and II-2 are as follows and as described above in Example I. The compound amounts listed in the tables represent solid amounts.
[0116] (Compound (A2) having an amino group and a hydroxyl group) Copolymer 1: amine value 130 mg KOH / g, hydroxyl value 1146 mg KOH / g, number average molecular weight 22000 Copolymer 2: amine value 213 mg KOH / g, hydroxyl value 1065 mg KOH / g, number average molecular weight 32000 Copolymer 3: amine value 300 mg KOH / g, hydroxyl value 980 mg KOH / g, number average molecular weight 27000
[0117] (Resin (D)) Polyethyleneimine (P-1000): manufactured by Nippon Shokubai Co., Ltd., solid content 30%, amine value 18 mmol / g (=1010 mg KOH / g)
[0118] [Preparation of Laminates] In Examples II-1 to II-19 and Comparative Examples II-1 to II-7, the prepared coating agents were applied to a PET substrate (Toyobo Co., Ltd., E-5102, film thickness 25 μm) using a Mayer bar. The number of the Mayer bar was selected so that the coating film thickness would fall within 3 to 5 μm when measured at multiple locations. After coating, the coated material was evaporated in a drying oven at 75°C for 3 minutes to remove the solvent, and then cured using an electron beam irradiator EC250 / 15 / 180L manufactured by Iwasaki Electric Co., Ltd. at an acceleration voltage of 130 kV and an electron beam dose of 70 kGy. Laminates were prepared as shown in Tables II-1 and II-2, and used as samples to evaluate the physical properties of the cured coating film.
[0119] [Evaluation of Physical Properties of Cured Coating Film] The physical properties of the cured coating film were evaluated in the same manner as in Example I. The evaluation results are shown in Tables II-1 and II-2.
[0120] As shown in II-1, the gas barrier coating material (cured coating film) of Example II not only exhibits excellent oxygen barrier properties under mild humidity conditions of 23°C and 65% RH, but also inhibits degradation of barrier properties under high humidity conditions of 23°C and 90% RH. Furthermore, it achieves high levels of substrate adhesion, transparency, and water resistance, demonstrating its suitability for top coating on packaging materials.
Claims
1. A gas barrier coating agent comprising: a water-soluble polysaccharide (A1); a compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more and less than 300; and a metal salt (C) having as a ligand a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more and less than 300.
2. The gas barrier coating agent according to claim 1, wherein the water-soluble polysaccharide (A1) includes chitosan.
3. A gas barrier coating agent according to claim 1 or 2, wherein, based on 100% by mass of the solid content of the gas barrier coating agent, the content of the water-soluble polysaccharide (A1) is 20 to 70% by mass, the content of the compound (B) is 10 to 60% by mass, and the content of the metal salt (C) is 10 to 70% by mass.
4. A gas barrier coating agent comprising: a compound (A2) having an amino group and a hydroxyl group; a compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond, and having a molecular weight of 50 or more and less than 300; and a metal salt (C) having as a ligand a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond, and having a molecular weight of 50 or more and less than 300, wherein the amine value of compound (A2) is 30 to 600 mg KOH / g and the hydroxyl value is 400 to 1,300 mg KOH / g.
5. The gas barrier coating agent according to claim 4, wherein the compound (A2) having an amino group and a hydroxyl group includes a vinylamine-vinyl alcohol copolymer.
6. The gas barrier coating agent according to claim 4 or 5, wherein the content of compound (A2) is 20 to 70 mass%, the content of compound (B) is 3 to 60 mass%, and the content of metal salt (C) is 10 to 70 mass%, based on 100 mass% of the solid content of the gas barrier coating agent.
7. The gas barrier coating agent according to any one of claims 1 to 6, wherein the central metal of the metal salt (C) includes at least one selected from the group consisting of zinc, calcium, magnesium, and aluminum.
8. The gas barrier coating agent according to any one of claims 1 to 7, which is used for packaging materials.
9. A laminate comprising a substrate and a gas barrier layer formed on the substrate using the gas barrier coating agent according to any one of claims 1 to 8.
10. A method for producing a laminate, comprising the steps of: applying the gas barrier coating agent according to any one of claims 1 to 8 to a substrate to obtain a coated product; and irradiating the coated product with ultraviolet light or electron beams to form a gas barrier layer on the substrate.
Citation Information
Patent Citations
Gas barrier coating
JP2004307731A
Aqueous coating agent and gas barrier film using the same
JP2018149779A
Gas-barrier film, gas-barrier layered product, and process for producing the same
WO2005108440A1
Aqueous polymerizable monomer composition, gas-barrier film, and method for producing such film
WO2006059773A1