Catalyst for methane reforming and manufacturing method thereof

A highly dispersed nickel catalyst with aluminum and magnesium, produced via hydrothermal synthesis, addresses the instability and activity issues of traditional methane reforming catalysts by enhancing structural stability and suppressing sintering and coke deposition, resulting in improved catalytic performance and reaction efficiency.

WO2024225637A1PCT designated stage expired Publication Date: 2024-10-31HANWHA SOLUTIONS CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/004221
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-02
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Catalysts for methane reforming using carbon dioxide suffer from instability and low activity due to sintering and coke deposition, especially at high temperatures, and existing methods using noble metals are economically impractical.

Method used

A highly dispersed nickel catalyst with aluminum and magnesium, produced through hydrothermal synthesis, which achieves structural stability and suppresses sintering and coke deposition, maintaining catalytic performance during methane reforming reactions.

Benefits of technology

The catalyst exhibits excellent structural stability and catalytic performance, with a faster methane reforming reaction rate and reduced coke deposition, even at high temperatures, outperforming traditional Ni-MgO catalysts in terms of activity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024004221_31102024_PF_FP_ABST
    Figure KR2024004221_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a nickel catalyst and a manufacturing method thereof, and more specifically, to provide: a structurally stable, highly dispersed nickel catalyst that can be used in methane reforming reactions using carbon dioxide; and a manufacturing method thereof. Provided is a nickel catalyst containing highly dispersed nickel and having excellent structural stability during methane reforming reactions, thus exhibiting excellent catalytic performance in methane reforming reactions using carbon dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Catalyst for methane reforming and method for producing the same

[0001] Cross-citation with related application(s)

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0055932, filed April 28, 2023, the entire contents of which are incorporated herein by reference.

[0003]

[0004] The present invention relates to a catalyst for methane reforming and a method for producing the same. In particular, the present invention relates to a highly dispersed nickel catalyst with guaranteed structural stability that can be used in a methane reforming reaction utilizing carbon dioxide, and a method for producing the same.

[0005]

[0006] As rising atmospheric carbon dioxide concentrations pose various challenges, active efforts are being made to convert carbon dioxide into useful substances. Among these, methane reforming using carbon dioxide involves reacting carbon dioxide and methane with a catalyst at high temperatures to produce industrially useful synthesis gases, such as a mixture of hydrogen and carbon monoxide. This synthesis gas offers the advantage of being directly applicable to reactions that synthesize various chemicals or hydrocarbons. However, despite these advantages, the catalysts used for reforming are unstable and have low activity, making practical application difficult.

[0007] In addition, since the methane reforming reaction using carbon dioxide shows a higher conversion as the temperature increases, the reaction must be carried out at a high temperature to obtain a high-purity product. However, in general, when the catalyst is exposed to high temperatures for a long time, the active metal sinters, reducing the active surface, or carbon (e.g., coke), a side reaction product, covers the surface of the active metal, causing a decrease in activity over time. Therefore, a method of using precious metals to minimize side reactions and sintering has been considered, but for economic reasons, a catalyst that can replace precious metals is currently needed.

[0008] Accordingly, a method of manufacturing a catalyst by impregnating an MgO carrier with nickel and molybdenum as active materials was devised, but there are still problems of reduction in active surface area and coke deposition due to calcination.

[0009]

[0010] The present invention provides a catalyst for methane reforming and a method for producing the same. In particular, the present invention provides a highly dispersed nickel catalyst with guaranteed structural stability that can be used in methane reforming reactions utilizing carbon dioxide, and a method for producing the same.

[0011]

[0012] A catalyst of one embodiment of the present invention is a catalyst comprising Al, Ni and Mg, and the Al content may be 5 to 50 molar parts with respect to 100 molar parts of Mg.

[0013]

[0014] In addition, the method for producing a catalyst of one embodiment of the present invention includes a step (step 1) of producing an aqueous solution mixture by mixing MgO, a Ni precursor, and an Al precursor; a step (step 2) of hydrothermally synthesizing the mixture of step 1; and a step (step 3) of drying and calcining the hydrothermally synthesized composition of step 2; wherein in step 1, the Al precursor can be mixed in an amount such that the Al content is 5 to 50 molar parts with respect to 100 molar parts of Mg content.

[0015]

[0016] According to the present invention, a nickel catalyst can be provided that exhibits excellent catalytic performance by suppressing sintering and coke deposition in a methane reforming reaction utilizing carbon dioxide, as nickel is highly dispersed and excellent structural stability is achieved during a methane reforming reaction.

[0017]

[0018] Figure 1 illustrates the results of nitrogen adsorption analysis of Examples 1 to 4 of the present disclosure and Comparative Example 1.

[0019] Figure 2 shows the TEM image results after the methane reforming reaction of Example 3 and Comparative Example 1 of the present disclosure.

[0020] The terminology used herein is for the purpose of describing exemplary embodiments only and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly dictates otherwise.

[0021] In this specification, it should be understood that terms such as “include,” “comprising,” or “having” are intended to specify the presence of a feature, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, steps, components, or combinations thereof.

[0022] The present invention is susceptible to various modifications and takes various forms. Specific embodiments are illustrated and described in detail below. However, this is not intended to limit the present invention to specific disclosed forms, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.

[0023] Hereinafter, the present invention will be described in detail.

[0024]

[0025] Although Ni-MgO catalysts are known to have high activity in methane reforming reactions using existing carbon dioxide, there was a problem that deactivation occurred quickly due to sintering of metal particles and coke formation under high-temperature reaction conditions.

[0026] Accordingly, a method utilizing hydrothermal synthesis has been proposed. Ni-MgO catalysts manufactured using hydrothermal synthesis have the advantage of achieving high Ni dispersion and suppressing coke deposition during the reaction compared to catalysts manufactured through other synthetic methods (e.g., impregnation, coprecipitation, etc.). However, structural stability is still significantly reduced due to sintering of the MgO support under high-temperature reaction conditions.

[0027] To overcome this, we attempted to manufacture a catalyst with improved structural stability by introducing a double metal (Al) during the hydrothermal synthesis of a Ni-MgO catalyst. The catalyst of the present disclosure achieves superior structural stability during methane reforming compared to the previously known Ni-MgO (hydrothermal synthesis) and Ni-MgAl2O4 (co-precipitation) catalysts, and thus exhibits superior catalytic performance in methane reforming using carbon dioxide.

[0028]

[0029] The catalyst of the present disclosure is a catalyst comprising Al, Ni, and Mg, wherein the Al content may be 5 to 50 molar parts relative to 100 molar parts of Mg. Specifically, the Al content may be 5 molar parts or more, or 10 molar parts or more, to 50 molar parts or less, 40 molar parts or less, 30 molar parts or less, or 20 molar parts or less relative to 100 molar parts of Mg.

[0030] The Al (aluminum) content must satisfy the above range to ensure catalyst structural stability in the methane reforming reaction process to be achieved in the present disclosure, and aluminum can be highly dispersed in the carrier MgO lattice to form a solid solution.

[0031] Conventional methane reforming catalysts containing nickel (Ni) in alumina (Al2O3) have acid sites in the alumina, which can cause coke deposition on the catalyst surface during the reforming reaction, leading to a decrease in catalytic activity during the reaction. Excessive aluminum content can lead to the formation of Al2O3 crystal structures on the catalyst surface, which can promote coke formation during the reforming reaction, significantly reducing catalytic activity.

[0032]

[0033] The Mg (magnesium) in the above methane reforming catalyst may exist in the form of MgO (magnesium oxide) as a carrier. Specifically, the catalyst of one embodiment of the present invention may be in the form of Al and Ni dispersed on MgO at atomic levels.

[0034]

[0035] The Ni content may be 2 to 10 parts by weight relative to 100 parts by weight of the total catalyst for methane reforming. Specifically, the Ni content may be 2 parts by weight or more, 3 parts by weight or more, 4 parts by weight or more, or 5 parts by weight or more to 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, or 6 parts by weight or less relative to the total weight of the catalyst.

[0036] When the Ni (nickel) content satisfies the above range, nickel can be suppressed from forming excessively large particles and promoting coke formation, thereby preventing adverse effects on catalytic activity, and a sufficient amount of nickel active phase required for the methane reforming reaction can be secured.

[0037] If the Ni content is too excessive, nickel may form large particles, which may promote coke formation and significantly reduce catalytic activity. If the Ni content is too small, the amount of nickel active phase required for the reaction may be insufficient, which may result in a problem of catalytic activity not being secured.

[0038]

[0039] In addition, the catalyst of the present disclosure may have a balance of the carrier MgO, excluding the Al content and the Ni content, based on the total weight of the catalyst.

[0040] Specifically, the catalyst of the present disclosure may be a catalyst containing only Al (aluminum), Ni (nickel), and Mg (magnesium) as metal elements.

[0041]

[0042] In addition, in the case of existing methane reforming catalysts containing Ni (nickel) on an alumina (Al2O3) support, there is a problem that the alumina has acid points, which causes coke deposition on the catalyst surface during the reforming reaction, that is, coking, and thus the catalytic activity decreases during the reaction. However, the catalyst of the present disclosure does not contain alumina, but instead contains MgO. Compared to alumina, MgO has very few acid points, that is, it can be considered to have no acid points, and therefore, coking occurs relatively less, which has the advantage of maintaining catalytic activity. In addition, MgO has excellent basicity, so it has excellent adsorption of reactants, resulting in good reactivity. However, in the case of manufacturing using the existing impregnation method, there is a problem that the nickel dispersion is low and the surface area is small. Therefore, the present disclosure intends to provide a manufacturing method including a hydrothermal synthesis method.

[0043]

[0044] The above catalyst has a cumulative pore volume of 0.20 to 0.50 cm by using a nitrogen adsorption method. 3 / g. Specifically, the N2 adsorption cumulative pore volume is 0.20 cm 3 / g or more, 0.25 cm 3 / g or more, 0.27 cm 3 / g or more, or 0.28 cm 3 / g or more to 0.50 cm 3 / g or less, 0.45 cm 3 / g or less, 0.40 cm 3 / g or less, 0.35 cm 3 / g or less, or 0.30 cm 3 / g can be less.

[0045] The catalyst pore volume range must satisfy the above range to obtain a desired level of rapid methane reforming reaction rate and suppress deactivation due to coke formation.

[0046] Furthermore, the catalyst manufactured using the manufacturing method of the present invention has a larger pore volume than that manufactured using the existing impregnation method. That is, the catalyst of the present invention is expected to exhibit a faster reforming reaction rate than that manufactured using the impregnation method, as the surface area increases due to the formation of pores.

[0047]

[0048] The above catalyst may have a Ni nanoparticle size of 3.0 to 8.0 nm upon reduction. Since the catalyst of the present invention does not observe any crystallization of Ni when it goes through only the calcination step, the size of the nanoparticles can be observed by reducing it in a hydrogen atmosphere to confirm the structural stability before and after the methane reforming reaction. In the case of a catalyst manufactured by an impregnation method, the size of the Ni nanoparticles may be 10 to 50 nm.

[0049] When Ni forms large particles, this can promote coke formation during the reforming reaction, which can significantly reduce catalytic activity.

[0050] In the present invention, since Ni is highly dispersed on MgO in atomic units to achieve high efficiency, even when used in a methane reforming reaction utilizing high-temperature carbon dioxide, the catalyst does not sinter or coke is deposited on the catalyst surface, resulting in a decrease in catalytic efficiency.

[0051]

[0052] MgO raw material is mixed with Al precursor and Ni precursor in an aqueous solution state and reacts at high temperature to form pores.

[0053] As with the N2 adsorption cumulative pore volume, the BET specific surface area of ​​the hydrothermally synthesized catalyst using the nitrogen adsorption method is larger than that of the catalyst manufactured by the impregnation method, so the active sites of the catalyst are expected to increase and the reforming reaction rate is expected to be faster.

[0054] The above catalyst has a BET specific surface area of ​​100 to 200 m measured using a nitrogen adsorption method. 2 / g. This is in the same context as the formation of pores in the MgO raw material, resulting in a large cumulative pore volume for N2 adsorption.

[0055] Specifically, the specific surface area of ​​the above catalyst is 100 m 2 / g or more, 110 m 2 / g or more, 115 m 2 / g or more, 120 m 2 / g or more, 125 m 2 / g or more, or 130 m 2 / g or more to 200 m 2 / g or less, 190 m 2 / g or less, 180 m 2 / g or less, 170 m 2 / g or less, 160 m 2 / g or less or 155 m 2 / g can be less.

[0056] The above catalyst may be used in a methane reforming reaction using carbon dioxide. As described above, the catalyst according to one embodiment of the present invention has the advantages of a fast methane reforming process, a large throughput, no or little sintering of the catalyst as the reaction progresses, and a small amount of coke deposition, so that the catalytic efficiency does not decrease during the reaction when used in a methane reforming reaction using carbon dioxide that is carried out at a high temperature due to a high BET specific surface area resulting from the highly dispersed and porous structure of Ni.

[0057]

[0058] The methane reforming catalyst of the present invention has excellent structural stability by introducing a double metal (Al) during the hydrothermal synthesis of a Ni-MgO catalyst. Accordingly, compared to existing Ni-MgO catalysts manufactured by a hydrothermal synthesis method without introducing a double metal, the catalyst of the present invention with the introduction of a double metal (Al) has a smaller decrease in BET specific surface area and a smaller decrease in N2 adsorption cumulative pore volume before and after a 24-hour methane reforming reaction.

[0059] This is because aluminum (Al), a double metal, is highly dispersed in the carrier MgO lattice to form a solid solution, which increases the lattice energy compared to the existing Ni-MgO catalyst to which the double metal is not introduced, thereby improving the structural stability of the catalyst before and after the reforming reaction.

[0060]

[0061] In addition, one embodiment of the present invention provides a method for preparing a catalyst, comprising the steps of: preparing an aqueous solution by mixing MgO, a Ni precursor, and an Al precursor (step 1); hydrothermally synthesizing the mixture of step 1 (step 2); and drying and calcining the hydrothermally synthesized composition of step 2 (step 3).

[0062]

[0063] In the above step 1, the Al precursor can be mixed in an amount such that the Al content is 5 to 50 molar parts relative to 100 molar parts of the Mg content. That is, the Al precursor can be added in an amount such that the Al content in the final product, the catalyst, is in the range of 5 to 50 molar parts relative to 100 molar parts of the Mg content. Specifically, the Al precursor can be mixed in an amount such that the Al content is 5 molar parts or more, or 10 molar parts or more, or 50 molar parts or less, 40 molar parts or less, 30 molar parts or less, or 20 molar parts or less relative to 100 molar parts of the Mg content.

[0064] The Al (aluminum) precursor content must satisfy the above range to ensure catalyst structural stability in the methane reforming reaction process to be achieved in the present disclosure, and aluminum can be highly dispersed in the MgO lattice of the support to form a solid solution. If the aluminum content is too low, it is difficult to maintain MgO support stability before and after the methane reforming reaction, and if the aluminum content is too high, an uneven Al2O3 or MgAl2O4 crystal phase may be formed on the catalyst surface, which may promote coke formation during the reaction and lower the catalytic activity.

[0065]

[0066] In the above step 1, the Ni precursor can be mixed in an amount such that the Ni content is 2 to 10 parts by weight based on 100 parts by weight of the entire catalyst. That is, the Ni precursor can be added to the final product, the catalyst, in an amount such that the Ni content is 2 to 10 parts by weight based on 100 parts by weight of the entire catalyst. Specifically, the Ni precursor can be mixed in an amount such that the Ni content is 2 parts by weight or more, 3 parts by weight or more, 4 parts by weight or more, or 5 parts by weight or more, and 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, or 6 parts by weight or less based on 100 parts by weight of the entire catalyst.

[0067] The content of the Ni precursor must satisfy the above range so that nickel can form excessively large particles, thereby preventing coke formation and adverse effects on catalytic activity, and a sufficient amount of nickel active phase required for the methane reforming reaction can be secured.

[0068]

[0069] The Al precursor of the above step 1 may be at least one selected from the group consisting of Al(NO3)3·9H2O, AlCl3·xH2O, Al(OH)3·xH2O, Al2(SO4)3·xH2O, Al2(SO4)3, AlNH4(SO4)2·12H2O, AlCl3·6H2O, AlCl3, AlBr3, AlO4P, AlI3, AlF3, Al(OH)3, Al2(SO4)3, Al2S3, AlN, Al(C5H7O2)3, Al(OC2H5)3, and Al[OCH(CH3)2]3. Specifically, the Al precursor of the step 1 may be Al(NO3)3·9H2O.

[0070]

[0071] The Ni precursor of the above step 1 may be at least one selected from the group consisting of Ni(CH3COO)2·4H2O), NiCl2, NiCl2·6H2O, Ni(NO3)2, NiSO4, (NH4)2Ni(SO4)2·6H2O, NiBr2, NiCO3, NiF2, NiI2, NiC2O4·2H2O and Ni(ClO4)2·6H2O. Specifically, the Ni precursor of the step 1 may be Ni(CH3COO)2·4H2O).

[0072]

[0073] The hydrothermal synthesis in step 2 can be carried out at a temperature of 100 to 300°C for 12 to 48 hours. Specifically, the hydrothermal synthesis can be carried out at a temperature of 100°C or higher, 110°C or higher, 120°C or higher, or 150°C or higher to 300°C or lower, 250°C or lower, or 200°C or lower.

[0074] Hydrothermal synthesis is a method of synthesizing a material using an aqueous solution under high temperature and high pressure. It is a single crystal synthesis method that depends on the solubility of the material, and performs material synthesis through heat treatment at a temperature higher than the boiling point of a commonly used solvent. Hydrothermal synthesis is a method that can be adopted to produce a solid solution in which Ni is uniformly dispersed on MgO, as in the present invention, because the particles are highly dispersed in the solution. In the present invention, in the synthesis step, a mixture of MgO and an aqueous solution of Ni precursor reacts, so that Ni is highly dispersed on MgO to form a solid solution, and MgO forms pores to increase the BET specific surface area.

[0075] Specifically, the hydrothermal synthesis of the present invention can be carried out at a temperature of 120 to 200°C for 22 to 26 hours.

[0076]

[0077] The mixture synthesized in step 2 can undergo the drying and calcination steps of step 3.

[0078] Drying in step 3 can be carried out at 50 to 150°C for 2 to 24 hours, specifically at 70 to 110°C for 10 to 16 hours.

[0079] The firing in step 3 above can be performed at 600 to 1000°C for 2 to 6 hours, specifically at 700 to 900°C for 3 to 5 hours.

[0080]

[0081] As described in the catalyst section above, the method for manufacturing the catalyst of the present invention uses a hydrothermal synthesis method, and thus, compared to an impregnation method such as a prior art, the manufactured catalyst is characterized in that the catalyst does not undergo calcination even in a high-temperature reforming reaction, there is no coke deposition on the surface, and the catalytic activity is maintained, and structural stability is maintained even when a methane reforming reaction is performed.

[0082]

[0083] Hereinafter, the present invention will be described in more detail with reference to the following experimental examples. However, the following experimental examples are intended only to illustrate the present invention and the scope of the present invention is not limited to these examples.

[0084]

[0085] [Experimental Example]

[0086]

[0087] <Example 1>

[0088] An attempt was made to prepare a Ni-Al-MgO catalyst using Ni, Al precursors and MgO raw materials.

[0089] First, 4 g of magnesium oxide [MgO] was added to 140 mL of distilled water and stirred (500 rpm) at room temperature to prepare an MgO aqueous solution.

[0090] At the same time, 0.893 g of nickel acetate tetrahydrate [Ni(CH3COO)2·4H2O], which has a Ni content of 5 parts by weight per 100 parts by weight of the total catalyst, was added to 20 mL of distilled water and stirred to dissolve, thereby preparing a Ni precursor aqueous solution.

[0091] Next, 1.899 g of aluminum nitrate nonahydrate [Al(NO3)3·9H2O] was added to the Ni precursor aqueous solution so that the Al content was 5 mol parts per 100 mol parts of Mg in the catalyst, and stirred to dissolve.

[0092]

[0093] Afterwards, Ni and Al precursor solutions were added dropwise to the stirred MgO suspension using a pipette and stirred at the same speed at room temperature for 2 hours. After stirring, the suspension was subjected to hydrothermal synthesis at 200°C for 24 hours in a Teflon-lined autoclave.

[0094] The suspension obtained thereafter was filtered and washed four times using distilled water through a filter device, and then dried at 100°C for 12 hours to remove moisture.

[0095] The dried sample was calcined in an air atmosphere at 800°C (heating rate: 2°C / min) for 4 hours.

[0096]

[0097] <Example 2>

[0098] The same method as Example 1 was performed except that 3.799 g of aluminum nitrate nonahydrate [Al(NO3)3·9H2O] was used so that the Al content was 10 mol parts per 100 mol parts of Mg in the catalyst.

[0099]

[0100]

[0101] <Example 3>

[0102] The same method as Example 1 was performed except that 7.598 g of aluminum nitrate nonahydrate [Al(NO3)3·9H2O] was used so that the Al content was 20 molar parts per 100 molar parts of Mg in the catalyst.

[0103]

[0104] <Example 4>

[0105] The same method as Example 1 was performed except that 11.398 g of aluminum nitrate nonahydrate [Al(NO3)3·9H2O] was used so that the Al content was 30 mol parts per 100 mol parts of Mg in the catalyst.

[0106]

[0107] <Comparative Example 1>

[0108] The same method as Example 1 was performed except that aluminum nitrate nonahydrate [Al(NO3)3·9H2O] was not used.

[0109]

[0110] <Comparative Example 2>

[0111] In a different manner from the examples, a Ni-MgAl2O4 spinel catalyst was prepared using a co-precipitation method as follows. 0.478 g of nickel nitrate hexahydrate [Ni(NO3)2·6H2O], 3.84 g of magnesium nitrate hexahydrate [Mg(NO3)2·6H2O], and 10 g of aluminum nitrate nonahydrate [Al(NO3)3·9H2O] were added to 200 mL of distilled water and stirred to dissolve such that the Ni content was 5 parts by weight per 100 parts by weight of the total catalyst, and the Al content was 200 parts by mol per 100 parts by mol of Mg. Thereafter, ammonia water [NH4OH] was added dropwise to the stirred solution using a pipette until the pH reached 10. The precipitated sample was filtered, dried, and calcined in the same manner as in Example 1.

[0112]

[0113] <Comparative Example 3>

[0114] In a different method from Comparative Example 2, a Ni-MgAl2O4 catalyst was prepared using the impregnation method as follows. 0.979 g of nickel nitrate hexahydrate [Ni(NO3)2·6H2O] was added to 0.5 mL of distilled water so that the Ni content was 5 parts by weight based on 100 parts by weight of the total catalyst, and sonication was performed to dissolve it until a transparent dark green solution was obtained. Thereafter, the Ni precursor solution was immersed in 4 g of MgAl2O4 using the impregnation method, and the immersed sample was dried and calcined in the same manner as in Example 1.

[0115]

[0116] Experimental Example 1

[0117] To determine the specific surface area and pore structure of the examples and comparative examples, nitrogen adsorption analysis was performed using a Tristar 2 3020 instrument. Prior to nitrogen adsorption analysis, the samples were pretreated in a vacuum at 150°C for 8 hours.

[0118] The BET surface area was calculated using the following equation: 0.15 from the graph of Adsorbed amout(v) / P / P0(A). <A<0.3 범위에서 y 축을 1 / v(1-A), x축을 A로 plot 했을 때 기울기가 1 / vm이다. vm은 촉매의 표면을 덮는 N2분자의 부피이다. N2분자 하나당 0.162 nm를 차지하며, BET 비표면적 S는 S=(vm x N x s) / mv와 같고, N은 아보가드로 숫자(6.02*10 23 ), s is 0.162 nm 2 (crosssection area), mv is the volume per mole of gas molecules (molar volume).

[0119]

[0120] The N2 adsorption cumulative volume, i.e., the total pore volume, was calculated using the following equation. When the Adsorbed amount value of the part where the value of P / P0(A) is 0.99 is B, the pore volume was calculated as B x density per mass of liquid nitrogen / molar volume x Avogadro's number.

[0121] The BET specific surface area and N2 adsorption cumulative volume values ​​are shown in Table 1 below.

[0122]

[0123] Experimental Example 2

[0124] To confirm the activity and stability of the examples and comparative examples, a methane reforming reaction using carbon dioxide was performed. Specifically, first, 0.08 g of catalyst particles (200-300 μm) were placed in a cylindrical quartz reactor (inner diameter: 10 mm), and the temperature was raised to 800°C (heating rate: 10°C / min) in a 100% hydrogen atmosphere for catalyst reduction. After that, the hydrogen atmosphere was maintained for 2 hours, purging was performed in a nitrogen atmosphere for 30 minutes, and then the methane-carbon dioxide mixed gas concentration was 90% of the total feed gas flow rate, and nitrogen gas, which was the internal standard gas, was injected together with the mixture gas (45.5 kPa CH4; 45.5 kPa CO2; 9.1 kPa N2). The GHSV (Gas Hourly Space Velocity) was fixed at 60 L / gh based on the reactants, and then the methane reforming reaction using carbon dioxide was performed for 24 hours. The products (H2, CO) and residual reactants (CH4, CO2) were quantified through gas chromatography (GC) equipped with a TCD detector and a carboxen-1000 column, and are shown in Table 1 below.

[0125] Methane reforming reaction using carbon dioxide was performed for 24 hours at a temperature of 800℃. The CH4 and CO2 treatment rates were calculated using the equation (treatment rate = GHSV x reactant concentration x conversion rate). After 24 hours of reaction, the amount of coke deposition on the catalyst was measured using elemental analysis.

[0126]

[0127] Division Unit Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Ni content (relative to 100 parts by weight of the entire catalyst) Weight parts 5 5 5 5 5 5 Al content (relative to 100 parts by mole of Mg) Mole parts 5 1 0 2 0 3 0 0 2 0 2 0 CH 4 treatment rate (initial reaction, 0 h) L / g · h 2 5.0 2 5.1 2 5.0 2 4.9 2 4.6 2 4.5 2 3.8 CO 2 treatment rate (initial reaction, 0 h) L / g · h 2 5.6 2 5.7 2 5.9 2 5.8 2 4.8 2 4.8 2 4.0 CH 4 treatment rate (after 24 h reaction) L / g · h 2 5.1 2 5.2 2 5.3 2 5.0 2 4.4 2 4.2 2 3.5 CO 2 treatment rate (24 h reaction) After)L / g·h25.725.826.025.924.724.923.7Total CH4 treatment amountL / g601.2603.6603.6598.8588.0584.4567.6Total CO-2 treatment amountL / g615.6618.0622.8620.4594.0596.4572.4BET ​​specific surface area (before reaction)m 2 / g118133152128917953Total pore volume (before reaction)cm 3 / g0.2770.2560.2970.2740.1650.1470.115BET specific surface area (after 24 h reaction)m 2 / g82919884487139Total pore volume (after 24 h reaction)cm 3 / g0.1580.1740.1960.1410.0760.1310.101Ni crystallite size (before 24 h reaction, after hydrogen reduction)nm5.15.05.15.25.311.810.7Ni crystallite size (after 24 h reaction)nm10.49.88.511.314.312.520.3Coke production (after 24 h reaction)wt%0.840.750.620.810.911.142.51

[0128] As a result of the reaction progress for 24 hours, the CH4 treatment rate after 24 hours in the example was 25.0 to 25.3 L / g·h, and the CO2 treatment rate was 25.7 to 26.0 L / g·h, showing higher activity than the comparative example. In addition, the coke production amount after 24 hours in the example was 0.6 to 0.8 wt%, and a smaller amount of coke was deposited than in the comparative example.

[0129] The BET surface area of ​​the example is 110 to 160 m 2 / g, and the N2 adsorption cumulative volume, i.e., the total pore volume, is 0.25 to 0.30 cm 3 It was confirmed that a wider specific surface area and larger pores were formed than in the comparative example. After the methane reforming reaction at 800 ℃ for 24 hours, the BET specific surface area of ​​the example was 80 to 100 m 2 / g, and the N2 adsorption cumulative volume, i.e., the total pore volume, is 0.14 to 0.20 cm 3 / g It was confirmed that a wider surface area and larger pores were maintained than the comparative example.

[0130] In addition, in the TEM image after the reaction, Ni nanoparticles with a size of 8 to 12 nm were observed, which is smaller than that of the comparative example. Specifically, when comparing the examples in which the double metal Al was introduced with the comparative example 1 in which the double metal was not introduced, it was confirmed that the size of the Ni nanoparticles before the modification reaction and after the reaction increased by about 60 to 120%, but the size of the Ni nanoparticles after the modification reaction of the comparative example 1 increased by about 180% compared to before the reaction.

[0131] As a result, it was confirmed that Examples 1 to 4 enabled higher activity and structural stability compared to the comparative examples.

Claims

1. A catalyst containing Al, Ni and Mg, With respect to 100 mol parts of Mg, the Al content is 5 mol parts to 50 mol parts, Catalyst for methane reforming.

2. In paragraph 1, In the above methane reforming catalyst, Mg exists in the form of MgO as a carrier. Catalyst for methane reforming.

3. In paragraph 1, The Ni content is 2 to 10 parts by weight based on 100 parts by weight of the total methane reforming catalyst. Catalyst for methane reforming.

4. In paragraph 1, The above methane reforming catalyst has a BET surface area of ​​100 m using nitrogen adsorption method. 2 / g to 200 m 2 / g person, Catalyst for methane reforming.

5. In paragraph 1, The above methane reforming catalyst has a cumulative pore volume of 0.20 cm for N2 adsorption using a nitrogen adsorption method. 3 / g to 0.50 cm 3 / g person, Catalyst for methane reforming.

6. In paragraph 1, The above catalyst is used in a methane reforming reaction using carbon dioxide. Catalyst for methane reforming.

7. Step of preparing an aqueous solution mixture by mixing MgO, Ni precursor and Al precursor (Step 1); A step of synthesizing the mixture of step 1 above (step 2); and A step of drying and calcining the composition synthesized in the above step 2 (step 3); Including, In the above step 1, the Al precursor is mixed in an amount such that the Al content is 5 to 50 mol parts per 100 mol parts of Mg content. Method for producing a catalyst for methane reforming.

8. In paragraph 7, In the above step 1, the Ni precursor is mixed in an amount such that the Ni content is 2 to 10 parts by weight based on 100 parts by weight of the total catalyst for methane reforming. Method for producing a catalyst for methane reforming.

9. In paragraph 7, The Al precursor of the above step 1 is at least one selected from the group consisting of Al(NO3)3·9H2O, AlCl3·xH2O, Al(OH)3·xH2O, Al2(SO4)3·xH2O, Al2(SO4)3, AlNH4(SO4)2·12H2O, AlCl3·6H2O, AlCl3, AlBr3, AlO4P, AlI3, AlF3, Al(OH)3, Al2(SO4)3, Al2S3, AlN, Al(C5H7O2)3, Al(OC2H5)3, and Al[OCH(CH3)2]3. Method for producing a catalyst for methane reforming.

10. In paragraph 7, The Ni precursor of the above step 1 is at least one selected from the group consisting of Ni(CH3COO)2·4H2O), NiCl2, NiCl2·6H2O, Ni(NO3)2, NiSO4, (NH4)2Ni(SO4)2·6H2O, NiBr2, NiCO3, NiF2, NiI2, NiC2O4·2H2O and Ni(ClO4)2·6H2O. Method for producing a catalyst for methane reforming.

11. In paragraph 7, The hydrothermal synthesis in step 2 is carried out at a temperature of 100 to 300°C for 12 to 48 hours. Method for producing a catalyst for methane reforming.

12. In paragraph 7, The drying in step 3 above is carried out at 50 to 150°C for 2 to 24 hours. Method for producing a catalyst for methane reforming.

13. In paragraph 7, The firing of the above step 3 is carried out at 600 to 1000℃ for 2 to 6 hours. Method for producing a catalyst for methane reforming.

Citation Information

Patent Citations

  • Composite Oxide Catalyst for Oxidizing Methane and Method for Preparing the Same

    KR101759183B1

  • Wearable Device and Control Method thereof

    KR1020200108725A

  • Supported nickel-magnesium oxide catalysts and processes for the production of syngas