Method for depolymerizing polyester
The described method efficiently depolymerizes polyester into dicarboxylic acids by using a mixture of alkaline compounds and solvents, addressing inefficiencies in existing recycling methods and enabling effective industrial recycling of polyester.
Patent Information
- Application Number
- PCT/JP2024/016555
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
Current chemical recycling methods for polyester, such as hydrolysis, alcoholysis, and glycolysis, face inefficiencies in terms of reaction rate and require special equipment or conditions, while microorganism-based methods need improvement in efficiency and conditions for depolymerization.
A method involving a mixture of polyester, an alkaline compound (like sodium hydroxide), and a solvent (alcohol or ketone) at specific ratios and temperatures to efficiently depolymerize polyester into dicarboxylic acids under mild conditions, optimizing the conversion rate of polyethylene terephthalate to terephthalic acid.
This method achieves a high conversion rate of polyester to dicarboxylic acids like terephthalic acid under mild conditions, making it suitable for industrial recycling and reducing the need for pressurized equipment.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Method for depolymerizing polyester
[0001] The present invention relates to a method for depolymerizing polyester.
[0002] Recently, environmental pollution caused by plastic waste has become a problem. In order to reduce the environmental impact, there is an urgent need to develop fundamental technologies for efficiently recycling plastic products. Among plastic products, polyester is used in large quantities as beverage bottles and fibers. Therefore, there is a strong demand for the establishment of an efficient recycling method.
[0003] There are two known methods for recycling used polyester products: material recycling and chemical recycling. Material recycling involves sorting used polyester products, then melting and remolding them as resin, but it is difficult to restore the quality to that before recycling because it is not possible to completely remove impurities. On the other hand, chemical recycling involves chemically breaking down the polyester into low-molecular-weight compounds, which in principle makes it possible to produce products of the same quality as the original polyester product.
[0004] Chemical recycling methods for polyester can be broadly classified into hydrolysis, which uses water as a solvent, alcoholysis, which uses alcohol as a solvent, and glycolysis, which uses glycol as a solvent. In addition to these three methods, the use of microorganisms for depolymerization has also been investigated in recent years.
[0005] The hydrolysis method involves reacting molten polyethylene terephthalate with steam and then with ammonium hydroxide to decompose it into terephthalic acid and ethylene glycol. This method has the advantage of not requiring glycol or alcohol for the reaction, but the reaction is carried out under high pressure, so a special pressure-resistant device is required.
[0006] The alcoholysis method is a method for depolymerizing polyester by heating in an alcohol solvent. This method has the advantage that, for example, when polyethylene terephthalate (PET) is depolymerized using methanol as a solvent, dimethyl terephthalate is produced as a monomer through the depolymerization reaction, making it efficient and allowing the depolymerization reaction to proceed relatively quickly. However, since the alcohol used as the solvent has a low boiling point and pressure is required to drive the reaction, a special pressure-resistant device is required.
[0007] The glycolysis method involves depolymerizing polyester by heating it in an excess of alkylene glycol solvent together with a depolymerization catalyst such as sodium carbonate to produce bis(hydroxyalkyl) terephthalate and ethylene glycol. Although the glycolysis method can be carried out at atmospheric pressure, it has the drawback of a relatively long reaction time.
[0008] The method using microorganisms involves hydrolyzing polyethylene terephthalate with an enzyme to obtain terephthalic acid. Although the hydrolysis reaction can proceed under mild reaction conditions, there is room for improvement in terms of efficiency.
[0009] In addition to these chemical recycling methods, a method has been proposed in which polyethylene terephthalate can be decomposed into monomers in a short time under relatively mild conditions, in which an alcohol and an ether are added to the polyethylene terephthalate and the mixture is reacted with an equivalent or excess amount of alkali to produce a terephthalate salt (Patent Document 1, Non-Patent Document 1, etc.).
[0010] Japanese Patent Application Publication No. 10-087529
[0011] Oku et. al, Polymer Journal, vol. 29, No. 9, 708-712 (1997)
[0012] Patent Document 1 describes that polyethylene terephthalate can be depolymerized by reacting it with sodium hydroxide to decompose it into terephthalic acid salts and ethylene glycol, and that the depolymerization reaction proceeds at 40 to 75°C. However, there is still room for improvement in terms of the depolymerization reaction rate (i.e., the conversion rate of polyethylene terephthalate to terephthalic acid). In addition, since ethers can produce peroxides upon degradation, there are concerns about industrially using ethers to depolymerize polyesters.
[0013] The present disclosure relates to a method for depolymerizing polyester, which achieves an excellent conversion rate to dicarboxylic acid (e.g., terephthalic acid) or hydroxycarboxylic acid through depolymerization even under mild reaction conditions.
[0014] The present inventors have prepared a composition containing a specific alkaline compound such as sodium hydroxide and an alcohol-based solvent and / or a ketone-based solvent, and have found that when the composition is used to depolymerize a polyester, the conversion rate to terephthalic acid is significantly affected by the amount of solvent used. The present disclosure is based on these findings.
[0015] The present disclosure includes the following: [1] A method for depolymerizing a polyester, the method comprising forming a mixture containing the following components (a), (b), and (c): (a) a polyester, (b) one or more alkali compounds selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, alkali metal bicarbonates, alkaline earth metal hydroxides, alkaline earth metal carbonates, and alkaline earth metal bicarbonates, and (c) a solvent containing at least one of an alcohol solvent or a ketone solvent, and depolymerizing the polyester in the mixture, wherein the temperature of the mixture containing the total amount of the polyester, the alkali compound, and the solvent is 75°C or less when the mixture is formed, and the ratio of the amount of the polyester to the amount of the solvent is 0.2 to 20 by mass. [2] The method according to [1], wherein the alkali compound dissolves in an amount of 100 g or more in 100 g of water at 20±5°C. [3] The method according to [1] or [2], wherein the alkali compound is one or more selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, and alkali metal hydrogencarbonates. [4] The method according to [1] or [2], wherein the alkali compound is an alkali metal hydroxide, an alkaline earth metal hydroxide, or both. [5] The method according to any one of [1] to [4], wherein the alkali compound is one or more of an alkali metal hydroxide and an alkaline earth metal hydroxide, and the total amount of hydroxide ions in the alkali metal hydroxide and the total amount of hydroxide ions in the alkaline earth metal hydroxide is in the range of 0.9 to 3.0 relative to the amount of repeating units of the polyester before the mixture is formed. [6] The method according to any one of [1] to [5], wherein the temperature of the mixture containing the total amount of the polyester, the alkali compound, and the solvent when the mixture is formed is 0 to 75°C. [7] The method according to any one of [1] to [6], wherein the temperature of the mixture containing the polyester, the alkali compound, and the total amount of the solvent when the mixture is formed is 35 to 55°C.[8] The method according to any one of [1] to [7], wherein the ratio of the amount of the polyester to the amount of the solvent is 0.25 to 2.2 by mass. [9] The method according to any one of [1] to [8], wherein the polyester is polyethylene terephthalate.
[10] The method according to any one of [1] to [9], wherein the alkaline compound is sodium hydroxide, potassium hydroxide, or both.
[11] The method according to any one of [1] to
[10] , wherein the alcohol-based solvent is a lower alcohol.
[12] The method according to any one of [1] to
[11] , wherein the mixture contains particles containing the polyester.
[13] The method according to
[12] , wherein the particles containing the polyester are granular with an average particle size of 150 to 350 μm.
[14] The method according to
[12] or
[13] , wherein the crystallinity of the particles containing the polyester is 50% or less.
[15] The method according to any one of
[12] to
[14] , wherein the mixture is a powder mixture containing particles containing the polyester and the solvent integrated with the particles.
[16] The method according to any one of [1] to
[15] , wherein the polyester before the mixture is formed has an intrinsic viscosity of 0.8 dl / g or less.
[17] The method according to any one of [1] to
[16] , wherein the polyester is prepared from used bottle containers containing a polyester.
[18] A method for producing a diol and a dicarboxylic acid, comprising producing a diol and a dicarboxylic acid salt from a polyester by the method according to any one of [1] to
[17] .
[19] A method for recycling polyester, comprising producing a polyester by polymerizing a polymerization raw material containing at least one of the diol and the dicarboxylic acid produced from the dicarboxylic acid salt obtained by the method according to
[18] .
[0016] [1]' A method for depolymerizing a polyester, comprising mixing the following components (a), (b), and (c): (a) a polyester; (b) one or more alkali metal compounds selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, alkali metal bicarbonates, alkaline earth metal hydroxides, alkaline earth metal carbonates, and alkaline earth metal bicarbonates; and (c) a solvent including an alcohol solvent and / or a ketone solvent, wherein the mixing is carried out at 75°C or less, and the components (a), (b), and (c) are mixed in such a manner that the ratio of component (a) to component (c) is 0.2 to 20 by mass. [2]' The method according to [1]', wherein the component (b) is an alkali metal hydroxide and / or alkaline earth metal hydroxide, and the amount of hydroxide ions of the alkali metal hydroxide and / or alkaline earth metal hydroxide is in the range of 1.8 to 3.0 relative to the amount of repeating units of the polyester added to the alcohol-based solvent and / or ketone-based solvent. [3]' The method according to [1]' or [2]', wherein the mixing is carried out at 35 to 55°C. [4]' The method according to any one of [1]' to [3]', wherein the ratio of component (a) to component (c) is 0.25 to 2.2 by mass. [5]' The method according to any one of [1]' to [4]', wherein the (a) polyester is polyethylene terephthalate. [6]' The method according to any one of [1]' to [5]', wherein the component (b) is sodium hydroxide or potassium hydroxide. [7]' The method according to any one of [1]' to [6]', wherein the alcohol-based solvent is a lower alcohol. [8]' The method according to any one of [1]' to [7]', wherein the (a) polyester is a granular material having an average particle size of 150 to 350 μm. [9]' The method according to any one of [1]' to [8]', wherein the (a) polyester has a crystallinity of 50% or less.
[10] ' The method according to any one of [1]' to [9]', wherein the (a) polyester has an intrinsic viscosity of 0.8 dl / g or less.
[11] ' The method according to any one of [1]' to
[10] ', wherein the (a) polyester is prepared from used bottle containers made of polyester.
[12] ' A method for producing a diol component and a dicarboxylic acid component by depolymerizing a polyester, the method being carried out by the method according to any one of [1]' to
[11] '.
[13] ' A method for recycling polyester, comprising regenerating polyester by using a product obtained by the method according to any one of [1]' to
[11] ' as at least a part of a polyester polymerization raw material.
[0017] According to the present disclosure, there is provided a method for depolymerizing polyesters that achieves an excellent conversion rate to dicarboxylic acids such as terephthalic acid or hydroxycarboxylic acids through depolymerization even under mild reaction conditions. The method of the present disclosure can be used for industrial recycling of used polyester products.
[0018] <Method for Depolymerizing Polyester> One example of a method for depolymerizing polyester includes mixing a polyester (hereinafter also referred to as "component (a)"), a predetermined alkali compound (hereinafter also referred to as "component (b)"), and a solvent containing an alcohol-based solvent and / or a ketone-based solvent (hereinafter also referred to as "component (c)"). The alkali compound includes at least one of an alkali metal compound or an alkaline earth metal compound. The solvent includes at least one of an alcohol-based solvent or a ketone-based solvent. Mixing the polyester, the alkali compound, and the solvent includes first mixing them together to form a mixture, and then stirring or kneading the formed mixture. The polyester is depolymerized in the formed mixture. A powder containing particles containing the polyester may be mixed with the alkali compound and the solvent. An example of a method for depolymerizing polyester according to the present disclosure will be described in detail below.
[0019] Polyesters are typically polymers formed by polycondensation of one or more dicarboxylic acids and one or more diols. The alkali compound (component (b)) reacts with the polyester (component (a)) to produce a dicarboxylate and a diol. That is, a depolymerization reaction occurs in which the polyester is decomposed into a dicarboxylate and a diol. Taking polyethylene terephthalate as an example, terephthalate and ethylene glycol are produced. In this reaction (depolymerization reaction), the presence of a solvent containing an alcoholic solvent and / or a ketone solvent in a predetermined ratio relative to the amount of polyester allows the depolymerization reaction to proceed efficiently even under mild conditions such as 75°C or below. Specifically, the ratio of the amount of polyester to the amount of solvent (component (c)) in the mixture can be 0.2 to 20 by mass. That is, by mixing components (a), (b), and (c) so that the ratio of the polyester to the alcohol-based solvent and / or ketone-based solvent of component (c) is in the range of 0.2 to 20 by mass, the polyester can be efficiently decomposed into a dicarboxylate salt and a diol even under mild conditions. The polyester may be a polymer formed by polycondensation of a hydroxycarboxylic acid compound (e.g., lactic acid) having a hydroxy group and a carboxy group. In this case, a salt of the hydroxycarboxylic acid compound can be formed by depolymerization of the polyester under mild conditions. In the salt of the hydroxycarboxylic acid compound, the carboxy group usually forms the salt. The polyester may contain dicarboxylic acid units derived from a dicarboxylic acid, diol units derived from a diol, and hydroxycarboxylic acid units derived from a hydroxycarboxylic acid.
[0020] If the ratio of the amount of polyester to the amount of solvent (component (a) to component (c)) is less than 0.2 by mass, the conversion rate to dicarboxylates and the like tends to be low under mild conditions. On the other hand, if the ratio of the amount of polyester to the amount of solvent (component (a) to component (c)) is more than 20 by mass, the amount of solvent is too small, making it difficult or impossible for the depolymerization reaction of the polyester to proceed uniformly, and instead the conversion rate to dicarboxylates and the like tends to be low. From a similar perspective, the ratio of the amount of polyester to the amount of solvent may be 0.25 or more, 0.3 or more, or 0.35 or more by mass, or may be 10 or less, 5.0 or less, 3.0 or less, 2.2 or less, 2.0 or less, or 1.0 or less. The ratio of the amount of polyester to the amount of solvent may be from 0.25 to 10, 0.3 to 10, 0.35 to 10, 0.25 to 5.0, 0.3 to 5.0, 0.35 to 5.0, 0.25 to 3.0, 0.3 to 3.0, 0.35 to 3.0, 0.25 to 2.2, 0.3 to 2.2, 0.35 to 2.2, 0.25 to 2.0, 0.3 to 2.0, 0.35 to 2.0, 0.25 to 1.0, 0.3 to 1.0, or 0.35 to 1.0 by weight.
[0021] The alkali compound (component (b)) used in the present disclosure is not particularly limited as long as it is at least one selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, alkali metal bicarbonates, alkaline earth metal hydroxides, alkaline earth metal carbonates, and alkaline earth metal bicarbonates.
[0022] Examples of alkali metal hydroxides include lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide, and francium hydroxide. Examples of alkali metal carbonates include lithium carbonate, sodium carbonate, potassium carbonate, rubidium carbonate, cesium carbonate, and francium carbonate. Examples of alkali metal bicarbonates include lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, rubidium bicarbonate, cesium bicarbonate, and francium bicarbonate. Examples of alkaline earth metal hydroxides include beryllium hydroxide, magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, and radium hydroxide. Examples of alkaline earth metal carbonates include beryllium carbonate, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, and radium carbonate. Examples of alkaline earth metal bicarbonates include beryllium bicarbonate, magnesium bicarbonate, calcium bicarbonate, strontium bicarbonate, barium bicarbonate, and radium bicarbonate.
[0023] The alkali compound may be one that is easily soluble in the solvents that make up the mixture. Since both alcohol-based solvents and ketone-based solvents are solvents with relatively high hydrophilicity, alkali compounds that exhibit higher solubility in water generally tend to exhibit higher solubility in solvents containing at least one of alcohol-based solvents or ketone-based solvents. Therefore, using the degree of solubility in water as an indicator, an alkali compound that is easily soluble in a solvent containing at least one of alcohol-based solvents or ketone-based solvents can be selected. From this perspective, the alkali compound may be one that dissolves at a rate of 100 g or more in 100 g of water at 20±5°C. Here, "100 g or more" means that the amount of alkali compound that dissolves in 100 g of water at 20±5°C is 100 g or more, and 100 g / 100 g-H 2 The amount of alkali compound dissolved in water at 20±5°C is sometimes written as 100g / 100g-H 2 0 or more, and preferably 102 g / 100 g-H2 0 or more, more preferably 104g / 100g-H 2 0 or more, more preferably 106 g / 100 g-H 2 The upper limit of the amount of the alkali compound dissolved in water at 20±5° C. is not particularly limited, but for example, it is 300 g / 100 g-H 2 The amount of the alkali compound dissolved in water at 20±5°C is 100 to 300 g / 100 g-H 2 O, and preferably 102 to 300 g / 100 g-H 2 0, more preferably 104 to 300 g / 100 g-H 2 0, more preferably 106 to 300 g / 100 g-H 2 It is O.
[0024] The alkali compound may be one or more alkali metal compounds selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, and alkali metal bicarbonates. In particular, the alkali compound may be sodium hydroxide, potassium hydroxide, or both.
[0025] In one example of the present disclosure, the amount of hydroxide ions of alkali metal hydroxide and / or alkaline earth metal hydroxide contained in the mixture together with the solvent containing an alcohol-based solvent and / or a ketone-based solvent, in other words, the total amount of hydroxide ions in the alkali metal hydroxide and the alkaline earth metal hydroxide, may be adjusted to be in the range of 1.8 to 3.0 relative to the amount of repeating units of the polyester added. The "amount of substance relative to the amount of repeating units of the polyester" refers to the sum, expressed in molar units, of the total amount of repeating units consisting of polycarboxylic acid units and diol units contained in the polyester and the total amount of repeating units consisting of hydroxycarboxylic acid units contained in the polyester. When the amount of hydroxide ions of alkali metal hydroxide and / or alkaline earth metal hydroxide is 1.8 or more relative to the amount of repeating units of the polyester, the conversion rate to carboxylate salt or hydroxycarboxylic acid salt is likely to reach 90% or more when all of the hydroxide ions of the alkali metal hydroxide and / or alkaline earth metal hydroxide are consumed in the depolymerization reaction. On the other hand, if the amount of hydroxide ions of alkali metal hydroxide and / or alkaline earth metal hydroxide relative to the amount of hydroxide ions based on the repeating units of the polyester is 3.0 or less, when the produced polyester salt (dicarboxylic acid salt or hydroxycarboxylic acid salt) is neutralized with an acid to convert it into a free form, the cost of chemicals for neutralizing excess hydroxide ions of alkali metal hydroxide and / or alkaline earth metal hydroxide and the cost of disposing of the neutralized salt are reduced, which can be economically advantageous.
[0026] In another embodiment, when the amount of hydroxide ions of the alkali metal hydroxide and / or alkaline earth metal hydroxide is 0.9 or more relative to the amount of repeating units of the polyester, the conversion rate to carboxylate salt or hydroxycarboxylic acid salt is likely to reach 90% or more when all of the hydroxide ions of the alkali metal hydroxide and / or alkaline earth metal hydroxide are consumed in the depolymerization reaction. On the other hand, when the amount of hydroxide ions of the alkali metal hydroxide and / or alkaline earth metal hydroxide is 1.5 or less relative to the amount of repeating units of the polyester, when the produced polyester salt (dicarboxylate salt or hydroxycarboxylic acid salt) is neutralized with acid to convert it to a free form, the cost of chemicals for neutralizing excess hydroxide ions of the alkali metal hydroxide and / or alkaline earth metal hydroxide and the cost of disposing of the neutralized salt are reduced, which can be economically advantageous.
[0027] From the above, the amount of hydroxide ions of alkali metal hydroxides and / or alkaline earth metal hydroxides may be 0.7 to 5.0, preferably 0.9 to 3.0, and more preferably 1.8 to 3.0, relative to the amount of repeating units of the polyester. In another embodiment, the amount of hydroxide ions of alkali metal hydroxides and / or alkaline earth metal hydroxides is preferably 0.7 to 2.0, and more preferably 0.9 to 1.5.
[0028] The entire amount of the alkali compound may be dissolved in the solvent, or some or all of the alkali compound may not dissolve in the solvent and be dispersed in the mixture as a solid. In particular, the alkali metal hydroxide and / or alkaline earth metal hydroxide may be dissolved in a solvent containing an alcohol-based solvent and / or a ketone-based solvent. The alkali metal hydroxide and / or alkaline earth metal hydroxide may be dispersed as a solid that does not dissolve in the solvent.
[0029] By setting the concentrations of the component (a) polyester, component (c) solvent including an alcohol-based solvent and / or a ketone-based solvent, and component (b) alkali compound within the above-described ranges, the polyester can be efficiently decomposed into dicarboxylates, diols, and the like, even under mild reaction conditions such as 75°C or below. The depolymerization reaction can be carried out at a temperature lower than the boiling point of the alcohol-based solvent (or ketone-based solvent) used, for example, 0 to 75°C, 1 to 75°C, 10 to 75°C, 15 to 75°C, 20 to 70°C, or 35 to 55°C. In other words, the temperature of the mixture at the time when the polyester, alkali compound, and solvent are mixed to initially form a mixture containing all of these components may be 75°C or below, 0 to 75°C, 1 to 75°C, 10 to 75°C, 20 to 70°C, or 35 to 55°C. The depolymerization reaction can also proceed at temperatures above 75°C, but in such cases, the solvent used is more likely to volatilize. Although solvent volatilization can be suppressed by carrying out the depolymerization reaction under pressurized conditions even at high temperatures, low temperatures are advantageous from an industrial perspective because they do not necessarily require complex pressurizing equipment. After the mixture is formed, the temperature of the mixture during stirring or kneading may be within the above range. However, the temperature of the mixture may exceed 75°C due to reaction heat or the like. The temperature of the mixture during stirring or kneading may be below the boiling point of the solvent. The mixture may be stirred or kneaded at room temperature (5 to 45°C) without heating.
[0030] The alcohol-based solvent used is not particularly limited, but examples include methanol, ethanol, propanol, isopropanol, butanol, and benzyl alcohol. The alcohol-based solvent may be a lower alcohol. The lower alcohol may be an alkyl alcohol having 1 to 5 carbon atoms. The alcohol-based solvent may include butanol, propanol, isopropanol, ethanol, methanol, or a combination of two or more selected from these, and may particularly include ethanol, methanol, or a combination of these. The alcohol-based solvent may be one type, or two or more types. The alcohol-based solvent mixed with the polyester and the alkali compound may contain a trace amount of water.
[0031] The ketone solvent to be used is not particularly limited, but examples include acetone, methyl ethyl ketone, diethyl ketone, methyl propyl ketone, methyl isobutyl ketone, methyl amyl ketone, cyclohexanone, isophorone, acetophenone, and benzophenone. One type of ketone solvent may be used, or two or more types may be used. The ketone solvent to be mixed with the polyester and the alkali compound may contain a trace amount of water.
[0032] In one example of the present disclosure, the solvent includes an alcohol-based solvent, particularly methanol or ethanol. However, the solvent contained in the mixture together with the predetermined alkali compound may also include solvents other than alcohol-based solvents and / or ketone-based solvents. For example, the solvent may include water. In this case, the ratio of the amount of polyester to the total mass of the solvent, including solvents other than alcohol-based solvents and / or ketone-based solvents, may be 0.2 to 20 by mass. If the composition containing the alkali compound mixed with the polyester or the solvent contains a solvent capable of dissolving a dicarboxylate or a hydroxycarboxylic acid salt, such as water, the depolymerization reaction rate tends to be slow, resulting in a relatively low conversion rate of the polyester to a dicarboxylate or a hydroxycarboxylic acid salt. Therefore, the combined proportion of the alcohol-based solvent and the ketone-based solvent in the solvent contained in the mixture together with the alkali compound may be 50% by mass or more, 70% by mass or more, or 90% by mass or more, or 100% by mass or less, based on the total mass of the solvent. In the solvent contained in the mixture together with the alkali compound, the ratio of the total amount of the alcohol solvent and the ketone solvent may be 50 to 100 mass%, 70 to 100 mass%, or 90 to 100 mass% based on the total amount of the solvent.
[0033] The polyesters applicable to the depolymerization method of the present disclosure may be polyesters obtained by polycondensation of a diol component (diol) and a dicarboxylic acid component (dicarboxylic acid), or polyesters obtained by polycondensation of a compound having both a hydroxy group and a carboxy group in the molecule. Examples of polyesters include aromatic polyesters such as polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and polyethylene furanoate; wholly aromatic polyesters such as polyarylates and liquid crystal polymers; polycarbonates such as polycarbonates; aliphatic polyesters such as polylactic acid polymers, polybutylene succinate polymers, polyethylene adipate polymers, polyethylene succinate polymers, polycaprolactone polymers, and polyhydroxyalkanoate polymers; and aliphatic aromatic polyesters such as polybutylene adipate terephthalate, polyethylene adipate terephthalate, and polyethylene succinate terephthalate. Among these, polyethylene terephthalate, which is widely used as a material for bottle containers, is particularly useful.
[0034] Polyethylene terephthalate is obtained by polycondensation of two main constituent monomers, ethylene glycol and terephthalic acid. In addition to these two components, polyethylene terephthalate may contain other monomers as copolymerization components, such as diol components or dicarboxylic acid components.
[0035] Examples of dicarboxylic acid components as copolymerization components of polyethylene terephthalate include malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, sebacic acid, dodecanedioic acid, eicosanedioic acid, pimelic acid, azelaic acid, methylmalonic acid, ethylmalonic acid, adamantanedicarboxylic acid, norbornenedicarboxylic acid, cyclohexanedicarboxylic acid, decalindicarboxylic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 5-sodiumsulfoisophthalic acid, phenylendanedicarboxylic acid, anthracenedicarboxylic acid, phenanthrenedicarboxylic acid, 9,9'-bis(4-carboxyphenyl)fluorene acid, 2,5-furandicarboxylic acid, and ester derivatives thereof.
[0036] Examples of diol components as copolymerization components for polyethylene terephthalate include 1,2-propanediol, 1,3-propanediol, butanediol, 2-methyl-1,3-propanediol, hexanediol, neopentyl glycol, cyclohexanedimethanol, cyclohexanediethanol, decahydronaphthalenedimethanol, decahydronaphthalenediethanol, norbornanedimethanol, norbornanediethanol, tricyclodecanedimethanol, tricyclodecaneethanol, tetracyclododecanedimethanol, tetracyclododecanediethanol, decalindimethanol, decalindiethanol, 5-methylol-5-ethyl-2-(1,1-dimethyl-2-hydroxyethyl)-1,3-dioxane, cyclohexanediol, bicyclohexyl-4,4'-diol, 2,2-bis(4-hydroxycyclohexylpropane), 2,2-bis(4-(2-hydroxyethoxy)cyclohexyl)propane, cyclopentanediol, 3-methyl-1,2-cyclopentadiol, 4-cyclopentene-1,3-diol, adamantanediol, paraxylene glycol, bisphenol A, bisphenol S, styrene glycol, trimethylolpropane, pentaerythritol, and bis-β-hydroxyethyl terephthalate (BHET).
[0037] Polyethylene terephthalate, the raw material for PET bottles, is known to be a partially crystalline polymer that contains both amorphous and crystalline portions. The polyester may contain a copolymer component that reduces crystallinity. For example, polyethylene terephthalate containing copolymer components such as isophthalic acid and adipic acid as dicarboxylic acid components has a relatively low degree of crystallinity and exhibits an excellent conversion rate to dicarboxylic acid salts upon depolymerization.
[0038] The crystallinity of the polyester subjected to depolymerization is not limited, but may be 50% or less. The crystallinity of the particles containing the polyester may be 50% or less. From the viewpoint of the efficiency of conversion of the polyester to a dicarboxylate or a hydroxycarboxylic acid, a lower crystallinity of the polyester subjected to depolymerization is advantageous. However, according to the method of the present disclosure, even a polyester (crystallized polyester) with a crystallinity of approximately 50% can be efficiently converted to a dicarboxylate or a hydroxycarboxylic acid under mild conditions. The lower the crystallinity of the polyester, the more easily the depolymerization reaction proceeds, and therefore, the efficiency of conversion to a dicarboxylate or a hydroxycarboxylic acid can be particularly improved. The crystallinity of the polyester (particles containing polyester) may be 40% or less, or 20% or less. As described above, the crystallinity can be adjusted by adding a copolymerizable monomer to the polyester, by stretching and orientation treatment, or the like. The crystallinity refers to the crystallinity obtained from wide-angle X-ray diffraction measurement, and specifically, it can be calculated from the wide-angle X-ray diffraction measurement profile using the following formula: Crystallinity (%) = {integral value of crystalline peak / (integral value of crystalline peak+integral value of amorphous peak)} × 100.
[0039] The intrinsic viscosity (IV) of the polyester may be 0.8 dl / g or less. A lower intrinsic viscosity tends to result in a smaller molecular weight of the polyester, which may contribute to more efficient depolymerization reaction. Even if the intrinsic viscosity of the polyester constituting a used polyester product (e.g., a bottle container) is high, the intrinsic viscosity of flakes formed after remelting the polyester for recycling may be reduced. There is no particular lower limit for the intrinsic viscosity, but the lower limit of the intrinsic viscosity may be about 0.3 dl / g. The intrinsic viscosity of the polyester may be 0.3 to 0.8 dl / g.
[0040] The shape of the polyester may be a powder composed of particles containing the polyester. According to the Powder Technology Glossary, the fundamental physical properties of a powder are characterized by particle shape and particle size. The particles constituting the polyester powder can have a variety of geometric shapes, such as cubical, granular, blocky, platy, flaky, film-like (thin flaky powder particles, thinner than flakes), prismoidal, rod-like, acicular, needle-like, fibrous, dendritic, sponge, angular, sharp-edged, sharp-cornered, modular, rounded, irregular, or crystalline, resulting from various processes. The shape of the particles is based on the mechanical and crystallographic properties of the material that constitutes the particle, and also depends on the production process (http: / / www.sptj.jp / powderpedia / words / 12474 / ). In the present disclosure, the particles containing polyester can have any shape, including those mentioned above. The particles containing polyester may be thin (flake-like), fibrous, film-like, or granular, and may be flake-like or granular, or may be granular. That is, the mixture may contain granular material containing polyester.
[0041] The average particle size of the polyester-containing granular material is not particularly limited, but may be 150 to 350 μm, or 200 to 300 μm. Here, the average particle size refers to the 50% particle size (D50: median size) when the particle size distribution measured by a laser diffraction scattering method is expressed as a cumulative distribution. The maximum particle size of the polyester-containing granular material may be 200 to 1000 μm, 250 to 500 μm, or 250 to 400 μm.
[0042] The longest side of the flaky particles containing polyester may be, for example, 1 to 50 mm, 1 to 20 mm, or 5 to 15 mm. Although small pieces obtained by collecting used PET bottles generally have a flake shape, the flake particles are not limited to those collected from used PET bottles.
[0043] The longest side of the fibrous particles containing polyester (the length of the fibrous particles) may be 1 to 500 mm, or 1 to 200 mm. The fibrous particles may be short fibers having the longest side (length) of about 1 to 100 mm. The fibrous polyester may be PET fiber used in clothing, but is not limited to these.
[0044] The longest side of the film-like particle containing polyester may be, for example, about 1 to 200 mm, 1 to 100 mm, or 1 to 50 mm.
[0045] In the present disclosure, components (a), (b), and (c) are mixed so that the blending ratio of each component falls within the above-described range. In other words, components (a), (b), and (c) are mixed so that the blending ratio of each component falls within the above-described range to form a mixture, and the mixture is then stirred or kneaded. The mixture may be a dispersion containing a solution containing an alkali compound and a solvent and polyester-containing particles dispersed in the solution. Alternatively, the mixture may be a powder mixture containing polyester-containing particles and a solvent integrated with the particles. The powder mixture may contain a solid alkali compound. The solid alkali compound may be integrated with the polyester-containing particles or may form particles separate from the polyester-containing particles. The solvent and / or alkali compound integrated with the polyester-containing particles may adhere to the surface of the polyester-containing particles or may penetrate into the interior of the polyester-containing particles. In a powder mixture, depolymerization of polyester can proceed particularly efficiently.
[0046] According to one example of the present disclosure, the depolymerization reaction of the polyester proceeds even when the components are mixed under mild conditions, such as at 75°C or below. From the perspective of the conversion rate to the dicarboxylate or hydroxycarboxylic acid salt, mixing (stirring or kneading) may be carried out for approximately 50 minutes or approximately 30 minutes. This facilitates a conversion rate to the dicarboxylate or hydroxycarboxylic acid salt of 50% or more. "Mixing" refers to the act of stirring or kneading the composition containing an alkali compound (a composition containing an alkali compound and a solvent) and the polyester in a container to achieve a uniform state. Specifically, mixing refers to stirring or kneading a mixture containing these components. The stirring and kneading speeds are not limited. Considering operational safety and equipment capacity, the stirring speed (e.g., the rotation speed of the stirring blade) may be, for example, 250 to 1500 rpm or 500 to 1000 rpm. The kneading speed (for example, the rotation speed of the kneading blades) may be, for example, 5 to 150 rpm, or 10 to 100 rpm.
[0047] <Method for Recycling Polyester> In another example of the present disclosure, a recycling method is provided in which a product produced by the above-described method for depolymerizing a polyester is used as at least a part of a polyester polymerization raw material to regenerate a polyester. That is, by applying the method for depolymerizing a polyester, a dicarboxylate salt and a dialcohol are obtained as products from a polyester prepared from a used polyester product (e.g., a used bottle container containing a polyester). The dicarboxylate salt can be separated as a solid. The dicarboxylate salt is usually converted to a dicarboxylic acid before being used as a polyester polymerization raw material. The dialcohol can be separated from a mixture with an alcohol solvent and / or a ketone solvent by a known operation such as fractional distillation. A product containing a salt of a hydroxycarboxylic acid is obtained from a polyester containing hydroxycarboxylic acid units. The salt of a hydroxycarboxylic acid is usually converted to a hydroxycarboxylic acid before being used as a polyester polymerization raw material.
[0048] In one example of the present disclosure, polyethylene terephthalate is used, methanol is used as the solvent containing an alcoholic solvent and / or a ketone solvent, and sodium hydroxide is used as the alkali metal hydroxide. In this case, sodium terephthalate is obtained as a solid by depolymerization of polyethylene terephthalate, and ethylene glycol can be obtained by fractional distillation of a mixture of ethylene glycol and methanol. The obtained sodium terephthalate can be converted into terephthalic acid by adding an acid. Polyethylene terephthalate can be regenerated from the terephthalic acid and ethylene glycol obtained in this manner. The mixture of sodium terephthalate, ethylene glycol, and methanol obtained after depolymerization can be dissolved in water to obtain an aqueous solution containing sodium terephthalate, ethylene glycol, and methanol, and then terephthalic acid can be crystallized and recovered by adding an acid. In this case, the methanol and ethylene glycol remaining in the aqueous solution can be recovered by fractional distillation, respectively. Polyethylene terephthalate can be regenerated or produced from the terephthalic acid and ethylene glycol obtained in this manner. The terephthalic acid and ethylene glycol obtained by the method of the present disclosure may be used as part of the diol component and dicarboxylic acid component used in producing polyester.
[0049] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to these examples.
[0050] <Sample Preparation> (1) Polyester - PET Sample 1 A commercially available amorphous PET resin (PBK-1, intrinsic viscosity 0.65 dl / g, manufactured by Bell Polyester Products) was prepared. This PET resin was freeze-pulverized to obtain PET Sample 1, a granular material containing polyethylene terephthalate. The particle size distribution of PET Sample 1 was measured by a wet method using a laser diffraction particle size distribution analyzer (Anton Paar, PSA1190) employing a scattering method. From the obtained particle size distribution, the 50% particle size (D50 median size) expressed as a cumulative distribution was calculated, and this value was used as the average particle size. The average particle size of PET Sample 1 was 218 μm. Wide-angle X-ray diffraction measurement of PET Sample 1 was performed using a wide-angle X-ray diffractometer (RINT2500HL, manufactured by Rigaku). The conditions for the wide-angle X-ray diffraction measurement were: X-ray source Cukα radiation (λ = 0.1542 nm), output 50 kV-250 mA, scanning speed 0.5 deg / min, slit width DS 0.6 mm + 10 mmH. Peak fitting was performed in the range of 2θ = 1.5 to 70° of the obtained diffraction pattern, and the integrated intensities of the angular peaks were summed for the crystalline component and the amorphous component, respectively. These values were designated as the crystalline component integrated intensity I and the amorphous component integrated intensity Ia. The crystallinity X was calculated from I and Ia according to the following formula: X = {I / (I + Ia)} × 100 (%) X: crystallinity I: crystalline component integrated intensity Ia: amorphous component integrated intensity The crystallinity of PET sample 1 calculated as above was 0.40%.
[0051] PET Sample 2 A commercially available crystalline PET resin (TK-3, intrinsic viscosity 0.65 dl / g, manufactured by Bell Polyester Products Co., Ltd.) was prepared. This PET resin was freeze-pulverized to obtain PET Sample 2, a granular material containing polyethylene terephthalate. The average particle size of PET Sample 2 was calculated in the same manner as above and was found to be 268 μm. The crystallinity of PET Sample 2 was determined in the same manner as above and was found to be 22.8%.
[0052] Examples 1-2, Comparative Examples 1-2 A solution was prepared by dissolving potassium hydroxide in ethanol. The temperature of this solution was adjusted to 40°C, and then PET Sample 1 was added to the solution to form a dispersion mixture containing PET Sample 1, potassium hydroxide, and ethanol in the masses shown in Table 1. After the mixture was formed, it was stirred for 10 minutes at 760 rpm using a mechanical stirrer (BL600, manufactured by Shinto Scientific Co., Ltd.) without heating. The amount of PET Sample 1 added was varied between 5 g (26 mmol) and 30 g (156 mmol), as shown in Table 1. The mixture was stirred under four conditions. The amount of potassium hydroxide in the solution was adjusted to 2.2 relative to the mass of the PET repeating units under each of the four conditions. The depolymerization rate and terephthalic acid conversion rate calculated as described below were as shown in Table 1. As is clear from Table 1, the depolymerization efficiency increased and a more effective effect was achieved as the amount of PET Sample 1 added relative to the reaction solvent increased on a mass basis. The "mol number of repeating units" in the table indicates the number of repeating units (C 10 H 8 O 4 The initial temperature in the table is the temperature of the mixture at the time when the entire amount of the PET sample was added to the solution, i.e., when a mixture containing the entire amount of the solution and the PET sample was formed.
[0053] <Depolymerization Rate> After 10 minutes had elapsed since the start of stirring the mixture, a sufficient amount of water was added to the mixture (reaction liquid) to dissolve the product. The unreacted PET sample 1 was recovered by centrifugation. The recovered unreacted PET sample 1 was dried by heating in an oven at 100°C for 12 hours or more, and its mass W fin The depolymerization rate was calculated using the following formula: Depolymerization rate (%) = [(W int -W fin ) / W int ]×100 In the above formula, W int represents the mass (g) of PET sample 1 subjected to the reaction, and W fin represents the mass (g) of the unreacted PET sample 1 recovered after the reaction.
[0054] <Terephthalic Acid Conversion Rate> The supernatant obtained during centrifugation to recover unreacted PET Sample 1 was placed in a volumetric flask, and water was added to bring the total volume to 1 L. A portion of the solution in the volumetric flask was diluted 100-fold with a diluent (1 N HCl aqueous solution: isopropanol = 1:9 (v / v)). The diluted solution was used as a sample to quantify terephthalic acid by HPLC. The HPLC measurement conditions were as follows: Column: L-column 2 ODS 2.1 mm x 150 mm, particle size 2 μm (Chemicals Evaluation and Research Institute, Japan) Column temperature: 35°C Mobile phase A: water containing 0.1% acetic acid Mobile phase B: acetonitrile containing 0.1% acetic acid Flow rate: 0.2 mL / min Linear gradient: 15% B (0 min) → 80% B (26 min) Detector: photodiode array (wavelength 190 to 600 nm)
[0055] Based on the quantitative results of HPLC, the terephthalic acid conversion rate was calculated using the following formula: Conversion rate (%) = [(W tpa / 166) / (W int / 192)] × 100 In the above formula, W int is the mass (g) of PET sample 1 subjected to the reaction, W tpa is the amount of terephthalic acid (g) produced in free form calculated based on the quantitative results of HPLC, 166 is the molecular weight of terephthalic acid, and 192 is the repeating unit of PET (C 10 H 8 O 4 ) is the formula mass of
[0056]
[0057] [Examples 3-4, Comparative Examples 3-4] The temperature of a solution in which potassium hydroxide was added to ethanol was adjusted to 50°C, and then PET sample 2 was added to the solution to form a mixture, which was a dispersion containing PET sample 2, potassium hydroxide, and ethanol in the masses shown in Table 2. Experiments were conducted in the same manner as in Examples 1-2 and Comparative Examples 1-2, except that the formed mixture was stirred, and the depolymerization rate and terephthalic acid conversion rate were calculated. The results obtained were as shown in Table 2. As is clear from Table 2, the depolymerization efficiency increased and a higher effect was achieved as the amount of PET sample 2 added increased on a mass basis relative to the reaction solvent.
[0058]
[0059] Example 5 A solution was prepared by dissolving sodium hydroxide in methanol. The temperature of this solution was adjusted to 40°C, and then 30 g of PET sample 1 was added to the solution to form a mixture, which was a dispersion containing PET sample 1, sodium hydroxide, and methanol in the masses shown in Table 3. An experiment was conducted in the same manner as in Example 1, except that the formed mixture was stirred, and the depolymerization rate and terephthalic acid conversion rate were calculated. The results obtained are shown in Table 3. For comparison, Example 1 is also listed in Table 3.
[0060]
[0061] Example 6 A solution of sodium hydroxide in a methanol / water mixed solvent (methanol:water (by mass) = approximately 7:3) was adjusted to 40°C, and then PET sample 1 was added to the solution to form a mixture that was a dispersion containing PET sample 1, sodium hydroxide, and the mixed solvent (methanol / water) in the masses shown in Table 4. An experiment was conducted in the same manner as in Example 1, except that the formed mixture was stirred, and the depolymerization rate and terephthalic acid conversion rate were calculated. The results obtained are shown in Table 4.
[0062] Example 7 A solution of sodium hydroxide in a methanol / water mixed solvent (methanol:water (by mass) = approximately 7:3) was adjusted to 50°C, and then PET sample 2 was added to the solution to form a mixture that was a dispersion containing PET sample 2, sodium hydroxide, and the mixed solvent (methanol / water) in the masses shown in Table 4. An experiment was conducted in the same manner as in Example 3, except that the formed mixture was stirred, and the depolymerization rate and terephthalic acid conversion rate were calculated. The results obtained are shown in Table 4.
[0063] Comparative Example 5 After adjusting the temperature of a solution of sodium hydroxide in water to 40°C, PET sample 1 was added to the solution to form a mixture that was a dispersion containing PET sample 1, sodium hydroxide, and water in the masses shown in Table 4. An experiment was conducted in the same manner as in Example 6, except that the formed mixture was stirred, and the depolymerization rate and terephthalic acid conversion rate were calculated. The results obtained are shown in Table 4.
[0064] As is clear from Table 4, under the conditions of Examples 6 and 7, which used a mixed solvent containing methanol and water in a ratio of approximately 7:3 by mass, a high depolymerization rate of 70% or more was observed. In contrast, in Comparative Example 5, which used only water as the solvent, the depolymerization rate was low, less than 3%, even though the amount of PET added was high, at 0.613 by mass relative to the reaction solvent. This result suggests that using an alcohol-based solvent as the solvent is advantageous in terms of increasing the depolymerization efficiency.
[0065]
[0066] Example 8 A commercially available crystalline PET resin powder (granular material, ES30-PD-000132, intrinsic viscosity 0.80 dl / g, maximum particle size 300 μm, manufactured by Goodfellow) was prepared as PET sample 3. The crystallinity of PET sample 3 was determined in the same manner as for PET sample 1 and was found to be 39.5%.
[0067] 150 g of methanol was heated to 50°C in a kneader (Hivis Dispermix 3D-2, manufactured by Primix Corporation). 137 g (3.43 mol) of sodium hydroxide and 300 g of PET sample 3 (amount of substance based on the repeating unit: 1.56 mol) were added thereto to form a powdery mixture containing PET sample 3, sodium hydroxide, and methanol with the mass shown in Table 5. The formed powdery mixture was kneaded for 15 minutes at a rotation speed of 40 rpm without heating. The depolymerization rate and terephthalic acid conversion rate were as shown in Table 5.
[0068]
[0069] Example 9: PET sample 4 was prepared by flaking recycled PET bottles. PET sample 4 was a powder containing flake-like particles measuring 0.5 to 1 cm on a side. The crystallinity of the sample obtained by freeze-pulverizing PET sample 4 was measured in the same manner as for PET sample 1, and was found to be 8.8%.
[0070] The flake-like PET sample 4 was subjected to a depolymerization test as is. 150 g of methanol was placed in a benchtop kneader (PNV-1, Irie Shokai Co., Ltd.) and heated to 50°C. 137 g (3.43 mol) of sodium hydroxide and 300 g of PET sample 4 (amount of substance based on the repeating unit: 1.56 mol) were added to form a powdery mixture containing PET sample 4, sodium hydroxide, and methanol with the mass shown in Table 6. The formed powdery mixture was kneaded for 30 minutes at 40 rpm without heating. The depolymerization rate and terephthalic acid conversion rate were as shown in Table 6.
[0071]
[0072] Example 10 155 g of methanol was placed in a benchtop kneader (PNV-1, Irie Shokai Co., Ltd.) and heated to 50°C. 114 g (2.85 mol) of sodium hydroxide and 250 g (amount of substance based on the repeating unit: 1.30 mol) of PET sample 3 were added thereto to form a powdery mixture containing PET sample 4, sodium hydroxide, and methanol with the mass shown in Table 7. The formed powdery mixture was kneaded for 30 minutes at a rotation speed of 50 rpm without heating. The depolymerization rate and terephthalic acid conversion rate were as shown in Table 7.
[0073] Example 11 155 g of methanol was placed in a benchtop kneader (PNV-1, Irie Shokai Co., Ltd.). 114 g (2.85 mol) of sodium hydroxide and 250 g (amount of substance based on the repeating unit: 1.30 mol) of PET sample 3 were added to the methanol in the kneader at room temperature (21°C) to form a powdery mixture containing PET sample 4, sodium hydroxide, and methanol with the mass shown in Table 7. The formed powdery mixture was kneaded for 30 minutes at a rotation speed of 50 rpm without heating. The depolymerization rate and terephthalic acid conversion rate were as shown in Table 7.
[0074] Example 12 125 g of methanol was placed in a benchtop kneader (PNV-1, Irie Shokai Co., Ltd.). 114 g (2.85 mol) of sodium hydroxide and 250 g of PET sample 3 (amount of substance based on the repeating unit: 1.30 mol) were added to the methanol in the kneader at room temperature (19°C) to form a powdery mixture containing PET sample 3, sodium hydroxide, and methanol with the mass shown in Table 7. The formed powdery mixture was kneaded at 50 rpm for 8 minutes without heating. The depolymerization rate and terephthalic acid conversion rate were as shown in Table 7.
[0075] Example 13 125 g of ethanol was placed in a benchtop kneader (PNV-1, Irie Shokai Co., Ltd.). 114 g (2.85 mol) of sodium hydroxide and 250 g of PET Sample 3 (amount of substance based on the repeating unit: 1.30 mol) were added to the ethanol in the kneader at room temperature (15°C) to form a powdery mixture containing PET Sample 3, sodium hydroxide, and ethanol with the mass shown in Table 7. The formed powdery mixture was kneaded at 50 rpm for 8 minutes without heating. The depolymerization rate and terephthalic acid conversion rate were as shown in Table 7.
[0076]
Claims
1. A method for depolymerizing a polyester, the method comprising: forming a mixture containing the following components (a), (b) and (c): (a) a polyester; (b) one or more alkali compounds selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, alkali metal hydrogencarbonates, alkaline earth metal hydroxides, alkaline earth metal carbonates and alkaline earth metal hydrogencarbonates; and (c) a solvent containing at least one of an alcohol solvent and a ketone solvent; and depolymerizing the polyester in the mixture; wherein the temperature of the mixture when the mixture containing the total amount of the polyester, the alkali compound and the solvent is formed is 75°C or less; and the ratio of the amount of the polyester to the amount of the solvent is 0.2 to 20 on a mass basis.
2. The method according to claim 1, wherein the alkaline compound dissolves in an amount of 100 g or more in 100 g of water at 20±5° C.
3. The method of claim 1, wherein the alkali compound is one or more alkali metal compounds selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, and alkali metal bicarbonates.
4. The method of claim 1, wherein the alkaline compound is an alkali metal hydroxide, an alkaline earth metal hydroxide, or both.
5. The method according to claim 1, wherein the alkali compound is an alkali metal hydroxide, an alkaline earth metal hydroxide, or both, and the total amount of hydroxide ions in the alkali metal hydroxide and hydroxide ions in the alkaline earth metal hydroxide is in the range of 0.9 to 3.0 based on the amount of repeating units of the polyester before the mixture is formed.
6. The method of claim 1, wherein the mixture containing the polyester, the alkaline compound, and the total amount of the solvent is at a temperature of 0 to 75°C when the mixture is formed.
7. The method of claim 1, wherein the mixture containing the polyester, the alkaline compound, and the total amount of the solvent is at a temperature of 35 to 55°C when the mixture is formed.
8. The method of claim 1, wherein the ratio of the amount of said polyester to the amount of said solvent is from 0.25 to 2.2 by weight.
9. The method of claim 1, wherein said polyester is polyethylene terephthalate.
10. The method of claim 1, wherein the alkaline compound is sodium hydroxide, potassium hydroxide or both.
11. The method of claim 1, wherein the alcoholic solvent is a lower alcohol.
12. The method of claim 1, wherein said mixture comprises particles comprising said polyester.
13. The method according to claim 12, wherein the particles containing the polyester are particulate matter having an average particle size of 150 to 350 μm.
14. The method of claim 12, wherein the polyester-containing particles have a crystallinity of 50% or less.
15. The method of claim 12, wherein said mixture is a powder mixture comprising particles comprising said polyester and said solvent associated with said particles.
16. The method of claim 1, wherein the polyester before the mixture is formed has an intrinsic viscosity of 0.8 dl / g or less.
17. The method of claim 1, wherein the polyester is prepared from used bottle containers containing polyester.
18. A method for producing a diol and a dicarboxylic acid comprising producing a diol and a dicarboxylate from a polyester by the method of any one of claims 1 to 17.
19. A method for recycling polyester, comprising producing a polyester by polymerizing a polymerization raw material containing at least one of the diol obtained by the method according to claim 18 and a dicarboxylic acid produced from the dicarboxylate.
Citation Information
Patent Citations
Method for treating plastic molded form
JP1996253619A
A chemical recycling method for waste polyethylene terephthalate (pet)
JP2007519798A
Method for dissolving saturated polyester, solution for decomposing saturated polyester and method for decomposition using the same
WO2003042288A1
A process for preparing a monoester of terephthalic acid and its derivatives
WO2022150016A1
Cited By
Decomposition method for polyester-based resin and decomposition apparatus for polyester-based resin
EP4806950A1