Cathode active material powder having core-shell structure and method for producing same

The core-shell structured positive electrode active material powder with a uniformly coated oxide protective film addresses the issue of battery performance deterioration by stabilizing the cathode active material, enhancing ion conductivity and lifespan, and improving electrical conductivity.

WO2024225845A1PCT designated stage expired Publication Date: 2024-10-31ALPES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005788
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-29
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing methods for stabilizing cathode active materials in batteries face challenges with side reactions at the electrode-electrolyte interface, leading to battery performance deterioration, particularly due to non-uniform and high-temperature-dependent protective film coatings on electrode plates, which are not effective for all-solid-state batteries.

Method used

A core-shell structured positive electrode active material powder is developed with a uniformly coated, highly ionic conductive oxide protective film of controlled thickness (0.1-10 nm) on the surface of the active material powder, ensuring mechanical and electrochemical stability, high uniformity, and improved ion conductivity.

Benefits of technology

The solution significantly enhances battery lifespan and performance by suppressing interfacial side reactions, improving electrical conductivity, and maintaining excellent capacity retention through precise control of the protective film's composition and thickness, resulting in superior physical and chemical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005788_31102024_PF_FP_ABST
    Figure KR2024005788_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a cathode active material powder having a core-shell structure and a method for producing same and, more specifically, to: a cathode active material powder having a core-shell structure of which physical properties are excellent and which is stabilized due to the formation of a protective film by uniformly depositing an atomic layer of a mechanically and electrochemically stable compound on the surface of a cathode active material powder; and a method for producing same. The present invention provides a cathode active material powder having a core-shell structure, in which, by controlling production process conditions and the total number of iterations of an ALD process, the thickness of the protective film formed on the particle surface of the cathode active material powder can be adjusted enabling the thickness of the protective film to be very small and uniformity thereof to be excellent and thus interfacial side reactions are inhibited and electrical conductivity is excellent, mechanical and electrochemical stability is obtained and when applied in batteries, the capacity and lifespan thereof can be substantially improved.
Need to check novelty before this filing date? Find Prior Art

Description

Core-shell structured cathode active material powder and its manufacturing method

[0001] The present invention relates to a core-shell structured positive electrode active material powder and a method for producing the same, and more particularly, to a core-shell structured positive electrode active material powder having a stabilized form and excellent physicochemical properties, and a method for producing the same, by uniformly depositing an atomic layer of a mechanically and electrochemically stable compound on the particle surface of the positive electrode active material powder to form a protective film.

[0002] Unless otherwise indicated herein, the matters described in this section are not prior art to the claims of this application, and their inclusion in this section is not an admission that they are prior art.

[0003] With the growth of the electric vehicle market, demand for high-performance batteries is increasing. To achieve both performance and cost-effectiveness, high-nickel, high-manufactured, or cobalt-free cathode materials are attracting significant attention. However, these cathode materials are prone to side reactions at the electrolyte interface, which degrades battery performance and is a critical challenge that the industry must address.

[0004] Accordingly, various studies are being conducted to stabilize cathode active materials, including composition gradients, doping, and surface coating. Among these, surface coating is the most intuitive stabilization method. The protective coating formed on the surface of the cathode active material must be mechanically and electrochemically stable, and possess high ionic conductivity to ensure smooth ion transport between the electrode and electrolyte. In particular, precise thickness control, high uniformity, and high-quality coating are essential to maximize stability.

[0005] As a technology for coating a protective film on an electrode plate manufactured by mixing a positive electrode active material or a negative electrode active material and a binder, etc., U.S. Patent No. 9196901 proposes an electrode material for a lithium-ion battery coated with an alumina layer (Lithium battery electrodes with ultra-thin alumina coatings, 2015.11), and Korean Patent Publication No. 10-2020-0136684 proposes an atomic layer deposition coating method and device for a secondary battery electrode.

[0006] However, in the case of these conventional technologies, there is a difficulty in uniformly applying a protective film over the entire surface of the active material. The protective film of the active material can be formed by atomic layer deposition (ALD). Although this ALD method is a relatively low-temperature deposition process, it is generally 150 to deposit a higher quality / higher uniformity thin film. o High-temperature deposition temperatures of C or higher are required. However, these high-temperature conditions can cause deterioration of the organic binder contained in the electrode plate, limiting the selection of protective film materials and process conditions. In particular, all-solid-state battery cells implement composite positive electrodes by mixing positive active materials and solid electrolytes. In other words, to maximize the positive electrode / electrolyte interfacial protective film effect, a protective film coating must be applied directly on the positive active material powder, rather than on the electrode plate.

[0007] In this way, there have been attempts to improve existing electrode active materials for secondary batteries, such as coating active materials, but there was a need to overcome technological limitations and improve physical properties.

[0008] {Prior art literature}

[0009] [Patent Document]

[0010] (Patent Document 1) U.S. Patent No. 9196901

[0011] (Patent Document 2) Korean Patent Publication No. 10-2020-0136684

[0012] In order to solve the problems of the prior art as described above, the present invention aims to provide a cathode active material having excellent physical properties by effectively depositing a high ion conductivity oxide protective film directly on the surface of cathode active material powder to maximize the stabilization effect of the electrode active material for the protective film forming the electrode active material.

[0013] Accordingly, the purpose of the present invention is to provide a core-shell structured cathode active material powder having an oxide protective film uniformly coated on the surface of the cathode active material powder, and a method for manufacturing the same.

[0014] In addition, another object of the present invention is to suppress interfacial side reactions between the cathode and the electrolyte by modifying the surface of the cathode material through the production of a cathode active material powder having a high stability core-shell structure.

[0015] In addition, another object of the present invention is to precisely control the composition and thickness of the coating protective film of the positive electrode active material powder having a core-shell structure, thereby improving ionic conductivity and thereby providing excellent electrical conductivity and suppressing deterioration and degradation of battery performance.

[0016] In addition, another object of the present invention is to improve the uniformity and coverage of a protective film coated on the surface of a positive electrode active material powder, thereby improving the characteristics of the protective film, and thereby improving the life characteristics of a battery cell.

[0017] The purpose or technical solution of the present invention is not limited to what is described above, and should be understood to include all purposes that can be inferred from the detailed description of the present invention or the composition of the invention described in the claims, or all purposes that can be achieved by the description or technical idea of ​​the present invention.

[0018] The present invention provides a core-shell structured positive electrode active material powder having novel physicochemical properties for solving the above-described technical problems, wherein the positive electrode active material powder has a protective film having a mechanically and electrochemically stabilized form by uniformly coating at least one of an oxide, a metal, a sulfide, and a nitride with a controlled thickness on the surface of the positive electrode active material powder, wherein the protective film has an average thickness of 0.1 to 10 nm and a uniformity in which the average thickness deviation of the protective film is ±10% or less over the entire surface of the positive electrode active material powder.

[0019] According to a preferred embodiment of the present invention, the protective film is LiOH, Al2O3, ZrO2, NbOx, TiO2, ZnO, CoO x , may be formed of a single oxide such as SnOx, or a heterooxide, a metal, a sulfide, and a nitride.

[0020] According to a preferred embodiment of the present invention, the protective film is formed on at least 95% of the entire surface area of ​​the positive electrode active material powder, and may be uniformly formed over the entire surface area.

[0021] According to a preferred embodiment of the present invention, the protective film may have a uniformity of 90% or more according to the following mathematical expression 1.

[0022] [Mathematical Formula 1]

[0023] Uniformity (%) = [1-(max-min) / (2×avg)]×100

[0024] According to a preferred embodiment of the present invention, the protective film can have a uniformity of an average thickness deviation of within ±2.5%.

[0025] According to a preferred embodiment of the present invention, the protective film may be amorphous.

[0026] According to a preferred embodiment of the present invention, the protective film may contain crystal grain boundaries of 20% or less.

[0027] According to a preferred embodiment of the present invention, the protective film has an ionic conductivity of 10 -7 It can be more than S / cm.

[0028] In addition, the present invention forms a protective film by coating at least one of oxide, metal, sulfide and nitride with a uniformly controlled thickness on the surface of a cathode active material powder.

[0029] The step of coating the protective film includes: a step of providing a precursor A to the surface of a positive electrode active material powder particle; a first dwell step in which the precursor A sufficiently reacts with the surface of the powder particle; a step of performing a first purge under reaction conditions in which the precursor A is provided; a step of providing a first reactant of at least one of O3, H2O, O2, NH3, and H2S after the first purge step; a second dwell step in which the first reactant sufficiently reacts with the surface of the positive electrode active material powder; and a second purge step in which the reactant is provided, so that the average thickness of the protective film is 0.1 to 10 nm and the average thickness deviation of the protective film has a uniformity of ±10% or less over the entire surface of the positive electrode active material powder. A method for producing a high-stability core-shell positive electrode active material powder is provided.

[0030] According to a preferred embodiment of the present invention, the step of providing the precursor A, the first dwell step, the first purge step, the first reactant providing step, the second dwell step, and the second purge step are defined as a first unit process, and the first unit process can be repeatedly performed one or more times.

[0031] According to a preferred embodiment of the present invention, the step of coating the protective film further includes a step of providing a precursor B on the positive electrode active material powder using a precursor B different from the precursor A; a third dwell step: a third purge step; a step of providing a second reactant of at least one of O3, H2O, O2, NH3, and H2S; a fourth dwell step and a fourth purge step, wherein the step of providing the precursor B, the third dwell step, the third purge step, the second reactant providing step, the fourth dwell step, and the fourth purge step are defined as a second unit process, and the second unit process can be repeatedly performed one or more times.

[0032] The positive electrode active material powder having a core-shell structure of the present invention effectively coats a protective film to excellently modify the surface properties of the positive electrode material, thereby suppressing interfacial side reactions between the positive electrode and the electrolyte when applied as a positive electrode active material, thereby having the effect of improving battery life characteristics.

[0033] In addition, the cathode active material powder having a core-shell structure of the present invention has the effect of improving the electronic conductivity function compared to existing cathode active materials.

[0034] In this way, the present invention can greatly improve the life of a battery cell by very precisely controlling the coating thickness of a protective film formed on the surface of a positive electrode active material powder and ensuring very excellent coating uniformity.

[0035] In addition, the core-shell structured cathode active material powder of the present invention can secure high ionic conductivity by efficiently depositing oxides by optimizing the composition of the protective film coated on its surface, thereby suppressing deterioration of battery performance.

[0036] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the detailed description of the present invention or the composition of the invention described in the claims.

[0037] Figure 1 is a schematic diagram conceptually showing a cross-section of a core-shell structure positive electrode active material powder according to an embodiment of the present invention.

[0038] FIG. 2 is a schematic diagram comparing an uncoated cathode active material powder (a) and a core-shell structure cathode active material powder (b) coated with a lithium ion conductive heterooxide according to an example of the present invention to form a protective film, to explain why coating of a cathode active material is necessary in a secondary battery.

[0039] FIG. 3 is a drawing for explaining an atomic layer deposition process of a cathode active material powder for manufacturing a core-shell structure cathode active material powder according to one embodiment of the present invention.

[0040] FIG. 4 is a graph for comparing ionic conductivity of protective film materials manufactured according to the composition of heterooxides through ALD supercycle control according to an embodiment of the present invention.

[0041] FIG. 5 is a TEM photograph of each part for observing the protective film coating state of the core-shell cathode active material powder implemented according to an embodiment of the present invention.

[0042] Below, preferred embodiments of the present invention will be described in detail with reference to the attached drawings. However, the technical concept of the present invention is not limited to the embodiments described herein and may be embodied in other forms. Rather, the embodiments introduced herein are provided to ensure that the disclosed content is thorough and complete and to sufficiently convey the technical concept of the present invention to those skilled in the art.

[0043] In this specification, when a component is referred to as being on another component, it means that the component may be formed directly on the other component, or a third component may be interposed between them. Furthermore, in the drawings, the thicknesses of films and regions may be expressed in exaggerated form, etc., for the purpose of effectively explaining the technical content.

[0044] Additionally, although terms such as first, second, and third have been used to describe various components in various embodiments of this specification, these components should not be limited by such terms. These terms are only used to distinguish one component from another. Thus, what is referred to as a first component in one embodiment may be referred to as a second component in another embodiment. Each embodiment described and illustrated herein also includes its complementary embodiments.

[0045] In the specification, singular expressions include plural expressions unless the context clearly dictates otherwise. Furthermore, terms such as "comprises" or "has" are intended to indicate the presence of a feature, number, step, component, or combination thereof described in the specification, but should not be construed as excluding the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0046] In addition, when describing the present invention below, if it is determined that a detailed description of a related known function or configuration may unnecessarily obscure the gist of the present invention, the detailed description will be omitted.

[0047] The present invention provides a core-shell structured cathode active material powder having stabilized high functionality and a method for manufacturing the same, in order to improve the lifespan and ease of handling of a cathode active material, which is a key material of a secondary battery, or to improve physicochemical properties such as suppression of interfacial side reactions and electrical conductivity.

[0048] The cathode active material powder with a stabilized core-shell structure provided in the present invention exhibits significantly superior properties compared to existing materials. In particular, the cathode active material powder of the present invention exhibits superior uniformity of the protective film formed on the surface of the powder (core) compared to existing materials, and the shell (protective film) has a very thin and consistent thickness, exhibiting excellent mechanical and electrochemical properties. Furthermore, due to its superior properties, it exhibits excellent capacity retention after charge and discharge and extended service life.

[0049] The attached drawing 1 is a schematic diagram conceptually showing a cross-section of a structure of a positive electrode active material powder having a core-shell structure according to one embodiment of the present invention.

[0050] The novel core-shell structured cathode active material powder that can be provided in the present invention has a structure in which a uniform protective film is coated on the surface of the cathode active material powder compared to the conventional one, and has a mechanically and electrochemically stable form, and in particular, can be composed of a cathode active material in powder form and a protective film for stabilizing the interface between the cathode and the electrolyte and improving the electrical conductivity function.

[0051] In this way, in the present invention, a protective film formed on the surface of a 'positive electrode active material powder' is defined as a 'positive electrode active material powder'. Therefore, the positive electrode active material powder can be defined as the core, the protective film as the shell, and the positive electrode active material powder means having a core-shell structure.

[0052] The positive electrode active material powder used in the present invention may be, for example, a metal oxide particle, and the metal oxide particle may be Li x M 1-a-b Md a Me b O y(0≤a, b≤0.5, 0≤x≤2, 2≤y≤4) components, wherein M, Md, and Me may be a transition metal or one of Mg, Ca, and F. Specifically, cathode active material powders such as LiNiCoMnOx, LiNiMnOx, and LiCoOx may be used. These cathode active material powders include typical forms as materials that can be used as cathode active materials of lithium secondary batteries, and it is preferable to use powders having an average particle size of, for example, 100 nm to 900 μm. These cathode active material powders may have one or more forms selected from, for example, spherical, elliptical, or amorphous powder particles, nanowires, porous material particles, nanorods, nanotubes, nanosheets, hollows, and yolk-shells.

[0053] At this time, the component used as a protective film is not limited to oxides or lithium-based compounds, and application of metals, sulfides, or nitrides is also possible. Here, the oxide used to form the protective film may be a single oxide or a heterogeneous oxide, and a preferred example of a heterogeneous oxide may include a heterogeneous oxide containing lithium. Here, the term "heterogeneous oxide" refers to a material that contains two or more different components to form an oxide.

[0054] The protective film of the present invention may be, for example, LiOH, Al2O3, ZrO2, NbOx, TiO2, ZnO, CoO x , SnOx, etc., may be formed of a component including at least one of a single oxide, a heterooxide, a metal, a sulfide, and a nitride. Here, the heterooxide may preferably be a heterooxide containing lithium, and an example thereof is LiAlO. x , LiZrO x , LiNbO x , LiCoO x , LiSnO x and LiTiOx One or more selected from may be included. In addition, as the metal, for example, a transition metal may be used, and preferably, one or more selected from Nb, Zr, Al, Co, Ru, Ir, Pt, Ag may be included. As the sulfide, for example, Li x Ge y P z S (1-x-y-z) , Li x PS y One or more of Cl, MoS2, and ZnS may be included. In addition, one or more selected from, for example, TiN, AlN, and SiN may be used as the nitride.

[0055] According to a preferred embodiment of the present invention, the protective film may be formed in a multi-layer form rather than a single layer. As a particularly preferred example, the protective film may comprise one or more layers of a lithium-ion conductive composite material comprising the lithium-containing heterooxides listed above. For example, a preferred form of the protective film may be a composite material comprising lithium oxide and another metal oxide.

[0056] According to a preferred embodiment of the present invention, the protective film can be formed substantially over the entire surface area of ​​the positive electrode active material powder. Preferably, the protective film is formed over at least 95% of the total surface area of ​​the positive electrode active material powder, and may be uniformly formed over the entire surface area.

[0057] The cathode active material powder used in the present invention exhibits a very rough surface structure. Therefore, although the technology for forming an ALD protective film on the surface of such cathode active material powder can form a protective film over a certain area, it is not easy to uniformly coat the entire area. However, the present invention is characterized by having a protective film that is uniformly formed over the entire surface despite the unevenness formed on the surface of the cathode active material powder, and in particular, has a protective film that is coated so as to maintain excellent uniformity with a very uniform thin thickness over the entire area.

[0058] Therefore, the present invention is characterized by a high-stability core-shell cathode active material powder having a core-shell structure and a protective film, wherein the protective film can be uniformly formed to have an average thickness of 0.1 to 10 nm, more preferably 0.1 to 5 nm, and wherein the average thickness deviation of the protective film over the entire surface of the cathode active material powder has a uniformity of ±10% or less.

[0059] If the average thickness deviation of the protective film exceeds ±10%, the performance of the positive electrode active material may be impaired due to the uneven thickness of the protective film, and in particular, the thick part may act as a resistance layer for lithium ion movement during the charge / discharge process, and lithium ion movement may occur only in the part where the protective film is thin, which may reduce the lithium ion movement speed and cause a decline in battery performance.

[0060] According to a preferred embodiment of the present invention, the average thickness deviation of the protective film can be manufactured to have a uniform thickness, more preferably within ±7.5%, within ±5%, within ±3%, within ±2%, within ±1.5%, or within ±1%. According to a preferred embodiment of the present invention, the protective film can preferably have a uniformity in average thickness deviation of within ±2.5%.

[0061] According to a preferred embodiment of the present invention, the protective film may have a uniformity of 90% or more according to the following mathematical formula 1. More preferably, it may have a uniformity of 95% or more, and most preferably, it may have a uniformity of 98% or more.

[0062] [Mathematical Formula 1]

[0063] Uniformity (%) = [1-(max-min) / (2×avg.)]×100

[0064] In addition, since the surface of each of the positive electrode active material powders of the present invention is very uniformly coated with a nano-thick protective film over the entire surface, when the positive electrode active material powder has such excellent uniformity, the interfacial stability between the positive electrode and the electrolyte as well as the ionic conductivity and electrical conductivity can be significantly improved due to the modification of the surface properties of the positive electrode active material. In addition, when applied to secondary batteries, the physical properties, capacity, and electrode lifespan can also be significantly improved.

[0065] According to a preferred embodiment of the present invention, the protective film formed on the surface of the powder may be amorphous. This means that the protective film is substantially amorphous overall.

[0066] Therefore, according to a preferred embodiment of the present invention, the protective film may contain grain boundaries of 20% or less, more preferably 15% or less, 10% or less, 5% or less, or 3% or less. Since the grain boundary content is low, the entire protective film has amorphous properties, so that the protective film can be formed in a coating state with desirable properties and excellent uniformity. If the protective film contains grain boundaries of 20% or more, it is difficult to form a uniform protective film coating, and after coating formation, there is a problem that the surface coating surface state cannot be maintained in the initial state during the use and process application processes such as transport, storage, mixing, and use of the positive electrode active material powder.

[0067] According to a preferred embodiment of the present invention, the protective film has an ionic conductivity of 10 -7S / cm or more, preferably 10 -6 It can be S / cm or more. This characteristic may be possible due to the characteristics of the protective film that has excellent uniformity across the entire surface of the positive electrode active material powder as described above. The improvement in ionic conductivity due to these characteristics of the protective film is significantly superior to existing methods.

[0068] FIG. 2 is a diagram illustrating why a coating protective film is required for a cathode active material powder in a secondary battery. If there is no coating protective film, a CEI (Cathode Electrolyte Interphase) is formed at the cathode / electrolyte interface, which causes a decline in battery performance due to an electrolyte decomposition reaction. Therefore, application of a protective film is essential to prevent direct contact between the electrode and the electrolyte. Accordingly, FIG. 2 is a schematic diagram comparing an uncoated cathode active material powder (a) and a core-shell structure cathode active material powder (b) coated using a lithium ion conductive heterooxide according to an example of the present invention. Here, CAM (Cathode Active Material) means a cathode active material, reference numeral 10 means CEI, and 100 means a protective film.

[0069] As shown in Fig. 2, in the case of the cathode active material powder according to the present invention presented as (b), it shows a mechanism that can significantly improve cell performance compared to the existing one by very uniformly coating a protective film on the surface of the cathode active material powder. This effect is that in the case of the cathode active material powder of the present invention, the uniform protective film functions as a protective film that suppresses interfacial side reactions between the cathode and the electrolyte, and at the same time, as the cathode voltage increases during the charging process, the decomposition reaction of the electrolyte is induced, thereby suppressing the formation of CEI (Cathode Electrolyte Interphase) at the interface between the cathode and the electrolyte, which causes a decline in cell performance.

[0070] In this way, in the case of a cathode using a cathode active material powder, a protective film is essential to prevent direct contact between the electrolyte and the cathode. Therefore, a cathode active material powder with a core-shell structure on which a protective film is formed is required to maximize the protective film effect.

[0071] Therefore, in the present invention, a protective film with excellent uniformity is formed on the surface of the positive electrode active material powder, thereby ensuring life stability without deterioration of cell performance.

[0072] In particular, in the present invention, the positive electrode active material powder having a core-shell structure has excellent uniformity of the protective film formed on the surface and has an ionic conductivity of 10 -7 Since a protective film having a density of S / cm or more is coated very uniformly, the function of the protective film is not limited to simply suppressing interfacial side reactions, but also provides a cathode active material having excellent functionality through improvement of the ion conductivity of the protective film.

[0073] In this way, the present invention can control the thickness of the protective film formed on the particle surface of the positive electrode active material powder by adjusting the manufacturing process conditions and the total number of repetitions of the ALD process, so that the thickness of the protective film is very thin and the uniformity is very excellent, thereby suppressing interfacial side reactions and providing a positive electrode active material powder with a core-shell structure that is mechanically and electrochemically stable and can significantly improve capacity and lifespan when applied to a battery.

[0074] Hereinafter, a method for manufacturing a core-shell structured positive electrode active material powder according to the present invention will be described.

[0075] The protective film formed on the positive electrode active material powder of the core-shell structure of the present invention can be formed by ALD coating on the positive electrode active material powder.

[0076] Typically, ALD coatings comprise a single cycle of atomic layer formation, consisting of precursor injection and adsorption, self-limiting reaction, dwell, and reactant injection onto the coating target. This cycle can be repeated. However, controlling this process cycle can result in ALD coating layers with a wide variety of structures and can also affect the properties of the resulting protective film. Therefore, process control is crucial, and forming a protective film with specific properties is not easy.

[0077] Here, 'precursor' means a precursor to a material that is coated on a coating target to form a protective film.

[0078] For ALD coating, for example, after precursor injection, precursor adsorption and reactants are generated through ligand exchange between hydroxyl groups and the precursor on the surface of the coating target. Next, a self-limiting reaction occurs. After all reactions have occurred at the surface reaction sites, any excess precursor no longer reacts with the surface and is emitted through the carrier gas, along with the generated reactants.

[0079] In this process, a dwell process is performed to ensure sufficient reaction. The dwell process provides reaction time, for example, after precursor injection, to allow sufficient reaction time for residual precursors to react with unreacted surfaces. During this time, no additional precursors are supplied or pumped. This provides sufficient time for chemical reaction in cases where precursors are weakly physically adsorbed on the particle surface, and also allows surfaces hidden between particles to sufficiently react with precursors remaining within the reactor.

[0080] Next, one or more reactants among H2O, O3, O2, H2S, and NH3- are injected, and the remaining byproducts and unreacted precursors that react with the surface of the coating target are purged, and then the reactants are injected to react with the new surface formed by the precursor injection, and the remaining reactants are similarly discharged.

[0081] This process is one cycle of ALD coating, and through this process, a coating layer is formed at the atomic layer level.

[0082] Therefore, a thin film can be deposited by repeating the ALD cycle, and a protective film can be formed by depositing a layer of oxide through the process of precursor injection → purge → oxidant injection → purge, etc. Such a layer can be formed by a multiple coating method in which it is repeatedly laminated through a repetitive process.

[0083] According to a preferred embodiment of the present invention, in order to manufacture a core-shell structured cathode active material powder, as a process for forming a protective film by ALD coating, an ALD coating method is used to form a protective film by uniformly coating at least one of oxide, metal, sulfide, and nitride with a controlled thickness on the surface of the cathode active material powder.

[0084] In order to coat the above protective film, a step of providing precursor A on the particle surface of the positive electrode active material powder is performed; a first dwell step isolating the precursor A in a reactor so that the precursor A can sufficiently react with the particle surface of the powder, thereby providing time for the particle surface covered by other particles to sufficiently react with the precursor; a first purge step is performed so that the speed at which the precursor A is injected or pumped is too fast to prevent the precursor A from being adsorbed on the surface of the positive electrode active material powder; and a first purging step is performed under reaction conditions in which the precursor A is provided.

[0085] Here, 'precursor A' means a precursor for at least one of an oxide, metal, sulfide or nitride that forms the protective film.

[0086] Next, after the first purge step, a step of providing at least one first reactant selected from O3, H2O, O2, NH3, and H2S to deposit at least one of, for example, a single oxide, a heterooxide, a metal, a sulfide, and a nitride, a second dwell step to allow the first reactant to sufficiently react with the particle surface of the cathode active material powder, and a second purge step for the reaction environment in which the reactant is provided, is included, so that a protective film having an average thickness of 0.1 to 10 nm and a uniformity of an average thickness deviation of the protective film within ±10% over the entire surface area can be formed, thereby manufacturing a core-shell cathode active material powder.

[0087] Through this process, a core-shell structured cathode active material powder according to the present invention can be obtained. However, after completing this basic process, additional processes may be repeatedly applied to manufacture the cathode active material powder using a more improved method to ensure sufficient functionality.

[0088] According to a preferred embodiment of the present invention, the step of providing the precursor A, the first dwell step, the first purge step, the first reactant providing step, the second dwell step, and the second purge step are defined as a first unit process, and the first unit process can be repeatedly performed one or more times.

[0089] According to a preferred embodiment of the present invention, the second unit process may be performed in the same manner as the first unit process, but using a precursor B having a different component instead of the precursor A; a step of providing the precursor B; a third dwell step; a third purge step; a step of providing at least one second reactant selected from O3, H2O, O2, NH3, and H2S for deposition of at least one of a single oxide, a heterooxide, a metal, a sulfide, and a nitride; a fourth dwell step, and a fourth purge step. Here, each or all of the first unit process and the second unit process may be repeated one or more times.

[0090] Here, 'precursor B' means a precursor for at least one of an oxide, metal, sulfide or nitride that forms a protective film, and means a precursor for a protective film component different from precursor A.

[0091] Figure 3 schematically illustrates an example of this process. Figure 3 illustrates an atomic layer deposition process of a cathode active material powder for manufacturing a core-shell structure cathode active material powder according to one embodiment of the present invention.

[0092] To explain this in more detail with an example, in a process for depositing an atomic layer on the particle surface of a positive electrode active material powder, the first unit process (unit process A) can form a protective film of, for example, lithium oxide through the following steps.

[0093] (1) Step of injecting precursor A into the reactor

[0094] A liquid or solid precursor A (e.g., Li precursor) is vaporized as a component for forming a protective film and injected into a reactor together with a carrier gas.

[0095] (2) 1st dwell stage

[0096] A dwell step is performed to allow precursor A injected into the reactor to sufficiently react with the cathode active material powder, and a process is performed to induce the powder surface to sufficiently react with the precursor A gas already injected by rotating only the reactor without additional supply or pumping of the injected precursor A.

[0097] (3) 1st fuzzy stage

[0098] A purge step is performed to remove the product resulting from the reaction between the above precursor A and the positive electrode active material powder surface and the unreacted precursor A remaining.

[0099] (4) First reactant injection stage

[0100] This is the step of injecting gaseous reactants, and by injecting these reactants, a protective film is formed.

[0101] (5) 2nd dwell stage

[0102] This is a process for forming a protective film made of precursor A oxide. The reaction time at this time is the same as that of step (3) above.

[0103] (6) Second fuzzy stage

[0104] A purge step is performed to remove products and unreacted reactants resulting from surface reaction of the positive electrode active material powder.

[0105] After the first unit process (unit process A) as described above is performed, a second unit process can be applied. This second unit process (unit process B) can be performed in a similar manner to the first unit process, for example, in a step of forming a protective film (e.g., a metal oxide protective film such as NbOx or ZrOx) using precursor B.

[0106] As an example of this process, a protective film of a composite oxide of, for example, Li and Nb can be formed.

[0107] According to a preferred embodiment of the present invention, the first unit process and the second unit process form a protective film made of different oxides. For example, it is preferred that at least one of the unit processes forms a protective film made of lithium oxide.

[0108] According to a preferred embodiment of the present invention, by alternately performing the first unit process and the second unit process, a protective film having desirable properties can be formed on the surface of the positive electrode active material powder using a specific compound. For example, the first and second unit processes can each be performed separately one or more times, and separately, the first unit process and the second unit process can be performed one or more times in a continuous manner and repeated several times. In this way, the present invention can manufacture positive electrode active material powder having a uniform thickness of the protective film and excellent physicochemical properties by appropriately repeating each process as needed and controlling the process conditions.

[0109] In the present invention, each of the first and second unit processes (unit processes A and B) exemplified above is referred to as a sub-cycle, and a cycle including both the first and second unit processes is defined as a super cycle.

[0110] According to a preferred embodiment of the present invention, the film thickness of the protective film formed on the surface of the positive electrode active material powder can be controlled through repetition and control of the above unit process. Such a protective film can be manufactured to a thickness of 0.1 to 10 nm, more preferably 0.1 to 5 nm, or 0.1 to 3 nm.

[0111] According to a preferred embodiment of the present invention, in the process conditions for the above manufacturing, the reaction temperature is preferably 210 to 400°C, more preferably 230 to 350°C, and this process can be carried out under stirring in a reactor, preferably at 10 to 50 rpm, more preferably at 15 to 35 rpm.

[0112] According to a preferred embodiment of the present invention, the thickness of the protective film can be precisely controlled during the manufacturing process to form a very uniform coating of the protective film on the positive electrode active material powder. To this end, according to a preferred embodiment of the present invention, a process of controlling mechanical and process conditions, such as designing a reactor structure and controlling rotation speed, may be included during the unit process for coating to prevent agglomeration between particles of the positive electrode active material powder and maximize dispersion.

[0113] According to a preferred embodiment of the present invention, a high-ionic conductivity coating can be formed on the particle surface of a cathode active material powder by controlling the composition of the protective film. This involves a process of controlling the supercycle of an atomic layer deposition method. By controlling the composition of components applied as the protective film, such as lithium and metals, high ionic conductivity can be secured, thereby preventing degradation of battery performance.

[0114] According to a preferred embodiment of the present invention, the surface of the positive electrode active material powder can be modified through the production of a core-shell structured positive electrode active material powder, thereby suppressing deterioration due to reaction with the electrolyte. At this time, by depositing a composite oxide on the surface of the positive electrode active material powder through a supercycle as described above, deterioration of ionic conductivity can be prevented, and stability can be maximized by precisely controlling the thickness and uniformity, thereby significantly contributing to improved cell life characteristics.

[0115] The core-shell structured cathode active material powder of the present invention exhibits excellent structure and physical properties, and thus has excellent and stable mechanical and electrochemical properties. The excellence of these properties can be confirmed in the attached drawings, such as FIG. 4 and FIG. 5.

[0116] FIG. 4 is a graph comparing ionic conductivity of a cathode active material powder having a protective film formed of a heterooxide composition through control of supercycle conditions for ALD coating according to one embodiment of the present invention, and it is confirmed that the electrochemical properties are excellent.

[0117] In Fig. 4, (a) shows that the Li:Nb composition of the actually deposited LiNbOx thin film changes according to the repetition ratio of the process, such as the subcycle for each of Li and Nb, among the supercycles using ALD.

[0118] In Fig. 4, (b) is a Nyquist plot according to the electrochemical impedance spectroscopy (EIS) measurement of LiNbOx thin films with different Li:Nb composition ratios. In general, materials with ionic conductivity appear as a combination of a hemisphere and a straight line. Here, a smaller hemisphere size means a smaller resistance to ion movement, and the ionic conductivity can be calculated by dividing the resistance by the thickness.

[0119] In addition, (c) in Fig. 4 shows the Nyquist diagram of the sample by Si:Nb composition and the ionic conductivity value calculated from the sample thickness.

[0120] FIG. 5 is a TEM photograph of each part for observing the protective film coating state of a core-shell cathode active material powder implemented according to one embodiment of the present invention, and it can be confirmed that the uniformity is excellent in all parts of the protective film despite the surface roughness of the cathode active material powder.

[0121] According to a preferred embodiment of the present invention, when performing the process exemplified in FIG. 3, by controlling the number of repetitions of unit processes A and B, for example, when forming a protective film of lithium oxide and a metal oxide such as Nb, Zr, or Al, the ratio of each subcycle of the unit process for forming lithium and metal oxide is controlled, the actual molar ratio of lithium:metal can be controlled.

[0122] Therefore, the difference in lithium ion conductivity may occur due to this difference in composition, and this lithium ion conductivity is, for example, 10 when the lithium content ratio of lithium / (lithium + metal) is around 40-80%. -7 It shows the level of S / cm, but the protective film above that, especially the lithium content ratio of 55-70%, is 10 -6 It was confirmed that a protective film with excellent physical properties and an ionic conductivity of about S / cm can be manufactured.

[0123] Therefore, the core-shell structured cathode active material powder according to the present invention can form a protective film having various thicknesses and properties by controlling the process conditions of the protective film coating process, and in this process, the protective film can be manufactured in a form with excellent uniformity.

[0124] The core-shell structured cathode active material powder according to the present invention has excellent surface uniformity of the protective film formed over the entire surface, so when used as an electrode material, it has excellent ionic conductivity compared to the existing one and can maintain electrode function excellently by suppressing interfacial side reactions, so it is useful for manufacturing a high-functionality battery with excellent electrical conductivity and capacity characteristics and can also extend the battery life.

[0125]

[0126] Hereinafter, the present invention will be described in detail by way of examples, but the present invention is not limited to the examples.

[0127] <Example 1>

[0128] Unit 1 process (Unit process A)

[0129] NCM (nickel-cobalt-manganese) cathode active material powder with an average particle size of 1 to 30 ㎛ was used as the cathode active material powder, and ALD coating was performed by injecting the NCM cathode active material powder into a rotating reactor. The cathode active material powder used here had a surface area of ​​approximately 0.4 m 2 / g NCM 811 powder was applied by loading 10g.

[0130] (1) Step of injecting Li precursor (precursor A) into the reactor

[0131] A solid precursor such as LiOtBu was heated / vaporized to 140°C, and carrier gas Ar was injected into the reactor at 200 sccm for 10 seconds. At this time, the reactor was maintained at 230 to 400°C and rotated at 10 to 50 rpm to disperse the positive electrode active material powder.

[0132] The LiOtBu precursor injected into the reactor is adsorbed on the surface of the NCM cathode active material powder by ligand conversion with the surface hydroxyl group.

[0133] (2) 1st dwell stage

[0134] A dwell process is performed to ensure that the precursor injected into the reactor can sufficiently react with the surface of the cathode active material powder. Here, the reactor is kept in an isolated state and rotated at 10–50 rpm without additional precursor supply. The dwell process is maintained for approximately 10 seconds to ensure sufficient reaction between the precursor and the surface of all cathode active material powders within the reactor.

[0135] In this process, the surface of the positive electrode active material powder that has already reacted with the precursor through a self-limiting reaction does not react any more, and some of the precursor remains as residue after the reaction.

[0136] (3) 1st fuzzy stage

[0137] In the above process, purging was performed to remove reaction by-products generated by the reaction between the precursor and the positive electrode active material powder surface and the unreacted precursor remaining.

[0138] In this process, the conditions of the reactor were maintained, but only Ar gas, not the precursor, was flowed at 200 sccm for 10 seconds to remove residual precursor and reaction products within the reactor.

[0139] (4) First reactant injection stage

[0140] After the above purging, the gaseous reactant is injected into the reactor to form a protective film with a lithium oxide (lithium oxide) forming film. In this process, the concentration is 180 g / m under the same reactor conditions. 3 O3 was injected at 500 sccm for 10 seconds to react with the precursor adsorbed on the surface of the cathode active material powder to form a LiOH layer.

[0141] (5) Second dwell and second purge stages

[0142] After the first reactant injection, a second dwell was performed for the reaction, and the residue was removed by a second purge. Here, the dwell and purge steps were performed under the same conditions as the first dwell and purge steps.

[0143] (6) Formation of lithium oxide coating layer

[0144] The above processes (1) to (5) were performed repeatedly three times to manufacture a core-shell structured cathode active material powder having a lithium oxide coating layer as a protective film on the surface of the cathode active material powder particles.

[0145]

[0146] <Example 2>

[0147] 2nd unit process (Unit process B)

[0148] Additional ALD coating was performed on the positive electrode active material powder (referred to as the first powder) on which a lithium oxide protective film was formed in the first unit process.

[0149] (1) Step of injecting Nb precursor (precursor B) into the reactor

[0150] A liquid precursor such as TBTDENb was heated to 70°C and vaporized, and Ar gas was injected into the reactor at 200 sccm as a carrier gas for 10 seconds. At this time, the reactor was maintained at 230-400°C and rotated at 10-50 rpm to disperse the first powder.

[0151] The TBTDENb precursor injected into the reactor in this way is adsorbed on the surface of the first powder, where a LiOH layer is formed by ligand conversion with the hydroxyl group present on the surface of the first powder.

[0152] (2) Third dwell stage

[0153] A dwell phase is performed to ensure that the precursor injected into the reactor can sufficiently react with the first powder. During this phase, the reactor is isolated and rotated at 10-50 rpm without additional precursor supply. This process is maintained for approximately 10 seconds to ensure that the precursor already injected into the reactor can sufficiently react with the entire first powder.

[0154] In this process, the surface of the first powder that has already reacted with the precursor through a self-limiting reaction does not react any more, and some of the precursor remains as residue after the reaction.

[0155] (3) Third fuzzy stage

[0156] In the above process, purging was performed to remove reaction by-products generated by the reaction between the precursor and the first powder surface and the unreacted precursor remaining.

[0157] In this process, the conditions of the reactor were maintained, but only Ar gas, not the precursor, was flowed at 200 sccm for 10 seconds to remove residual precursor and reaction products within the reactor.

[0158] (4) Second reactant injection stage

[0159] After the above purging, the gaseous reactant is injected into the reactor to form a Nb oxide thin film. In this process, under the same reactor conditions, the concentration is 180 g / m 3 O3 was injected at 500 sccm for 10 seconds to react with the precursor adsorbed on the surface of the first powder to form a first layer of NbOx.

[0160] (5) 4th dwell and 4th purge stage

[0161] After the injection of the second reactant, a fourth dwell was performed for the reaction, and the residue was removed by a fourth purge. Here, the dwell and purge steps were performed under the same conditions as the third dwell and purge step.

[0162] (6) Formation of Nb oxide coating layer

[0163] The above processes (1) to (5) were performed repeatedly three times to manufacture a core-shell structured cathode active material powder (second powder) by additionally forming a Nb oxide coating layer on the surface of the cathode active material powder (first powder) on which a lithium oxide protective film was formed in Example 1.

[0164] Experimental Example 1

[0165] In order to confirm the effect of improving the physical properties, such as ionic conductivity, of the protective film formed on the positive electrode active material powder, the number of repetitions of the unit processes A and B exemplified above was adjusted, and the Li:Nb ratio was adjusted by controlling the cycle for each unit process of lithium (Li) and metal (Nb), thereby manufacturing the protective film.

[0166] Through this process, the changes in physical properties such as ionic conductivity of the protective film were compared and analyzed while controlling the actual lithium:metal molar ratio in various forms, and the results are shown in Figure 3.

[0167] As confirmed in the experimental results in Fig. 3, it was confirmed that the characteristics of the protective film formed on the particle surface of the positive electrode active material powder can be changed by controlling the manufacturing process of the protective film, and that a difference in lithium ion conductivity occurs depending on the properties of the changed protective film.

[0168] As a result, lithium ion conductivity was confirmed to be excellent at a lithium molar ratio of lithium / (lithium + metal) of approximately 40-80%. In particular, it was confirmed to exhibit the best activity when the lithium molar ratio was around 60%, i.e., 55-70%.

[0169] Experimental Example 2

[0170] In order to confirm the physicochemical properties of the positive electrode active material powder manufactured by the method of Example 2 above, the structure of the manufactured positive electrode active material powder having a core-shell structure with a protective film formed was observed.

[0171] Figure 5 is a TEM image of each part obtained as a result of this experiment, which was used to observe the protective film coating state of the core-shell cathode active material powder. As seen in this image, a TEM image of a cross-section of a single particle of the cathode active material powder can be observed.

[0172] As confirmed in Fig. 5, the positive electrode active material powder is not a perfect spherical and smooth shape, and shows a shape in which small primary particles are aggregated to form secondary particles. In this way, the particle shape of the positive electrode active material powder has a roughness of 1, and it shows a shape in which it is difficult to form a perfect coating between small particles and on the curves. Therefore, it is impossible to implement a core-shell structure with a perfect protective film using a general wet chemical process.

[0173] However, in the drawing of FIG. 5 according to the present invention, in the photos ① to ⑤ showing partial enlarged photos, when comparing the thickness of the protective film by enlarging at any location on the particle surface of the positive electrode active material powder, when comparing the thickness of the protective film at each of 5 or more locations, it was confirmed that the uniformity calculated by the above mathematical formula 1 was 98.2% with almost the same thickness at most locations.

[0174] Furthermore, as a result of observing the properties and thickness of the protective film formed on the positive electrode active material powder of Fig. 5, it was confirmed that the protective film is very thin and mostly exists in an amorphous form. If the protective film forms a crystal, the crystal lattice is prominent as in the interior of the positive electrode in the TEM image, but the protective film side of Fig. 5 showed almost no crystallization tendency. The crystalline content state for this was predicted to be within approximately 5%.

[0175] In addition, in Fig. 5, the coating state of the protective film formed on the particle surface of the positive electrode active material powder was measured to have a protective film formation area of ​​98% or more compared to the total area, and it was confirmed that the protective film was practically formed over the entire area. In addition, the thickness of the protective film was measured as 2.74, 2.75, 2.82, 2.83, 2.84 nm at each position, and was confirmed to be in the range of 2.74 to 2.84, and the thickness deviation was measured to be 3.6%, or ±1.8.

[0176] From these experimental results, it was confirmed that the protective film of the core-shell structured cathode active material powder manufactured in the examples according to the present invention was formed at least 95%, and substantially 98%, of the protective film overall despite the highly irregular surface of the cathode active material powder, and at the same time, the thickness was formed to be 5 nm or less, and substantially 3 nm or less, the uniformity was 90% or more, and actually 98% or more, and the average deviation of the thickness was confirmed to be at least ±10% or less, and actually ±2% or less.

[0177] Therefore, the core-shell structured cathode active material powder having a surface protective film formed according to the present invention has excellent interfacial protection effects such as suppression of interfacial side reactions, as well as excellent ionic conductivity, and is therefore very useful as a cathode active material material, and in particular, can exhibit a remarkable effect in extending battery capacity and lifespan.

[0178]

[0179] While the present invention has been described in detail using preferred embodiments, the scope of the present invention is not limited to the specific embodiments and should be construed in accordance with the appended claims. Furthermore, those skilled in the art will appreciate that numerous modifications and variations are possible without departing from the scope of the present invention.

Claims

1. A high-stability core-shell structured cathode active material powder characterized in that the surface of the cathode active material powder is coated with at least one of oxide, metal, sulfide, and nitride with a uniformly controlled thickness to form a mechanically and electrochemically stabilized protective film, wherein the protective film has an average thickness of 0.1 to 10 nm and a uniformity in which the average thickness deviation of the protective film over the entire surface of the cathode active material powder is ±10% or less.

2. In claim 1, the protective film LiOH, Al2O3, ZrO2, NbOx, TiO2, ZnO, CoO x , a single oxide selected from SnOx; LiAlO x , LiZrO x , LiNbO x , LiCoO x , LiSnO x and LiTiO x A heterooxide containing lithium selected from; A cathode active material powder having a high stability core-shell structure formed from a component including one or more of the following.

3. In claim 1, the protective film is formed on at least 95% of the entire surface area of ​​the positive electrode active material powder, and is characterized by being uniformly formed over the entire surface area. A positive electrode active material powder having a high stability core-shell structure.

4. In claim 1, the protective film is a cathode active material powder having a high stability core-shell structure with a uniformity of 90% or more according to the following mathematical formula 1. [Mathematical Formula 1] Uniformity (%) = [1-(max-min) / (2×avg)]×100 5. In claim 1, the protective film is a high-stability core-shell structure positive electrode active material powder having a uniformity of an average thickness deviation of within ±2.5%.

6. In claim 1, the protective film is a high-stability core-shell structure positive electrode active material powder characterized by having amorphous properties.

7. In claim 1, the protective film is a positive electrode active material powder having a high stability core-shell structure containing grain boundaries of 20% or less.

8. In claim 1, the protective film has an ionic conductivity of 10 -7 A high-stability core-shell structured cathode active material powder having a density of S / cm or more.

9. Form a protective film on the surface of the positive electrode active material powder by coating at least one of oxide, metal, sulfide, and nitride with a uniformly controlled thickness. The step of coating the above protective film is: A step of providing precursor A on the above positive electrode active material powder; A first dwell step for sufficiently reacting the precursor A with the surface of the positive electrode active material powder; A step of first purging the precursor A under the provided reaction conditions; A step of providing at least one first reactant among O3, H2O, O2, NH3, and H2S after the first purge step; A second dwell step for sufficiently reacting the first reactant with the surface of the positive electrode active material powder; and A step of purging the above reactants for the second time under the provided reaction conditions. A method for producing a cathode active material powder having a high-stability core-shell structure, characterized in that the average thickness of the protective film is 0.1 to 10 nm, and the average thickness deviation of the protective film over the entire surface of the cathode active material powder has a uniformity of ±10% or less.

10. In claim 9, the step of providing the precursor A, the first dwell step, the first purge step, the first reactant providing step, the second dwell step, and the second purge step are defined as a first unit process, and a method for producing a cathode active material powder having a high-stability core-shell structure by repeating the first unit process at least once.

11. In claim 9, The step of coating the protective film further includes a step of providing a precursor B on the positive electrode active material powder using a precursor B different from the precursor A; a third dwell step; a third purge step; a step of providing a second reactant of at least one of O3, H2O, O2, NH3, and H2S; a fourth dwell step and a fourth purge step, wherein the step of providing the precursor A, the third dwell step, the third purge step, the second reactant providing step, the fourth dwell step, and the fourth purge step are defined as a second unit process, and a method for producing a positive electrode active material powder having a high-stability core-shell structure is performed by repeating the second unit process at least once.

Citation Information

Patent Citations

  • Manufacturing method of cathode active material powder for lithium secondary battery

    KR1020160100854A

  • Jig for fabricating window and fabricating method of window using the same

    KR1020220115676A

  • Method, server and computer program for providing food company matching service customized for users

    KR102425214B1

  • Reactor core for load follow operation

    KR102463008B1

  • Lithium battery electrodes with ultra-thin alumina coatings

    US9196901B2