Method for producing metal-lithium fluoride composite for positive electrode additive for negative electrode pre-doping, and lithium-ion capacitor including metal-lithium fluoride composite
The method of forming a metal-lithium fluoride complex by mixing lithium metal oxide with ammonium fluoride and heat treating it addresses the cost and safety issues of metallic lithium in lithium-ion capacitors, achieving high capacity and cost-effectiveness as a positive electrode additive for lithium-ion capacitors.
Patent Information
- Application Number
- PCT/KR2023/012940
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2023-08-31
- Publication Date
- 2024-10-31
AI Technical Summary
Existing lithium-ion capacitors face challenges with high manufacturing costs and safety issues due to the use of metallic lithium for pre-doping, which also complicates control over pre-doping levels, and lithium transition metal oxides are expensive and difficult to process.
A method involving the mixing of lithium metal oxide with ammonium fluoride and subsequent heat treatment in a reducing or inert gas atmosphere to form a metal-lithium fluoride complex, which is used as a positive electrode additive for negative electrode pre-doping in lithium ion capacitors, reducing costs and simplifying the manufacturing process.
The metal-lithium fluoride complex exhibits high capacity (400 mAh/g or more at 4.5 V or less) and is suitable as a positive electrode additive, offering improved scalability, cost-effectiveness, and easier control of pre-doping levels compared to traditional methods.
Smart Images

Figure KR2023012940_31102024_PF_FP_ABST
Abstract
Description
Method for manufacturing a metal-lithium fluoride complex for cathode additives for cathode pre-doping and a lithium-ion capacitor comprising the same
[0001] The present invention relates to a method for producing a metal-lithium fluoride complex for a cathode additive for anode pre-doping and a lithium ion capacitor including the same, and more particularly, to a method for producing a metal-lithium fluoride complex for a cathode additive for anode pre-doping and a lithium ion capacitor including the same, which can produce a metal-lithium fluoride complex for a cathode additive for anode pre-doping at a low cost by producing the metal-lithium fluoride complex through a simple method of mixing lithium metal oxide and ammonium fluoride and then heat-treating the mixture.
[0002]
[0003] A lithium-ion capacitor is a hybrid type of energy storage device consisting of a positive electrode based on the physical adsorption / desorption reaction of a supercapacitor and a negative electrode based on the chemical ion insertion and desorption reaction of a lithium-ion battery.
[0004] These lithium-ion capacitors exhibit superior output and life characteristics compared to conventional lithium-ion batteries, while also exhibiting higher energy density compared to conventional supercapacitors.
[0005] To achieve high energy density of these lithium-ion capacitors, pre-doping of the negative electrode is required.
[0006]
[0007] Figure 1 is a cross-sectional view showing a lithium ion capacitor using a pre-doping method in which lithium metal is added to the negative electrode.
[0008] As illustrated in FIG. 1, a conventional pre-doped lithium ion capacitor (1) includes a negative electrode (10) having a negative current collector (12) and a negative active material layer (14) formed on both sides of the negative current collector (12), a positive electrode (20) laminated on the negative electrode (10) and having a positive current collector (22) and a positive active material layer (24) formed on both sides of the positive current collector (22), and a separator (30) disposed between the negative electrode (10) and the positive electrode (20).
[0009] The existing pre-doping type lithium ion capacitor (1) is mainly used by additionally using metallic lithium (50) in the negative electrode (10).
[0010] However, the use of metallic lithium (50) raises safety issues and there is the problem that it is difficult to control the level of pre-doping. In addition, in order to additionally use metallic lithium (50), a porous current collector must be used instead of a general current collector, but the use of such a porous current collector has the disadvantage of significantly increasing the manufacturing cost.
[0011] A related prior art document is Republic of Korea Patent Publication No. 10-2019-0101778 (published on September 2, 2019), which describes a cost-saving lithium ion capacitor electrode material and manufacturing method.
[0012]
[0013] The purpose of the present invention is to provide a method for producing a metal-lithium fluoride complex for a cathode additive for anode pre-doping, which can produce a metal-lithium fluoride complex for a cathode additive for anode pre-doping at a low cost by producing a metal-lithium fluoride complex through a simple method of mixing lithium metal oxide and ammonium fluoride and then heat-treating the mixture, and a lithium ion capacitor including the same.
[0014]
[0015] In order to achieve the above object, a method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to an embodiment of the present invention comprises the steps of (a) preparing a lithium metal oxide; (b) mixing the lithium metal oxide with ammonium fluoride; and (c) heat-treating the mixed mixture in a reducing gas atmosphere or an inert gas atmosphere to form a metal-lithium fluoride complex.
[0016] In the above step (a), the lithium metal oxide is Li x NiO y , Li x FeO y , Li x CoO y , Li x CuO y , Li x ZnO y , Li x MgO y and Li x CaO y Include any one of the selected ones (where 0.1 ≤ x ≤ 6 and 1 ≤ y ≤ 6).
[0017] In the above step (b), the ammonium fluoride is mixed in an amount of 10 to 150 parts by weight per 100 parts by weight of the lithium metal oxide.
[0018] In the above step (b), only the ammonium fluoride is mixed alone, or a carbon precursor is further mixed together with the ammonium fluoride.
[0019] The above carbon precursor is mixed in an amount of 10 to 150 parts by weight per 100 parts by weight of the above lithium metal oxide.
[0020] The above carbon precursor comprises at least one selected from sucrose, cellulose, xylose, and galactose.
[0021] In the above step (c), when only the ammonium fluoride is mixed alone, the heat treatment is performed at 300 to 750°C for 30 to 120 minutes.
[0022] In the above step (c), it is preferable that the reducing gas atmosphere is a gas atmosphere of any one of hydrogen, hydrogen-nitrogen mixed gas, and hydrogen-argon mixed gas, and the inert gas atmosphere is a gas atmosphere containing at least one of nitrogen and argon.
[0023] In the above step (c), when a carbon precursor is further mixed with the ammonium fluoride, the heat treatment is performed at 500 to 750°C for 30 to 120 minutes.
[0024] In the step (c), the metal-lithium fluoride complex includes any one of nickel (Ni) / lithium fluoride, iron (Fe) / lithium fluoride, cobalt (Co) / lithium fluoride, copper (Cu) / lithium fluoride, zinc (Zn) / lithium fluoride, magnesium (Mg) / lithium fluoride, and calcium (Ca) / lithium fluoride.
[0025]
[0026] A method for producing a metal-lithium fluoride complex for a cathode additive for anode pre-doping according to a modified example of the present invention for achieving the above object is characterized by comprising the steps of (a) mixing a metal hydroxide and lithium hydroxide; (b) first heat-treating the mixed mixture in an air or oxygen atmosphere to form a lithium metal oxide; (c) mixing the formed lithium metal oxide with ammonium fluoride; and (d) second heat-treating the mixed mixture in a reducing gas atmosphere or an inert gas atmosphere to form a metal-lithium fluoride complex.
[0027] In the above step (b), the first heat treatment is performed at 500 to 900°C for 10 to 180 minutes.
[0028] In the above step (c), only the ammonium fluoride is mixed alone, or a carbon precursor is further mixed together with the ammonium fluoride.
[0029] In the above step (d), when only the ammonium fluoride is mixed alone, the secondary heat treatment is performed at 300 to 750°C for 30 to 120 minutes.
[0030] In the above step (d), it is preferable that the reducing gas atmosphere is a gas atmosphere of any one of hydrogen, hydrogen-nitrogen mixed gas, and hydrogen-argon mixed gas, and the inert gas atmosphere is a gas atmosphere containing at least one of nitrogen and argon.
[0031] In the above step (d), when a carbon precursor is further mixed with the ammonium fluoride, the secondary heat treatment is performed at 500 to 750°C for 30 to 120 minutes.
[0032] In the step (d), the metal-lithium fluoride complex includes any one of nickel (Ni) / lithium fluoride, iron (Fe) / lithium fluoride, cobalt (Co) / lithium fluoride, copper (Cu) / lithium fluoride, zinc (Zn) / lithium fluoride, magnesium (Mg) / lithium fluoride, and calcium (Ca) / lithium fluoride.
[0033]
[0034] According to an embodiment of the present invention for achieving the above object, a lithium ion capacitor including a metal-lithium fluoride complex for a cathode additive for cathode pre-doping comprises: a cathode having a cathode current collector and a cathode active material layer formed on both sides of the cathode current collector; a cathode laminated on the cathode and having a cathode current collector and a cathode active material layer formed on both sides of the cathode current collector; and a separator disposed between the cathode and the cathode, wherein the cathode active material layer includes a cathode active material, a cathode additive, a conductive material, and a binder, and the cathode additive is characterized in that a metal-lithium fluoride complex manufactured by the above method is used.
[0035] The above lithium ion capacitor has a metal-lithium fluoride complex added as a cathode additive, which exhibits a capacity of 400 mAh / g or more at a charging voltage of 4.5 V or less.
[0036] The above metal-lithium fluoride complex comprises any one of nickel (Ni) / lithium fluoride, iron (Fe) / lithium fluoride, cobalt (Co) / lithium fluoride, copper (Cu) / lithium fluoride, zinc (Zn) / lithium fluoride, magnesium (Mg) / lithium fluoride, and calcium (Ca) / lithium fluoride.
[0037]
[0038] A method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to the present invention and a lithium ion capacitor comprising the same use a material in which a lithium source is mixed with a lithium metal oxide or metal compound as a raw material, and manufacture a metal-lithium fluoride complex through a simple method of mixing ammonium fluoride and then heat-treating, and utilize the metal-lithium fluoride complex as a cathode additive for a lithium ion capacitor.
[0039] In this way, the method for manufacturing a metal-lithium fluoride complex for a cathode additive for anode pre-doping according to the present invention and a lithium ion capacitor including the same is a method for mixing ammonium fluoride with lithium metal oxide and then heat-treating, so the manufacturing process is simple, and thus the metal-lithium fluoride complex for a cathode additive for cathode pre-doping can be manufactured at a lower cost than lithium transition metal oxide, which is a general cathode additive.
[0040] In addition, the method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to the present invention and the lithium ion capacitor including the same manufacture a metal-lithium fluoride complex exhibiting a high capacity of 400 mAh / g or more at a charging voltage of 4.5 V or less, and when such a metal-lithium fluoride complex is utilized as a cathode additive, it can exhibit suitable properties as a cathode additive because the irreversibility during discharge after charging is very large.
[0041]
[0042] Figure 1 is a cross-sectional view showing a lithium-ion capacitor using a pre-doping method of adding lithium metal to the negative electrode.
[0043] Figure 2 is a cross-sectional view showing a lithium-ion capacitor using a pre-doping method that introduces a cathode additive to the cathode.
[0044] FIG. 3 is a cross-sectional view showing a lithium ion capacitor including a metal-lithium fluoride complex as a cathode additive for cathode pre-doping according to an embodiment of the present invention.
[0045] Figure 4 is a process flow diagram showing a method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to an embodiment of the present invention.
[0046] Figure 5 is a process flow diagram showing a method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to a modified example of the present invention.
[0047] Figure 6 is a graph showing the results of XRD analysis of a nickel-lithium fluoride composite manufactured according to Example 1.
[0048] Figure 7 is a graph showing the results of a half-cell test conducted after manufacturing an electrode using a nickel-lithium fluoride composite manufactured according to Example 1.
[0049] Figure 8 is a graph showing the results of a half-cell test conducted after manufacturing an electrode using a nickel-lithium fluoride composite manufactured according to Example 3.
[0050] Figure 9 is a graph showing the results of a half-cell test conducted after manufacturing an electrode using a nickel-lithium fluoride composite manufactured according to Comparative Example 1.
[0051] Figure 10 is a graph showing the results of a half-cell test conducted after manufacturing an electrode using a nickel-lithium fluoride composite manufactured according to Comparative Example 2.
[0052]
[0053] The advantages and features of the present invention, and the methods for achieving them, will become clearer with reference to the embodiments described in detail below together with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, but may be implemented in various different forms. These embodiments are provided only to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention, and the present invention is defined only by the scope of the claims. Like reference numerals designate like elements throughout the specification.
[0054] Hereinafter, with reference to the attached drawings, a method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to a preferred embodiment of the present invention and a lithium ion capacitor including the same will be described in detail.
[0055]
[0056] Figure 2 is a cross-sectional view showing a lithium-ion capacitor using a pre-doping method that introduces a cathode additive to the cathode.
[0057] As illustrated in FIG. 2, a lithium ion capacitor (100) of a pre-doping method for introducing a positive electrode additive to a positive electrode includes a negative electrode (110) having a negative electrode current collector (112) and a negative electrode active material layer (114) formed on both sides of the negative electrode current collector (112), a positive electrode (120) laminated on the negative electrode (110) and having a positive electrode current collector (122) and a positive electrode active material layer (124) formed on both sides of the positive electrode current collector (122), and a separator (130) disposed between the negative electrode (110) and the positive electrode (120).
[0058] This lithium ion capacitor (100) introduces a lithium metal compound as a cathode additive (160) into a carbon-based material used as a cathode (120), and then electrochemically pre-dopes the cathode (110). This method has various advantages over the existing pre-doping method, such as reduced process costs, increased convenience, easy process scalability, and easy control of the pre-doping level.
[0059] Lithium metal compounds used as these positive electrode additives (160) include, as shown in Table 1, representative lithium transition metal oxides such as Li2MoO3, Li5FeO4, Li2CuO2, and Li2Cu. 0.9 Zn 0.1 O2 and Li6CoO4 have been reported.
[0060]
[0061] [Table 1]
[0062]
[0063] By mixing the cathode additive shown in Table 1 with a carbon material to provide a lithium source to the cathode (120) on its own, the manufacturing process for cathode pre-doping can be simplified, and side reactions due to residual lithium after lithium doping can be suppressed, which has the advantage of being possible.
[0064] However, the lithium transition metal oxides shown in Table 1 are materials having a composition that is not used in secondary batteries such as general lithium ion batteries, and have the disadvantages of high raw material prices or difficult and high cost process conditions for manufacturing materials having the above composition.
[0065]
[0066] To solve this problem, a lithium ion capacitor including a metal-lithium fluoride complex as a cathode additive for cathode pre-doping according to an embodiment of the present invention was manufactured by a simple method of mixing lithium metal oxide and ammonium fluoride and then heat-treating the metal-lithium fluoride complex, and the metal-lithium fluoride complex was utilized as a cathode additive for a lithium ion capacitor.
[0067] As a result, a lithium ion capacitor including a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to an embodiment of the present invention can manufacture a metal-lithium fluoride complex for a cathode additive for cathode pre-doping at a lower cost than a lithium transition metal oxide, which is a general cathode additive.
[0068]
[0069] FIG. 3 is a cross-sectional view showing a lithium ion capacitor including a metal-lithium fluoride complex as a positive electrode additive for negative electrode pre-doping according to an embodiment of the present invention, and will be described in more detail with reference to this.
[0070] Referring to FIG. 3, a lithium ion capacitor (200) including a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to an embodiment of the present invention includes a cathode (210) having a cathode current collector (212) and a cathode active material layer (214) formed on both sides of the cathode current collector (212), a cathode (220) laminated on the cathode (210) and having a cathode current collector (222) and a cathode active material layer (224) formed on both sides of the cathode current collector (222), and a separator (230) disposed between the cathode (210) and the cathode (220).
[0071] The negative electrode active material layer (214) may include a negative electrode active material, a conductive material, and a binder, and the positive electrode active material layer (224) may include a positive electrode active material, a positive electrode additive, a conductive material, and a binder.
[0072] The negative active material may be a carbon-based material capable of inserting and de-inserting lithium ions, and is not particularly limited.
[0073] Any cathode active material known in the art may be used without limitation. Examples of such cathode active materials include, but are not limited to, carbon-based materials such as activated carbon.
[0074] A cathode additive (260) is added for cathode pre-doping. A metal-lithium fluoride complex is used as this cathode additive (260). This metal-lithium complex (260) includes any one of nickel (Ni) / lithium fluoride, iron (Fe) / lithium fluoride, cobalt (Co) / lithium fluoride, copper (Cu) / lithium fluoride, zinc (Zn) / lithium fluoride, magnesium (Mg) / lithium fluoride, and calcium (Ca) / lithium fluoride.
[0075] The metal-lithium fluoride complex (260), which is a cathode additive, may be added in an amount of less than 20 wt% of the total weight of the cathode active material layer (224), but is not limited thereto.
[0076] Each of the conductive materials of the negative and positive active material layers (214, 224) is not particularly limited as long as it is a conductive material commonly used in the relevant technical field, and may include at least one selected from graphite, carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, metal powder, and metal oxide.
[0077] Each of the binders of the negative and positive active material layers (214, 224) is not particularly limited as long as it is commonly used in the relevant technical field, and may include, for example, at least one selected from polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene butylene rubber, and fluororubber.
[0078] Here, the negative electrode current collector (212) and the positive electrode current collector (222) perform a support function that supports the negative electrode active material layer (214) and the positive electrode active material layer (224), respectively, and can be connected to an external electrode to provide a path for current movement. The negative electrode current collector (212) and the positive electrode current collector (222) can be in any one form selected from a film, a porous body, a foam, a mesh shape, etc., and the material thereof can be a conductive material such as copper, stainless steel, or aluminum, but is not limited thereto.
[0079] The separator (230) may include pores through which lithium ions can pass, and may be made of a polymer material such as a polypropylene film, but is not limited thereto.
[0080]
[0081] In particular, a lithium ion capacitor (200) including a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to an embodiment of the present invention was manufactured by simply mixing lithium metal oxide and ammonium fluoride (NH4F) and then heat-treating the metal-lithium fluoride complex (260), and utilizing this as a cathode additive.
[0082] In addition, a lithium ion capacitor (200) including a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to an embodiment of the present invention uses a material in which lithium hydroxide, which is a lithium source, is mixed with lithium metal oxide or metal hydroxide as a raw material, and a simple process method of mixing this with ammonium fluoride and performing heat treatment allows for manufacturing a metal-lithium fluoride complex (260) for a cathode additive at low cost.
[0083] As a result, when the metal-lithium fluoride composite (260) of the present invention was applied as a positive electrode additive of a lithium ion capacitor (200), it had a voltage of 4.5 V (vs. Li / Li + ) exhibits a high capacity of more than 400 mAh / g at a charging voltage below 100 mAh / g, which can provide a large amount of lithium for negative electrode pre-doping.
[0084] This metal-lithium fluoride complex (260) provides lithium to the negative electrode (210) through a conversion reaction as shown in Scheme 1 below during the charging process.
[0085]
[0086] Reaction Scheme 1: M + xLiF → MF x + xLi +
[0087] For example, Ni / LiF nanocomposites undergo Ni + 2LiF → NiF2+ 2Li during the charging process. + Lithium is supplied to the cathode (210) through a reaction.
[0088] At this time, since the mass of the material constituting the metal-lithium fluoride complex is relatively light, a large amount of lithium can be provided per mass of the metal-lithium fluoride complex.
[0089] The cathode additive, a metal-lithium fluoride complex, was used to produce a 4.5 V (vs. Li / Li) +) When the capacity is expressed at a high voltage of 4.5 V or higher, side reactions may occur excessively on the surface of the anode, but the metal-lithium fluoride composite of the present invention exhibits a capacity of 4.5 V (vs. Li / Li + ) and develops capacity at charging voltages below.
[0090] That is, after the first charge, the voltage is 2.5 to 2.6 V (vs. Li / Li + ) when discharged to a lower level, the amount of lithium ions re-acquired by the metal-lithium fluoride complex from the cathode is very small. Accordingly, it has suitable conditions for application as a cathode additive for lithium-ion capacitors.
[0091] Thus, an ideal cathode additive for cathode pre-doping should be able to provide a large amount of lithium to the cathode during the first charging stage, and it is advantageous to not re-accept lithium ions during the subsequent discharging stage.
[0092]
[0093] A lithium ion capacitor including a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to the above-described embodiment of the present invention can manufacture a metal-lithium fluoride complex through a simple method of mixing lithium metal oxide and ammonium fluoride and then heat-treating it, and utilize it as a cathode additive, thereby manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping at a lower cost than a lithium transition metal oxide, which is a general cathode additive.
[0094] In addition, a lithium ion capacitor including a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to an embodiment of the present invention produces a metal-lithium fluoride complex exhibiting a high capacity of 400 mAh / g or more at a charging voltage of 4.5 V or less, and when such a metal-lithium fluoride complex is used as a cathode additive, it can exhibit suitable characteristics as a cathode additive because the irreversibility during discharge after charging is very large.
[0095]
[0096] Hereinafter, a method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to an embodiment of the present invention will be described with reference to the attached drawings.
[0097] Figure 4 is a process flow diagram showing a method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to an embodiment of the present invention.
[0098] As illustrated in FIG. 4, a method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to an embodiment of the present invention includes a lithium metal oxide preparation step (S210), a lithium metal oxide and ammonium fluoride mixing step (S220), and a heat treatment step (S230).
[0099]
[0100] Preparation of lithium metal oxide
[0101] In the lithium metal oxide preparation step (S210), lithium metal oxide is prepared.
[0102] These lithium metal oxides include Li x NiO y , Li x FeO y , Li x CoO y , Li x CuO y , Li x ZnO y , Li x MgO y and Lix CaO y It includes one selected from among. Here, it is preferable that 0.1 ≤ x ≤ 6 and 1 ≤ y ≤ 6. At this time, the lithium metal oxide may be used in a powder state, but is not limited thereto.
[0103]
[0104] Lithium metal oxide and ammonium fluoride mixture
[0105] In the lithium metal oxide and ammonium fluoride mixing step (S220), lithium metal oxide is mixed with ammonium fluoride. Thus, in this step (S220), only ammonium fluoride can be mixed with lithium metal oxide.
[0106] Here, it is preferable to mix ammonium fluoride in an amount of 10 to 150 parts by weight per 100 parts by weight of lithium metal oxide, a more preferable range may be 30 to 100 parts by weight, and a most preferable range may be 50 to 75 parts by weight.
[0107] If the amount of ammonium fluoride added is less than 10 parts by weight per 100 parts by weight of lithium metal oxide, it may be difficult to sufficiently form lithium fluoride. Conversely, if the amount of ammonium fluoride added exceeds 150 parts by weight per 100 parts by weight of lithium metal oxide, there is a problem that the reaction proceeds excessively, resulting in a decrease in capacity.
[0108]
[0109] heat treatment
[0110] In the heat treatment step (S230), the mixed mixture is heat treated in a reducing gas atmosphere or an inert gas atmosphere to form a metal-lithium fluoride complex.
[0111] It is preferable that the reducing gas atmosphere is a gas atmosphere of any one of hydrogen, hydrogen-nitrogen mixed gas, and hydrogen-argon mixed gas, and the inert gas atmosphere is a gas atmosphere containing at least one of nitrogen and argon.
[0112] At this stage, when only ammonium fluoride is mixed alone, the heat treatment is preferably performed at 300 to 750°C for 30 to 120 minutes, and more preferably at 400 to 600°C for 50 to 100 minutes.
[0113] When the heat treatment temperature is less than 300℃ or the heat treatment time is less than 30 minutes, the metal ions (M) present in the lithium metal oxide x+ ) is a metal (M 0 ) may not be completely reduced. Conversely, if the heat treatment temperature exceeds 750℃ or the heat treatment time exceeds 120 minutes, the metal and lithium fluoride constituting the metal-lithium fluoride complex grow excessively, which lowers the efficiency of the electrochemical reaction when applied to a lithium-ion capacitor.
[0114]
[0115] Meanwhile, in the aforementioned lithium metal oxide and ammonium fluoride mixing step (S220), a carbon precursor may be further mixed with ammonium fluoride into the lithium metal oxide.
[0116] Here, the carbon precursor is preferably mixed in an amount of 10 to 150 parts by weight per 100 parts by weight of lithium metal oxide, and a more preferable range is 30 to 100 parts by weight. The carbon precursor may include at least one selected from sucrose, cellulose, xylose, and galactose.
[0117] The reason for using additional carbon precursors, such as sucrose, is that carbon precursors, such as sucrose, can improve the electrical conductivity of the metal-lithium fluoride complex as they are converted to carbon during the heat treatment process. Accordingly, utilizing a metal-lithium fluoride complex manufactured by mixing in additional carbon precursors, such as sucrose, as a cathode additive results in improved capacity during charging of the lithium-ion capacitor.
[0118] When a carbon precursor such as sucrose is additionally mixed, it is preferable that the heat treatment be performed at 500°C or higher in the heat treatment step (S230) to convert the carbon precursor into carbon. This is because if the heat treatment is performed at a temperature lower than 500°C, the carbon precursor may not be converted into carbon, which may have the adverse effect of lowering the electrochemical reactions of other substances, thereby reducing the capacity. Therefore, when a carbon precursor is further mixed with ammonium fluoride, the heat treatment is preferably performed at 500°C or higher, more preferably at 500 to 750°C for 30 to 120 minutes.
[0119] In this way, since the embodiment of the present invention manufactures a metal-lithium fluoride composite by mixing ammonium fluoride alone with lithium metal oxide, or by further mixing a carbon precursor together with ammonium fluoride and then performing a heat treatment, the process method is simple, so that a metal-lithium fluoride composite for a cathode additive can be easily manufactured at low cost.
[0120] These metal-lithium fluoride complexes include any one of nickel (Ni) / lithium fluoride, iron (Fe) / lithium fluoride, cobalt (Co) / lithium fluoride, copper (Cu) / lithium fluoride, zinc (Zn) / lithium fluoride, magnesium (Mg) / lithium fluoride, and calcium (Ca) / lithium fluoride.
[0121] With this, the method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to an embodiment of the present invention can be completed.
[0122]
[0123] Hereinafter, with reference to the attached drawings, a method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to a modified example of the present invention will be described.
[0124] FIG. 5 is a process flow diagram showing a method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to a modified example of the present invention.
[0125] As illustrated in FIG. 5, a method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to a modified example of the present invention includes a step of mixing metal hydroxide and lithium hydroxide (S310), a first heat treatment step (S320), a step of mixing lithium metal oxide and ammonium fluoride (S330), and a second heat treatment step (S340).
[0126]
[0127] Mixture of metal hydroxides and lithium hydroxide
[0128] In the metal hydroxide and lithium hydroxide mixing step (S310), the metal hydroxide and lithium hydroxide are mixed.
[0129] In this step, the metal hydroxide may be, but is not limited to, nickel hydroxide. It is preferable to mix the metal hydroxide and lithium hydroxide in a weight ratio of 1:1 to 1:3.
[0130]
[0131] Primary heat treatment
[0132] In the first heat treatment step (S320), the mixed mixture is subjected to a first heat treatment in an air or oxygen atmosphere to form lithium metal oxide.
[0133] At this stage, it is preferable to perform the primary heat treatment at 500 to 900°C for 10 to 180 minutes.
[0134]
[0135] Lithium metal oxide and ammonium fluoride mixture
[0136] In the lithium metal oxide and ammonium fluoride mixing step (S330), the formed lithium metal oxide is mixed with ammonium fluoride. Thus, in this step (S330), only ammonium fluoride can be mixed with lithium metal oxide.
[0137] Here, it is preferable to mix ammonium fluoride in an amount of 10 to 150 parts by weight per 100 parts by weight of lithium metal oxide, a more preferable range may be 30 to 100 parts by weight, and a most preferable range may be 50 to 75 parts by weight.
[0138] If the amount of ammonium fluoride added is less than 10 parts by weight per 100 parts by weight of lithium metal oxide, it may be difficult to sufficiently form lithium fluoride. Conversely, if the amount of ammonium fluoride added exceeds 150 parts by weight per 100 parts by weight of lithium metal oxide, there is a problem that the reaction proceeds excessively, resulting in a decrease in capacity.
[0139]
[0140] Secondary heat treatment
[0141] In the second heat treatment step (S340), the mixed mixture is subjected to a second heat treatment in a reducing gas atmosphere or an inert gas atmosphere to form a metal-lithium fluoride complex.
[0142] It is preferable that the reducing gas atmosphere is a gas atmosphere of any one of hydrogen, hydrogen-nitrogen mixed gas, and hydrogen-argon mixed gas, and the inert gas atmosphere is a gas atmosphere containing at least one of nitrogen and argon.
[0143] In this step, when only ammonium fluoride is mixed alone, the secondary heat treatment is preferably performed at 300 to 750°C for 30 to 120 minutes, and more preferably at 400 to 600°C for 50 to 100 minutes.
[0144] If the secondary heat treatment temperature is less than 300℃ or the secondary heat treatment time is less than 30 minutes, the metal ions (M) present in the lithium metal oxide x+ ) is a metal (M 0 ) may not be completely reduced. Conversely, if the secondary heat treatment temperature exceeds 750℃ or the secondary heat treatment time exceeds 120 minutes, the metal and lithium fluoride constituting the metal-lithium fluoride complex grow excessively, which lowers the efficiency of the electrochemical reaction when applied to a lithium ion capacitor.
[0145]
[0146] Meanwhile, in the aforementioned lithium metal oxide and ammonium fluoride mixing step (S330), a carbon precursor may be further mixed with ammonium fluoride into the lithium metal oxide.
[0147] Here, the carbon precursor is preferably mixed in an amount of 10 to 150 parts by weight per 100 parts by weight of lithium metal oxide, and a more preferable range is 30 to 100 parts by weight. The carbon precursor may include at least one selected from sucrose, cellulose, xylose, and galactose.
[0148] The additional use of a carbon precursor, such as sucrose, is due to the fact that sucrose, when converted to carbon during the heat treatment process, can improve the electrical conductivity of the metal-lithium fluoride composite. Accordingly, utilizing a metal-lithium fluoride composite manufactured by further mixing in a carbon precursor, such as sucrose, as a cathode additive can significantly improve the capacity of a lithium-ion capacitor during charging.
[0149] When a carbon precursor such as sucrose is further mixed, it is preferable that the second heat treatment be performed at 500°C or higher in the second heat treatment step (S340) to convert the carbon precursor into carbon. This is because if the heat treatment is performed at less than 500°C, the carbon precursor may not be converted into carbon, which may have the adverse effect of lowering the electrochemical reactions of other substances, thereby reducing the capacity. Therefore, when a carbon precursor is further mixed with ammonium fluoride, it is preferable that the second heat treatment be performed at 500°C or higher, more preferably at 500 to 750°C for 30 to 120 minutes.
[0150] In this way, in a modified example of the present invention, a metal-lithium fluoride complex is manufactured by mixing lithium hydroxide, which is a lithium source, with a metal hydroxide and performing a first heat treatment to form a lithium metal oxide, and then mixing ammonium fluoride alone with the lithium metal oxide, or further mixing a carbon precursor together with ammonium fluoride, and then performing a second heat treatment. Therefore, since the process method is simple, a metal-lithium fluoride complex for a cathode additive can be easily manufactured at low cost.
[0151] These metal-lithium fluoride complexes include any one of nickel (Ni) / lithium fluoride, iron (Fe) / lithium fluoride, cobalt (Co) / lithium fluoride, copper (Cu) / lithium fluoride, zinc (Zn) / lithium fluoride, magnesium (Mg) / lithium fluoride, and calcium (Ca) / lithium fluoride.
[0152] With this, the method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to a modified example of the present invention can be completed.
[0153]
[0154] As discussed so far, the method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to the present invention and the lithium ion capacitor including the same uses a material in which a lithium source is mixed with a lithium metal oxide or metal compound as a raw material, and manufactures a metal-lithium fluoride complex through a simple method of mixing ammonium fluoride and then heat-treating, and utilizes the metal-lithium fluoride complex as a cathode additive for a lithium ion capacitor.
[0155] In this way, the method for manufacturing a metal-lithium fluoride complex for a cathode additive for anode pre-doping according to the present invention and a lithium ion capacitor including the same is a method for mixing ammonium fluoride with lithium metal oxide and then heat-treating, so the manufacturing process is simple, and thus the metal-lithium fluoride complex for a cathode additive for cathode pre-doping can be manufactured at a lower cost than lithium transition metal oxide, which is a general cathode additive.
[0156] In addition, the method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to the present invention and the lithium ion capacitor including the same manufacture a metal-lithium fluoride complex exhibiting a high capacity of 400 mAh / g or more at a charging voltage of 4.5 V or less, and when such a metal-lithium fluoride complex is utilized as a cathode additive, it can exhibit suitable properties as a cathode additive because the irreversibility during discharge after charging is very large.
[0157]
[0158] The method for manufacturing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping according to the present invention and the lithium ion capacitor including the same are not limited to the methods of the embodiments and modified examples described with reference to FIGS. 4 and 5. That is, all electrode manufacturing and cell manufacturing methods for general lithium ion capacitors or lithium ion batteries can be applied.
[0159] In the present invention, the types and weight ratios of the conductive material and binder for electrode manufacturing, the solvent and drying method for slurry manufacturing, and the types of the counter electrode, electrolyte, and separator for cell manufacturing are one example method for confirming electrochemical performance.
[0160] Therefore, the metal-lithium fluoride composite manufactured according to the present invention can be equally utilized as a cathode additive for lithium-ion batteries as well as a cathode additive for lithium-ion capacitors. In other words, by utilizing both the electrode manufacturing and cell manufacturing methods of the present invention, it can be equally utilized as a cathode additive for lithium-ion batteries.
[0161]
[0162] Example
[0163] Hereinafter, the structure and operation of the present invention will be described in more detail through preferred embodiments of the present invention. However, these are presented as preferred examples of the present invention and should not be construed as limiting the present invention in any way.
[0164] Anything not described here will be omitted as it is technically feasible for those skilled in this field to infer.
[0165]
[0166] 1. Half-cell manufacturing
[0167]
[0168] Example 1
[0169]
[0170] Manufacturing of metal-lithium fluoride complexes
[0171] Commercial lithium nickel oxide (Li2NiO2) powder was prepared without any separate treatment.
[0172] Next, lithium nickel oxide (Li2NiO2) was mixed with ammonium fluoride (NH4F) at a weight ratio of 1:0.7.
[0173] Next, the mixed mixture was heat-treated at 600°C for 60 minutes in an inert gas atmosphere supplied with Ar gas to produce a metal-lithium fluoride composite.
[0174]
[0175] Electrode fabrication using metal-lithium fluoride complexes
[0176] Nickel-lithium fluoride composite manufactured by the above method: conductive material (super-P): binder (polyvinylidene fluoride, PVDF) were mixed in a weight ratio of 6:3:1, and then a slurry was manufactured using 1-methyl-2-pyrrolidone (NMP) as a solvent.
[0177] Next, the prepared slurry was applied onto aluminum foil using the doctor blade method, dried, and then dried in a vacuum at 110°C for 12 hours.
[0178] Next, a half-cell was manufactured using the dried sheet as a working electrode (cathode), a lithium metal foil as a counter electrode (anode), a polyethylene (PE) film as a separator, and a 1M LiPF6in EC / DEC (1:1) solution as an electrolyte.
[0179]
[0180] Example 2
[0181]
[0182] Manufacturing of metal-lithium fluoride complexes
[0183] Commercial nickel hydroxide (Ni(OH)2) powder and lithium hydroxide (LiOH) were mixed in a weight ratio of 1:2.
[0184] Next, lithium nickel oxide was prepared by heat treatment at 750°C in air for 60 minutes.
[0185] Next, the manufactured lithium nickel oxide was mixed with ammonium fluoride at a weight ratio of 1:0.65.
[0186] Next, the mixed mixture was heat-treated at 600°C for 60 minutes in an inert gas atmosphere supplied with Ar gas to produce a metal-lithium fluoride composite.
[0187]
[0188] Electrode fabrication using metal-lithium fluoride complexes
[0189] A half cell was manufactured using the nickel-lithium fluoride composite manufactured by the above method in the same manner as in Example 1.
[0190]
[0191] Example 3
[0192]
[0193] Manufacturing of metal-lithium fluoride complexes
[0194] Commercial lithium nickel oxide (Li2NiO2) powder was prepared without any separate treatment.
[0195] Next, lithium nickel oxide, ammonium fluoride, and sucrose were mixed in a weight ratio of 1:0.7:0.5.
[0196] Next, the mixed mixture was heat-treated at 600°C for 60 minutes in an inert gas atmosphere supplied with Ar gas to produce a metal-lithium fluoride composite.
[0197]
[0198] Electrode fabrication using metal-lithium fluoride complexes
[0199] A half cell was manufactured using the nickel-lithium fluoride composite manufactured by the above method in the same manner as in Example 1.
[0200]
[0201] Comparative Example 1
[0202] A half-cell was manufactured in the same manner as in Example 3, except that lithium nickel oxide, ammonium fluoride, and sucrose were mixed in a weight ratio of 1:1.5:0.5 when manufacturing a metal-lithium fluoride complex.
[0203]
[0204] Comparative Example 2
[0205] When manufacturing the metal-lithium fluoride composite, a half-cell was manufactured in the same manner as in Example 3, except that heat treatment was performed at 500°C.
[0206]
[0207] 2. Physical property evaluation
[0208] FIG. 6 is a graph showing the results of XRD analysis of a nickel-lithium fluoride composite manufactured according to Example 1, and FIG. 7 is a graph showing the results of a half-cell test performed after manufacturing an electrode using a nickel-lithium fluoride composite manufactured according to Example 1.
[0209] As shown in Fig. 6, the XRD analysis results of the nickel-lithium fluoride composite manufactured according to Example 1 confirmed that nickel and lithium fluoride crystal peaks were observed.
[0210] In addition, as shown in Fig. 7, a half-cell test was performed after manufacturing an electrode using the nickel-lithium fluoride composite manufactured according to Example 1. At this time, the prepared half-cell was tested at 4.5 V (vs. Li / Li) with a current of 10 mA / g. + ) When the voltage was increased to 2.5 V and the battery was delithiated, the capacity was 436 mAh / g at the first charge. After that, when the voltage was lowered to 2.5 V and the battery was discharged, the capacity was 4.9 mAh / g, resulting in an irreversibility of approximately 431 mAh / g and a coulombic efficiency of approximately 1.1%.
[0211] In addition, when an electrode was manufactured using a nickel-lithium fluoride composite manufactured according to Example 2 and a half-cell test was conducted, charge and discharge capacities similar to those in Example 1 were observed.
[0212]
[0213] Figure 8 is a graph showing the results of a half-cell test conducted after manufacturing an electrode using a nickel-lithium fluoride composite manufactured according to Example 3.
[0214] As shown in Fig. 8, an electrode was manufactured using a nickel-lithium fluoride composite manufactured according to Example 3, and then a half-cell test was conducted. At this time, the prepared half-cell was tested at 4.5 V (vs. Li / Li) with a current of 10 mA / g. + ) and charging was performed by increasing the voltage to 2.6 V, and the capacity was 568 mAh / g. After that, discharging (lithiation) was performed by lowering the voltage to 2.6 V, and the capacity was 6.9 mAh / g, resulting in an irreversibility of approximately 561 mAh / g and a coulombic efficiency of approximately 1.2%.
[0215]
[0216] Figure 9 is a graph showing the results of a half-cell test conducted after manufacturing an electrode using a nickel-lithium fluoride composite manufactured according to Comparative Example 1.
[0217] As shown in Fig. 9, after manufacturing an electrode using the nickel-lithium fluoride composite manufactured according to Comparative Example 1, a half-cell test was performed, and a reduced low capacity of 185 mAh / g was exhibited when the first charge was performed.
[0218]
[0219] Figure 10 is a graph showing the results of a half-cell test conducted after manufacturing an electrode using a nickel-lithium fluoride composite manufactured according to Comparative Example 2.
[0220] As shown in Fig. 10, when an electrode was manufactured using a nickel-lithium fluoride composite manufactured according to Comparative Example 2 and a half-cell test was performed, a low capacity of 74 mAh / g was observed upon the first charge.
[0221]
[0222] While the above description focuses on specific embodiments of the present invention, those skilled in the art will appreciate that various modifications and variations can be made. Such modifications and variations, as long as they do not depart from the scope of the technical concept provided by the present invention, are considered to be within the scope of the present invention. Therefore, the scope of the present invention should be determined by the claims set forth below.
[0223]
[0224] [Explanation of symbols]
[0225] S210: Lithium metal oxide preparation step
[0226] S220: Lithium metal oxide and ammonium fluoride mixed stage
[0227] S230: Heat treatment stage
[0228]
[0229] S310: Mixed metal hydroxide and lithium hydroxide step
[0230] S320: 1st heat treatment stage
[0231] S330: Lithium metal oxide and ammonium fluoride mixed stage
[0232] S340: Second heat treatment stage
Claims
1. (a) Step of preparing lithium metal oxide; (b) a step of mixing the lithium metal oxide with ammonium fluoride; and (c) a step of heat-treating the above-mentioned mixed mixture in a reducing gas atmosphere or an inert gas atmosphere to form a metal-lithium fluoride complex; A method for producing a metal-lithium fluoride complex for cathode additives for cathode pre-doping, characterized in that it comprises:
2. In paragraph 1, In step (a) above, The above lithium metal oxide is Li x NiO y , Li x FeO y , Li x CoO y , Li x CuO y , Li x ZnO y , Li x MgO y and Li x CaO y A method for producing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping, characterized in that it comprises one selected from among: (where 0.1 ≤ x ≤ 6 and 1 ≤ y ≤ 6) 3. In paragraph 1, In step (b) above, The above ammonium fluoride A method for producing a metal-lithium fluoride complex for a cathode additive for anode pre-doping, characterized in that 10 to 150 parts by weight are mixed with respect to 100 parts by weight of the above lithium metal oxide.
4. In paragraph 1, In step (b) above, A method for producing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping, characterized in that only the above ammonium fluoride is mixed alone, or a carbon precursor is further mixed together with the above ammonium fluoride.
5. In paragraph 4, The above carbon precursor is A method for producing a metal-lithium fluoride complex for a cathode additive for anode pre-doping, characterized in that 10 to 150 parts by weight are mixed with respect to 100 parts by weight of the above lithium metal oxide.
6. In paragraph 4, The above carbon precursor is A method for producing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping, characterized in that it comprises at least one selected from sucrose, cellulose, xylose and galactose.
7. In paragraph 1, In step (c) above, When the above ammonium fluoride is mixed alone, A method for manufacturing a metal-lithium fluoride complex for cathode additives for cathode pre-doping, characterized in that the above heat treatment is performed at a temperature of 300 to 750°C for 30 to 120 minutes.
8. In paragraph 1, In step (c) above, The above reducing gas atmosphere is one of hydrogen, hydrogen-nitrogen mixed gas, and hydrogen-argon mixed gas, A method for producing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping, characterized in that the above inert gas atmosphere is a gas atmosphere containing at least one of nitrogen and argon.
9. In paragraph 4, In step (c) above, When a carbon precursor is further mixed with the above ammonium fluoride, A method for manufacturing a metal-lithium fluoride complex for cathode additives for cathode pre-doping, characterized in that the above heat treatment is performed at 500 to 750°C for 30 to 120 minutes.
10. In paragraph 1, In step (c) above, The above metal-lithium fluoride complex is A method for producing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping, characterized in that it comprises any one of nickel (Ni) / lithium fluoride, iron (Fe) / lithium fluoride, cobalt (Co) / lithium fluoride, copper (Cu) / lithium fluoride, zinc (Zn) / lithium fluoride, magnesium (Mg) / lithium fluoride, and calcium (Ca) / lithium fluoride. 11.(a) A step of mixing metal hydroxide and lithium hydroxide; (b) a step of forming lithium metal oxide by first heat treating the above-mentioned mixed mixture in an air or oxygen atmosphere; (c) a step of mixing the formed lithium metal oxide with ammonium fluoride; and (d) a step of forming a metal-lithium fluoride complex by performing a secondary heat treatment on the above-mentioned mixed mixture in a reducing gas atmosphere or an inert gas atmosphere; A method for producing a metal-lithium fluoride complex for cathode additives for cathode pre-doping, characterized in that it comprises:
12. In paragraph 11, In step (b) above, The above first heat treatment A method for producing a metal-lithium fluoride complex for cathode additives for cathode pre-doping, characterized in that the process is performed at 500 to 900°C for 10 to 180 minutes.
13. In paragraph 11, In step (c) above, A method for producing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping, characterized in that only the above ammonium fluoride is mixed alone, or a carbon precursor is further mixed together with the above ammonium fluoride.
14. In paragraph 11, In step (d) above, When the above ammonium fluoride is mixed alone, A method for manufacturing a metal-lithium fluoride complex for cathode additives for cathode pre-doping, characterized in that the above secondary heat treatment is performed at 300 to 750°C for 30 to 120 minutes.
15. In paragraph 11, In step (d) above, The above reducing gas atmosphere is one of hydrogen, hydrogen-nitrogen mixed gas, and hydrogen-argon mixed gas, A method for producing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping, characterized in that the above inert gas atmosphere is a gas atmosphere containing at least one of nitrogen and argon.
16. In paragraph 11, In step (d) above, When a carbon precursor is further mixed with the above ammonium fluoride, A method for manufacturing a metal-lithium fluoride complex for cathode additives for cathode pre-doping, characterized in that the above secondary heat treatment is performed at 500 to 750°C for 30 to 120 minutes.
17. In paragraph 11, In step (d) above, The above metal-lithium fluoride complex is A method for producing a metal-lithium fluoride complex for a cathode additive for cathode pre-doping, characterized in that it comprises any one of nickel (Ni) / lithium fluoride, iron (Fe) / lithium fluoride, cobalt (Co) / lithium fluoride, copper (Cu) / lithium fluoride, zinc (Zn) / lithium fluoride, magnesium (Mg) / lithium fluoride, and calcium (Ca) / lithium fluoride.
18. A negative electrode having a negative current collector and a negative active material layer formed on both sides of the negative current collector; A positive electrode laminated on the negative electrode, having a positive electrode current collector and a positive electrode active material layer formed on both sides of the positive electrode current collector; and A separator disposed between the cathode and the anode; The above positive electrode active material layer includes a positive electrode active material, a positive electrode additive, a conductive material, and a binder, A lithium ion capacitor comprising a metal-lithium fluoride complex for anode pre-doping, characterized in that the cathode additive uses a metal-lithium fluoride complex manufactured by any one of the methods of claims 1 to 17.
19. In paragraph 18, The above lithium ion capacitor A lithium ion capacitor comprising a metal-lithium fluoride complex for cathode additive for anode pre-doping, characterized in that a metal-lithium fluoride complex exhibiting a capacity of 400 mAh / g or more at a charging voltage of 4.5 V or less is added as a cathode additive.
20. In paragraph 18, The above metal-lithium fluoride complex is A lithium ion capacitor comprising a metal-lithium fluoride complex for a cathode additive for anode pre-doping, characterized in that it comprises any one of nickel (Ni) / lithium fluoride, iron (Fe) / lithium fluoride, cobalt (Co) / lithium fluoride, copper (Cu) / lithium fluoride, zinc (Zn) / lithium fluoride, magnesium (Mg) / lithium fluoride, and calcium (Ca) / lithium fluoride.
Citation Information
Patent Citations
Pre-lithiation additive of lithium ion battery cathode material and preparation method and application thereof
CN112164796A
Cathode active material added with fluorine compound for lithium secondary batteries And Method of producing thereof
KR100701532B1
Positive electrode active material coated with fluorine compounds for lithium secondary battery and preparation method thereof
KR101490406B1
A System for Paying a Toll Through with a Mobile Application
KR1020220050862A
Pipe fixture for plastic house frame
KR102452793B1