Borate-based solid electrolyte and manufacturing method thereof
The boroxide-based lithium chloroboracite solid electrolyte addresses safety and performance issues in lithium-ion batteries by providing a high-ionic-conductivity, safe alternative to traditional liquid and sulfide-based electrolytes, enhancing energy density and stability across varying temperatures.
Patent Information
- Application Number
- PCT/KR2024/095761
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-22
- Filing Date
- 2024-04-23
- Publication Date
- 2024-10-31
AI Technical Summary
Lithium-ion batteries face safety concerns due to the risk of ignition and explosion from liquid electrolytes, and existing sulfide-based solid electrolytes pose challenges with high interface resistance and hazardous material handling, necessitating a safe and mass-producible alternative with improved ionic conductivity.
Development of a boroxide-based solid electrolyte, specifically lithium chloroboracite with a composition of Li4+x B7 O12+x/2 Cl (x=0~1), synthesized using LiOH, Li2 CO3, H3 BO3, and LiCl raw materials, exhibiting high ionic conductivity and nanoparticle form, manufactured through a melting and quenching process to replace traditional liquid electrolytes.
The boroxide-based solid electrolyte enhances safety, reduces volume and cost, and maintains high ionic conductivity, eliminating the risk of hydrogen sulfide generation, enabling efficient and stable battery performance across a wide temperature range, particularly at low temperatures, and allowing for higher energy density and simplified battery design.
Smart Images

Figure KR2024095761_31102024_PF_FP_ABST
Abstract
Description
Boron oxide-based solid electrolyte and its manufacturing method
[0001] The present invention relates to an all-solid-state electrolyte for an all-solid-state secondary battery with improved safety and ionic conductivity.
[0002] Secondary batteries consist of one or more electrochemical cells capable of recharging and discharging. Currently, lithium-ion batteries are leading the pack, essential for small electronic devices (such as smartphones). Lithium-ion batteries are advantageous over traditional lead-acid batteries due to their environmental hazards and memory effect (the phenomenon in which discharge voltage decreases and discharge capacity decreases below the nominal capacity with repeated charging and discharging). They also offer superior energy density per mass and volume.
[0003] While secondary batteries typically have a higher initial cost than disposable batteries, they can be recharged multiple times before needing replacement, which significantly reduces overall costs and environmental impact. Some types of secondary batteries are available in the same size and voltage as disposable batteries and can be replaced.
[0004] However, the electrolyte (liquid or gel) inside lithium-ion batteries poses a risk of fire and explosion due to thermal propagation. Concerns about safety are growing due to numerous actual explosion incidents.
[0005] Therefore, to compensate for these shortcomings, replacing the liquid electrolyte with a solid electrolyte has the following advantages:
[0006] - The risk of fire and explosion due to temperature changes and external impacts is significantly reduced, and since there is no need for safety devices or separators to prepare for temperature changes and external impacts, cost reduction and high capacity implementation are possible with the same size.
[0007] - Since there is no risk of fire, the energy density can be increased by filling the space where the cooling device, which takes up more than 30% of the battery pack space, has been removed with additional battery cells.
[0008] - Since there is no need for a separator that physically blocks the positive and negative electrodes in the liquid electrolyte to prevent electrical short-circuiting, volume reduction and cost reduction are possible.
[0009] - Lithium metal, which has superior performance, such as a capacity 10 times that of graphite, but was not used due to the risk of fire and explosion between electrodes, can be used as an anode active material, enabling high capacity to be achieved with the same size.
[0010] Meanwhile, as a solid electrolyte, a sulfide-based solid electrolyte using a Li2S-P2S5-LiCl ternary raw material with an argyrodite crystal structure has been developed. However, these existing sulfide-based solid electrolytes are hazardous because they can generate hazardous compounds such as hydrogen sulfide (H2S). In other words, the reality is that there are many controversies and challenges in the solid electrolyte material, high resistance at the active material-electrolyte boundary (interfacial resistance), and manufacturing process. Therefore, the need for the development of a safe and mass-producible solid electrolyte that can fundamentally eliminate the risks of existing sulfide-based solid electrolytes has emerged.
[0011] The purpose of the present invention is to manufacture a boron oxide-based solid electrolyte material having high purity and ionic conductivity and a particle shape, and to apply the same to a lithium ion conductor of an all-solid-state battery.
[0012] In addition, the purpose is to provide boron oxide-based solid electrolyte materials to the industry, thereby achieving economic advantages and ensuring superior safety in handling raw materials.
[0013] After years of research to develop a solid electrolyte that meets the needs of these industries, the researchers synthesized a lithium chloroboracite-based solid electrolyte. The solid electrolyte of the present invention is composed of Li4 + x B7O 12 +x / It is lithium chloroborasite with a composition of 2Cl (x=0~1).
[0014] The above lithium chloroborasite is characterized by being manufactured from LiOH or Li2CO3 and H3BO3 or B2O3 and LiCl raw materials, and has a Li ion conductivity of 1.0 x 10 at room temperature (25°C). -6 It is characterized by a value of S / cm or more.
[0015] In addition, the lithium chloroborasite is characterized by being a nanoparticle having a diameter of 10 nm to 300 μm. Preferably, the particle size is 0.8 to 80 μm, more preferably 1 to 20 μm. As the particle size decreases, the density can be increased, which is advantageous for ionic conductivity, but there are difficulties in the process, and if the particles are too large, there are disadvantages in that the density and homogeneity of the solid electrolyte membrane decrease.
[0016] Li4 of the present invention + x B7O 12 +x / A lithium chloroboracite solid electrolyte having a composition of 2Cl (x=0~1) is characterized in that it is manufactured including the steps of mixing LiOH or Li2CO3 and H3BO3 or B2O3 and LiCl raw materials; melting and quenching the raw material mixture at 600°C or higher; and cooling, recovering, and pulverizing the melt.
[0017] The lithium chloroboracite-based solid electrolyte of the present invention can solve the problem of environmental stability in which P2S5 and Li2S, which are used as raw materials for existing argyrodite-based sulfide solid electrolytes, react with moisture to generate hydrogen sulfide (H2S), and thus, by manufacturing a secondary battery including the lithium chloroboracite-based solid electrolyte, it is possible to replace secondary batteries using existing liquid electrolytes in the market.
[0018] The present invention provides a solid electrolyte of lithium chloroboracite type, which has a particle shape and high purity and ionic conductivity.
[0019] In addition, the lithium chloroboracite-based solid electrolyte of the present invention can solve the problem of environmental stability in which P2S5 and Li2S, which are used as raw materials for existing argyrodite-based sulfide solid electrolytes, react with moisture to generate hydrogen sulfide (H2S).
[0020] In addition, by manufacturing a secondary battery including the lithium chloroboracite-based solid electrolyte of the present invention, it is possible to replace secondary batteries using existing liquid electrolytes in the market.
[0021] Figure 1 is XRD data of lithium chloroborasite.
[0022] Figure 2 is a SEM image showing lithium chloroborasite particle sizes of 2 to 40 μm.
[0023] Figure 3 is an image after lithium chloroborasite gold coating.
[0024] Figure 4 is a photograph showing the coating thickness of lithium chloroborasite after the gold coating of Figure 3 using SEM-BSE (Back Scattered Electron).
[0025] Figure 5 shows data measuring Li ion conductivity at room temperature after gold coating.
[0026] Figure 6 is a graph showing the change in ionic conductivity according to temperature of the solid electrolyte of the present invention.
[0027] Preferred embodiments of the present invention are described in detail, and the description of the following embodiments is provided by way of example, but is not limited thereto.
[0028]
[0029] 1. Composition of solid electrolyte
[0030] The solid electrolyte of the embodiment of the present invention has a composition of lithium chloroboracite as shown below. (See XRD Data of Fig. 1)
[0031] Li 4+x B7O 12+x / 2 Cl (x=0~1)
[0032] The lithium chloroborasite of the above composition is manufactured from LiOH or Li2CO3 and H3BO3 or B2O3 and LiCl raw materials, and has higher ionic conductivity and lower activation energy.
[0033]
[0034] 2. Measurement of ionic conductivity according to sample conditions
[0035] The solid electrolyte of one embodiment of the present invention has a Li ion conductivity of 1.0 x 10 when measured at room temperature of 25°C after sintering. -6 It was more than S / cm.
[0036] - Electrical conductivity model / measurement conditions -
[0037] EIS SP-300, Scan fi=7.0MHz, ff=1.0 Hz, Nd=10 points per decade
[0038] sinus amplitude Va=20.0 mV, pw=0.10, Na=2, E Range=-10V~10V
[0039]
[0040] 3. Manufacturing of all-solid-state secondary batteries
[0041] An all-solid-state secondary battery is manufactured by manufacturing a positive electrode layer, a negative electrode layer, and a solid electrolyte layer using the method described below and then laminating them.
[0042] The solid electrolyte may be a solid electrolyte having a composition according to one embodiment of the present invention. In one embodiment, the boron oxide-based solid electrolyte is produced by treating the starting material of the boron oxide-based solid electrolyte using a melting quenching method or mechanical milling method. Furthermore, after such treatment, additional calcination may be performed. When additional calcination is performed, crystallization of the solid electrolyte progresses, resulting in improved electrical conductivity characteristics.
[0043] A solid electrolyte of one embodiment of the present invention is manufactured by the following manufacturing method. First, LiOH or Li2CO3 and H3BO3 or B2O3 and LiCl raw materials are mixed with Li4 + x B7O 12 +x / Mix in a mixing ratio corresponding to lithium chloroborasite having a composition of 2Cl (x=0~1).
[0044] An all-solid-state secondary battery according to one embodiment of the present invention can be manufactured by laminating and rolling a positive electrode layer, a negative electrode layer, and a solid electrolyte layer so that the positive electrode layer and the negative electrode layer sandwich the solid electrolyte layer.
[0045]
[0046] Comparative examples and examples
[0047]
[0048] Comparative Example 1; Bulk lithium chloroboracite
[0049] Comparative Example 2: Implementation of ionic conductivity according to grinding
[0050] Comparative Example 2 vs. Examples 1 and 2; Comparison according to particle size
[0051] Comparative Example 2 vs. Example 3; Comparison according to firing time
[0052] Example 3 vs. Example 4; Comparison of sizes at different firing times
[0053] Comparative Example 2 vs. Example 5; Comparison according to firing temperature
[0054] Comparative Example 2 vs. Example 6; Comparison according to size at changed firing temperature
[0055]
[0056] Examples 1-6. Preparation of solid electrolyte
[0057] Lithium chloroboracite having the following composition was prepared by mixing LiOH or Li2CO3 and H3BO3 or B2O3 and LiCl raw materials. (See XRD data in Fig. 1)
[0058] Li 4+x B7O 12+x / 2 Cl (x=0~1)
[0059]
[0060] Comparative Examples 1 to 2; Lithium chloroboracite having the following composition was manufactured by mixing LiOH or Li2CO3 and H3BO3 or B2O3 and LiCl raw materials in the same manner as in Examples 1 to 6, and a solid electrolyte was manufactured to evaluate ionic conductivity and stability.
[0061] Li 4+x B7O 12+x / 2 Cl (x=0~1)
[0062]
[0063] <Evaluation of ionic conductivity of solid electrolytes>
[0064] The ionic conductivity of the solid electrolyte obtained in the present invention was measured by the following method (see Table 1).
[0065] Press the solid electrolyte (pressure 100 MPa / cm) 2 ) to produce a pellet. Then, as shown in Fig. 2, Au coating was performed to produce a pellet for measuring ionic conductivity, and the Li ion conductivity at room temperature (25°C) was measured using an AC impedance measuring device at room temperature, and the ionic conductivity was 1.8 x 10 -6 It was more than S / cm.
[0066] Additionally, ionic conductivity was measured while changing the temperature to 40℃, 50℃, 60℃, 70℃, and 80℃.
[0067] As shown in Fig. 4, it was confirmed by SEM-BSE (Back Scattered Electron) that the coating thickness of lithium chloroborasite after gold coating of Fig. 3 was 90 to 100 nm.
[0068]
[0069] <Stability of solid electrolytes>
[0070] The stability of a general lithium electrolyte is due to the reaction between cations and anions, and thus requires a separator, but in the case of the solid electrolyte of the present invention, the cations and anions are separated by the solid electrolyte and do not meet, so they are stable.
[0071] It is widely known that in the case of sulfide as a material for all-solid-state electrolytes, hydrogen sulfide is generated according to the chemical formula below, and therefore, it must be manufactured in an environment without moisture during manufacturing.
[0072] MS (sulfide) + H2O → MO (metal oxide) + H2S
[0073] 2MS(sulfide) + O2→ 2MO(metal oxide) + 2S
[0074] On the other hand, the lithium chloroborasite oxide of the present invention has a very low reactivity with moisture in the air, and even if it reacts, it does not contain sulfur, so it has the advantage of not generating hydrogen sulfide, a harmful substance.
[0075] The solid electrolyte of the present invention manufactured as described above has the following advantages.
[0076] 1) Solid electrolytes have excellent safety as there is no risk of evaporation due to temperature changes or leakage due to external impact, no swelling, and no explosion or ignition characteristics even under extreme external conditions such as heat and pressure.
[0077] 2) Stackable bipolar electrodes, in which a cathode and anode are combined on both sides of a current collector, can be manufactured. The application of bipolar electrodes enables high voltages of over 10 V to be generated from a single cell. For example, to achieve 14.4 V in a lithium-ion battery, four 3.6 V cells must be arranged, but this is possible with an all-solid-state battery from a single cell. The effect of single cellization reduces the separator, current collector, and cell external materials (pouches), thereby reducing volume. Furthermore, by minimizing the BMS (battery management system), high energy density per volume can be achieved.
[0078] 3) Unlike liquid electrolytes, a desolvation reaction, where lithium ions separate from the solvent, is unnecessary. The charge / discharge reaction is directly reflected in the diffusion reaction of lithium ions within the solid, enabling high output.
[0079] 4) Compared to existing organic electrolytes, it can ensure stable performance across a wide temperature range. High ionic conductivity is expected, particularly at low temperatures. A major concern for electric vehicle users is the decline in battery performance in winter, resulting in reduced driving range. If a Tesla Model X is left parked on a cold night with a 50% charge, its charge rate drops to 30% the next morning. The advent of the all-solid-state battery era will eliminate this concern regarding low-temperature environments.
[0080] 5) The battery structure is simple and does not require a separator. During the manufacturing process, a slurry-like solid electrolyte is coated onto the cathode active material. This continuous process, without the need for a liquid electrolyte injection process, allows for the creation of various multilayer cell configurations.
Claims
1. Li 4+x B7O 12+x / 2 Lithium chloroboracite solid electrolyte having a composition of Cl (x=0~1).
2. A solid electrolyte according to claim 1, characterized in that the lithium chloroboracite is manufactured from LiOH or Li2CO3 and H3BO3 or B2O3 and LiCl raw materials.
3. In paragraph 1, Li ion conductivity is 1.0 x 10 at room temperature (25℃). -6 A solid electrolyte characterized by having a density of S / cm or more.
4. In paragraph 1, A solid electrolyte characterized in that the lithium chloroborasite is a nanoparticle having a diameter of 10 nm to 300 μm.
5. A secondary battery comprising a solid electrolyte according to any one of claims 1 to 4.
6. Step of mixing LiOH or Li2CO3 and H3BO3 or B2O3 and LiCl raw materials; A step of melting and quenching the above raw material mixture at 600°C or higher; and Li comprising a step of cooling the above melt, recovering it, firing it, and crushing it; 4+x B7O 12+x / 2 A method for producing a lithium chloroboracite solid electrolyte having a composition of Cl (x=0~1).
Citation Information
Patent Citations
Black tea-based natural tea manufacturing method with anti-obesity