Optical film having low yellowness index change and display device comprising same
The use of a specific polymerizable composition in optical films, including bistrifluoromethylbenzidine and sulfone-based diamine monomers, addresses the issue of yellowness change at high temperatures, ensuring stable optical properties and mechanical integrity for display devices.
Patent Information
- Application Number
- PCT/KR2024/004469
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-05
- Publication Date
- 2024-10-31
AI Technical Summary
Optical films used as cover windows or TFT substrates in display devices face challenges in maintaining excellent optical properties, particularly low yellowness change, at high temperatures due to heat treatment, which affects their mechanical and thermal stability.
A polymerizable composition comprising a diamine monomer, such as bistrifluoromethylbenzidine, bis(3-aminophenyl)sulfone, and bis(4-aminophenyl)sulfone, along with a dianhydride and dicarbonyl compound, is used to create an optical film with controlled molecular structure and packing, inhibiting yellowness increase at high temperatures, while maintaining mechanical and thermal stability.
The optical film exhibits a yellowness change of 1 or less and high light transmittance, ensuring excellent optical properties and resistance to high-temperature treatments, thereby maintaining transparency and display quality over time.
Smart Images

Figure KR2024004469_31102024_PF_FP_ABST
Abstract
Description
Optical film having low yellowness change and display device including the same
[0001] The present invention relates to an optical film having low yellowness change and a display device including the same.
[0002] Polyimide (PI) resins have insolubility, chemical resistance, heat resistance, radiation resistance, and excellent mechanical strength, and are used as automotive materials, aviation materials, spacecraft materials, insulating coatings, insulating films, and protective films.
[0003] Recently, due to the trend toward thinner, lighter, and more flexible display devices, research is underway to utilize optical films for cover windows or TFT substrates. For optical films to be used as cover windows or TFT substrates in display devices, they must possess excellent mechanical and optical properties.
[0004] In particular, the change in yellowness should be small so that excellent optical properties can be maintained even during high-temperature processing.
[0005] One embodiment of the present invention seeks to provide an optical film having low yellowness.
[0006] One embodiment of the present invention seeks to provide an optical film having low yellowness at high temperatures.
[0007] One embodiment of the present invention is to provide an optical film in which yellowness increase is prevented or suppressed at high temperatures.
[0008] One embodiment of the present invention is to provide an optical film having low yellowness change after high-temperature heat treatment.
[0009] One embodiment of the present invention is to provide an optical film having excellent haze.
[0010] One embodiment of the present invention seeks to provide an optical film having excellent light transmittance.
[0011] To solve the above-mentioned problem, the present invention may include the following configuration.
[0012] One embodiment of the present invention provides an optical film prepared from a polymerizable composition comprising a diamine monomer and at least one of a dianhydride compound and a dicarbonyl compound, and having a yellowness change (△YI) of 1 or less based on a thickness of 50 μm. Here, the yellowness change is calculated from the following equation 1.
[0013] [Formula 1]
[0014] △YI =│YI(300℃) - YI(270℃)│
[0015] In the above formula 1, the YI (300°C) is the yellowness (YI) of the optical film measured after cooling to room temperature following heat treatment at 300°C for 10 minutes, and the YI (270°C) is the yellowness (YI) of the optical film measured after cooling to room temperature following heat treatment at 270°C for 10 minutes.
[0016] The above diamine monomer may include bistrifluoromethylbenzidine (TFDB), bis(3-aminophenyl)sulfone (3DDS), and bis(4-aminophenyl)sulfone (4DDS).
[0017] The content of the above bis(3-aminophenyl)sulfone (3DDS) may be less than the content of bistrifluoromethylbenzidine (TFDB) and greater than the content of bis(4-aminophenyl)sulfone (4DDS).
[0018] With respect to the total mole number of the above diamine monomer, the content of the bis(3-aminophenyl)sulfone (3DDS) may be 30 mol% or less and the content of the bis(4-aminophenyl)sulfone (4DDS) may be 10 mol% or less.
[0019] With respect to the total mole number of the above diamine monomer, the content of the bis trifluoromethylbenzidine (TFDB) may be 65 to 80 mol%, the content of the bis (3-aminophenyl) sulfone (3DDS) may be 15 to 25 mol%, and the content of the bis (4-aminophenyl) sulfone (4DDS) may be 5 to 10 mol%.
[0020] The polymerizable composition may include the dianhydride compound and the dicarbonyl compound.
[0021] The molar ratio of the above dianhydride compound and the above dicarbonyl compound may be in the range of 20:80 to 2:98.
[0022] The above dianhydride compounds are 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FDA), 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride (TDA), pyromellitic acid dianhydride (1,2,4,5-Benzene tetracarboxylic dianhydride, Pyromellicticacid dianhydride, PMDA), benzophenone tetracarboxylic dianhydride (3,3,4,4-Benzophenone tetracarboxylic dianhydride, BTDA), biphenyl tetracarboxylic dianhydride (3,3,4,4-Biphenyltetracarboxylic dianhydride, BPDA), naphthalenetetracarboxylic dianhydride (NTDA), diphenylsulfonetetracarboxylic dianhydride Among 4,4-Oxydiphthalic dianhydride (ODPA), Bis(3,4-dicarboxyphenyl)dimethyl-silane dianhydride (SiDA), Bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride (BDSDA), Sulfonyldiphthalic anhydride (SO2DPA), Cyclobutane-1,2,3,4-tetracarboxylic dianhydride (CBDA), and Isopropylidenediphenoxy bis phthalic anhydride (4,4'-(4,4'-Isopropylidenediphenoxy)bis(phthalic anhydride, BPADA) It can contain at least one.
[0023] The above dicarbonyl compound may include at least one of phthaloyl chloride, terephthaloyl chloride (TPC), isophthaloyl chloride (IPC), 4,4'-Biphenyldicarbonyl chloride (DPDOC), 4,4'-Oxybis(benzoyl chloride) (OBBOC), and naphthalene-2,3-dicarbonyl dichloride.
[0024] The above optical film may have a haze of 1.0 or less based on a thickness of 50㎛.
[0025] The above optical film can have a light transmittance of 88% or more based on a thickness of 50㎛.
[0026] Another embodiment of the present invention provides a display device including a display panel and the optical film disposed on the display panel.
[0027] An optical film according to one embodiment of the present invention has a low yellowness change, so that the transmittance of the optical film does not decrease even at high temperatures and excellent transparency can be maintained.
[0028] A display device including an optical film according to one embodiment of the present invention has excellent display quality and can maintain excellent display quality even when used for a long period of time.
[0029] FIG. 1 is a cross-sectional view of a portion of a display device according to another embodiment of the present invention.
[0030] Figure 2 is an enlarged cross-sectional view of portion “P” of Figure 1.
[0031] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. However, the embodiments described below are presented for illustrative purposes only to facilitate a clear understanding of the present invention and do not limit the scope of the present invention.
[0032] The shapes, sizes, ratios, angles, numbers, etc. disclosed in the drawings for explaining embodiments of the present invention are merely illustrative, and the present invention is not limited to the details depicted in the drawings. Throughout the specification, identical components may be designated by identical reference numerals. In describing the present invention, detailed descriptions of related known technologies will be omitted if they are deemed to unnecessarily obscure the gist of the present invention.
[0033] In this specification, where "includes," "has," and "consists of" are used, other parts may be added, unless the expression "only" is used. When a component is expressed in the singular, the plural is included unless otherwise explicitly stated. Furthermore, when interpreting a component, it is interpreted to include a margin of error even if there is no explicit indication otherwise.
[0034] When describing a positional relationship, for example, when the positional relationship between two parts is described as 'on top of', 'upper part of', 'lower part of', 'next to', etc., one or more other parts may be located between the two parts, unless the expression 'right' or 'directly' is used.
[0035] Spatially relative terms such as "below," "beneath," "lower," "above," and "upper" can be used to easily describe the relationship of one element or component to another, as illustrated in the drawings. Spatially relative terms should be understood to include different orientations of the elements during use or operation in addition to the orientations depicted in the drawings. For example, if an element depicted in the drawings were flipped over, an element described as "below" or "beneath" another element could end up being placed "above" the other element. Thus, the exemplary term "below" can encompass both the above and below directions. Similarly, the exemplary term "above" or "above" can encompass both the above and below directions.
[0036] When describing a temporal relationship, for example, when the temporal relationship is described as 'after', 'following', 'next to', 'before', etc., it can also include cases where it is not continuous, as long as the expression 'immediately' or 'directly' is not used.
[0037] While terms like "first" and "second" are used to describe various components, these components are not limited by these terms. These terms are used merely to distinguish one component from another. Therefore, a "first" component referred to below may also be a "second" component within the technical scope of the present invention.
[0038] The term "at least one" should be understood to include all possible combinations of one or more associated items. For example, "at least one of the first, second, and third items" can mean not only the first, second, or third items, but also any combination of items that can be represented by two or more of the first, second, and third items.
[0039] The individual features of the various embodiments of the present invention can be partially or wholly combined or combined with each other, and various technical linkages are possible.
[0040] The present invention can be modified in various ways and has various embodiments. Hereinafter, specific embodiments will be described in detail based on the attached drawings.
[0041] One embodiment of the present invention provides an optical film (100). The optical film (100) according to one embodiment of the present invention includes a polymer resin.
[0042] An optical film (100) according to one embodiment of the present invention may include at least one of an imide repeating unit and an amide repeating unit. For example, an optical film (100) according to one embodiment of the present invention may include at least one of a polyimide-based polymer, a polyamide-based polymer, and a polyamide-imide-based polymer.
[0043] An optical film (100) according to one embodiment of the present invention may include an imide repeating unit formed by a diamine monomer and a dianhydride compound.
[0044] An optical film (100) according to one embodiment of the present invention may include an amide repeating unit formed by a diamine monomer and a dicarbonyl compound.
[0045] An optical film (100) according to one embodiment of the present invention may include both amide repeating units and imide repeating units formed by a diamine monomer, a dianhydride compound, and a dicarbonyl compound.
[0046] An optical film (100) according to one embodiment of the present invention can be manufactured from a polymerizable composition.
[0047] An optical film (100) according to one embodiment of the present invention can be manufactured from at least one polymerizable composition among, for example, a polyimide polymerizable composition, a polyamide polymerizable composition, and a polyamide-imide polymerizable composition.
[0048] An optical film (100) according to one embodiment of the present invention may be any one of a polyimide-based film, a polyamide-based film, and a polyamide-imide-based film. However, the present invention is not limited thereto, and any film having light transmittance may be the optical film (100) according to one embodiment of the present invention.
[0049] A polymerizable composition for producing an optical film may include a diamine monomer. In addition, the polymerizable composition for producing an optical film may include at least one of a dianhydride compound and a dicarbonyl compound.
[0050] During the formation of an optical film, packing between polymer chains can cause the optical film to exhibit a yellow tint. The higher the heat treatment temperature, the higher the yellowness of the optical film. Furthermore, the higher the degree of packing between polymer chains, the higher the yellowness of the optical film.
[0051] Depending on the type of diamine monomer, the degree of packing of the polymer chain may vary. According to one embodiment of the present invention, the polymerizable composition for manufacturing an optical film (100) may include one or more diamine monomers. In addition, according to one embodiment of the present invention, the polymerizable monomer for manufacturing an optical film (100) may include two or more diamine monomers, and may also include three or more diamine monomers.
[0052] According to one embodiment of the present invention, the diamine monomer may include, for example, bistrifluoromethylbenzidine (TFDB), bis(3-aminophenyl)sulfone (3DDS), and bis(4-aminophenyl)sulfone (4DDS).
[0053] According to one embodiment of the present invention, when three or more types of diamine monomers are used, various combinations can be formed, thereby increasing the irregularity of the molecular structure. Furthermore, as the irregularity of the molecular structure increases, the packing of polymer chains at high temperatures can be inhibited or suppressed. Accordingly, the effect of not significantly changing the yellowness of the optical film (100) even at high temperatures can be achieved.
[0054] According to one embodiment of the present invention, the diamine monomer may include bistrifluoromethylbenzidine (TFDB), bis(3-aminophenyl)sulfone (3DDS), and bis(4-aminophenyl)sulfone (4DDS).
[0055] The content of bis-trifluoromethylbenzidine (TFDB) may be 60 mol% or more based on the total mole number of diamine monomers. When the content of bis-trifluoromethylbenzidine (TFDB) is less than 60 mol%, the yellowness of the optical film may increase. Specifically, the content of bis-trifluoromethylbenzidine (TFDB) may be 65 to 80 mol% based on the total mole number of diamine monomers.
[0056] Bis(3-aminophenyl)sulfone (3DDS) and bis(4-aminophenyl)sulfone (4DDS) have a folded structure. When at least one of bis(3-aminophenyl)sulfone (3DDS) and bis(4-aminophenyl)sulfone (4DDS) is used to form a polymer chain, packing of the polymer chain is inhibited or suppressed, so that an increase in yellowness of the optical film (100) at high temperatures can be inhibited or prevented.
[0057] As the length of the polymer chain constituting the optical film (100) increases, the mechanical properties or heat resistance of the optical film (100) may deteriorate. Therefore, in terms of mechanical properties or heat resistance, a polymer chain with a short length is required.
[0058] When forming a polymer chain, the length of bis(3-aminophenyl)sulfone (3DDS) is shorter than that of bis(4-aminophenyl)sulfone (4DDS). Therefore, in order to secure the mechanical properties or heat resistance of the optical film (100) according to one embodiment of the present invention, the content of bis(3-aminophenyl)sulfone (3DDS) may be greater than that of bis(4-aminophenyl)sulfone (4DDS).
[0059] According to one embodiment of the present invention, for example, the content of bis(3-aminophenyl)sulfone (3DDS) may be less than the content of bistrifluoromethylbenzidine (TFDB) and greater than the content of bis(4-aminophenyl)sulfone (4DDS).
[0060] According to one embodiment of the present invention, there is no particular limitation on the content of bis(3-aminophenyl)sulfone (3DDS) and the content of bis(4-aminophenyl)sulfone (4DDS), but the content of bis(3-aminophenyl)sulfone (3DDS) is set to be greater than the content of bis(4-aminophenyl)sulfone (4DDS).
[0061] With respect to the total mole number of diamine monomers, the content of bis(3-aminophenyl)sulfone (3DDS) may be 30 mol% or less. When the content of bis(3-aminophenyl)sulfone (3DDS) exceeds 30 mol%, the content of bistrifluoromethylbenzidine (TFDB) with respect to the total mole number of diamine monomers decreases, and thus the thermal stability or optical properties of the optical film (100) according to one embodiment of the present invention may deteriorate.
[0062] Specifically, the content of bis(3-aminophenyl)sulfone (3DDS) may be 10 to 30 mol% based on the total number of moles of diamine monomers. More specifically, the content of bis(3-aminophenyl)sulfone (3DDS) may be 15 to 25 mol% based on the total number of moles of diamine monomers.
[0063] The content of bis(4-aminophenyl)sulfone (4DDS) may be 10 mol% or less based on the total mole number of diamine monomers. When the content of bis(4-aminophenyl)sulfone (4DDS) exceeds 10 mol%, the length of the polymer chain may increase, thereby deteriorating the mechanical properties or heat resistance of the optical film according to one embodiment of the present invention.
[0064] Specifically, the content of bis(4-aminophenyl)sulfone (4DDS) may be 2 to 10 mol% based on the total number of moles of diamine monomers. More specifically, the content of bis(4-aminophenyl)sulfone (4DDS) may be 5 to 10 mol% based on the total number of moles of diamine monomers.
[0065] A polymerizable composition according to one embodiment of the present invention may include both a dianhydride compound and a dicarbonyl compound.
[0066] According to one embodiment of the present invention, the molar ratio of the dianhydride compound and the dicarbonyl compound of the polymerizable composition may be, for example, in the range of 20:80 to 2:98. More specifically, the molar ratio of the dianhydride compound and the dicarbonyl compound of the polymerizable composition may be in the range of 10:90 to 2:98.
[0067] According to one embodiment of the present invention, the total equivalents of the dianhydride compound and the dicarbonyl compound and the equivalents of the diamine monomer may be substantially the same.
[0068] Dianhydride compounds include 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FDA), 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride (TDA), pyromellitic acid dianhydride (1,2,4,5-Benzene tetracarboxylic dianhydride, Pyromellicticacid dianhydride, PMDA), benzophenone tetracarboxylic dianhydride (3,3,4,4-Benzophenone tetracarboxylic dianhydride, BTDA), biphenyl tetracarboxylic dianhydride (3,3,4,4-Biphenyltetracarboxylic dianhydride, BPDA), naphthalenetetracarboxylic dianhydride (NTDA), diphenylsulfonetetracarboxylic dianhydride Among 4,4-Oxydiphthalic dianhydride (ODPA), Bis(3,4-dicarboxyphenyl)dimethyl-silane dianhydride (SiDA), Bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride (BDSDA), Sulfonyldiphthalic anhydride (SO2DPA), Cyclobutane-1,2,3,4-tetracarboxylic dianhydride (CBDA), and Isopropylidenediphenoxy bis phthalic anhydride (4,4'-(4,4'-Isopropylidenediphenoxy)bis(phthalic anhydride, BPADA) It can contain at least one.
[0069] Dicarbonyl compounds possess a benzene ring, which allows them to exhibit high thermal stability and mechanical properties. However, this characteristic also leads to high birefringence values. However, when bistrifluoromethylbenzidine (TFDB) is used as a diamine monomer, thermal stability and optical properties can be improved. Furthermore, when the contents of the dianhydride compound, dicarbonyl compound, and diamine monomer are controlled within appropriate ranges during polymerization, thermal stability, mechanical properties, and optical properties can be balanced and improved.
[0070] According to one embodiment of the present invention, the dicarbonyl compound of the polymerizable composition may include at least one of phthaloyl chloride, terephthaloyl chloride (TPC), isophthaloyl chloride (IPC), 4,4'-biphenyldicarbonyl chloride (DPDOC), 4,4'-oxybis(benzoyl chloride) (OBBOC), and naphthalene-2,3-dicarbonyl dichloride.
[0071] An optical film (100) according to one embodiment of the present invention may have a yellowness of 5 or less, for example, based on a thickness of 50 μm. More specifically, the optical film (100) may have a yellowness of 3 or less based on a thickness of 50 μm.
[0072] An optical film (100) according to one embodiment of the present invention may have a yellowness change (△YI) of 1 or less based on a thickness of 50 μm.
[0073] The above yellowness change (△YI) is calculated from the following equation 1.
[0074] [Formula 1]
[0075] △YI =│YI(300℃) - YI(270℃)│
[0076] In the above equation 1, YI(300℃) is the yellowness (YI) of the optical film (100) measured after cooling to room temperature following a heat treatment at 300℃ for 10 minutes, and YI(270℃) is the yellowness (YI) of the optical film (100) measured after cooling to room temperature following a heat treatment at 270℃ for 10 minutes. According to one embodiment of the present invention, the yellowness change (△YI) can be calculated from the absolute value of the difference between YI(300℃) and YI(270℃) (│YI(300℃) - YI(270℃)│).
[0077] The yellowness for calculating the above yellowness change (△YI) can be measured by a spectrophotometer according to the standard specification ASTM E313. As a spectrophotometer, for example, CM-3700D from KONICA MINOLTA can be used.
[0078] According to one embodiment of the present invention, the temperature for measuring the yellowness change of the optical film (100) was set to 270°C and 300°C. 270°C corresponds to a temperature at which the solvent used in manufacturing the optical film can be sufficiently removed. 300°C corresponds to a temperature that can be applied in the manufacturing process of other products using the optical film (100). For example, a temperature of approximately 300°C can be applied in the TFT manufacturing process.
[0079] An optical film (100) according to one embodiment of the present invention may have a yellowness change (△YI) of 0.8 or less based on a thickness of, for example, 50 μm.
[0080] An optical film (100) according to one embodiment of the present invention may have a haze of 1.0 or less. The haze according to one embodiment of the present invention is measured before heat-treating the optical film (100).
[0081] Haze can be measured using a haze meter according to the standard ASTM D1003. For example, the HM-150 from MURAKAMI can be used as a haze meter.
[0082] An optical film (100) according to one embodiment of the present invention may have, for example, a haze of 0.7 or less.
[0083] An optical film (100) according to one embodiment of the present invention may have a light transmittance of 88% or more based on a thickness of 50 μm. The light transmittance of the optical film (100) according to one embodiment of the present invention is measured before heat-treating the optical film (100).
[0084] Light transmittance can be measured over a wavelength range of 360 to 740 nm using a spectrophotometer according to the standard ASTM E313. For example, the CM-3700D from KONICA MINOLTA can be used as a spectrophotometer.
[0085] Hereinafter, a method for manufacturing an optical film (100) according to one embodiment of the present invention will be described.
[0086] A method for manufacturing an optical film (100) according to one embodiment of the present invention includes the steps of forming a first reaction solution using a diamine monomer and a dianhydride compound, adding a dicarbonyl compound to the first reaction solution and reacting it to form a second reaction solution, adding a dehydrating agent and an imidization catalyst to the second reaction solution and reacting it to form a third reaction solution, treating the third reaction solution to produce a solid-state polymer resin, dissolving the solid-state polymer resin to produce a polymer resin solution, and casting the polymer resin solution. Hereinafter, each step will be described in detail.
[0087] First, a first reaction solution is formed using a diamine monomer and a dianhydride compound.
[0088] As a solvent for preparing the first reaction solution, for example, an aprotic polar organic solvent such as dimethylacetamide (DMAc, N,N-dimethylacetamide), dimethylformamide (DMF, N,N-dimethylformamide), methylpyrrolidone (NMP, 1-methyl-2-pyrrolidinone), m-cresol, tetrahydrofuran (THF, tetrahydrofuran), chloroform, methyl ethyl ketone (MEK), and mixtures thereof may be used. However, the solvent according to one embodiment of the present invention is not limited thereto, and other solvents may be used.
[0089] The above diamine monomers may include bistrifluoromethylbenzidine (TFDB), bis(3-aminophenyl)sulfone (3DDS), and bis(4-aminophenyl)sulfone (4DDS).
[0090] However, the diamine monomer according to one embodiment of the present invention is not limited thereto, and other diamine monomers may be used.
[0091] With respect to the total mole number of diamine monomers, the content of bis(3-aminophenyl)sulfone (3DDS) may be 30 mol% or less, and the content of bis(4-aminophenyl)sulfone (4DDS) may be 10 mol% or less.
[0092] More specifically, with respect to the total mole number of diamine monomers, the content of bis trifluoromethylbenzidine (TFDB) may be 65 to 80 mol%, the content of bis (3-aminophenyl) sulfone (3DDS) may be 15 to 25 mol%, and the content of bis (4-aminophenyl) sulfone (4DDS) may be 5 to 10 mol%.
[0093] Dianhydride compounds include 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FDA), 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride (TDA), pyromellictic acid dianhydride (1,2,4,5-benzene tetracarboxylic dianhydride, pyromellicticacid dianhydride, PMDA), benzophenone tetracarboxylic dianhydride (3,3,4,4-Benzophenone tetracarboxylic dianhydride, BTDA), biphenyl tetracarboxylic dianhydride (3,3,4,4-Biphenyltetracarboxylic dianhydride, BPDA), naphthalenetetracarboxylic dianhydride (NTDA), diphenylsulfonetetracarboxylic dianhydride Among 4,4-Oxydiphthalic dianhydride (ODPA), Bis(3,4-dicarboxyphenyl)dimethyl-silane dianhydride (SiDA), Bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride (BDSDA), Sulfonyldiphthalic anhydride (SO2DPA), Cyclobutane-1,2,3,4-tetracarboxylic dianhydride (CBDA), and Isopropylidenediphenoxy bis phthalic anhydride (4,4'-(4,4'-Isopropylidenediphenoxy)bis(phthalic anhydride, BPADA) At least one may be included.
[0094] However, the dianhydride compound according to one embodiment of the present invention is not limited thereto, and other dianhydride compounds may be used.
[0095] According to one embodiment of the present invention, the first reaction solution may include polyamic acid and polyimide repeating units.
[0096] Next, a dicarbonyl compound is added to the first reaction solution and reacted to form a second reaction solution. For example, the dicarbonyl compound may be added to the first reaction solution 1 to 24 hours after the formation of the first reaction solution. More specifically, the dicarbonyl compound may be added to the first reaction solution 1 to 20 hours after the formation of the first reaction solution.
[0097] According to one embodiment of the present invention, when a dicarbonyl compound is added to the first reaction solution, the reaction solution is called a second reaction solution.
[0098] The above dicarbonyl compound may include at least one of phthaloyl chloride, terephthaloyl chloride (TPC), isophthaloyl chloride (IPC), 4,4'-biphenyldicarbonyl chloride (DPDOC), 4,4'-oxybis(benzoyl chloride) (OBBOC), and naphthalene-2,3-dicarbonyl dichloride.
[0099] However, the dicarbonyl compound according to one embodiment of the present invention is not limited thereto, and other dicarbonyl compounds may be used.
[0100] According to one embodiment of the present invention, the molar ratio of the dianhydride compound and the dicarbonyl compound may be in the range of 20:80 to 2:98.
[0101] Next, a dehydrating agent and an imidization catalyst are added to the second reaction solution and reacted to form a third reaction solution.
[0102] According to one embodiment of the present invention, after a dehydrating agent and an imidization catalyst are added to the second reaction solution, reflux stirring is performed at a temperature of 60°C to 80°C for 30 minutes to 2 hours. As a result, a third reaction solution can be formed.
[0103] As a dehydrating agent, acid anhydrides such as acetic anhydride, propionic anhydride, isobutyric anhydride, pivalic anhydride, butyric anhydride, and isovaleric anhydride can be used.
[0104] Tertiary amines such as isoquinoline, β-picoline, and pyridine can be used as imidization catalysts.
[0105] Next, the third reaction solution is processed to produce a solid polymer resin.
[0106] To produce a solid polymer resin, a solvent may be added to the third reaction solution. Examples of solvents that can be used include ethanol, methanol, hexane, and the like. The solvent may be used alone, or two or more types may be mixed.
[0107] When a solvent that mixes well with the polymerization solvent and has low solubility in the polymer resin is added to the third reaction solution, a powdered solid polymer resin precipitates. The precipitate can be filtered and dried to obtain a high-purity solid polymer resin. When the liquid components are removed during the filtering process, unreacted monomers, oligomers, additives, and reaction byproducts can also be removed.
[0108] The polymer resin thus obtained is in a solid powder state and may contain imide repeating units and amide repeating units. The polymer resin may be, for example, a polyamide-imide resin.
[0109] Next, the solid polymer resin is dissolved to produce a polymer resin solution. The step of dissolving the solid polymer resin in a solvent to produce a polymer resin solution is also called the re-dissolution step.
[0110] As a solvent for dissolving the solid-state polymer resin, the same solvents as those used in the polymerization process can be used. For example, aprotic polar organic solvents such as dimethylacetamide (DMAc, N,N-dimethylacetamide), dimethylformamide (DMF, N,N-dimethylformamide), methylpyrrolidone (NMP, 1-methyl-2-pyrrolidinone), m-cresol, tetrahydrofuran (THF, tetrahydrofuran), chloroform, methyl ethyl ketone (MEK), and mixtures thereof can be used as a solvent for dissolving the solid-state polymer resin.
[0111] However, the solvent according to one embodiment of the present invention is not limited thereto, and other known solvents may be used.
[0112] Next, the polymer resin solution is cast.
[0113] A casting substrate is used for casting. There are no specific limitations on the type of casting substrate. Examples of casting substrates that can be used include glass substrates, aluminum substrates, stainless steel (SUS) substrates, and Teflon substrates. According to one embodiment of the present invention, for example, a glass substrate can be used as the casting substrate.
[0114] Specifically, casting is performed by applying a polymer resin solution to a casting substrate. A coater, blade, or the like may be used for casting. According to one embodiment of the present invention, for example, a Baker Film Applicator may be used for casting.
[0115] After casting the polymer resin solution, drying at a temperature ranging from 80°C to 120°C can produce a polymer resin coating film. The coating film produced in this manner can be considered an intermediate for an optical film. After the coating film is tautly stretched and fixed on a pin-shaped tenter, additional heat treatment can be performed.
[0116] There are no specific limitations on the additional heat treatment conditions for the coating film, but the heat treatment may be performed at a temperature of, for example, 200°C or higher. The heat treatment temperature may be, for example, 200°C, 220°C, 240°C, 270°C, or 300°C.
[0117] Additionally, the additional heat treatment may be performed in an isothermal atmosphere where the heat treatment temperature is maintained constant, or in a variable temperature atmosphere where the heat treatment temperature is gradually increased or decreased.
[0118] The heat treatment time may vary depending on the need and may be performed for, for example, one minute or more. The heat treatment time may be performed for, for example, one minute, three minutes, five minutes, ten minutes, or twenty minutes.
[0119] According to one embodiment of the present invention, an additional heat treatment may be performed for, for example, 10 minutes in an isothermal atmosphere of 270°C. As a result, an optical film (100) according to one embodiment of the present invention may be manufactured.
[0120] An optical film (100) according to one embodiment of the present invention can be applied to a display device to protect the display surface of a display panel (501).
[0121] The optical film (100) according to one embodiment of the present invention may have a thickness sufficient to protect the display panel (501). For example, the optical film (100) may have a thickness of 10 to 100 μm.
[0122] Hereinafter, with reference to FIGS. 1 and 2, a display device (200) using an optical film (100) according to one embodiment of the present invention will be described.
[0123] FIG. 1 is a cross-sectional view of a portion of a display device (200) according to another embodiment of the present invention, and FIG. 2 is an enlarged cross-sectional view of a portion “P” of FIG. 1.
[0124] Referring to FIG. 1, a display device (200) according to another embodiment of the present invention includes a display panel (501) and an optical film (100) on the display panel (501).
[0125] Referring to FIGS. 1 and 2, the display panel (501) includes a substrate (510), a thin film transistor (TFT) on the substrate (510), and an organic light-emitting element (570) connected to the thin film transistor (TFT). The organic light-emitting element (570) includes a first electrode (571), an organic light-emitting layer (572) on the first electrode (571), and a second electrode (573) on the organic light-emitting layer (572). The display device (200) disclosed in FIGS. 1 and 2 is an organic light-emitting display device.
[0126] The substrate (510) may be made of glass or plastic. Specifically, the substrate (510) may be made of plastic such as a polyimide-based resin. Although not shown, a buffer layer may be disposed on the substrate (510).
[0127] A thin film transistor (TFT) is disposed on a substrate (510). The thin film transistor (TFT) includes a semiconductor layer (520), a gate electrode (530) that is insulated from the semiconductor layer (520) and overlaps at least a portion of the semiconductor layer (520), a source electrode (541) connected to the semiconductor layer (520), and a drain electrode (542) that is spaced apart from the source electrode (541) and connected to the semiconductor layer (520).
[0128] Referring to FIG. 3, a gate insulating film (535) is disposed between a gate electrode (530) and a semiconductor layer (520). An interlayer insulating film (551) may be disposed on the gate electrode (530), and a source electrode (541) and a source electrode (541) may be disposed on the interlayer insulating film (551).
[0129] A planarization film (552) is placed on a thin film transistor (TFT) to planarize the upper portion of the thin film transistor (TFT).
[0130] The first electrode (571) is placed on the planarization film (552). The first electrode (571) is connected to a thin film transistor (TFT) through a contact hole provided in the planarization film (552).
[0131] The bank layer (580) is disposed on a portion of the first electrode (571) and the planarization film (552) to define a pixel area or a light-emitting area. For example, the bank layer (580) may be disposed in a matrix structure in a boundary area between a plurality of pixels, thereby defining a pixel area by the bank layer (580).
[0132] The organic light-emitting layer (572) is disposed on the first electrode (571). The organic light-emitting layer (572) may also be disposed on the bank layer (580). The organic light-emitting layer (572) may include one light-emitting layer, or may include two or more light-emitting layers stacked one above the other. Light having any one of red, green, and blue colors may be emitted from the organic light-emitting layer (572), and white light may also be emitted.
[0133] The second electrode (573) is placed on the organic light-emitting layer (572).
[0134] A first electrode (571), an organic light-emitting layer (572), and a second electrode (573) can be laminated to form an organic light-emitting element (570).
[0135] Although not shown, when the organic light-emitting layer (572) emits white light, each pixel may include a color filter for filtering the white light emitted from the organic light-emitting layer (572) by wavelength. The color filter is formed on the path of light.
[0136] A thin film encapsulation layer (590) may be disposed on the second electrode (573). The thin film encapsulation layer (590) may include at least one organic film and at least one inorganic film, and at least one organic film and at least one inorganic film may be disposed alternately.
[0137] An optical film (100) is placed on a display panel (501) having the laminated structure described above.
[0138] Hereinafter, the present invention will be described through more specific examples and comparative examples. However, the following examples are provided solely to aid understanding of the present invention and are not intended to limit the scope of the present invention.
[0139] <Example 1>
[0140] While passing nitrogen through a 500 ml reactor equipped with a stirrer, nitrogen injection device, dropping funnel, temperature controller, and condenser, 313.34 g of N,N-dimethylacetamide (DMAc) was charged, and 24.02 g (0.075 mol) of bistrifluoromethylbenzidine (TFDB), an aromatic diamine, was slowly added and dissolved. Then, 4.97 g (0.020 mol) of bis(3-aminophenyl)sulfone (3DDS) and 1.24 g (0.005 mol) of bis(4-aminophenyl)sulfone (4DDS) were additionally added and dissolved.
[0141] After the diamine was dissolved, 0.89 g (0.002 mol) of 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FDA), a dianhydride compound, was added and stirred for 2 hours. [Formation of the first reaction solution]
[0142] Afterwards, 19.90 g (0.098 mol) of terephthaloyl chloride (TPC) was added at 10°C or lower and reacted for 1 hour. [Formation of the second reaction solution]
[0143] After the polymerization reaction was completed, the second reaction solution was warmed to room temperature, and then 0.35 g of pyridine and 0.45 g of acetic anhydride, corresponding to 2.2 times the mole number of the introduced dianhydride compound, were added and stirred at 80°C for 30 minutes. [Formation of the third reaction solution]
[0144] The flask was cooled to room temperature, and an excess of methanol was added dropwise to the third reaction solution to induce precipitation. The precipitate was filtered and dried using a vacuum filter to obtain a white solid polymer resin. The obtained polymer resin is in the form of a solid powder.
[0145] The polymer resin in a solid powder state obtained in this way was redissolved in N,N-dimethylacetamide (DMAc) to obtain a polymer resin solution having a solid concentration of 14 wt%.
[0146] The above solution was cast onto a glass plate. Specifically, the polymer resin solution was applied to the glass plate using a Baker Film Applicator, and dried for 20 minutes with hot air at 80°C and 20 minutes at 120°C to form a coating film.
[0147] After the above primary drying, it was peeled off from the glass plate and fixed to a pin frame. This was then dried a second time with hot air in an isothermal atmosphere at 270°C for 10 minutes, thereby producing an optical film with a thickness of 50 μm.
[0148] <Examples 2 and 3>
[0149] According to the conditions of Table 1 below, optical films according to Examples 2 and 3 were manufactured by applying the method disclosed in Example 1.
[0150] <Comparative Examples 1 and 2>
[0151] According to the conditions of Table 1 below, optical films according to Comparative Examples 1 and 2 were manufactured by applying the method disclosed in Example 1.
[0152] Classification Diamine Monomer (mol%) Dianhydride Compound (mol%) Dicarbonyl Compound (mol%) TFDB3DDS4DDS6FDABPDATPC Example 175 mol% 20 mol% 5 mol% 2 mol% - 98 mol% Example 270 mol% 20 mol% 10 mol% 2 mol% - 98 mol% Example 375 mol% 20 mol% 5 mol% - 10 mol% 90 mol% Comparative Example 180 mol% - 20 mol% - 100 mol% Comparative Example 260 mol% - 40 mol% - 100 mol%
[0153] The physical properties of the optical films manufactured in Examples 1 to 3 and Comparative Examples 1 and 2 were measured as follows.
[0154] (1) Light transmittance (TT) (%)
[0155] The optical transmittance (TT) of the 50 μm thick optical films manufactured in Examples 1 to 3 and Comparative Examples 1 and 2 at a wavelength of 360 to 740 nm was measured using a spectrophotometer (CM-3700D, KONICA MINOLTA) according to the standard specification ASTM E313.
[0156] (2) Yellowness (YI)
[0157] The yellowness index (YI) of the 50 μm thick optical films manufactured in Examples 1 to 3 and Comparative Examples 1 and 2 was measured using a spectrophotometer (CM-3700D, KONICA MINOLTA) according to the standard ASTM E313.
[0158] (3) Change in yellowness (△YI)
[0159] The yellowness (YI) after heat treatment at 270°C and the yellowness (YI) after heat treatment at 300°C of the 50 μm thick optical films manufactured in Examples 1 to 3 and Comparative Examples 1 and 2 were compared to obtain the yellowness change (△YI) value.
[0160] Specifically, the 50 μm thick optical films manufactured in Examples 1 to 3 and Comparative Examples 1 and 2 were each heat-treated at 270°C for 10 minutes, then cooled to room temperature and the yellowness was measured. This was referred to as YI (270°C).
[0161] The optical films manufactured in Examples 1 to 3 and Comparative Examples 1 and 2 were each heat-treated at 300°C for 10 minutes, then cooled to room temperature and the yellowness was measured. This was referred to as YI (300°C).
[0162] Using the yellowness (YI) values measured after heat treatment above, the change in yellowness (△YI) was calculated according to Equation 1 below.
[0163] [Formula 1]
[0164] △YI = │YI(300℃) - YI(270℃)│
[0165] (4) Haze
[0166] According to the standard specification ASTM D1003, using a Haze Meter (HM-150, MURAKAMI Co., Ltd.), optical film samples of 50 mm X 50 mm size were prepared using the 50 μm thick optical films manufactured in Examples 1 to 3 and Comparative Examples 1 and 2, and then the haze for each optical film sample was measured.
[0167] The measurement results are shown in Table 2 below.
[0168] Classification TT (%) YI (270℃) YI (300℃) △ YI Haze (%) Example 188.73 1.96 2.74 0.78 0.3 Example 288.79 1.5 1 1.85 0.3 4 0.3 Example 388.26 3.5 0 4.2 1 0.6 2 0.6 Comparative Example 188.5 6 4.0 8 5.9 2 1.84 0.5 Comparative Example 288.70 3.0 2 5.0 3 2.0 1 0.3
[0169] As disclosed in the measurement results in Table 2, the optical films according to Examples 1 to 3 of the present invention have excellent light transmittance and excellent haze, and have low yellowness and low yellowness change even after high-temperature treatment, confirming that they have excellent resistance to high temperatures.
[0170] On the other hand, the optical films according to Comparative Examples 1 and 2 had high yellowness and high yellowness change after high-temperature treatment, confirming that they lacked resistance to high temperatures.
[0171] The above description is merely an illustrative illustration of the technical idea of the present invention, and those skilled in the art will appreciate that various modifications and variations can be made without departing from the essential characteristics of the present invention. Furthermore, the embodiments disclosed in the present invention are intended to illustrate, rather than limit, the technical idea of the present invention, and the scope of the technical idea of the present invention is not limited by these embodiments. Therefore, the scope of protection of the present invention should be interpreted by the claims, and all technical ideas within a scope equivalent thereto should be interpreted as being included within the scope of the rights of the present invention.
[0172] [Explanation of symbols]
[0173] 100: Optical Film
[0174] 200: Display device
[0175] 501: Display panel
Claims
1. Diamine monomer; and At least one of a dianhydride compound and a dicarbonyl compound; is prepared from a polymerizable composition comprising: An optical film having a yellowness change (△YI) of 1 or less based on a thickness of 50㎛: Here, the change in yellowness is calculated from the following equation 1: [Formula 1] △YI = │YI(300℃) - YI(270℃)│ In the above formula 1, the YI (300°C) is the yellowness (YI) of the optical film measured after cooling to room temperature following heat treatment at 300°C for 10 minutes, and the YI (270°C) is the yellowness (YI) of the optical film measured after cooling to room temperature following heat treatment at 270°C for 10 minutes.
2. In paragraph 1, An optical film, wherein the above diamine monomer comprises bistrifluoromethylbenzidine (TFDB), bis(3-aminophenyl)sulfone (3DDS), and bis(4-aminophenyl)sulfone (4DDS).
3. In paragraph 2, An optical film wherein the content of bis(3-aminophenyl)sulfone (3DDS) is less than that of bistrifluoromethylbenzidine (TFDB) and greater than that of bis(4-aminophenyl)sulfone (4DDS).
4. In paragraph 2, For the total moles of the above diamine monomer, The content of the above bis(3-aminophenyl)sulfone (3DDS) is 30 mol% or less, An optical film having a content of the above bis(4-aminophenyl)sulfone (4DDS) of 10 mol% or less.
5. In paragraph 2, For the total moles of the above diamine monomer, The content of the above bistrifluoromethylbenzidine (TFDB) is 65 to 80 mol%, The content of the above bis(3-aminophenyl)sulfone (3DDS) is 15 to 25 mol%, An optical film having a content of the above bis(4-aminophenyl)sulfone (4DDS) of 5 to 10 mol%.
6. In paragraph 1, An optical film, wherein the polymerizable composition comprises the dianhydride compound and the dicarbonyl compound.
7. In paragraph 6, An optical film wherein the molar ratio of the dianhydride compound and the dicarbonyl compound is in the range of 20:80 to 2:
98.
8. In paragraph 1, The above dianhydride compounds are 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FDA), 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride (TDA), pyromellitic acid dianhydride (1,2,4,5-Benzene tetracarboxylic dianhydride, Pyromellicticacid dianhydride, PMDA), benzophenone tetracarboxylic dianhydride (3,3,4,4-Benzophenone tetracarboxylic dianhydride, BTDA), biphenyl tetracarboxylic dianhydride (3,3,4,4-Biphenyltetracarboxylic dianhydride, BPDA), naphthalenetetracarboxylic dianhydride (NTDA), diphenylsulfonetetracarboxylic dianhydride Among 4,4-Oxydiphthalic dianhydride (ODPA), Bis(3,4-dicarboxyphenyl)dimethyl-silane dianhydride (SiDA), Bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride (BDSDA), Sulfonyldiphthalic anhydride (SO2DPA), Cyclobutane-1,2,3,4-tetracarboxylic dianhydride (CBDA), and Isopropylidenediphenoxy bis phthalic anhydride (4,4'-(4,4'-Isopropylidenediphenoxy)bis(phthalic anhydride, BPADA) An optical film comprising at least one.
9. In paragraph 1, An optical film, wherein the dicarbonyl compound comprises at least one of phthaloyl chloride, terephthaloyl chloride (TPC), isophthaloyl chloride (IPC), 4,4'-biphenyldicarbonyl chloride (DPDOC), 4,4'-oxybis(benzoyl chloride) (OBBOC), and naphthalene-2,3-dicarbonyl dichloride.
10. In paragraph 1, An optical film having a haze of 1.0 or less based on a thickness of 50㎛.
11. In paragraph 1, An optical film having a light transmittance of 88% or more based on a thickness of 50㎛.
12. Display panel; and An optical film according to any one of claims 1 to 11, disposed on the display panel; A display device including:
Citation Information
Patent Citations
Colorless and transparent polyamide-imide film and its manufacturing method
JP2019513887A
High strength transparent polyamide-imide and process for preparing same
KR1020170132459A
Electric brake system
KR1020200109430A
Rocket propulsion system
KR1020240019531A
KR20220092774A