Method for preparing ultraviolet blocking powder by using dry process and ultraviolet blocking powder prepared thereby

The dry process for forming a silica coating layer on porous silica with a solid organic sunscreen in ultraviolet blocking powders addresses environmental and efficiency issues, improving UV blocking performance and stability while preventing skin irritation, resulting in a more sustainable and effective sunscreen production method.

WO2024225524A1PCT designated stage expired Publication Date: 2024-10-31SUNJIN BEAUTY SCI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/006587
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-05-16
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional wet processes for manufacturing ultraviolet blocking powders generate significant wastewater, consume high energy, and result in poor stability and skin irritation due to leakage of chemical sunscreens, while also being inefficient in terms of raw material usage and production economics.

Method used

A dry process is employed to form a silica coating layer on porous silica supporting a solid organic sunscreen, using an aqueous silicic acid solution sprayed and condensed at 80-120°C, which reduces waste, energy consumption, and enhances coating efficiency, preventing sunscreen leakage and improving stability and skin safety.

Benefits of technology

The method significantly reduces environmental impact, saves energy, and enhances UV blocking performance, stability, and user experience by increasing the density of the coating layer, preventing sunscreen leakage and ensuring no skin irritation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023006587_31102024_PF_FP_ABST
    Figure KR2023006587_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing ultraviolet blocking powder by using a dry process and ultraviolet blocking powder prepared thereby, and may provide a method for preparing ultraviolet blocking powder by using a dry process and ultraviolet blocking powder prepared thereby, in which, by using a dry process instead of a wet process to form a coating layer formed of powder, the generation of a large amount of wastewater due to the wet process is prevented, thus being environmentally friendly, process time can be drastically reduced, process energy can be saved, the amounts of raw materials used can be reduced due to high coating efficiency, thus significantly improving the economic efficiency of production, and at the same time, excellent performance in blocking ultraviolet rays is exhibited, a chemical ultraviolet blocking agent inside the powder is prevented from leaking out, by increasing the density of the coating layer, so that there is no concern about skin irritation caused by organic ultraviolet blocking agents, and excellent stability and excellent texture are exhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing ultraviolet ray blocking powder using a dry process and ultraviolet ray blocking powder manufactured thereby

[0001] The present invention relates to a method for manufacturing a UV-blocking powder using a dry process and a UV-blocking powder manufactured thereby, and by using a dry process instead of a wet process in forming a coating layer of the powder, the generation of a large amount of wastewater due to the wet process is prevented, making it environmentally friendly, the process time can be drastically reduced, process energy can be saved, the coating efficiency is high, the amount of raw materials used can be reduced, and production economy can be significantly improved, and at the same time, the UV-blocking performance is excellent, the density of the coating layer is increased, so that the chemical UV-blocking agent inside the powder is prevented from leaking out, so there is no concern about skin irritation due to the organic UV-blocking agent, and the stability is excellent, and the feeling of use is excellent. The present invention relates to a method for manufacturing a UV-blocking powder using a dry process and a UV-blocking powder manufactured thereby.

[0002] The content described below merely provides background information related to the present invention and does not constitute prior art.

[0003] Normally, about 1% of the sunlight that reaches the Earth's surface is ultraviolet rays, which are harmful to humans.

[0004] These ultraviolet rays are light with a shorter wavelength than visible light or infrared rays, and since the energy of light is inversely proportional to the wavelength, ultraviolet rays are light with greater energy than visible light or infrared rays.

[0005] Therefore, the more ultraviolet rays a person is exposed to, the more chemical reactions can occur due to the large energy of the ultraviolet rays, and this can induce physiological changes.

[0006] Because ultraviolet rays have high energy, they activate many chemicals, changing their structure or paralyzing their functions.

[0007] Organic pigments, which are particularly widely used in cosmetics and daily necessities, are substances that easily lose their original function as they are activated by ultraviolet rays.

[0008] For this reason, sunscreens have long been essential in the formulation of cosmetics and daily necessities.

[0009] Recently, the market for products aimed at blocking ultraviolet rays has been growing significantly every year due to the increase in the amount of ultraviolet radiation on the surface of the earth caused by the destruction of the ozone layer.

[0010] Most chemical (organic) sunscreens can cause physiological damage when in direct contact with the human body.

[0011] In addition, chemical sunscreens have poor stability to heat and light and poor solubility in solvents, which limits their use and makes them feel uncomfortable to use.

[0012] To overcome these problems, Korean Patent Application No. 10-2009-0059107 discloses a composite pigment in which an organic UV blocker is supported on hollow silica. However, when the organic UV blocker supported on silica is applied to a cosmetic, it is eluted from the silica and comes into direct contact with the skin, resulting in poor skin stability and poor photostability and heat stability.

[0013] In addition, Korean Patent Publication No. 10-2018-0126270 discloses a silica-based composite powder for UV protection, which includes porous silica; an inorganic UV blocker doped on the surface inside the pores of the porous silica; an organic UV blocker impregnated on the pores of the porous silica; and a coating layer coated on the outer surface of the porous silica. However, the surface strength of the coating layer is weak, so the surface coating layer is easily broken, which increases the risk of skin irritation, and the usability is poor, so improvements are requested.

[0014] In addition, the applicant's Korean Patent Application No. 10-2020-0174433 discloses a method for manufacturing a UV-blocking powder by loading a chemical UV blocking agent that is solid at room temperature into the pores of porous silica and then coating the silica surface with an aqueous silicic acid solution through a wet process. However, there was a request for the development of an environmentally friendly manufacturing method that can replace the wet process and reduce environmental pollution-causing factors caused by the wet process.

[0015] The technical problem to be achieved by the present invention is to solve the problems of the past, and by using a dry process instead of a wet process in forming a powder coating layer, it is environmentally friendly by preventing a large amount of wastewater generated by the wet process, and the process time can be drastically reduced, process energy can be saved, and the coating efficiency is high so that the amount of raw materials used can be reduced, and production economy can be significantly improved, and at the same time, the ultraviolet ray blocking performance is excellent, and the density of the coating layer is increased so that the chemical ultraviolet ray blocker inside the powder is prevented from leaking out, so that there is no concern about skin irritation due to the organic ultraviolet ray blocker, and the purpose is to provide a method for manufacturing a UV-blocking powder using a dry process and a UV-blocking powder manufactured thereby.

[0016] The present invention

[0017] S1) A step of loading an organic UV blocking agent that is in a solid state at room temperature into the pores of porous silica;

[0018] S2) Step of preparing a silicate solution; and

[0019] S3) A step of forming a silica coating layer by dry-coating a silicic acid aqueous solution on the porous silica surface in which an organic UV blocking agent is loaded in the pores;

[0020] A method for manufacturing a UV blocking powder including .

[0021] Preferably, the content of Silicic Acid in the Silicic Acid aqueous solution of the above step S2) is 3 to 30 wt%.

[0022] Preferably, the dry coating of the above step S3) is performed by spraying an aqueous solution of Silicic Acid so that it is applied to the surface of a porous silica carrying an organic UV blocker, and then a silica coating layer is formed through a condensation reaction of Silicic Acid.

[0023] Specifically, the above condensation reaction can be carried out by stirring porous silica, which has an organic UV blocker impregnated on its surface with a silicic acid aqueous solution, at 80 to 120°C at 100 to 1000 rpm.

[0024] Preferably, the silica coating layer (30) is 5 to 100 parts by weight based on 100 parts by weight of the total of the porous silica (10) and the ultraviolet ray blocking agent (20).

[0025] Preferably, after the step S3), a step of drying the ultraviolet ray blocking powder having a silica coating layer formed on the surface with silicic acid may be further included.

[0026] Preferably, the step S3) may further include a step of forming an organic coating layer or an inorganic coating layer on the outermost surface of the ultraviolet ray blocking powder on which a silica coating layer is formed using silicic acid on the surface.

[0027] In addition, the present invention

[0028] In UV blocking powder,

[0029] Porous silica having pores (10);

[0030] A chemical UV blocker (20) that is solid at room temperature and is contained in the pores of the porous silica; and

[0031] A silica coating layer (30) formed by dry-coating silicic acid on the surface of porous silica in which the chemical UV blocking agent is contained in the pores;

[0032] Provides a UV blocking powder (100) including:

[0033] Preferably, the above UV blocking powder (100) is characterized by being manufactured by the manufacturing method described above.

[0034] Preferably, the silica coating layer (30) is 5 to 100 parts by weight based on 100 parts by weight of the total of the porous silica (10) and the ultraviolet ray blocking agent (20).

[0035] Preferably, the absorption amount of the above UV blocking powder (100) is 0.20 to 0.49 mL / g.

[0036] In addition, the present invention provides a cosmetic comprising the UV blocking powder (100) described above.

[0037] According to the present invention, by using a dry process instead of a wet process in forming a powder coating layer, the production of a large amount of wastewater due to the wet process is prevented, which is environmentally friendly, the process time can be drastically reduced, process energy can be saved, the coating efficiency is high, the amount of raw materials used is reduced, production economy can be significantly improved, and at the same time, the UV blocking performance is excellent, the density of the coating layer is increased, so that the chemical UV blocking agent inside the powder is prevented from leaking out, so there is no concern about skin irritation due to the organic UV blocking agent, and the stability and usability are excellent. A method for manufacturing a UV blocking powder using a dry process and a UV blocking powder manufactured thereby can be provided.

[0038] Figure 1 is a schematic diagram of a UV blocking powder according to one embodiment of the present invention.

[0039] Figure 2 is a schematic diagram of a UV blocking powder according to another embodiment of the present invention.

[0040] Figure 3 is a schematic diagram showing a method for manufacturing a UV blocking powder according to an embodiment of the present invention.

[0041] Embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0042] Throughout this specification, whenever a part is said to "include" a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise stated.

[0043] The present invention has been devised to solve the disadvantages of the conventional wet coating method, such as environmental pollution, large energy consumption, and long manufacturing time, on the surface of a porous silica in which an organic UV blocking agent is supported in the pores, by a dry coating method, and a silica coating layer can be formed using a silicic acid aqueous solution. In this case, the generation of a large amount of wastewater due to the wet process is prevented, making it environmentally friendly, the process time can be drastically reduced, process energy can be saved, the coating efficiency is high, the amount of raw materials used can be reduced, and the production economy can be significantly improved. At the same time, the UV blocking performance is excellent, and the density of the coating layer is increased, preventing the chemical UV blocking agent inside the powder from leaking out, so there is no concern about skin irritation due to the organic UV blocking agent, and it has been confirmed that it is possible to manufacture a UV blocking powder having excellent stability and a good feeling of use, thereby completing the present invention.

[0044] The method for manufacturing the ultraviolet ray blocking powder of the present invention is

[0045] S1) A step of loading an organic UV blocking agent that is in a solid state at room temperature into the pores of porous silica;

[0046] S2) Step of preparing a silicate solution; and

[0047] S3) A step of forming a silica coating layer by dry-coating a silicic acid aqueous solution on the porous silica surface in which an organic UV blocking agent is loaded in the pores;

[0048] It is characterized by including.

[0049] In the present invention, a known method can be applied to the method of loading the chemical UV blocker (20) of the step S1) into the pores of the porous silica (10), and specifically, when the chemical UV blocker (20) and the porous silica (10) are mixed in a Henschel mixer and then stirred at a temperature higher than the melting point of the chemical UV blocker (20) but below the thermal decomposition temperature and then cooled, the chemical UV blocker (20) can be loaded into the pores of the porous silica (10), and more specifically, when the temperature is maintained at about 60 to 100° C. and stirred at 200 to 500 rpm and then cooled, the chemical UV blocker (20) can be loaded into the pores of the porous silica (10).

[0050] The porous silica (10) above can be used with a pore size of 10 to 90%, and the content of the chemical UV blocking agent (20) carried can be adjusted depending on the use of the product.

[0051] The content of the chemical UV blocker (20) loaded on the porous silica (10) can be arbitrarily adjusted, and specifically, it can be loaded in an amount of 10 to 200 parts by weight per 100 parts by weight of the porous silica (10).

[0052] The chemical UV blocker (20) having a solid state at room temperature may be a known chemical UV blocker, and specifically, at least one selected from the group consisting of butyl methoxydibenzoylmethane, ethylhexyl methoxycinnamate, ethylhexyl silicate, octyldimethyl para-aminobenzoic acid, octyl methoxycinnamate, octyl salicylate, octocrylene, butyl methoxydibenzoylmethane, oxybenzone, octyltriazone, menthyl anthranilate, 3,4-methylbenzylidenekempfer, and bis-ethylhexyloxyphenol methoxyphenyl triazine.

[0053] The present invention includes a step of preparing a silica aqueous solution in the step S2), and preferably, the silica content of the silica aqueous solution is 3 to 30 wt%. In this case, the coating efficiency is high, so that the amount of raw materials used can be reduced, thereby significantly improving the production economy, and at the same time, the UV blocking performance is excellent, and the density of the coating layer is increased, so that the chemical UV blocking agent inside the powder is prevented from leaking out, so that there is no concern about skin irritation due to the organic UV blocking agent, and a UV blocking powder having excellent stability and excellent usability can be manufactured.

[0054] Specifically, the above-mentioned Silicic Acid aqueous solution can be prepared by dissolving TEOS in distilled water having a pH of 2 to 3 while stirring.

[0055] The present invention includes a step S3) of forming a silica coating layer by dry-coating a silicic acid aqueous solution on a porous silica surface in which an organic UV blocking agent is loaded in the pores.

[0056] Preferably, the dry coating in step S3) is performed by spraying an aqueous solution of Silicic Acid so that it is evenly applied to the surface of a porous silica loaded with an organic UV blocking agent, and then a silica coating layer is formed through a condensation reaction of Silicic Acid.

[0057] Specifically, the condensation reaction can be carried out at 80 to 120°C for 1 to 5 hours while stirring the porous silica impregnated with an organic UV blocker and having a silicic acid aqueous solution on the surface at 100 to 1000 rpm. The stirring can be performed using a Henschel mixer, and the condensation reaction can be performed while maintaining a vacuum inside the mixer. Preferably, the temperature of the condensation reaction is 100 to 120°C. In this case, the coating efficiency is high, so that the amount of raw materials used can be reduced, thereby significantly improving the production economy. At the same time, the UV blocking performance is excellent, and the density of the coating layer is increased, so that the chemical UV blocker inside the powder is prevented from leaking to the outside, so that there is no concern about skin irritation due to the organic UV blocker, and a UV blocking powder having excellent stability and a good feeling of use can be manufactured.

[0058] The content of the above silica coating layer (30) can be arbitrarily adjusted, and is preferably 5 to 100 parts by weight based on 100 parts by weight of the total of the porous silica (10) and the ultraviolet ray blocker (20).

[0059] The present invention may further preferably include a step of drying the UV-blocking powder having a silica coating layer formed on the surface with silicic acid after the step S3). Conventional powder drying methods may be applied for the drying.

[0060] In addition, the present invention may further preferably include a step of forming an organic coating layer or an inorganic coating layer on the outermost surface of the ultraviolet ray blocking powder having a silica coating layer formed with silicic acid on the surface after the step S3).

[0061] In the present invention, the coating material of the organic coating layer (40) may be specifically selected from monohydric alcohols including cetyl alcohol, lauryl alcohol, myristyl alcohol, lauryl-myristyl alcohol, lauryl-cetyl alcohol, caprylic alcohol, capric alcohol, stearyl alcohol, cetyl-stearyl alcohol, and decyl alcohol, and / or dihydric alcohols including hexanediol, propanediol, butanediol, pentandiol, and octanediol, but is not limited thereto. Preferably, the organic coating may be a coating using cetyl alcohol. In this case, the stability of the UV-blocking powder in a cosmetic can be further improved.

[0062] In addition, the above-mentioned inorganic coating layer (40) may be formed of a silane compound or may be formed of titanium dioxide or zinc oxide, and the inorganic coating layer (40) may be formed in an amount of 5 to 100 parts by weight based on 100 parts by weight of the total of the porous silica (10) and the UV blocking agent (20). In this case, the stability of the cosmetic can be further improved.

[0063] In addition, the present invention may further include a step of cooling the powder to room temperature, crushing the powder in which some agglomeration has occurred, and then filtering the powder through a 100 to 200 mesh sieve.

[0064] In addition, the present invention

[0065] In UV blocking powder,

[0066] Porous silica having pores (10);

[0067] A chemical UV blocker (20) that is solid at room temperature and is contained in the pores of the porous silica; and

[0068] A silica coating layer (30) formed by dry-coating silicic acid on the surface of porous silica in which the chemical UV blocking agent is contained in the pores;

[0069] Provides a UV blocking powder (100) including:

[0070] Preferably, the above UV blocking powder (100) is manufactured by the manufacturing method of the above UV blocking powder (100).

[0071] Preferably, the silica coating layer (30) is 5 to 100 parts by weight based on 100 parts by weight of the total of the porous silica (10) and the UV blocking agent (20). In this case, the UV blocking performance is excellent, and the density of the coating layer is increased to prevent the chemical UV blocking agent inside the powder from leaking out, so there is no concern about skin irritation due to the organic UV blocking agent, and the stability is excellent and the usability is excellent.

[0072] Preferably, the absorption amount of the above UV blocking powder (100) is 0.20 to 0.49 mL / g, more preferably 0.20 to 0.40 mL / g. In this case, when applied to cosmetics, even if the formulation changes, the density of the coating layer is increased to prevent the chemical UV blocking agent inside the powder from leaking out, so there is no concern about skin irritation due to the organic UV blocking agent, and the stability is excellent and the usability is excellent.

[0073] In addition, the pore volume of the above UV blocking powder (100) is 0.05 to 0.015 cm 3 / g is recommended, and more preferably 0.05 to 0.01 cm 3 / g is recommended. In this case, when applied to cosmetics, it prevents chemical UV blockers from leaking out, so there is no concern about skin irritation caused by organic UV blockers, and it has excellent stability and a good feel when used.

[0074] The present invention also provides a cosmetic comprising the UV-blocking powder described above.

[0075] Hereinafter, the present invention will be described in detail through examples. However, the following examples are only illustrative of the present invention, and the present invention is not limited to the following examples.

[0076] Test 1: Comparison of physical properties of UV-blocking powders according to condensation temperature ([Examples 1] to [Examples 4] and [Comparative Example 1])

[0077] A UV blocking powder was manufactured according to the manufacturing method of Fig. 3, and the oil absorption and pore volume of the manufactured UV blocking powder according to the temperature of the condensation reaction were measured, and the results are shown in Table 1 below. Here, the silica aqueous solution was set to 10 wt%.

[0078] Sample temperature (℃) Oil absorption of powder after coating (n=5) (mL / g) Pore volume (cm 3 / g) Comparative Example 1600.520.1622 Embodiment 1800.490.1233 Embodiment 21000.320.0814 Embodiment 31100.290.0515 Embodiment 41200.260.0511

[0079] As shown in Table 1 above, the temperature of the condensation reaction was suitable at 80°C or higher, and more preferably, 100°C or higher.

[0080] Test 2: Comparison of the properties of UV-blocking powder after dry coating and wet coating [Example 3] and [Comparative Example 2]

[0081] A UV-blocking powder was manufactured by forming a silica coating layer using the same silicic acid aqueous solution through dry coating and wet coating, respectively. The dry coating used the UV-blocking powder manufactured in Example 3, and the wet coating used the method described in the applicant's prior application, Republic of Korea Patent Application No. 10-2020-0174433, to manufacture the UV-blocking powder (Comparative Example 2). The oil absorption was measured and is shown in Table 2 below.

[0082] Oil absorption of powder after sample coating (n=5) (mL / g) Example 30.29 Comparative example 20.45

[0083] As shown in Table 2 above, the UV-blocking powder manufactured using dry coating according to the present invention (Example 3) has a higher density of the coating layer than the UV-blocking powder manufactured using a wet process (Comparative Example 2), thereby preventing the chemical UV-blocking agent inside the powder from leaking out, and thus eliminating concerns about skin irritation due to organic UV-blocking agents, and confirming excellent stability.

[0084] Although the embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention.

Claims

1. S1) A step of loading an organic UV blocking agent that is in a solid state at room temperature into the pores of porous silica; S2) Step of preparing a silicate solution; and S3) A step of forming a silica coating layer by dry-coating a silicic acid aqueous solution on the porous silica surface in which an organic UV blocking agent is loaded in the pores; Method for manufacturing ultraviolet ray blocking powder including 2. In paragraph 1, A method for producing a UV blocking powder, characterized in that the silica content of the silica aqueous solution of the above step S2) is 3 to 30 wt%.

3. In paragraph 1, The dry coating of the above step S3) is a method for manufacturing an ultraviolet ray blocking powder, characterized in that a silica coating layer is formed by spraying a silica aqueous solution and depositing it on a porous silica surface containing an organic ultraviolet ray blocking agent, and then performing a condensation reaction of the silica.

4. In paragraph 3, A method for producing a UV blocking powder, characterized in that the above condensation reaction is carried out by stirring porous silica, on the surface of which an organic UV blocking agent is supported, with an aqueous solution of silicic acid at 100 to 1000 rpm at 80 to 120°C.

5. In paragraph 1, A method for manufacturing a UV-blocking powder further comprising a step of drying the UV-blocking powder having a silica coating layer formed with silicic acid on the surface after the above step S3).

6. In paragraph 1, A method for manufacturing a UV-blocking powder, further comprising a step of forming an organic coating layer or an inorganic coating layer on the outermost surface of a UV-blocking powder having a silica coating layer formed with silicic acid on the surface after the above step S3).

7. In UV blocking powder, Porous silica having pores; A chemical UV blocker having a solid state at room temperature, which is contained in the pores of the porous silica; and A silica coating layer formed by dry-coating silicic acid on the surface of porous silica in which the chemical UV blocking agent is contained in the pores; UV blocking powder containing .

8. In paragraph 7, The above ultraviolet ray blocking powder is characterized in that it is manufactured by the manufacturing method described in any one of claims 1 to 7.

9. In paragraph 7, A UV blocking powder characterized in that the silica coating layer (30) is 5 to 100 parts by weight based on 100 parts by weight of the total of porous silica (10) and UV blocking agent (20).

10. In paragraph 7, A UV blocking powder (100) characterized in that the absorption amount of the above UV blocking powder is 0.20 to 0.49 mL / g.

11. A cosmetic comprising a UV-blocking powder as described in any one of Articles 7 to 10.

Citation Information

Patent Citations

  • Cosmetic preparation, surface-hydrophobizedsilica-coated metal oxide particles, sol ofsilica-coated metal oxide, and processes for producingthese

    KR1020010101455A

  • Self-heating non-aqueous cosmetic composition

    KR1020130073154A

  • A anti-UV complexed powder coated with inorganic UV block agent, organic UV absorbent and anti-UV cosmetic composition using the same

    KR1020160031982A

  • Manufacturing device of packaging film

    KR102533758B1

  • Organic UV blocker-supported silica aerogel composite