Method for recovering alkali metal salt and apparatus for recovering alkali metal salt

The described method addresses the inefficiency in recovering high-purity alkali metal salts by adjusting pH, adding aluminum salts, and using nanofiltration to separate alkali metal ions, effectively reducing fluorine impurities and enhancing the recovery of alkali metal salts from waste materials and liquids.

WO2024225409A1PCT designated stage expired Publication Date: 2024-10-31TORAY INDUSTRIES INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016357
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-25
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Current methods for recovering high-purity alkali metal salts from waste materials and liquids, such as lithium ion battery electrolytes, are inefficient due to residual fluorine impurities, which hinder the production of high-purity lithium carbonate or hydroxide.

Method used

A method involving pH adjustment, aluminum salt addition, and nanofiltration using a specific nanofiltration membrane to separate alkali metal ions, effectively reducing fluorine impurities and achieving high-purity alkali metal salt recovery.

Benefits of technology

The method enables the efficient recovery of high-purity alkali metal salts like lithium and cesium by minimizing fluorine contamination, improving the purity and recovery efficiency of alkali metal salts from waste materials and liquids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention is a method for recovering an alkali metal salt from a solution X that contains: a compound HA having a pKa value of 3.0-5.0 and / or an anion A that forms compound HA; and an alkali metal ion. The method includes: (1) a pH adjustment step for adjusting the pH of the solution X to 0-4.0 when the pH exceeds 4; (2) an aluminum salt addition step for adding an aluminum salt to the solution X so that the molar concentration of aluminum is at least 0.25 times the total molar concentration of anions A, which is the sum of the molar concentration of compound HA in the solution X and the molar concentration of anions A present as ions in the solution X; and (3) a nanofiltration step for separating alkali metal ions to the permeation side from the solution X by means of a nanofiltration membrane following step (1) and step (2).
Need to check novelty before this filing date? Find Prior Art

Description

Method and apparatus for recovering alkali metal salts

[0001] The present invention relates to a method for recovering alkali metal salts and an apparatus for recovering alkali metal salts.

[0002] In recent years, the demand for mineral resources has expanded significantly in line with global industrial and economic development. While mineral resources are essential for a wide range of industries, including the semiconductor industry, many resources are technically difficult to extract in their entirety, making mining and refining them uneconomical, even when they are abundant in the Earth's crust. Furthermore, many resources are concentrated in specific regions. Meanwhile, environmental issues have also come into sharp focus, spurring the creation of a recycling-oriented society. In particular, the development of electric vehicles, their motors, and batteries has accelerated, due to their potential to reduce carbon dioxide emissions. With regard to batteries in particular, lithium-ion secondary batteries are expected to become the primary battery for electric vehicles due to their energy density and light weight.

[0003] Lithium compounds are used, for example, for lithium carbonate, which is used as an electrode material for lithium-ion batteries, an additive for heat-resistant glass, and for surface acoustic wave filters. High-purity lithium carbonate is used in filters and transmitters for mobile phones and car navigation systems. Lithium bromide is used as a refrigerant absorber in absorption refrigerators for large air conditioning systems in buildings and factories. Lithium hydroxide is used as a raw material for grease in automobiles and for lithium batteries (primary and secondary). Metallic lithium is used as foil for the anode material in primary batteries and as a raw material for butyl lithium, a synthetic rubber catalyst.

[0004] Lithium is extracted from resources such as salt lake brine and ores, but new lithium supply sources are needed to meet the increasing demand for lithium for use in electric vehicles. In particular, there is a need for technology to efficiently recover lithium from waste materials and waste liquids generated in the manufacturing process of lithium-ion batteries.

[0005] For example, the electrolyte of a lithium ion battery is generally a lithium salt containing fluorine as a constituent element (LiPF 6 , LiBF 4 , LiAsF 6However, it is known that hydrolysis occurs when water gets mixed in (see, for example, Non-Patent Document 1). When the electrolyte undergoes hydrolysis, the battery performance deteriorates, so the electrolyte that deteriorates during use in the manufacturing process of lithium-ion batteries is discarded. Since the electrolyte contains a large amount of lithium, it needs to be recovered, but the fluorine contained in the electrolyte becomes an impurity when lithium is recovered as lithium carbonate or lithium hydroxide, so it needs to be separated.

[0006] Patent Document 1 describes a method in which an electrolyte is heated, the fluorine-containing solvent is removed, and the residue is leached with water to obtain an aqueous solution of lithium hydroxide.

[0007] Japanese Patent Application Publication No. 2005-197149

[0008] Tetsuya Kawamura and two others, "Decomposition Reaction of LiPF6 Electrolyte for Lithium Batteries," Kyushu University Graduate School of Science and Engineering Bulletin, Kyushu University Graduate School of Science and Engineering, December 2002, Vol. 24, No. 3, pp. 281-288

[0009] However, in the method described in Patent Document 1, although the amount of fluorine in the electrolyte is significantly reduced, some fluorine remains as lithium fluoride, and therefore, this method is insufficient for obtaining high-purity lithium hydroxide or lithium carbonate.

[0010] SUMMARY OF THE INVENTION An object of the present invention is to provide a method for recovering highly pure alkali metal salts from waste materials, waste liquids, ores, etc. containing mineral resources.

[0011] In order to achieve the above object, the present invention has the following configuration: [1] A method for recovering an alkali metal salt from a solution X containing a compound HA having a pKa of 3.0 or more and 5.0 or less and at least one of an anion A forming said compound HA and an alkali metal ion, the method comprising the following steps (1) to (3): (1) A pH adjustment step of adjusting the pH of the solution X to between 0 and 4.0 when the pH of the solution X exceeds 4.0. (2) An aluminum salt addition step of adding an aluminum salt to the solution X so that the aluminum molar concentration (mol / L) is 0.25 times or more the total anion A molar concentration (mol / L) of the sum of the molar concentration (mol / L) of the compound HA in the solution X and the molar concentration (mol / L) of the anion A present as ions in the solution X. (3) A nanofiltration step of separating alkali metal ions from the solution X after steps (1) and (2) to the permeate side using a nanofiltration membrane. [2] The method for recovering an alkali metal salt according to [1], wherein in step (1), the pH of the solution X is adjusted to between 1.0 and 3.0. [3] The method for recovering an alkali metal salt according to [1] or [2], wherein the pKa of the compound HA is between 3.0 and 4.0. [4] The method for recovering an alkali metal salt according to any one of [1] to [3] above, wherein in the step (2), an aluminum salt is added to the solution X so as to satisfy any one of the following conditions (a) to (d): Condition (a): When the pH of the solution X is 1.0 or more and 1.4 or less, the molar concentration of the aluminum relative to the total anion A molar concentration in the solution X is 0.5 times or more; Condition (b): When the pH of the solution X is greater than 1.4 and 1.9 or less, the molar concentration of the aluminum relative to the total anion A molar concentration in the solution X is 0.4 times or more; Condition (c): When the pH of the solution X is greater than 1.9 and 2.4 or less, the molar concentration of the aluminum relative to the total anion A molar concentration in the solution X is 0.3 times or more; and Condition (d): When the pH of the solution X is greater than 2.4 and 3.0 or less, the molar concentration of the aluminum relative to the total anion A molar concentration in the solution X is 0.25 times or more.[5] The method for recovering an alkali metal salt according to any one of [1] to [4], wherein the difference between the magnesium sulfate rejection rate when a 2000 mg / L aqueous magnesium sulfate solution at 25°C and pH 6.5 is passed through the nanofiltration membrane at an operating pressure of 0.5 MPa and the magnesium chloride rejection rate when a 2000 mg / L aqueous magnesium chloride solution at 25°C and pH 6.5 is passed through the nanofiltration membrane at an operating pressure of 0.5 MPa is 20% or less. [6] The method for recovering an alkali metal salt according to any one of [1] to [5], wherein the difference between the glucose rejection rate when a 1000 mg / L aqueous glucose solution at 25°C and pH 6.5 is passed through the nanofiltration membrane at an operating pressure of 0.5 MPa and the isopropyl alcohol rejection rate when a 1000 mg / L aqueous isopropyl alcohol solution at 25°C and pH 6.5 is passed through the nanofiltration membrane at an operating pressure of 0.5 MPa is 40% or more, and the glucose rejection rate is 70% or more and 95% or less. [7] The method for recovering an alkali metal salt according to any one of [1] to [6] above, wherein the compound HA contains fluorine. [8] The method for recovering an alkali metal salt according to any one of [1] to [7] above, wherein the alkali metal salt contains lithium. [9] An apparatus for recovering an alkali metal salt, comprising: a tank for storing a solution containing alkali metal ions; an aluminum salt adding means for adding an aluminum salt to the solution; and a nanofiltration means for separating alkali metal ions from the solution.

[10] The apparatus for recovering an alkali metal salt according to [9] above, comprising a pH adjusting means for adjusting the pH of the solution.

[0012] The method and apparatus for recovering alkali metal salts of the present invention make it possible to recover highly pure salts of alkali metals such as lithium and cesium from a solution containing alkali metal ions.

[0013] The following describes in detail the embodiments of the present invention, but the present invention is not limited to the following description and can be modified as desired without departing from the spirit of the present invention. In this specification, the unit of "molar concentration" is mol / L. In addition, in this specification, "mass" is synonymous with "weight."

[0014] <1> Method for recovering alkali metal salt The method for recovering alkali metal salt of the present invention is a method for recovering an alkali metal salt from a solution X containing a compound HA having a pKa of 3.0 to 5.0 and at least one of an anion A forming the compound HA and alkali metal ions, and includes the following steps (1) to (3): (1) a pH adjustment step of adjusting the pH of solution X to 0 to 4.0 when the pH of solution X exceeds 4.0; (2) an aluminum salt addition step of adding an aluminum salt to solution X so that the molar concentration of aluminum (mol / L) is 0.25 or more times the total molar concentration of anion A (mol / L), which is the sum of the molar concentration (mol / L) of compound HA in solution X and the molar concentration (mol / L) of anion A present as ions in solution X; and (3) a nanofiltration step of separating alkali metal ions from solution X after steps (1) and (2) to the permeate side using a nanofiltration membrane.

[0015] <2> Solution X Solution X contains alkali metal ions. The alkali metal ions contained in Solution X are ions that constitute alkali metal salts, and alkali metal salts consist of alkali metal ions and one or more conjugate bases (e.g., fluoride ions, chloride ions, nitrate ions, sulfate ions, carbonate ions, acetate ions, etc.). Examples of alkali metal salts include salts of lithium, sodium, potassium, rubidium, and cesium, but from the perspective of the value of the object to be recovered, it is preferable that Solution X contains a salt of lithium. That is, Solution X contains lithium ions (hereinafter referred to as "Li") as alkali metal ions. + Preferably, the compound includes a polyimide-containing polymer.

[0016] The alkali metal ion-containing solution X is preferably a solution prepared by dissolving a lithium-containing material in an acid, such as waste materials, waste liquids, ores, and slags generated in the manufacturing process of lithium-ion batteries.

[0017] A lithium ion battery is composed of components such as a positive electrode material, a negative electrode material, a separator, and an electrolyte. Any of these components containing lithium can be used as the material for solution X. The acid that dissolves the lithium-containing material preferably contains at least one acid selected from the group consisting of hydrochloric acid, sulfuric acid, and nitric acid.

[0018] The method for dissolving the lithium-containing material with an acid includes, for example, immersing the material in an acidic aqueous solution, but other methods may also be used as long as they can elute the desired alkali metal ions.

[0019] When the lithium-containing material is the electrolyte, for example, LiPF 5 is dissolved in an organic solvent such as ethylene carbonate (EC) or dimethyl carbonate (DMC). 6 However, it is preferable to dilute it with water from the viewpoint of the separation property of the nanofiltration membrane described later. 6 is hydrolyzed to hydrofluoric acid, phosphoric acid, and lithium hydroxide, and lithium becomes more easily permeable through the nanofiltration membrane, while fluorine easily forms a compound with aluminum, as described below. 6 The hydrolysis of

[0020] The temperature of the acidic aqueous solution to be contacted is preferably 10° C. or higher and 100° C. or lower from the viewpoint of elution efficiency of alkali metal ions. Furthermore, from the viewpoints of cost and safety, the temperature of the acidic aqueous solution is more preferably 20° C. or higher and 90° C. or lower.

[0021] The solution obtained by dissolving a lithium-containing material in acid does not always have a constant composition, and the composition may vary depending on the variations in the composition of various ions in the material, the dissolution conditions in the acid, and the like.

[0022] Furthermore, solution X contains at least one of compound HA having a pKa of 3.0 or more and 5.0 or less and an anion A that forms said compound HA. Compound HA generates anion A upon ionization. As a result of extensive research, the inventors have found that compound HA having a pKa of 3.0 or more and 5.0 or less and / or anion A that forms said compound HA form a compound with aluminum ions under acidic conditions of pH 4.0 or less, resulting in a significant decrease in the permeability of the nanofiltration membrane. Because the alkali metal salt to be recovered permeates the nanofiltration membrane, a decrease in the permeability of the compound formed from compound HA and / or anion A that forms said compound HA contributes to an improvement in the purity of the alkali metal salt in the nanofiltration membrane permeate.

[0023] The pKa of the compound HA is more preferably 3.0 or more and 4.0 or less, from the viewpoint of facilitating the formation of a compound with aluminum.

[0024] pKa is defined by the following equation (1) in the ionization equilibrium equation of HA → H + A at 25°C, using the concentration of compound HA at equilibrium [HA], the concentration of anions constituting compound HA [A], and the acid concentration [H]: pKa = -log([H] × [A] / [HA]) (1)

[0025] The pKa can be determined by any method such as titration. Examples of the compound HA include hydrogen fluoride, acetic acid, and formic acid. Among these, hydrogen fluoride is more preferred as the compound HA from the viewpoint of ease of forming a compound with aluminum ions.

[0026] If the concentration ratio of the total anion A molar concentration (mol / L) (hereinafter simply referred to as "total anion A molar concentration"), which is the sum of the molar concentration (mol / L) of compound HA and the molar concentration (mol / L) of anion A present as ions in solution X, to the molar concentration (mol / L) of alkali metal ions to be recovered in solution X, is P, P can be expressed by the following formula (2): Concentration ratio P = {total anion A molar concentration (mol / L)} / {molar concentration of alkali metal ions to be recovered (mol / L)} (2) The total anion A molar concentration specifically corresponds to the sum of the concentration [HA] of compound HA at equilibrium contained in solution X and the concentration [A] of anions constituting compound HA. Note that when anion A originates solely from compound HA added to solution X, the total anion concentration A corresponds to the anion concentration A when compound HA is fully ionized.

[0027] The concentration ratio P of the solution X is preferably 0.01 or more and 10 or less, and more preferably 0.05 or more and 7 or less.

[0028] Solution X may contain an organic compound. When the solution is an electrolyte for a lithium-ion battery, examples of the organic compounds include those described above. These organic compounds may act as foulants and may reduce the efficiency of alkali metal ion recovery. Therefore, these foulants may be removed by a pretreatment process described below.

[0029] When solution X contains lithium ions as alkali metal ions, the lithium ion concentration in the solution is preferably 0.5 mg / L or more and 10,000 mg / L or less. Having a lithium ion concentration in the solution of 0.5 mg / L or more improves the efficiency of lithium ion recovery by membrane separation. Having a lithium ion concentration in the solution of 10,000 mg / L or less prevents the osmotic pressure difference from increasing, improving the efficiency of membrane separation. The lithium ion concentration in the solution is more preferably 10 mg / L or more and 8,000 mg / L or less, and even more preferably 100 mg / L or more and 6,000 mg / L or less.

[0030] <3> Step (1): pH Adjustment Step Step (1) is a step of adjusting the pH of solution X to between 0 and 4.0. The pH adjustment step is performed when the pH of solution X exceeds 4.0. When the pH of solution X to be treated is 4.0 or less, a compound can be efficiently formed between aluminum ions and anions A ionized from compound HA in solution X and / or anions A that form compound HA contained in solution X. Furthermore, when the pH of solution X is 4.0 or less, precipitation of aluminum hydroxide on the membrane surface can be suppressed in the nanofiltration step described below, allowing efficient membrane separation using a nanofiltration membrane.

[0031] An example of a method for adjusting the pH of solution X to 0 or more and 4.0 or less is to add an acid. There are no particular limitations on the acid to be added, and examples thereof include sulfuric acid, hydrochloric acid, and nitric acid.

[0032] The pH of solution X is preferably adjusted to 0 or more and 3.0 or less, and more preferably 1.0 or more and 3.0 or less. When the pH is 0 or more, deterioration of the nanofiltration membrane due to acid can be suppressed, and when the pH is 3.0 or less, the nanofiltration membrane can maintain high alkali metal ion permeability.

[0033] The pH adjustment step is preferably carried out before the aluminum salt addition step described below. By carrying out the pH adjustment step before the aluminum salt addition step, precipitation of aluminum hydroxide can be suppressed, and the nanofiltration step described below can be carried out efficiently.

[0034] <4> Step (2): Aluminum Salt Addition Step Step (2) is a step of adding an aluminum salt at a molar concentration of 0.25 or more times the total anion A molar concentration (mol / L) (total anion A molar concentration), which is the sum of the molar concentration (mol / L) of compound HA in solution X and the molar concentration (mol / L) of anion A present as ions in solution X. By adding aluminum salt so that the molar concentration (mol / L) of aluminum is 0.25 or more times the total anion A molar concentration (mol / L), most of the anions A forming compound HA in solution X form compounds with aluminum ions, which are removed by the nanofiltration membrane in the subsequent stage. For example, when anion A is a fluoride ion, if the molar concentration of aluminum ions is relatively low relative to the molar concentration of fluoride ions, a compound AlF, which is a fluoride of aluminum ions, is formed. 4 - As the molar concentration of aluminum ions relative to fluorine ions increases, the main component of the aluminum ion fluoride becomes AlF 4 - →AlF 3 →AlF 2 + →AlF 2+ and transitions to.

[0035] The aluminum salt to be added in step (2) is not particularly limited, and examples thereof include aluminum sulfate, aluminum nitrate, and aluminum chloride.

[0036] Aluminum ions more easily form compounds with anions A at higher pH levels. Therefore, it is preferable to adjust the amount of aluminum salt added depending on the pH of solution X. Specifically, the amount of aluminum salt added is adjusted to satisfy one of the following conditions (a) to (d): Condition (a): When the pH of solution X is 1.0 or higher and 1.4 or lower, the molar concentration of aluminum relative to the total molar concentration of anions A in solution X is 0.5 or higher; Condition (b): When the pH of solution X is higher than 1.4 and 1.9 or lower, the molar concentration of aluminum relative to the total molar concentration of anions A in solution X is 0.4 or higher; Condition (c): When the pH of solution X is higher than 1.9 and 2.4 or lower, the molar concentration of aluminum relative to the total molar concentration of anions A in solution X is 0.3 or higher; Condition (d): When the pH of solution X is higher than 2.4 and 3.0 or lower, the molar concentration of aluminum relative to the total molar concentration of anions A in solution X is 0.25 or higher.

[0037] The aluminum salt is preferably added in an amount such that the molar concentration of aluminum relative to the total anion A molar concentration is 10 times or less, more preferably 1 time or less, and even more preferably 0.7 times or less. By adding an aluminum salt in an amount of 10 times or less, it is possible to prevent excessive aluminum from being mixed into the permeate in the subsequent nanofiltration step. In other words, it is preferable to adjust the molar concentration of aluminum relative to the total anion A molar concentration in accordance with the pH of solution X within the range of 0.25 to 10 times.

[0038] The metal ion concentration can be determined, for example, by analyzing the solution to be measured using an ICP optical emission spectrometer (e.g., Hitachi P-4010 ICP (inductively coupled plasma optical emission spectrometry) instrument) and quantifying the concentration (mol / L) of various ions.

[0039] The means for measuring the total anion A concentration in solution X is not particularly limited as long as it can measure the molar concentration of compound HA in solution X and the molar concentration of anion A in solution X, but for example, an ion chromatograph can be used for analysis in the case of inorganic substances, or a gas chromatograph can be used in the case of organic substances, and the concentrations (mol / L) of various ions can be determined by quantifying them. The ion chromatograph can measure the concentration of anion A when compound HA is completely ionized.

[0040] When a precipitate containing aluminum hydroxide is produced in the aluminum salt addition step, it is preferable to remove the precipitate by performing solid-liquid separation using a filter press or the like.

[0041] <5> Step (3): Nanofiltration Step In the present invention, the solution X (hereinafter also referred to as "solution X'") obtained after the steps (1) and (2) is treated with a nanofiltration membrane to separate the alkali metal salt into the permeate side.

[0042] <5-1> Nanofiltration Membrane The nanofiltration membrane used in this embodiment may have fractionation characteristics that fall between those of reverse osmosis membranes and ultrafiltration membranes. Membranes commonly known as reverse osmosis membranes can remove most organic substances and ions. On the other hand, ultrafiltration membranes typically do not remove most ionic species, but remove high-molecular-weight organic substances.

[0043] In order to separate alkali metal ions and polyvalent metal ions, the nanofiltration membrane preferably has a charge on the membrane surface, enabling both separation by pores (size separation) and electrostatic separation due to the charge. Such a nanofiltration membrane preferably satisfies either of the following conditions 1 and 2. <Condition 1 for nanofiltration membrane> The difference between the magnesium sulfate rejection rate when a 2000 mg / L aqueous magnesium sulfate solution at 25°C and pH 6.5 is passed through the membrane at an operating pressure of 0.5 MPa and the magnesium chloride rejection rate when a 2000 mg / L aqueous magnesium chloride solution at 25°C and pH 6.5 is passed through the membrane at an operating pressure of 0.5 MPa is 20% or less. <Nanofiltration membrane condition 2> The difference between the glucose removal rate when a 1000 mg / L aqueous glucose solution at pH 6.5 is passed through at an operating pressure of 0.5 MPa, 25°C, and 25°C and the isopropyl alcohol removal rate when a 1000 mg / L aqueous isopropyl alcohol solution at pH 6.5 is passed through at an operating pressure of 0.5 MPa is 40% or more, and the glucose removal rate is 70% or more and 95% or less. Hereinafter, in this specification, when simply referred to as "magnesium sulfate removal rate", it means the magnesium sulfate removal rate when a 2000 mg / L aqueous magnesium sulfate solution at 25 ° C. and pH 6.5 is permeated at an operating pressure of 0.5 MPa. When referred to as "magnesium chloride removal rate", it means the magnesium chloride removal rate when a 2000 mg / L aqueous magnesium chloride solution at 25 ° C. and pH 6.5 is permeated at an operating pressure of 0.5 MPa. When referred to as "glucose removal rate", it means the glucose removal rate when a 1000 mg / L aqueous glucose solution at 25 ° C. and pH 6.5 is permeated at an operating pressure of 0.5 MPa. When referred to as "isopropyl alcohol removal rate", it means the isopropyl alcohol removal rate when a 1000 mg / L aqueous isopropyl alcohol solution at 25 ° C. and pH 6.5 is permeated at an operating pressure of 0.5 MPa.

[0044] In condition 1, it is more preferable that the difference between the magnesium sulfate rejection rate and the magnesium chloride rejection rate is 15% or less. In condition 2, it is more preferable that the difference between the glucose rejection rate and the isopropyl alcohol rejection rate is 50% or more, and the glucose rejection rate is 80% or more and 90% or less. It is even more preferable that the nanofiltration membrane satisfies both conditions 1 and 2.

[0045] By having the glucose rejection rate, the difference between the glucose rejection rate and the isopropyl alcohol rejection rate, and the difference between the magnesium sulfate rejection rate and the magnesium chloride rejection rate of the nanofiltration membrane within the above ranges, the selective separation and recovery of alkali metal ions and polyvalent metal ions can be performed with high efficiency and over a long period of time, resulting in a highly efficient process. In particular, the inventors have found that by having the glucose rejection rate and the difference between the glucose rejection rate and the isopropyl alcohol rejection rate within the above ranges, the selective separation of alkali metal ions and compounds of aluminum anions A with various valences is high. Furthermore, the inventors have found that by having the difference between the magnesium sulfate rejection rate and the magnesium chloride rejection rate within the above ranges, the charge on the membrane surface becomes nearly neutral, making fouling by inorganic scale such as aluminum fluoride less likely to occur, and enabling long-term operation. Inorganic scale is likely to form during filtration in a relatively high pH range.

[0046] Nanofiltration membranes are made from polymers such as cellulose acetate polymers, polyamides, sulfonated polysulfones, polyacrylonitriles, polyesters, polyimides, and vinyl polymers. Nanofiltration membranes may be made from a single material or multiple materials. The membrane structure may be an asymmetric membrane with a dense layer on at least one side of the membrane and gradually increasing pore sizes from the dense layer toward the interior of the membrane or toward the other side, or a composite semipermeable membrane with a very thin separation functional layer made of a different material on the dense layer of the asymmetric membrane.

[0047] The composite semipermeable membrane is preferably, for example, a membrane having a porous support membrane containing polysulfone and a separation functional layer containing polyamide provided on the porous support membrane. The composite semipermeable membrane may also have a substrate in addition to the porous support membrane and the separation functional layer, in which case the porous support membrane is provided on the substrate. The polyamide is a thin film formed on the porous support membrane by a polycondensation reaction between a polyfunctional aliphatic amine and a polyfunctional aromatic acid halide.

[0048] The separating functional layer in the composite semipermeable membrane preferably contains 50% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, of a semi-aromatic crosslinked polyamide obtained by interfacial polycondensation of a divalent or higher polyfunctional aliphatic amine compound and a divalent or higher polyfunctional aromatic acid halide. The semi-aromatic crosslinked polyamide is particularly preferably composed solely of the polyamide. By containing 50% by mass or more of the semi-aromatic crosslinked polyamide, excessive densification due to π-π interactions derived from the aromatic rings in the semi-aromatic crosslinked polyamide is suppressed, resulting in excellent alkali metal ion permeability. Furthermore, the inventors have found, after extensive research, that when the relative humidity during interfacial polycondensation is controlled to 80% or more, the resulting composite semipermeable membrane exhibits particularly excellent membrane performance under acidic conditions. The relative humidity can be adjusted, for example, by using a precision air conditioning device.

[0049] The polyfunctional aliphatic amine is preferably an alicyclic diamine, more preferably a 4,4'-bipiperidine or piperazine derivative.

[0050] In addition, the molecular weight of the alicyclic diamine is preferably 90 or more and 160 or less. When the molecular weight of the alicyclic diamine is 90 or more, the diffusion coefficient of the amine is reduced, and polyamide is gradually formed during interfacial polycondensation, making it easier to form a separation functional layer with a uniform pore size in the film thickness direction from the early to middle stages of polycondensation. Also, usually, at the end of the early stage of polycondensation, excessive oligomers are generated on the surface of the support in contact with the organic layer, blocking the pores on the support surface, causing the pore size distribution in the film thickness direction to become non-uniform. However, when the molecular weight of the alicyclic diamine is 160 or less, the molecular weight of the generated oligomers is reduced and the interaction with the semi-aromatic crosslinked polyamide is reduced. Therefore, after forming the separation functional layer by the polycondensation reaction, the oligomers are easily detached from the separation functional layer, making it easier to form a separation functional layer with a uniform pore size in the film thickness direction. In addition, when the molecular weight of the alicyclic diamine is 90 or more and 160 or less, it is easier to form a membrane pore size that satisfies the above condition 2.

[0051] Examples of alicyclic diamines having a molecular weight of 90 or more and 160 or less include substituted piperazines in which the piperazine ring is substituted with an alkyl group having 1 to 3 carbon atoms (e.g., 2-methylpiperazine, 2-ethylpiperazine, 2-normal propylpiperazine, 2,2-dimethylpiperazine, 2,2-diethylpiperazine, 2,3-dimethylpiperazine, 2,3-diethylpiperazine, 2,5-dimethylpiperazine, 2,5-diethylpiperazine, 2,6-dimethylpiperazine, 2,6-diethylpiperazine, and 2,3,5,6-tetramethylpiperazine), and homopiperazine.

[0052] The polyfunctional aromatic acid halide is an aromatic acid halide having two or more halocarbonyl groups in one molecule, and is not particularly limited as long as it gives a semi-aromatic crosslinked polyamide upon reaction with the polyfunctional aliphatic amine. Examples of polyfunctional aromatic acid halides that can be used include halides of 1,3,5-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,3-benzenedicarboxylic acid, 1,4-benzenedicarboxylic acid, 1,3,5-benzenetrisulfonic acid, and 1,3,6-naphthalenetrisulfonic acid. Among polyfunctional aromatic acid halides, acid chlorides are preferred, and in particular, from the standpoints of economy, availability, ease of handling, ease of reactivity, and the like, trimesoyl chloride, which is an acid halide of 1,3,5-benzenetricarboxylic acid, isophthaloyl chloride, which is an acid halide of 1,3-benzenedicarboxylic acid, terephthaloyl chloride, which is an acid halide of 1,4-benzenedicarboxylic acid, 1,3,5-benzenetrisulfonic acid chloride, which is an acid halide of 1,3,5-benzenetrisulfonic acid, and 1,3,6-naphthalenetrisulfonic acid chloride, which is an acid halide of 1,3,6-naphthalenetrisulfonic acid. The polyfunctional aromatic acid halides may be used alone or in combination of two or more. However, by mixing the trifunctional trimesic acid chloride, 1,3,5-benzenetrisulfonic acid chloride, or 1,3,6-naphthalenetrisulfonic acid chloride with either the bifunctional isophthalic acid chloride or terephthalic acid chloride, the intermolecular gaps of the polyamide crosslinked structure are expanded, allowing for the production of membranes with a uniform pore size distribution over a wide range. The molar ratio of the trifunctional acid chloride to the bifunctional acid chloride is preferably 1:20 to 50:1, more preferably 1:1 to 20:1. Furthermore, by appropriately adjusting the ratio of the polyfunctional aromatic acid halide to the polyfunctional aliphatic amine added during interfacial polycondensation, it becomes easier to form membrane pores with a size that satisfies the above condition 1.

[0053] The composite semipermeable membrane can be obtained, for example, by forming a porous support membrane on a substrate, and then forming a separation functional layer containing a semi-aromatic crosslinked polyamide on the porous support membrane by polycondensation of a polyfunctional aliphatic amine and a polyfunctional aromatic acid halide.

[0054] <5-2> Separation by Nanofiltration Membrane Because alkali metal ions easily permeate nanofiltration membranes and aluminum ions have difficulty permeating nanofiltration membranes, it is possible to separate alkali metal ions from a compound composed of aluminum and anion A (hereinafter also referred to as "compound B") in solution X (solution X') after steps (1) and (2) have been performed. The nanofiltration membrane is preferably used in a state incorporated into an element such as a spiral-type element.

[0055] By sending solution X' to the nanofiltration membrane unit, a permeate having a lower concentration ratio P relative to solution X' and a concentrated solution having a higher concentration ratio P can be obtained. Alkali metal ions that easily pass through the nanofiltration membrane are separated on the permeate side. To increase the purity of the alkali metal salt, the permeate may be passed through the nanofiltration membrane unit again to obtain a permeate with an even lower concentration ratio P. Nanofiltration of the permeate may also be performed multiple times.

[0056] In the nanofiltration step, it is preferable to supply the solution to the nanofiltration membrane at an operating pressure in the range of 0.1 MPa to 8 MPa. An operating pressure of 0.1 MPa or higher improves the membrane permeation rate, while an operating pressure of 8 MPa or lower can prevent damage to the nanofiltration membrane. The operating pressure is more preferably 0.5 MPa to 6 MPa, and even more preferably 1 MPa to 4 MPa.

[0057] <6> Concentration step The alkali metal ion concentration (mg / L) in the permeate of the final-stage nanofiltration membrane unit is preferably 1 mg / L or more, more preferably 10 mg / L or more, and even more preferably 100 mg / L or more. An alkali metal ion concentration of 1 mg / L or more improves the recovery efficiency of alkali metal salts in the subsequent stages.

[0058] To increase the alkali metal ion concentration (mg / L) in the permeate from the final nanofiltration membrane unit, the permeate from the final nanofiltration membrane unit may be concentrated by any method, including, but not limited to, evaporation or reverse osmosis.

[0059] <7> Organic substance removal step An organic substance removal step may be performed on solution X' before the nanofiltration step of solution X'. When solution X' is a liquid containing an electrolyte and the organic solvent and water are separated, it is preferable to separate the oil phase and the aqueous phase using any oil-water separation method. Organic substances dissolved in water are preferably removed using an ultrafiltration membrane. Since high molecular weight organic substances can be removed by ultrafiltration, fouling of the nanofiltration membrane can be suppressed by removing high molecular weight organic substances. The aqueous phase in the oil-water separation or the permeate from the ultrafiltration is used in the nanofiltration step of solution X'.

[0060] <8> Recovery Step In this step, the alkali metal salt is recovered from the permeate (aqueous alkali metal salt solution) obtained in the nanofiltration step of step (3).

[0061] The recovery of alkali metal salts can be carried out by known methods. For example, when the alkali metal salt is a potassium salt, this can be achieved by utilizing the temperature dependence of solubility or by adding a poor solvent such as ethanol. Lithium salts have lower solubility than other alkali metal salts. For example, sodium carbonate and potassium carbonate have high solubility in water (20 g or more per 100 mL of water), but lithium carbonate dissolves only 1.33 g per 100 mL of water at 25°C. Therefore, by adding a carbonate to the permeate, lithium can be recovered as lithium carbonate. Since the solubility of lithium carbonate further decreases at high temperatures, the aqueous solution may be heated.

[0062] <Recovery Apparatus> The alkali metal salt recovery apparatus of the present invention for carrying out the alkali metal salt recovery method of the present invention comprises a tank for storing a solution containing alkali metal ions (solution X), an aluminum salt adding means for adding an aluminum salt to the solution, and a nanofiltration means for separating the alkali metal ions from the solution. It is more preferable that the recovery apparatus of the present invention further comprises a pH adjusting means for adjusting the pH of the solution.

[0063] The nanofiltration means preferably includes a pressure vessel (hereinafter also referred to as a "vessel") filled with spiral-wound elements (hereinafter also referred to as "nanofiltration membrane elements") incorporating nanofiltration membranes capable of separating alkali metal ions, and a nanofiltration membrane unit capable of supplying a solution to the vessel using a high-pressure pump. The nanofiltration membrane unit may be configured by connecting multiple vessels in parallel or series, with each vessel being filled with multiple nanofiltration membrane elements. Nanofiltration membrane elements of any diameter and length can be used. Nanofiltration membrane elements vary in size depending on the membrane area; for the same membrane type, the larger the membrane area, the greater the amount of liquid that can be processed per unit time. The size and number of nanofiltration membrane elements can be determined arbitrarily depending on the scale of the solution to be processed.

[0064] The aluminum salt adding means provided in the recovery apparatus of the present invention is not particularly limited as long as it has a mechanism capable of adding aluminum salt to a solution. For example, it may be equipment that adds aluminum salt as a solid to a tank storing a solution having a stirring means, or equipment that adds aluminum salt directly to the solution from a tank storing an aqueous solution of high concentration aluminum salt using a chemical feed pump. Among these, from the viewpoints of the size of the equipment and the solubility of aluminum salt in the solution, it is preferable to have a mechanism that adds aluminum salt to the solution from a tank storing high concentration aluminum salt using a chemical feed pump.

[0065] Methods for adding a highly concentrated aluminum salt from a chemical feed pump include a flow rate proportional method in which a constant amount of a highly concentrated aqueous aluminum salt solution is added from the chemical feed pump in proportion to the permeation flow rate of the nanofiltration means, and a timer method in which a constant amount of a highly concentrated aqueous aluminum salt solution is added from the chemical feed pump at regular intervals, and of these, the flow rate proportional method is more preferred.

[0066] The pH adjusting means is not particularly limited as long as it has a mechanism capable of adjusting the pH of the solution. For example, a chemical feed pump for adding an acidic or alkaline aqueous solution to the solution and equipment for measuring the pH of the solution, such as a pH meter, may be installed in a tank storing the solution. Furthermore, it is preferable to have a mechanism for feeding back the pH value of the solution to the chemical feed pump and adjusting the pH of the solution.

[0067] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. Measurements in the examples and comparative examples were carried out as follows.

[0068] <Nanofiltration Membrane Performance> (Glucose Removal Rate and Isopropyl Alcohol Removal Rate of Nanofiltration Membrane) The isopropyl alcohol removal rate and glucose removal rate were calculated using the following formulas from the permeate obtained when a 1000 mg / L glucose aqueous solution at 25°C and pH 6.5 was permeated through the nanofiltration membrane at an operating pressure of 0.5 MPa as feed water, and the permeate obtained when a 1000 mg / L isopropyl alcohol aqueous solution at 25°C and pH 6.5 was permeated through the nanofiltration membrane at an operating pressure of 0.5 MPa as feed water, and the glucose concentration and isopropyl alcohol concentration of each feed water. Isopropyl alcohol removal rate (%) = 100 × {1 - (isopropyl alcohol concentration in permeate water / isopropyl alcohol concentration in feed water)} Glucose removal rate (%) = 100 × {1 - (glucose concentration in permeate water / glucose concentration in feed water)} The isopropyl alcohol concentration was determined using a gas chromatograph (GC-18A, manufactured by Shimadzu Corporation), and the glucose concentration was determined using a refractometer (RID-6A, manufactured by Shimadzu Corporation).

[0069] (Magnesium sulfate rejection rate and magnesium chloride rejection rate of nanofiltration membrane) The permeate obtained when a 2000 mg / L aqueous magnesium sulfate solution at pH 6.5 at 25°C was passed through the nanofiltration membrane at an operating pressure of 0.5 MPa as feed water, the permeate obtained when a 2000 mg / L aqueous magnesium chloride solution at pH 6.5 at 25°C was passed through the nanofiltration membrane at an operating pressure of 0.5 MPa as feed water, and the magnesium sulfate (MgSO 4 ) concentration and magnesium chloride (MgCl2 ) concentration was measured. 4 Concentration and MgCl 2 The concentration was determined by measuring the electrical conductivity of the feed water and permeate water using an electrical conductivity meter manufactured by Toa Denpa Kogyo Co., Ltd., and determining the practical salt content of each, i.e., MgSO 4 Concentration and MgCl 2 The concentration of MgSO 4 Concentration, MgCl 2 Based on the concentration and the following formula, MgSO 4 Removal rate and MgCl 2 The removal rate was calculated. 4 Removal rate (%) = 100 × {1 - (MgSO in permeate)} 4 Concentration / MgSO in feed water 4 Concentration)} MgCl 2 Removal rate (%) = 100 × {1 - (MgCl in permeate)} 2 Concentration / MgCl in feed water 2 concentration)}

[0070] <Nanofiltration membrane> (Nanofiltration membrane A) Nonwoven fabric made of polyester fiber (air permeability 1 cc / cm 2A 18.0 mass% dimethylformamide (DMF) solution of polysulfone was cast onto the porous support membrane (s) at room temperature (25 ° C.) to a thickness of 180 μm, and then immediately immersed in pure water and left for 5 minutes to prepare a porous support membrane (thickness 160 μm) made of fiber-reinforced polysulfone. Next, air adjusted to 25 ° C. was blown to remove excess moisture, and the membrane surface temperature of the porous support membrane was adjusted to 25 ° C. A 30 ° C. aqueous solution containing 2.0 mass% piperazine, 250 ppm sodium dodecyl diphenyl ether disulfonate, and 1.0 mass% trisodium phosphate was applied to the surface of the porous support membrane and left to stand for 15 seconds, after which nitrogen was blown from an air nozzle to remove excess aqueous solution, forming a coating layer of an amine aqueous solution on the porous support membrane. Furthermore, a 38°C n-decane solution containing 0.2% by mass of trimesoyl chloride (hereinafter referred to as "TMC") was uniformly applied to the entire surface of the porous support membrane, and then the membrane was left to stand for 1 minute at a relative humidity of 70% and a temperature of 25°C to carry out interfacial polycondensation. Two fluids (pure water and air) were sprayed onto the membrane surface to remove the solution from the surface. The membrane was then washed with 80°C pure water to obtain nanofiltration membrane A.

[0071] (Nanofiltration Membrane B) Nanofiltration Membrane B was prepared in the same manner as Nanofiltration Membrane A, except that the piperazine was changed to 2,5-dimethylpiperazine, and an n-decane solution at 38°C containing 0.2% by mass of TMC was uniformly applied to the entire surface of a porous support membrane, and then the solution was allowed to stand at a relative humidity of 80% and 25°C for 1 minute.

[0072] (Nanofiltration Membrane C) Nanofiltration membrane C was obtained by producing a nanofiltration membrane in the same manner as nanofiltration membrane A, except that the TMC concentration was 0.5% by mass.

[0073] The membrane performance of nanofiltration membrane A, nanofiltration membrane B, and nanofiltration membrane C is shown in Table 1.

[0074]

[0075] <Liquids to be treated> (Solutions Xa to Xf) On page 282, line 14 of Non-Patent Document 1, it is described that 1.0 mol / L LiPF 6 is used as an electrolyte. 6 The solution is described. The molar concentration of lithium (Li) and fluorine (F) was simulated when this electrolyte solution was diluted 10 times with water, and Li 2 SO4 To water, 0.05 mol / L of Li and 0.60 mol / L of HF were added, and the pH was adjusted with sodium hydroxide or sulfuric acid to the values ​​shown in Table 2 to prepare solutions Xa to Xf. The molar concentrations of Li and F in Table 2 are those in a fully ionized state.

[0076]

[0077] (Solution Xa-2) Solution Xa-2 was prepared by using the solution Xa, but containing acetate ions at the same molar concentration as the compound HA instead of fluorine.

[0078] (Solution Xa-3) Solution Xa-3 was prepared by using the solution Xa, but containing formate ions at the same molar concentration as the compound HA instead of fluorine.

[0079] (Solution Xa-4) Solution Xa-4 was prepared by using the solution Xa, but containing phosphate ions instead of fluorine as the compound HA at the same molar concentration.

[0080] (Solution Xa-5) Solution Xa-5 was prepared by using Solution Xa but containing cyanide ions at the same molar concentration as the compound HA instead of fluorine.

[0081] <Evaluation of Nanofiltration Process> (Concentration Ratio P) Using the molar concentrations of various ions in the solution, the concentration ratio P was calculated based on the following formula: Concentration ratio P = {molar concentration of total anions A in the solution (mol / L)} / {molar concentration of lithium ions (mol / L)}

[0082] (Pressure ratio) Nanofiltration membrane cross-flow filtration method, permeate flow rate: concentrate flow rate = 1:9, permeation flux 0.4 m 2 / m 3 Constant flow rate filtration was performed under the condition of 1 / s. The pressure ratio was defined as the ratio of the operating pressure (MPa) after 24 hours to the operating pressure (MPa) after 1 hour from the start of constant flow rate operation. A higher pressure ratio indicates more fouling of the nanofiltration membrane.

[0083] (Example 1) Aluminum sulfate was added to a solution Xa at 25°C so that the Al concentration was 0.20 mol / L, and the solution was filtered through a nanofiltration membrane A by cross-flow filtration at a permeate flow rate: concentrate flow rate = 1:9 and a permeation flux of 0.4 m2 / m 3 Filtration was carried out at a constant flow rate of 1 / s.

[0084] Example 2 The same procedure as in Example 1 was carried out, except that aluminum sulfate was added so that the Al concentration was 0.25 mol / L.

[0085] Example 3 The same procedure as in Example 1 was carried out, except that aluminum sulfate was added so that the Al concentration was 0.30 mol / L.

[0086] Example 4 The procedure of Example 1 was repeated except that solution Xb was used instead of solution Xa.

[0087] Example 5 The same procedure as in Example 4 was carried out, except that aluminum sulfate was added so that the Al concentration was 0.25 mmol / L.

[0088] Example 6 The procedure of Example 1 was repeated except that solution Xc was used instead of solution Xa.

[0089] Example 7 The procedure of Example 1 was repeated except that solution Xd was used instead of solution Xa.

[0090] Example 8 The procedure of Example 1 was repeated except that the solution Xe was used instead of the solution Xa.

[0091] Example 9 The same procedure as in Example 5 was repeated except that nanofiltration membrane B was used instead of nanofiltration membrane A.

[0092] Example 10 The procedure of Example 1 was repeated except that Solution Xa-2 was used instead of Solution Xa.

[0093] Example 11 The procedure of Example 1 was repeated, except that solution Xa-3 was used instead of solution Xa.

[0094] Example 12 The procedure of Example 8 was repeated except that nanofiltration membrane B was used instead of nanofiltration membrane A.

[0095] Example 13 The same procedure as in Example 8 was carried out, except that nanofiltration membrane C was used instead of nanofiltration membrane A.

[0096] Comparative Example 1 The same procedure as in Example 1 was carried out except that aluminum sulfate was not added.

[0097] Comparative Example 2 The same procedure as in Example 1 was carried out, except that aluminum sulfate was added so that the Al concentration was 0.05 mmol / L.

[0098] Comparative Example 3 The procedure was the same as in Example 1, except that solution Xf was used instead of solution Xa. As a result, precipitates clogged the membrane surface during the nanofiltration step, making it impossible to perform filtration.

[0099] Comparative Example 4 The procedure of Example 1 was repeated except that Solution Xa-4 was used instead of Solution Xa.

[0100] Comparative Example 5 The same procedure as in Example 1 was carried out except that Solution Xa-5 was used instead of Solution Xa.

[0101] The analysis results of the composition of the initial permeate one hour after the start of constant flow rate operation and the pressure ratios performed for Examples 1 to 13 and Comparative Examples 1, 2, 4, and 5 are shown in Tables 3 and 4. The molar ratios of "Al / total anions A" in Tables 3 and 4 were calculated from the concentration of anions A when compound HA was completely ionized.

[0102]

[0103]

[0104] In the above Examples and Comparative Examples, the lower the concentration ratio of the permeate through the nanofiltration membrane and the lower the pressure ratio, the more advantageous it is. From the above results, it was found that Examples 1 to 13, which are the alkali metal salt recovery methods of the present invention, can recover alkali metal salts with higher purity relative to impurities such as fluorine, compared to Comparative Examples 1 to 5.

[0105] Although the present invention has been described in detail using specific embodiments, it will be apparent to those skilled in the art that various modifications and variations are possible without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-075075) filed on April 28, 2023, the entire contents of which are incorporated by reference.

[0106] The present invention can be suitably used as a method for efficiently separating and recovering alkali metals such as lithium from waste materials, waste liquids, ores, slag, etc. generated in the manufacturing process of lithium ion batteries.

Claims

1. A method for recovering an alkali metal salt from a solution X containing at least one of a compound HA having a pKa of 3.0 to 5.0 and an anion A forming said compound HA, and alkali metal ions, comprising the following steps (1) to (3): (1) a pH adjustment step of adjusting the pH of said solution X to 0 to 4.0 when the pH of said solution X exceeds 4.0, (2) an aluminum salt addition step of adding an aluminum salt to said solution X such that the molar concentration of aluminum (mol / L) is 0.25 or more times the total molar concentration of anion A (mol / L) which is the sum of the molar concentration (mol / L) of said compound HA in said solution X and the molar concentration (mol / L) of anion A present as ions in said solution X, and (3) a nanofiltration step of separating alkali metal ions from the solution X after steps (1) and (2) to the permeate side using a nanofiltration membrane.

2. The method for recovering an alkali metal salt according to claim 1, wherein in the step (1), the pH of the solution X is adjusted to 1.0 or more and 3.0 or less.

3. The method for recovering an alkali metal salt according to claim 1 or 2, wherein the pKa of the compound HA is 3.0 or more and 4.0 or less.

4. The method for recovering an alkali metal salt according to claim 1 or 2, wherein in the step (2), an aluminum salt is added to the solution X so as to satisfy any one of the following conditions (a) to (d): Condition (a): When the pH of the solution X is 1.0 or more and 1.4 or less, the molar concentration of the aluminum is 0.5 times or more relative to the total molar concentration of the anion A in the solution X. Condition (b): When the pH of the solution X is greater than 1.4 and 1.9 or less, the molar concentration of the aluminum is 0.4 times or more relative to the total molar concentration of the anion A in the solution X. Condition (c): When the pH of the solution X is greater than 1.9 and 2.4 or less, the molar concentration of the aluminum is 0.3 times or more relative to the total molar concentration of the anion A in the solution X. Condition (d): When the pH of the solution X is greater than 2.4 and 3.0 or less, the molar concentration of the aluminum is 0.25 times or more relative to the total molar concentration of the anion A in the solution X.

5. The method for recovering an alkali metal salt according to claim 1 or 2, wherein the difference between the magnesium sulfate removal rate when a 2000 mg / L aqueous magnesium sulfate solution at 25°C and pH 6.5 is allowed to permeate through the nanofiltration membrane at an operating pressure of 0.5 MPa and the magnesium chloride removal rate when a 2000 mg / L aqueous magnesium chloride solution at 25°C and pH 6.5 is allowed to permeate through the nanofiltration membrane at an operating pressure of 0.5 MPa is 20% or less.

6. The method for recovering an alkali metal salt according to claim 1 or 2, wherein the difference between the glucose removal rate when a 1000 mg / L aqueous glucose solution at 25° C. and pH 6.5 is permeated through the nanofiltration membrane at an operating pressure of 0.5 MPa and the isopropyl alcohol removal rate when a 1000 mg / L aqueous isopropyl alcohol solution at 25° C. and pH 6.5 is permeated through the nanofiltration membrane at an operating pressure of 0.5 MPa is 40% or more, and the glucose removal rate is 70% or more and 95% or less.

7. The method for recovering an alkali metal salt according to claim 1 or 2, wherein said compound HA contains fluorine.

8. The method for recovering an alkali metal salt according to claim 1 or 2, wherein the alkali metal salt comprises lithium.

9. An apparatus for recovering an alkali metal salt, comprising: a tank for storing a solution containing alkali metal ions; an aluminum salt adding means for adding an aluminum salt to the solution; and a nanofiltration means for separating the alkali metal ions from the solution.

10. The apparatus for recovering alkali metal salts according to claim 9, further comprising a pH adjusting means for adjusting the pH of the solution.

Citation Information

Patent Citations

  • Lithium battery processing method

    JP2005197149A

  • Service subscription method and apparatus

    JP2023075075A

  • Method for deeply removing fluorine from LiHCO3 solution recycled and leached from waste lithium batteries

    CN112853120A

  • Method for removing phosphorus and / or fluorine, and method for recovering valuable metal from lithium ion battery

    JP2012036419A

  • Method for removing phosphorus and / or fluorine and method for recovering valuable metal

    JP2016003382A