Transparent coating composition

A transparent paint composition combining specific acrylic and polyester polyols with an isocyanate curing agent addresses adhesion and resistance issues in automotive coatings, offering improved workability and environmental sustainability.

WO2024225620A1PCT designated stage expired Publication Date: 2024-10-31KCC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/003575
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-03-21
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional clear paint compositions for automotive bumpers, particularly those using polyolefin substrates, face challenges with adhesion due to poor non-polar material compatibility, and existing low VOC paints suffer from reduced workability, slow drying, and inferior resistance properties.

Method used

A transparent paint composition is developed using a combination of acrylic and polyester polyols with specific hydroxyl values and molecular weights, along with an isocyanate curing agent, to enhance adhesion, drying speed, and crosslinking density, resulting in a high-solid, low-VOC paint with improved water, weather, and chemical resistance.

Benefits of technology

The paint composition achieves excellent workability, adhesion, and resistance properties, making it suitable for non-polar substrates like polyolefin resins while being environmentally friendly with reduced VOC content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTKR2024003575-APPB-IMG-000001
    Figure PCTKR2024003575-APPB-IMG-000001
  • Figure PCTKR2024003575-APPB-IMG-000002
    Figure PCTKR2024003575-APPB-IMG-000002
  • Figure PCTKR2024003575-APPB-IMG-000003
    Figure PCTKR2024003575-APPB-IMG-000003
Patent Text Reader

Abstract

The present invention relates to a transparent coating composition comprising a first acrylic polyol, a second acrylic polyol, a first polyester polyol, a second polyester polyol, a third polyester polyol, and an isocyanate compound, wherein: the first acrylic polyol has a lower hydroxyl value and a lower glass transition temperature than the second acrylic polyol; the first polyester polyol has a higher hydroxyl value and a higher weight average molecular weight than the second polyester polyol; and the first polyester polyol has a lower hydroxyl value and a higher weight average molecular weight than the third polyester polyol.
Need to check novelty before this filing date? Find Prior Art

Description

transparent paint composition

[0001] The present invention relates to a transparent paint composition that is environmentally friendly due to its low content of volatile organic compounds (VOCs), has excellent workability, and has excellent water resistance, weather resistance, chemical resistance, and appearance characteristics of the produced coating film.

[0002] Automotive bumpers are typically manufactured from compositions containing polyolefins such as polypropylene. These bumpers are often coated with paint to enhance their appearance and physical properties. Polyolefin resins such as polypropylene are generally non-polar and are known to have poor adhesion. Therefore, to enhance paint adhesion to polyolefin substrates, the surface is typically treated or a primer is applied to form a primer layer before additional coating.

[0003] Specifically, conventional automobile bumpers have been coated with multilayer films, such as a primer layer, a base coating layer, and a transparent coating layer, to improve their physical properties and appearance. At this time, each layer of the multilayer film was typically coated with an oil-based paint. For example, Korean Patent No. 1655621 (Patent Document 1) discloses a clear paint composition comprising an acrylic polyol resin and a polyester polyol resin having a specific hydroxyl value, a reactive silicone additive in which a polysiloxane side chain is bonded to an acrylate main chain, and a two-component type isocyanate curing agent. However, conventional oil-based paints, such as the clear paint composition of Patent Document 1, have a high content of volatile organic compounds (VOCs), and as their use has been regulated in many countries, the need for paints with a low VOC content is increasing.

[0004] Accordingly, low-VOC water-based paints or high-solids oil-based paints have been proposed. However, when the top transparent coating layer is formed with a water-based paint, problems arise in painting workability, such as a significant decrease in the paint film's adhesion. Furthermore, when a transparent coating layer is produced by painting with an oil-based high-solids paint, there are problems in that the drying is slow and the painting workability is significantly inferior to that of conventional oil-based paints.

[0005] Therefore, there is a need to develop a transparent paint that is environmentally friendly due to its low volatile organic compound (VOC) content, has excellent paint workability, and has excellent water resistance, weather resistance, chemical resistance, and appearance characteristics of the manufactured coating film.

[0006] The present invention provides a transparent paint composition having a high solid content and a low volatile organic compound (VOC) content, which is environmentally friendly, has excellent paint workability, and has excellent water resistance, weather resistance, chemical resistance, and appearance characteristics of the produced paint film.

[0007] In order to achieve the above purpose, the present invention comprises a first acrylic polyol, a second acrylic polyol, a first polyester polyol, a second polyester polyol, a third polyester polyol, and an isocyanate compound,

[0008] The first acrylic polyol has a lower hydroxyl value and glass transition temperature than the second acrylic polyol,

[0009] The first polyester polyol has a higher hydroxyl value and weight average molecular weight than the second polyester polyol,

[0010] The first polyester polyol provides a transparent paint composition having a lower hydroxyl value and a higher weight average molecular weight than the third polyester polyol.

[0011] The transparent paint composition according to the present invention is environmentally friendly due to its high solids content and low volatile organic compound (VOC) content, and exhibits excellent painting workability. Furthermore, a coating film prepared from the transparent paint composition exhibits excellent water resistance, weather resistance, chemical resistance, and appearance properties, making it highly suitable as a paint for automotive parts, particularly for substrates made of non-polar materials such as polyolefin resins.

[0012] Hereinafter, the present invention will be described in detail.

[0013] The “weight average molecular weight” used in this specification is measured by a conventional method known in the art, and can be measured by, for example, the GPC (gel permeation chromatography) method.

[0014] Additionally, the “glass transition temperature” is measured by a conventional method known in the art, and can be measured by, for example, differential scanning calorimetry (DSC).

[0015] Furthermore, functional groups such as “acid value” and “hydroxyl value” can be measured by methods well known in the art, and can represent values ​​measured by, for example, a titration method.

[0016] In this specification, “(meth)acrylic” means “acrylic” and / or “methacrylic”, and “(meth)acrylate” means “acrylate” and / or “methacrylate”.

[0017] A transparent paint composition according to the present invention comprises a first acrylic polyol, a second acrylic polyol, a first polyester polyol, a second polyester polyol, a third polyester polyol, and an isocyanate compound.

[0018] The above transparent paint composition forms a coating film by a urethane reaction between a hydroxyl group of an acrylic polyol and an isocyanate group of an isocyanate compound, and includes two types of acrylic polyols having different hydroxyl groups and glass transition temperatures, so that the different glass transition temperatures of the acrylic polyols control the drying speed of the produced coating film and the different hydroxyl groups of the acrylic polyols control the crosslinking density of the produced coating film, thereby improving the coating film's physical properties such as appearance, adhesion, water resistance, chemical resistance, and weather resistance.

[0019] In addition, the transparent paint composition comprises three kinds of polyester polyols having different hydroxyl groups and weight average molecular weights, in which a hydroxyl group of a polyester polyol and an isocyanate compound react with a urethane group to form a coating film, and the different weight average molecular weights of the polyester polyols appropriately control the viscosity of the composition, thereby improving workability, and the different hydroxyl groups of the polyester polyols control the crosslinking density of the produced coating film, thereby improving the physical properties of the coating film, such as appearance, adhesion, water resistance, chemical resistance, and weather resistance. Furthermore, the three kinds of polyester polyols have a high solid content, thereby making the paint composition highly solid, thereby improving the paintability, workability, and appearance characteristics of the coating film, while also improving the physical properties of the coating film, such as water resistance. In particular, the paint composition includes three types of polyester polyols, thereby improving the weather resistance of the produced coating film, thereby preventing discoloration even under harsh conditions, and is environmentally friendly due to its low organic solvent content. Specifically, a paint composition including only the first polyester polyol having a higher hydroxyl value and weight average molecular weight than the second polyester polyol improves the chemical resistance and abrasion resistance of the produced coating film, but may have poor workability due to the high viscosity of the paint composition. Therefore, when the first polyester polyol and the second polyester polyol having a relatively low hydroxyl value and weight average molecular weight are included, the viscosity of the paint composition is appropriately adjusted, thereby improving workability, preventing staining of the produced coating film, and improving appearance characteristics such as gloss. In addition, the paint composition further comprising a third polyester polyol having different hydroxyl groups and weight average molecular weights from the polyester polyols has the effect of improving the water resistance and weather resistance of the produced paint film by more closely controlling the crosslinking density of the produced paint film.

[0020]

[0021] 1st acrylic polyol

[0022] The first acrylic polyol serves to improve the appearance properties of the manufactured coating film.

[0023] The first acrylic polyol may be synthesized directly using a known method, or a commercially available product may be used. In this case, the first acrylic polyol may be prepared by polymerizing, for example, at least one of a vinyl monomer and a (meth)acrylate monomer.

[0024] The type of the above vinyl monomer is not particularly limited, but for example, at least one selected from the group consisting of styrene, methylstyrene, dimethylstyrene, fluorostyrene, ethoxystyrene, methoxystyrene, phenylene vinyl ketone, vinyl t-butyl benzoate, vinyl cyclohexanoate, vinyl acetate, vinyl pyrrolidone, vinyl chloride, vinyl alcohol, acetoxystyrene, t-butylstyrene, and vinyltoluene may be used.

[0025] The above (meth)acrylate monomers include, for example, 2-hydroxypropyl methacrylate, propyl methacrylate, t-butylaminoethyl methacrylate, dicyclopentenyl oxyethyl methacrylate, acrylic acid dimer, hexanediol diacrylate, t-butyl acrylate, triisopropylsilyl acrylate, benzyl methacrylate, 2-hydroxyethyl methacrylate, trimethylolpropane triacrylate, tripropylene glycol diacrylate, ethyl methacrylate, isobutyl methacrylate, hydroxyisopropyl methacrylate, isopropyl methacrylate, cyclohexyl methacrylate, triisopropyl silyl methacrylate, isobornyl acrylate, t-butylcyclohexyl methacrylate, trimethylcyclohexyl methacrylate, methyl methacrylate, acrylic acid, t-butyl methacrylate, One or more selected from the group consisting of isobornyl methacrylate, methacrylonitrile, methacrylic acid, acrylamide, methacrylamide, and cyclohexyl vinyl ether may be used.

[0026] The above first acrylic polyol can be manufactured using a radical polymerization method, and the weight average molecular weight can be controlled depending on the initiator and polymerization time.

[0027] At this time, the first acrylic polyol has a lower hydroxyl value and glass transition temperature than the second acrylic polyol. For example, the first acrylic polyol may have a hydroxyl value that is 5 to 40 mgKOH / g or 10 to 20 mgKOH / g lower than the second acrylic polyol. In addition, the first acrylic polyol may have a glass transition temperature that is 25°C to 50°C or 30°C to 45°C lower than the second acrylic polyol. Furthermore, the first acrylic polyol may have a lower weight average molecular weight than the second acrylic polyol.

[0028] The first acrylic polyol may have a hydroxyl value (OHv) of 80 to 100 mgKOH / g, or 90 to 100 mgKOH / g. When the hydroxyl value of the first acrylic polyol is within the above range, the sagging property of the produced coating film is improved. On the other hand, when the hydroxyl value of the first acrylic polyol is below the above range, the paintability of the produced coating film may be insufficient, and when it exceeds the above range, the appearance characteristics of the produced coating film may be deteriorated.

[0029] In addition, the first acrylic polyol may have a glass transition temperature (Tg) of 30 to 40°C or 31 to 37°C. When the glass transition temperature of the first acrylic polyol is within the above range, the drying time of the composition is appropriate, resulting in excellent workability and improved appearance properties and hardness of the produced coating film. On the other hand, when the glass transition temperature of the first acrylic polyol is below the above range, the hardness of the produced coating film may be insufficient, and paint staining and surface stickiness may occur, and when it exceeds the above range, the sagging property of the produced coating film may be reduced.

[0030] The above first acrylic polyol may have a weight average molecular weight (Mw) of 2,000 to 3,500 g / mol, or 2,700 to 3,200 g / mol. When the weight average molecular weight of the first acrylic polyol is within the above range, the manufactured coating film exhibits excellent chemical resistance and workability. On the other hand, when the weight average molecular weight of the first acrylic polyol is below the above range, the paintability of the manufactured coating film is reduced, and when it exceeds the above range, the curing time of the composition is prolonged, which may result in poor painting workability.

[0031] In addition, the solid content (NV) of the first acrylic polyol may be 60 to 75 wt%, or 63 to 72 wt%, based on the total weight of the first acrylic polyol. When the solid content of the first acrylic polyol is within the above range, the composition has excellent storage stability and can be stored in a high solid content form without agglomeration or precipitation of the solid content. In addition, when the solid content of the first acrylic polyol is less than the above range, there is a problem that the amount of use for other compositions that can be used is limited due to the low solid content and the high solvent content, and when it exceeds the above range, the high viscosity of the composition may result in insufficient painting workability and storage stability.

[0032] The first acrylic polyol may be included in the composition in an amount of 20 to 30 parts by weight, or 23 to 28 parts by weight, relative to 5 to 10 parts by weight of the second acrylic polyol. When the amount of the first acrylic polyol is within the above range, the produced coating film does not stain, thereby exhibiting good appearance characteristics. On the other hand, when the amount of the first acrylic polyol is less than or greater than the above range, the drying time of the composition may be prolonged, or the produced coating film may exhibit insufficient appearance characteristics.

[0033]

[0034] Second acrylic polyol

[0035] The second acrylic polyol plays a role in improving the appearance properties and adhesion of the manufactured coating film.

[0036] The second acrylic polyol may be synthesized directly using a known method, or a commercially available product may be used. In this case, the second acrylic polyol may be, for example, manufactured by polymerizing at least one of a vinyl monomer and a (meth)acrylate monomer.

[0037] The type of the above vinyl monomer is not particularly limited, but for example, at least one selected from the group consisting of styrene, methylstyrene, dimethylstyrene, fluorostyrene, ethoxystyrene, methoxystyrene, phenylene vinyl ketone, vinyl t-butyl benzoate, vinyl cyclohexanoate, vinyl acetate, vinyl pyrrolidone, vinyl chloride, vinyl alcohol, acetoxystyrene, t-butylstyrene, and vinyltoluene may be used.

[0038] The above (meth)acrylate monomers include, for example, 2-hydroxypropyl methacrylate, propyl methacrylate, t-butylaminoethyl methacrylate, dicyclopentenyl oxyethyl methacrylate, acrylic acid dimer, hexanediol diacrylate, t-butyl acrylate, triisopropylsilyl acrylate, benzyl methacrylate, 2-hydroxyethyl methacrylate, trimethylolpropane triacrylate, tripropylene glycol diacrylate, ethyl methacrylate, isobutyl methacrylate, hydroxyisopropyl methacrylate, isopropyl methacrylate, cyclohexyl methacrylate, triisopropyl silyl methacrylate, isobornyl acrylate, t-butylcyclohexyl methacrylate, trimethylcyclohexyl methacrylate, methyl methacrylate, acrylic acid, t-butyl methacrylate, One or more selected from the group consisting of isobornyl methacrylate, methacrylonitrile, methacrylic acid, acrylamide, methacrylamide, and cyclohexyl vinyl ether may be used.

[0039] The above second acrylic polyol can be manufactured using a radical polymerization method, and the weight average molecular weight can be controlled depending on the initiator and polymerization time.

[0040] At this time, the second acrylic polyol may have a hydroxyl value (OHv) of 101 to 120 mgKOH / g, or 106 to 120 mgKOH / g. When the hydroxyl value of the second acrylic polyol is within the above range, the adhesion of the manufactured coating film is improved. On the other hand, when the hydroxyl value of the second acrylic polyol is below the above range, the adhesion of the manufactured coating film may be insufficient, and when it exceeds the above range, the appearance characteristics of the manufactured coating film may deteriorate.

[0041] In addition, the second acrylic polyol may have a glass transition temperature (Tg) of 65 to 80°C or 70 to 77°C. When the glass transition temperature of the second acrylic polyol is within the above range, the drying time of the composition is appropriate, resulting in excellent workability and improved adhesion of the produced coating film. On the other hand, when the glass transition temperature of the second acrylic polyol is below the above range, the hardness of the produced coating film may be insufficient, and the painting workability of the composition may be insufficient, and when it exceeds the above range, the water resistance of the produced coating film may be reduced.

[0042] The above second acrylic polyol may have a weight average molecular weight (Mw) of more than 3,500 g / mol and less than or equal to 5,000 g / mol, or more than 3,500 g / mol and less than or equal to 4,000 g / mol. When the weight average molecular weight of the second acrylic polyol is within the above range, the manufactured coating film has excellent chemical resistance and water resistance. On the other hand, when the weight average molecular weight of the second acrylic polyol is less than the above range, the chemical resistance of the manufactured coating film is reduced, and when it exceeds the above range, the curing time of the composition is prolonged, which may result in poor painting workability.

[0043] In addition, the solid content (NV) of the second acrylic polyol may be 60 to 75 wt%, or 63 to 72 wt%, based on the total weight of the second acrylic polyol. When the solid content of the second acrylic polyol is within the above range, the composition has excellent storage stability and can be stored in a high solid content form without agglomeration or precipitation of the solid content. In addition, when the solid content of the second acrylic polyol is less than the above range, there is a problem that the amount of use for other compositions that can be used is limited due to the low solid content and the high solvent content, and when it exceeds the above range, the high viscosity of the composition may result in insufficient painting workability and storage stability.

[0044] The second acrylic polyol may be included in the composition in an amount of 5 to 10 parts by weight or 6 to 9 parts by weight based on 20 to 30 parts by weight of the first acrylic polyol. When the amount of the second acrylic polyol is within the above range, the produced coating film does not stain, thereby providing good appearance properties. On the other hand, when the amount of the second acrylic polyol is less than or greater than the above range, the drying time of the composition may be prolonged or the adhesiveness of the produced coating film may be insufficient.

[0045]

[0046] Meanwhile, the paint composition of the present invention may include the first acrylic polyol and the second acrylic polyol in a total amount of 25 to 40 parts by weight, 29 to 37 parts by weight, or 32 to 36 parts by weight, based on 100 parts by weight of the total paint composition. When the total amount of the first acrylic polyol and the second acrylic polyol is within the above range, the appearance characteristics and adhesion of the manufactured coating film may be excellent, and the workability of the composition may be excellent. On the other hand, when the total amount of the first acrylic polyol and the second acrylic polyol is less than the above range, there may be a problem that the hardness, water resistance, weather resistance, appearance, and especially gloss of the manufactured coating film are insufficient, and when it exceeds the above range, there may be a problem that the painting workability of the paint composition is insufficient or the appearance characteristics of the manufactured coating film are insufficient.

[0047] In addition, in the transparent paint composition of the present invention, the first acrylic polyol and the second acrylic polyol may be included in a weight ratio of 2:1 to 6:1, or a weight ratio of 2.5:1 to 5.0:1. When the mixing weight ratio of the first acrylic polyol and the second acrylic polyol is within the above range, there is an effect of improving the paintability and adhesion of the manufactured coating film and improving the appearance characteristics. On the other hand, when the mixing weight ratio of the first acrylic polyol and the second acrylic polyol is less than the above range, that is, when a small amount of the first acrylic polyol is included with respect to the weight of the second acrylic polyol, there is a problem that the paintability, adhesion, and appearance characteristics of the manufactured coating film are deteriorated, and when it exceeds the above range, that is, when an excessive amount of the first acrylic polyol is included with respect to the weight of the second acrylic polyol, there may occur a problem that the drying property of the composition is deteriorated.

[0048]

[0049] 1st polyester polyol

[0050] The first polyester polyol serves to improve the appearance properties, adhesion, and weather resistance of the manufactured coating film.

[0051] The first polyester polyol may be synthesized directly using a known method, or a commercially available product may be used. For example, the first polyester polyol may be prepared by reacting a carboxylic acid compound with a polyol compound.

[0052] At this time, the carboxylic acid compound may be at least one selected from the group consisting of, for example, adipic acid (AA), isophthalic acid (IPA), trimaletic anhydride (TMA), alicyclic acids, phthalic anhydride, isophthalic acid, terephthalic acid, succinic acid, adipic acid, fumaric acid, maleic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, and derivatives thereof.

[0053] In addition, the polyol compound may be at least one selected from the group consisting of methoxypolyethylene glycol, 1,6-hexanediol (1,6-HD), neopentyl glycol (NPG), trimethylol propane (TMP), ethylene glycol, propylene glycol, diethylene glycol, butanediol 1,4-hexanediol, and 3-methylpentanediol.

[0054] The first polyester polyol has a higher hydroxyl value and a higher weight average molecular weight than the second polyester polyol. For example, the first polyester polyol may have a lower hydroxyl value of 30 to 50 mgKOH / g, or 35 to 45 mgKOH / g, than the second polyester polyol. In addition, the first polyester polyol may have a higher weight average molecular weight of 2,000 to 4,000 g / mol, or 2,500 to 3,500 g / mol, than the second polyester polyol. Furthermore, the first polyester polyol may have a higher acid value (Av) than the second polyester polyol.

[0055] Additionally, the first polyester polyol has a lower hydroxyl value and a higher weight average molecular weight than the third polyester polyol. For example, the first polyester polyol may have a hydroxyl value that is 50 to 140 mgKOH / g, or 80 to 120 mgKOH / g lower than the third polyester polyol. Additionally, the first polyester polyol may have a weight average molecular weight that is 3,000 to 5,000 g / mol, or 3,200 to 3,800 g / mol higher than the third polyester polyol.

[0056] Specifically, the first polyester polyol may have a hydroxyl value (OHv) of 150 to 200 mgKOH / g, or 160 to 190 mgKOH / g. When the hydroxyl value of the first polyester polyol is within the above range, the manufactured coating film has excellent appearance characteristics and weather resistance. When the hydroxyl value of the first polyester polyol is outside the above range, the manufactured coating film may have stains or the weather resistance of the coating film may be insufficient.

[0057] In addition, the first polyester polyol may have a weight average molecular weight (Mw) of 3,500 to 6,000 g / mol, or 4,200 to 5,000 g / mol. When the weight average molecular weight of the first polyester polyol is within the above range, the drying time of the paint is appropriate, so that workability is excellent, and the produced coating film has excellent water resistance and weather resistance. When the weight average molecular weight of the first polyester polyol is less than the above range, the drying time of the paint may be long, so that workability may be poor, and when it exceeds the above range, the produced coating film may have stains or lack appearance characteristics.

[0058] The above first polyester polyol may have an acid value (Av) of 10 to 30 mgKOH / g, or 17 to 27 mgKOH / g. When the acid value of the first polyester polyol is within the above range, rapid hardening due to heat treatment is prevented, thereby preventing appearance defects of the coating film and reducing the formation of bubbles (popping). When the acid value of the first polyester polyol is below the above range, the appearance characteristics of the manufactured coating film are insufficient, and when it exceeds the above range, the water resistance and weather resistance of the manufactured coating film may be insufficient.

[0059] In addition, the solid content (NV) of the first polyester polyol may be 60 to 70 wt%, or 62 to 66 wt%, based on the total weight of the first polyester polyol. When the solid content of the first polyester polyol is within the above range, the composition has excellent storage stability and can be stored in a high solid content form without agglomeration or precipitation of the solid content. In addition, when the solid content of the first polyester polyol is less than the above range, there is a problem that the amount of use for other compositions that can be used is limited due to the low solid content and high solvent content, and when it exceeds the above range, the high viscosity of the composition may result in insufficient painting workability and storage stability.

[0060] The first polyester polyol may be included in the composition in an amount of 5 to 15 parts by weight, or 8 to 13 parts by weight, based on 20 to 30 parts by weight of the first acrylic polyol. When the first polyester polyol is included within the above content range, the appearance properties of the coating film, particularly the gloss properties, are improved and the formation of stains is prevented. When the content of the first polyester polyol is less than the above range, there is a problem of stains occurring in the manufactured coating film, and when it exceeds the above range, the drying property of the composition is delayed and the gloss of the manufactured coating film increases, which may result in poor appearance properties.

[0061]

[0062] Second polyester polyol

[0063] The second polyester polyol serves to improve the appearance properties, adhesion, and weather resistance of the manufactured coating film.

[0064] The second polyester polyol may be synthesized directly using a known method, or a commercially available product may be used. For example, the second polyester polyol may be prepared by reacting a carboxylic acid compound with a polyol compound.

[0065] At this time, the carboxylic acid compound may be at least one selected from the group consisting of, for example, adipic acid (AA), isophthalic acid (IPA), trimaletic anhydride (TMA), alicyclic acids, phthalic anhydride, isophthalic acid, terephthalic acid, succinic acid, adipic acid, fumaric acid, maleic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, and derivatives thereof.

[0066] In addition, the polyol compound may be at least one selected from the group consisting of methoxypolyethylene glycol, 1,6-hexanediol (1,6-HD), neopentyl glycol (NPG), trimethylol propane (TMP), ethylene glycol, propylene glycol, diethylene glycol, butanediol 1,4-hexanediol, and 3-methylpentanediol.

[0067] The second polyester polyol may have a hydroxyl value (OHv) of 130 to 149 mgKOH / g, or 131 to 140 mgKOH / g. When the hydroxyl value of the second polyester polyol is within the above range, the manufactured coating film has excellent appearance characteristics and weather resistance. When the hydroxyl value of the second polyester polyol is outside the above range, the manufactured coating film may be stained or have insufficient weather resistance.

[0068] In addition, the second polyester polyol may have a weight average molecular weight (Mw) of 1,000 to 3,400 g / mol, or 1,000 to 2,000 g / mol. When the weight average molecular weight of the second polyester polyol is within the above range, the drying time of the paint is appropriate, so that workability is excellent, and the produced coating film has excellent water resistance and weather resistance. When the weight average molecular weight of the second polyester polyol is less than the above range, the drying time of the paint is long, so that workability may be poor, and when it exceeds the above range, the produced coating film may be stained or have poor appearance characteristics.

[0069] The second polyester polyol may have an acid value (Av) of 10 to 30 mgKOH / g, or 17 to 27 mgKOH / g. When the acid value of the second polyester polyol is within the above range, rapid hardening due to heat treatment is prevented, thereby preventing appearance defects of the coating film and reducing the formation of bubbles (popping). When the acid value of the second polyester polyol is below the above range, the appearance characteristics of the manufactured coating film are insufficient, and when it exceeds the above range, the water resistance and weather resistance of the manufactured coating film may be insufficient.

[0070] In addition, the solid content (NV) of the second polyester polyol may be 40 to 50 wt%, or 42 to 47 wt%, based on the total weight of the second polyester polyol. When the solid content of the second polyester polyol is within the above range, the composition has excellent storage stability and can be stored in a high solid content form without agglomeration or precipitation of the solid content. In addition, when the solid content of the second polyester polyol is less than the above range, there is a problem that the amount of use for other compositions that can be used is limited due to the low solid content and high solvent content, and when it exceeds the above range, the high viscosity of the composition may result in insufficient painting workability and storage stability.

[0071] The second polyester polyol may be included in the composition in an amount of 1 to 10 parts by weight, or 2 to 7 parts by weight, based on 20 to 30 parts by weight of the first acrylic polyol. When the second polyester polyol is included within the above content range, the appearance properties of the coating film, particularly the gloss properties, are improved and the formation of stains is prevented. When the content of the second polyester polyol is less than the above range, there is a problem of stains occurring in the manufactured coating film, and when it exceeds the above range, the drying property of the composition is delayed and the gloss of the manufactured coating film increases, which may result in poor appearance properties.

[0072]

[0073] 3rd polyester polyol

[0074] The third polyester polyol serves to improve the appearance properties, adhesion, and weather resistance of the manufactured coating film.

[0075] The third polyester polyol may be synthesized directly using a known method, or a commercially available product may be used. For example, the third polyester polyol may be prepared by reacting a carboxylic acid compound with a polyol compound.

[0076] At this time, the carboxylic acid compound may be at least one selected from the group consisting of, for example, adipic acid (AA), isophthalic acid (IPA), trimaletic anhydride (TMA), alicyclic acids, phthalic anhydride, isophthalic acid, terephthalic acid, succinic acid, adipic acid, fumaric acid, maleic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, and derivatives thereof.

[0077] In addition, the polyol compound may be at least one selected from the group consisting of methoxypolyethylene glycol, 1,6-hexanediol (1,6-HD), neopentyl glycol (NPG), trimethylol propane (TMP), ethylene glycol, propylene glycol, diethylene glycol, butanediol 1,4-hexanediol, and 3-methylpentanediol.

[0078] The third polyester polyol may have a hydroxyl value (OHv) of 250 to 290 mgKOH / g, or 260 to 280 mgKOH / g. When the hydroxyl value of the third polyester polyol is within the above range, the manufactured coating film has excellent appearance characteristics and weather resistance. When the hydroxyl value of the third polyester polyol is outside the above range, the manufactured coating film may be stained or have insufficient weather resistance.

[0079] In addition, the third polyester polyol may have a weight average molecular weight (Mw) of 1,000 to 3,400 g / mol, or 1,000 to 2,000 g / mol. When the weight average molecular weight of the third polyester polyol is within the above range, the drying time of the paint is appropriate, so that workability is excellent, and the water resistance and weather resistance of the manufactured coating film are excellent. When the weight average molecular weight of the third polyester polyol is less than the above range, the drying time of the paint may be long, so that workability may be poor, and when it exceeds the above range, the manufactured coating film may be stained or have poor appearance characteristics.

[0080] The third polyester polyol may have an acid value (Av) of 10 to 30 mgKOH / g, or 17 to 27 mgKOH / g. When the acid value of the third polyester polyol is within the above range, rapid curing due to heat treatment is prevented, thereby preventing appearance defects of the coating film and reducing the formation of bubbles (popping). When the acid value of the third polyester polyol is below the above range, the appearance characteristics of the manufactured coating film are insufficient, and when it exceeds the above range, the water resistance and weather resistance of the manufactured coating film may be insufficient.

[0081] In addition, the third polyester polyol may have a solid content (NV) of 60 to 70 wt%, or 62 to 66 wt%, based on the total weight of the third polyester polyol. When the solid content of the third polyester polyol is within the above range, the composition has excellent storage stability and can be stored in a high solid content form without agglomeration or precipitation of the solid content. In addition, when the solid content of the third polyester polyol is less than the above range, there is a problem that the amount of use for other compositions that can be used is limited due to the low solid content and high solvent content, and when it exceeds the above range, the composition may have insufficient painting workability and storage stability due to the high viscosity.

[0082] The third polyester polyol may be included in the composition in an amount of 1 to 10 parts by weight, or 2 to 7 parts by weight, based on 20 to 30 parts by weight of the first acrylic polyol. When the third polyester polyol is included within the above content range, the appearance properties of the coating film, particularly the gloss properties, are improved and the formation of stains is prevented. When the content of the third polyester polyol is less than the above range, there is a problem of stains occurring in the manufactured coating film, and when it exceeds the above range, the drying property of the composition is delayed and the gloss of the manufactured coating film increases, which may result in poor appearance properties.

[0083]

[0084] Meanwhile, the transparent paint composition of the present invention may contain the first polyester polyol, the second polyester polyol, and the third polyester polyol in a total amount of 7 to 35 parts by weight, 12 to 27 parts by weight, or 18 to 25 parts by weight, based on 100 parts by weight of the total paint composition. When the total amount of the first polyester polyol, the second polyester polyol, and the third polyester polyol is within the above range, the appearance characteristics and adhesion of the manufactured coating film may be excellent, and the workability of the composition may be excellent. On the other hand, when the total amount of the first polyester polyol, the second polyester polyol, and the third polyester polyol is less than the above range, the solid content of the paint may be reduced, resulting in a lack of environmental friendliness or a problem in which the paintability, appearance characteristics, and paint workability of the manufactured coating film may be reduced, and when it exceeds the above range, the hardness, drying properties, and weather resistance of the manufactured coating film may be insufficient.

[0085] In addition, the transparent paint composition of the present invention may include the first polyester polyol and the second polyester polyol in a weight ratio of 1:0.1 to 1:2.0, or a weight ratio of 1:0.3 to 1:1.0. When the mixing weight ratio of the first polyester polyol and the second polyester polyol is within the above range, there is an effect of improving the paintability and chemical resistance of the manufactured coating film and improving the appearance characteristics. On the other hand, when the mixing weight ratio of the first polyester polyol and the second polyester polyol is less than the above range, that is, when a small amount of the second acrylic polyol is included with respect to the weight of the first polyester polyol, there is a problem that the paintability and appearance characteristics of the manufactured coating film are deteriorated, and when it exceeds the above range, that is, when an excessive amount of the second polyester polyol is included with respect to the weight of the first polyester polyol, there may occur a problem that the drying property of the composition and the chemical resistance of the manufactured coating film are deteriorated.

[0086] In addition, the transparent paint composition of the present invention may include the first polyester polyol and the third polyester polyol in a weight ratio of 1:0.1 to 1:0.9, or a weight ratio of 1:0.15 to 1:0.80. When the mixing weight ratio of the first polyester polyol and the third polyester polyol is within the above range, there is an effect of improving the paintability and chemical resistance of the manufactured coating film and improving the appearance characteristics. On the other hand, when the mixing weight ratio of the first polyester polyol and the third polyester polyol is less than the above range, that is, when a small amount of the third acrylic polyol is included with respect to the weight of the first polyester polyol, there is a problem that the paintability and appearance characteristics of the manufactured coating film are deteriorated, and when it exceeds the above range, that is, when an excessive amount of the third polyester polyol is included with respect to the weight of the first polyester polyol, there may occur a problem that the drying property of the composition and the chemical resistance of the manufactured coating film are deteriorated.

[0087]

[0088] isocyanate compounds

[0089] The above isocyanate compound acts as a curing agent, reacting with the hydroxyl groups of polyols to form a urethane bond, thereby curing the composition and forming a coating film.

[0090] In addition, the type of the isocyanate compound is not particularly limited as long as it can be applied as a curing agent in a typical urethane-based paint composition. For example, the isocyanate compound may include an aliphatic polyisocyanate compound that does not exhibit yellowing, and specifically, may include hexamethylene diisocyanate (HDI), isophorone diisocyanate, 4,4'-dicyclohexyl methane diisocyanate, tetramethyl xylene diisocyanate, or a mixture thereof.

[0091] The above isocyanate compound may have an unreacted isocyanate group content (NCO%) of 20 to 25 wt%, or 21 to 23 wt%, based on the total weight of the compound. If the NCO% of the isocyanate compound is less than the above range, the crosslinking density of the coating film may decrease, which may cause problems such as lowering the impact resistance, water resistance, and cold chipping resistance of the coating film. If it exceeds the above range, the curing speed may increase and the resin may aggregate, which may cause problems such as lowering the appearance characteristics, gloss, and mechanical properties of the coating film.

[0092] In addition, the isocyanate compound may be included in the composition in an amount of 15 to 25 parts by weight, or 18 to 22 parts by weight, based on 20 to 30 parts by weight of the first acrylic polyol. If the amount of the isocyanate compound is less than the above range, the composition may have insufficient reactivity, resulting in a decrease in crosslinking density and a decrease in mechanical properties. If the amount exceeds the above range, unreacted isocyanate groups may be generated in the coating film after curing, resulting in a decrease in the appearance and workability of the coating film.

[0093]

[0094] additives

[0095] The above transparent paint composition may further include one or more additives selected from the group consisting of ultraviolet absorbers, curing accelerators, surface conditioners, and solvents. In this case, the additives are not particularly limited as long as they can be typically added to paint compositions.

[0096] The above additive may be included in the composition in an amount of 15 to 40 parts by weight, or 20 to 30 parts by weight, based on 20 to 30 parts by weight of the first acrylic polyol.

[0097] The above transparent paint composition may have a solid content of 50 wt% or more, or 50 to 60 wt%.

[0098] Additionally, the transparent paint composition may have a volatile organic compound (VOC) content of 750 g / L or less, or 550 to 750 g / L.

[0099] The transparent paint composition according to the present invention, as described above, has a high solids content and a low volatile organic compound (VOC) content, making it environmentally friendly and exhibiting excellent painting workability. In addition, a coating film prepared from the transparent paint composition exhibits excellent water resistance, weather resistance, chemical resistance, and appearance properties, making it highly suitable as a paint for automotive parts, particularly for substrates made of non-polar materials such as polyolefin resins.

[0100] Hereinafter, the present invention will be described in more detail through examples. However, these examples are provided solely to aid understanding of the present invention and are not intended to limit the scope of the present invention in any way.

[0101]

[0102] [Example]

[0103] Experimental Examples 1 to 19. Preparation of transparent paint composition

[0104] A transparent paint composition was prepared by mixing ingredients in the amounts shown in Tables 1 to 4.

[0105]

[0106]

[0107]

[0108]

[0109]

[0110]

[0111]

[0112]

[0113] Below, the manufacturer and product name, or ingredient name, of each component used in the experimental example are shown in Table 5. Here, OHv is the hydroxyl value, Mw is the weight average molecular weight, NV is the solid content, Tg is the glass transition temperature, and Av is the acid value.

[0114]

[0115]

[0116] Test example. Evaluation of coating properties

[0117] An oil-based primer (manufacturer: KCC, product name: RP2143(H)) was applied onto a polypropylene material and dried at room temperature for 5 minutes to form a primer layer with a film thickness of approximately 10 μm. Thereafter, an oil-based base (manufacturer: KCC, product name: UT595(Y)) was applied onto the primer layer and dried at room temperature for 5 minutes to form a base layer with a film thickness of approximately 25 μm. Thereafter, a transparent paint composition of the experimental example was applied onto the base layer and dried at 80°C for 30 minutes to produce a transparent paint film with a film thickness of approximately 33 μm.

[0118] The painting workability of the transparent paint composition and the physical properties of the transparent paint film were measured as follows, and the results are shown in Table 6 below.

[0119] (1) Painting workability

[0120] The paint workability was evaluated by the paint film's thickness by applying a transparent paint composition twice back and forth on a tin plate measuring 30 cm wide × 40 cm long with 61 IWATA guns. Specifically, if the paint film's thickness was 38 ㎛ or more after leaving it at room temperature for 10 minutes after painting, it was evaluated as excellent (◎). If the paint film's thickness was 33 ㎛ or more and less than 38 ㎛, it was evaluated as good (○). If the paint film's thickness was 28 ㎛ or more and less than 33 ㎛, it was evaluated as average (△). If the paint film's thickness was less than 28 ㎛, it was evaluated as poor (×).

[0121] (2) Appearance

[0122] The appearance of the manufactured coating was measured using an appearance measuring device, Wave Scan DOI (BYK Gardner), for gloss (LU), clarity (SH), and orange peel (OP), and the measured properties were used to calculate the comprehensive appearance evaluation value (CF) using the following mathematical formula 1.

[0123] [Mathematical Formula 1]

[0124] CF = LU × 0.15 + SH × 0.35 + OP × 0.5

[0125] At this time, it was judged that the higher the CF value, the better the appearance characteristics of the coating film.

[0126] (3) Adhesion

[0127] According to the ASTM D3359 tape adhesion test method, 100 checkerboard grids measuring 2 mm wide × 2 mm long were drawn on the coating with a knife, and then peeling was evaluated after the tape adhesion test. Specifically, if there was no peeling along the straight line of the knife stroke, it was evaluated as excellent (◎), if less than 50% of one checkerboard grid was peeled, it was evaluated as good (○), if more than 50% but less than 90% of one checkerboard grid was peeled, it was evaluated as fair (△), and if more than 90% of one checkerboard grid was peeled, it was evaluated as poor (×).

[0128] (4) Water resistance

[0129] After immersing the coating in a 40℃ constant temperature bath for 10 days, the adhesion was evaluated using the same method as the adhesion in item (3). Specifically, if there were no bubbles on the surface of the coating and no breakage of the coating at the intersection of the cutting, it was evaluated as excellent (◎). If there were no bubbles on the surface of the coating but less than 50% of the area of ​​one checkerboard grid was peeled at the intersection of the cutting, it was evaluated as good (○). If bubbles occurred on the surface of the coating or more than 50% but less than 90% of the area of ​​one checkerboard grid was peeled at the intersection of the cutting, it was evaluated as average (△). If bubbles occurred on the surface of the coating and more than 90% of the area of ​​one checkerboard grid was peeled at the intersection of the cutting, it was evaluated as poor (×).

[0130] (5) Chemical resistance

[0131] A weight (diameter 4 cm) with a load of 4.9 N was wrapped in gauze, the gauze was sufficiently soaked with industrial acetone, and the surface of the coating was rubbed back and forth 10 times with the weight. Thereafter, the appearance of the coating was observed visually, left at room temperature for 1 hour, left in a constant temperature chamber at 80±2℃ for 3 hours, and then the surface condition of the coating was observed visually.

[0132] Specifically, if the Gray Scale is 5, it was evaluated as excellent (◎), if it is 4, it was evaluated as good (○), if it is 3, it was evaluated as average (△), and if it is 2 or lower, it was evaluated as poor (×).

[0133] (6) Weather resistance

[0134] The weathering resistance was evaluated by color difference after exposing the coating to a xenon weatherometer tester with an energy of 2500 kJ for 1,200 hours.

[0135] Specifically, when the color difference (△E) was 0.5 or less, it was evaluated as excellent (◎), when the color difference (△E) was more than 0.5 and less than 1.0, it was evaluated as good (○), when the color difference (△E) was more than 1.0 and less than 2.0, it was evaluated as average (△), and when the color difference (△E) was more than 2.0, it was evaluated as poor (×).

[0136]

[0137]

[0138] As shown in Table 6, the compositions of Experimental Examples 1 to 7 had excellent painting workability, and the coating films manufactured therefrom had excellent appearance, adhesion, water resistance, chemical resistance, and weather resistance.

[0139] Meanwhile, experimental examples 8 and 9, which contained a small amount of the first polyester polyol and an excessive amount of the second polyester polyol or the third polyester polyol, had poor painting workability of the composition and poor chemical resistance of the coating film.

[0140] In addition, Experimental Example 10, which includes a fourth polyester polyol having a high hydroxyl value instead of the second polyester polyol and a fifth polyester polyol having a low hydroxyl value and weight average molecular weight instead of the third polyester polyol, Experimental Example 11, which includes an excess of the second polyester polyol and includes the fifth polyester polyol and the sixth polyester polyol, Experimental Example 13, which includes a fourth polyester polyol having a high hydroxyl value instead of the first polyester polyol and a fifth polyester polyol having a low hydroxyl value and weight average molecular weight instead of the third polyester polyol, and Experimental Examples 14 and 15, which do not include the first acrylic polyol, had very poor painting workability of the composition, and very poor appearance and water resistance of the coating film. In particular, Experimental Example 11 had insufficient weather resistance of the coating, Experimental Example 14 had insufficient adhesion of the coating, and Experimental Example 15 had insufficient adhesion and weather resistance of the coating.

[0141] Experimental Example 12, which included an excess of a third polyester polyol, a sixth polyester polyol having a low hydroxyl value, and a seventh polyester polyol having a high hydroxyl value, Experimental Example 16, which included a third acrylic polyol having a low hydroxyl value, a sixth polyester polyol having a low hydroxyl value, and a seventh polyester polyol having a high hydroxyl value instead of the second acrylic polyol, and Experimental Example 17, which included a third acrylic polyol and a fourth acrylic polyol, a sixth polyester polyol having a low hydroxyl value, and a seventh polyester polyol having a high hydroxyl value instead of the first acrylic polyol and the second acrylic polyol, had poor paintability of the composition, and the appearance, adhesion, and weather resistance of the coating film were very poor.

[0142] In addition, experimental examples 18 and 19, which contained only one type of acrylic polyol and only one type of polyester polyol, had poor painting workability of the composition, and the appearance, adhesion, water resistance, chemical resistance, and weather resistance of the coating film were very poor.

Claims

1. Containing a first acrylic polyol, a second acrylic polyol, a first polyester polyol, a second polyester polyol, a third polyester polyol, and an isocyanate compound, The first acrylic polyol has a lower hydroxyl value and glass transition temperature than the second acrylic polyol, The first polyester polyol has a higher hydroxyl value and weight average molecular weight than the second polyester polyol, A transparent paint composition wherein the first polyester polyol has a lower hydroxyl value and a higher weight average molecular weight than the third polyester polyol.

2. In claim 1, The above first acrylic polyol has a hydroxyl value of 80 mgKOH / g to 100 mgKOH / g, a glass transition temperature of 30°C to 40°C, and a weight average molecular weight (Mw) of 2,000 g / mol to 3,500 g / mol. A transparent paint composition wherein the second acrylic polyol has a hydroxyl value of 101 mgKOH / g to 120 mgKOH / g, a glass transition temperature of 65°C to 80°C, and a weight average molecular weight (Mw) of more than 3,500 g / mol and less than or equal to 5,000 g / mol.

3. In claim 1, The above first polyester polyol has a hydroxyl value of 150 mgKOH / g to 200 mgKOH / g, a weight average molecular weight of 3,500 g / mol to 6,000 g / mol, and an acid value (Av) of 10 mgKOH / g to 30 mgKOH / g. The second polyester polyol has a hydroxyl value of 130 mgKOH / g to 149 mgKOH / g, a weight average molecular weight of 1,000 g / mol to 3,400 g / mol, and an acid value (Av) of 10 mgKOH / g to 30 mgKOH / g. A transparent paint composition wherein the third polyester polyol has a hydroxyl value of 250 mgKOH / g to 290 mgKOH / g, a weight average molecular weight of 1,000 g / mol to 3,400 g / mol, and an acid value (Av) of 10 mgKOH / g to 30 mgKOH / g.

4. In claim 1, A transparent paint composition comprising 20 to 30 parts by weight of a first acrylic polyol, 5 to 10 parts by weight of a second acrylic polyol, 5 to 15 parts by weight of a first polyester polyol, 1 to 10 parts by weight of a second polyester polyol, 1 to 10 parts by weight of a third polyester polyol, and 15 to 25 parts by weight of an isocyanate compound.

5. In claim 1, A transparent paint composition comprising the first acrylic polyol and the second acrylic polyol in a weight ratio of 2:1 to 6:

1.

6. In claim 1, A transparent paint composition comprising the first polyester polyol and the second polyester polyol in a weight ratio of 1:0.1 to 1:2.0, and the first polyester polyol and the third polyester polyol in a weight ratio of 1:0.1 to 1:0.9.

Citation Information

Patent Citations

  • Paint composition

    KR1020000041335A

  • A clear coat composition with antipollution

    KR1020160074319A

  • Transparent coating composition for prepairing automobile

    KR1020160113346A

  • Data recovery apparatus for USB memory

    KR102301761B1

  • Ball valve

    KR102302191B1