Method for manufacturing high-purity iron-nickel alloy for fine metal mask, and iron-nickel alloy manufactured thereby
The multi-step process of vacuum induction melting, electron beam cold hearth melting, and vacuum arc remelting, followed by hot and cold rolling, effectively reduces non-metallic inclusions in iron-nickel alloys, addressing the cleanliness issue in fine metal masks for OLED displays and enhancing their suitability for high-resolution applications.
Patent Information
- Application Number
- PCT/KR2023/010852
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2023-07-26
- Publication Date
- 2024-10-31
AI Technical Summary
Current methods for producing fine metal masks for OLED displays fail to achieve sufficient cleanliness, leading to defects due to non-metallic inclusions, particularly Al-Mg-O-based inclusions larger than 2㎛, which impede processing precision and are not suitable for high-resolution displays.
A multi-step process involving vacuum induction melting, electron beam cold hearth melting, primary and secondary vacuum arc remelting, and hot and cold rolling to produce an iron-nickel alloy with reduced non-metallic inclusions, specifically targeting the removal of Al-based oxides and other impurities, resulting in an alloy with fewer than 1 inclusion per mm² larger than 2㎛.
The process significantly reduces non-metallic inclusions, enhancing the cleanliness and precision of fine metal masks, making them suitable for high-resolution OLED display manufacturing by minimizing defects and improving processing accuracy.
Smart Images

Figure KR2023010852_31102024_PF_FP_ABST
Abstract
Description
Method for producing a high-purity iron-nickel alloy for fine metal masks and iron-nickel alloy produced thereby
[0001] The present invention relates to a method for producing a high-purity iron-nickel alloy for a fine metal mask and an iron-nickel alloy produced thereby.
[0002] Fine Metal Masks (FMMs) are thin plates used to deposit organic light-emitting materials on the substrates of OLED (Organic Light Emitting Diodes) displays. Specifically, as shown in Fig. 1 (a) of the FMM thin plate, fine holes of 10 to 20 μm are first processed at the locations where RGB organic materials are to be deposited, and then, as shown in Figs. 1 (b) to (c), the OLED source is vaporized to precisely deposit the RGB organic materials in the micro-hole areas. The micro-through holes must be processed uniformly and precisely, but if the holes are processed with a material containing a large number of non-metallic inclusions, it can cause defects in the processing location and dimensions. In particular, in the case of high-definition displays, the number of holes processed per unit area increases, so a cleaner fine metal mask is required.
[0003] Recently, with the increasing demand for high-resolution displays, various research results and patents have been reported on novel wet etching methods and laser-based processing methods to improve the processing accuracy of FMM plates, enabling more and finer holes than previously required by conventional FMMs. However, research on the cleanliness of FMM plates, a factor affecting processability, remains insufficient. Cleanliness can be assessed by the number and size of non-metallic inclusions within the plate, and higher cleanliness can reduce the defect rate in OLED display manufacturing.
[0004] Korean Patent Application No. 10-2019-700910 discloses a method for removing segregated and coarse oxide-based non-metallic inclusions using a VIM-VAR-VAR process to reduce inclusions larger than 6.0㎛ that affect the wet etching method, and applying hot rolling and cold rolling to the steel ingot obtained through this process to break up and crush the remaining coarse oxide-based non-metallic inclusions.
[0005] However, the patent document reports that the produced FMM sheet metal still contains 2 to 6 Al-Mg-O non-metallic inclusions of 6 to 10 μm in size per gram, and the cleanliness (amount of non-metallic inclusions per gram) of 2 to 6 non-metallic inclusions of 6 to 10 μm in size per gram is not suitable for producing high-resolution displays required by the current display industry.
[0006] This study describes a method for manufacturing ultra-clean FMM thin plates with reduced non-metallic inclusions (including Al-based oxides) with a size of 2 ㎛ or more that impair the processing precision of FMM thin plates.
[0007] The purpose of the present invention is to provide a method for manufacturing an ultra-clean FMM thin plate.
[0008] The present invention is a method for manufacturing a metal sheet having a non-metallic inclusion (including Al oxide) of 2 μm or more that affects etching processability. 2 The purpose of the present invention is to provide a method for manufacturing an Invar alloy sheet having less than 1 unit weight.
[0009] The purposes of the present disclosure are not limited to those mentioned above, and other purposes and advantages of the present disclosure not mentioned above can be understood through the following description and will be more clearly understood through the embodiments of the present disclosure. Furthermore, it will be readily apparent that the purposes and advantages of the present disclosure can be realized by the means and combinations thereof set forth in the claims.
[0010] The present invention provides a method for producing an iron-nickel alloy, comprising the steps of: preparing iron and nickel raw materials; vacuum induction melting the iron and nickel raw materials to provide a vacuum induction melted alloy; electron beam cold hearth melting the vacuum induction melted alloy to provide an electron beam melted alloy; first vacuum arc remelting the electron beam melted alloy; second vacuum arc remelting the first vacuum arc remelted alloy; and performing hot rolling and cold rolling on the second vacuum arc remelted alloy to produce an iron-nickel alloy in the form of a thin plate having a thickness of 0.5 mm or less.
[0011] The above vacuum induction melting is carried out under normal melting conditions, and the components of the vacuum induction melted alloy are, in wt% according to ASTM standards, Ni: 35 to 38%, C: 0.10% or less, Mn: 0.06% or less, P: 0.025% or less, S: 0.025% or less, Si: 0.35% or less, Cr: 0.50% or less, Mo: 0.50% or less, Co: 1.0% or less, and the remainder may be iron and impurities.
[0012] The above electron beam cold melting can be performed under conditions of a vacuum of 0.001 torr or less and a melting speed of 6 to 10 kg / min.
[0013] The above primary vacuum arc remelting can be performed under conditions of a current of 7 kA to 12 kA, a voltage of 20 to 30 V, and a vacuum of 0.001 torr or less.
[0014] In the above-mentioned secondary vacuum arc remelting, the current and vacuum level may be carried out under the same conditions as in the above-mentioned primary vacuum arc remelting, and the voltage may be carried out under relatively lower voltage conditions compared to the above-mentioned primary vacuum arc remelting.
[0015] The present invention also provides an alloy having an inclusion size exceeding 2㎛, which is 1 / mm 2 An iron-nickel alloy having a value less than 0.01% can be provided.
[0016] According to the present invention, the inclusion of 2㎛ or more in the alloy is 1 / mm 2 An iron-nickel alloy having a value less than 0.01% can be provided.
[0017] Figure 1 shows a description of a fine metal mask.
[0018] Fig. 2 shows a flow chart showing a method for manufacturing an iron-nickel alloy according to one embodiment of the present invention.
[0019] Figure 3 shows photographs of inclusions in alloys of examples and comparative examples of the present invention.
[0020] The present invention is described in more detail below through examples and experimental examples. However, these examples and experimental examples are intended to exemplify the present invention and the scope of the present invention is not limited to these examples and experimental examples.
[0021] Figure 2 is a flow chart showing a method for manufacturing an iron-nickel alloy according to one embodiment of the present invention.
[0022] First, referring to FIG. 2, a method for manufacturing an iron-nickel alloy according to one embodiment of the present invention includes a step of preparing iron and nickel raw materials for melting the alloy.
[0023] The above iron-nickel alloy is an alloy containing 64 wt% iron and 36 wt% nickel, and is preferably an iron-nickel alloy having a composition as shown in Table 1 below corresponding to ASTM F1684. The form of the iron-nickel alloy is not particularly limited, but is, for example, an ingot.
[0024]
[0025] A method for manufacturing an iron-nickel alloy according to one embodiment of the present invention includes a step of vacuum induction melting iron and nickel raw materials to provide a vacuum induction melted alloy.
[0026] Vacuum induction melting can be performed in a conventional manner, as is well known to those skilled in the art, to produce a melt with sufficient structural integrity to permit stable remelting. The vacuum induction melting is typically performed under a vacuum, or alternatively, under a partially inert gas atmosphere. This step focuses on controlling component content through real-time component analysis and controlling impurities through vacuum control. The vacuum is utilized to prevent and remove oxygen, a cause of inclusion formation, and the addition of a deoxidizer further controls the oxygen content.
[0027] A method for producing an iron-nickel alloy according to one embodiment of the present invention comprises the step of subjecting a vacuum induction melted alloy to electron beam cold hearth melting to provide an electron beam melted alloy.
[0028] The above electron beam cold hearth melting is carried out under the conditions of vacuum degree of 0.0001 torr or less and melting speed of 6~10kg / min. The main purpose of electron beam cold hearth melting in this step is to reduce the oxygen content in the alloy. When the above vacuum induction melting step is carried out, an electron beam accelerated in high vacuum is irradiated on the surface of the material, and melting proceeds due to the heat generated at this time. In particular, the vacuum degree in this step is 0.0001 This process is performed under a high vacuum of less than 10 torr, which is higher than the other two processes. This high vacuum allows for the removal of oxygen content within inclusions through evaporation and the removal of dissolved oxygen through the removal of gases within the alloy.
[0029] A method for manufacturing an iron-nickel alloy according to one embodiment of the present invention includes a step of first vacuum arc remelting an electron beam melted alloy.
[0030] The above first vacuum arc remelting step is carried out under the conditions of a current of 7 kA to 12 kA, a voltage of 20 to 30 V, and a vacuum of 0.001 torr or less. The main purpose of this step is to increase the heat input by increasing the power and to volatilize the Mg-based non-metallic inclusions that were not removed during the electron beam cold hearth melting.
[0031] A method for manufacturing an iron-nickel alloy according to one embodiment of the present invention includes a step of performing a second vacuum arc remelting of a first vacuum arc remelted alloy.
[0032] The above-mentioned second vacuum arc remelting step is characterized by applying the same current and vacuum degree as the first vacuum arc remelting step, and lowering the voltage compared to the first vacuum arc remelting. High-melting-point inclusions (such as Al-based oxides) that are difficult to volatilize in the first vacuum arc remelting are floated in this step and discharged to the surface of the ingot, thereby achieving the effect of reducing the inclusions inside the ingot.
[0033] A method for producing an iron-nickel alloy according to one embodiment of the present invention includes a step of performing hot rolling and cold rolling on a secondary vacuum arc remelted alloy to produce an iron-nickel alloy in the form of a thin plate having a thickness of 0.5 mm or less.
[0034] By segmenting and crushing the non-metallic inclusions in the steel ingot during the rolling process, it is possible to further refine the non-metallic inclusions. If necessary, a homogenizing heat treatment may be performed at approximately 900 to 1300°C before cold rolling, and during the cold rolling process, annealing at 800 to 1050°C may be performed one or more times to reduce the hardness of the cold-rolled material. The annealing time at this time may be selected from the range of 30 to 150 seconds. In the cold rolling process, a polishing process to remove surface scale, an edge cutting process to remove the off-gauge portion (the portion with a thick sheet thickness) at the end of the material, and an edge cutting process to remove the edge wave portion generated during the rolling process may be performed. During the heat treatment process, conventional furnaces such as vertical furnaces and horizontal furnaces can be used. However, to prevent bending during the process and to further increase the steepness of the material, it is preferable to use a vertical furnace that is less likely to sag due to its own weight. In addition, to suppress shape defects that occur in the iron-nickel alloy after the finish rolling, shape correction using deformation relief annealing or a tension leveler can be performed.
[0035] An iron-nickel alloy manufactured by a method for manufacturing an iron-nickel alloy according to one embodiment of the present invention has excellent cleanliness. The standard for cleanliness is related to the size or number of inclusions in the manufactured iron-nickel alloy. The inclusions are oxides generated or mixed during the process. An iron-nickel alloy manufactured by one embodiment of the present invention has 1 inclusion / mm having a size exceeding 2 μm in the alloy. 2 It is less than.
[0036]
[0037] Hereinafter, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the following examples.
[0038] Examples 1 and 2
[0039] Iron and nickel raw materials were prepared for alloy melting. The iron and nickel raw materials were formed into ingots by vacuum induction melting under standard conditions. The ingots met the compositional requirements of Invar36 alloy as specified in ASTM F1684.
[0040] The above vacuum-induced melted alloy was subjected to electron beam cold hearth melting under conditions of a high vacuum of 0.0001 torr or less at a melting rate of 8 kg / min to produce an electron beam melted alloy.
[0041] The above electron beam melted alloy was subjected to primary vacuum arc remelting under conditions of a current of 9.5 kA, a voltage of 25 V, and a vacuum of 0.001 torr or less.
[0042] Thereafter, the secondary vacuum arc remelting was performed under the same current and vacuum conditions as the primary vacuum arc remelting, with a difference in voltage conditions (Example 1: 23 V, Example 2: 21 V). The produced ingot was then hot rolled and cold rolled to produce an iron-nickel alloy in the form of a thin plate of 0.05 mm or less.
[0043] Comparative Example 1
[0044] The same iron and nickel raw materials as in Example 1 were prepared, and vacuum induction melting, electron beam cold hearth melting, and primary vacuum arc remelting were performed. Instead of performing secondary vacuum arc remelting, an iron-nickel alloy was manufactured through a rolling process. The conditions for each step were the same as in Examples 1 and 2.
[0045] Comparative Example 2-5
[0046] Iron and nickel raw materials were prepared under the same process conditions as in Example 1-2, and vacuum induction melting, electron beam cold hearth melting, and first vacuum arc remelting were performed. There was a difference in voltage conditions in the second vacuum arc remelting stage (Comparative Example 2: 19 V, Comparative Example 3: 25 V, Comparative Example 4: 27 V, Comparative Example 5: 29 V). The subsequent processes were the same as in Example 1-2.
[0047] Experimental example
[0048] The number of inclusions present in the iron-nickel alloys manufactured in the above examples and comparative examples was evaluated, and the results are shown in Table 2 below, and photographs of the inclusions in the alloys are shown in Fig. 3. The evaluation method was to photograph 20 random points on the alloy using an SEM and measure the number of inclusions photographed per unit area. The photograph shown in Fig. 3 is one of the photographs taken by randomly selecting 20 points on the alloy, and the number shown in Table 2 below is the average value of the 20 points.
[0049]
[0050] As shown in Table 2, in Comparative Example 1, where VAR was performed only once, the largest number of inclusions was observed, 1.25. On the other hand, it can be confirmed that there is an effect of reducing inclusions under the conditions of the remaining examples and comparative examples where VAR was performed twice. In particular, in Examples 1 and 2, where lower voltage conditions than those used in the first VAR were applied, inclusions larger than 2 μm were observed at 0.95 / mm2, respectively. 2 , 0.91 / mm 2 It can be confirmed that it is only a dog. Therefore, it can be seen that the iron-nickel alloy of the present invention has excellent purity. On the other hand, it was confirmed that Comparative Example 2 is not suitable for application to the production process because the ingot formation does not occur smoothly due to the voltage conditions that are too low in the second VAR process.
Claims
1. Step of preparing iron and nickel raw materials; A step of vacuum induction melting iron and nickel raw materials to provide a vacuum induction melted alloy; A step of providing an electron beam melted alloy by subjecting a vacuum induction melted alloy to electron beam cold hearth melting; A step of first vacuum arc remelting of an electron beam melted alloy; A step of remelting the first vacuum arc remelted alloy by a second vacuum arc; and A method for producing an iron-nickel alloy, comprising the step of producing an iron-nickel alloy in the form of a thin plate of 0.5 mm or less by performing hot rolling and cold rolling on a secondary vacuum arc remelted alloy.
2. In paragraph 1, A method for producing an iron-nickel alloy, wherein the above vacuum induction melting is performed in a normal vacuum, and the components of the vacuum induction melted alloy are, in wt% according to ASTM standards, Ni: 35 to 38%, C: 0.10% or less, Mn: 0.06% or less, P: 0.025% or less, S: 0.025% or less, Si: 0.35% or less, Cr: 0.50% or less, Mo: 0.50% or less, Co: 1.0% or less, and the remainder is iron and impurities.
3. In paragraph 1, A method for manufacturing an iron-nickel alloy, wherein the above electron beam cold hearth melting is performed under conditions of a vacuum of 0.0001 torr or less and a melting speed of 6 to 10 kg / min.
4. In paragraph 1, A method for manufacturing an iron-nickel alloy, wherein the above primary vacuum arc remelting is performed at a current of 7 kA to 12 kA, a voltage of 20 V to 30 V, and a vacuum of 0.001 torr or less.
5. In paragraph 1, A method for manufacturing an iron-nickel alloy, wherein the current and vacuum level in the second vacuum arc remelting are carried out under the same conditions as in the first vacuum arc remelting, and the voltage is carried out under relatively lower voltage conditions compared to the first vacuum arc remelting.
6. An iron-nickel alloy manufactured by the manufacturing method of paragraph 1, The number of inclusions exceeding 2㎛ in the alloy is 1 / mm 2 An iron-nickel alloy less than 100%.
Citation Information
Patent Citations
Metal mask material and method for manufacturing same
EP3514249B1
HIGH STRENGTH FREE-CUTTING Fe-Ni BASED ALLOY AND ITS PRODUCTION METHOD
JP2007197793A
Method for producing ultrahigh purity alloy ingot
JP2011021228A
METHOD FOR PRODUCTION OF Fe-Ni-BASED THIN ALLOY SHEET
JP2016135505A
Alloy melting and refining method
KR1020180019546A