A hydrogel composition, a method of preparing the same and uses thereof
The hydrogel substrate using functionalized graphene oxide addresses cytotoxicity and cost issues in cell culture by enabling triaxial mechanical manipulation and reducing serum usage, improving cell and seed growth through controlled magnetic manipulation and mechanical strength, thus enhancing cell culture and seed germination processes.
Patent Information
- Application Number
- PCT/SG2024/050270
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Current cell culture substrates face challenges such as cytotoxic and non-physiological effects from magnetic labeling, high costs due to expensive growth factors and serum, and significant cell mortality, while also struggling to replicate seed microenvironments effectively for agriculture and food production.
A hydrogel composition comprising functionalized graphene oxide, which allows for triaxial mechanical manipulation of cells without cytotoxic effects, reduces serum and growth factor usage, and replicates seed germination microenvironments through paramagnetic manipulation, enabling improved cell growth and seed germination.
The hydrogel substrate enhances cell proliferation, viability, and seed germination by providing mechanical strength and controlled magnetic manipulation, reducing costs and cell mortality, and facilitating imaging for research, while maintaining a physiologically relevant environment.
Smart Images

Figure IMGF000027_0001 
Figure 00000034_0000 
Figure 00000034_0001
Abstract
Description
[0001] A HYDROGEL COMPOSITION, A METHOD OF PREPARING THE SAME AND
[0002] USES THEREOF
[0003] CROSS-REFERENCE TO RELATED APPLICATIONS
[0004] This application claims priority to Singapore application number 10202301 148V filed with the Intellectual Property Office of Singapore on 25 April 2023, the contents of which is hereby incorporated by reference in its entirety for all purposes.
[0005] TECHNICAL FIELD
[0006] The present invention relates generally to a hydrogel and a method of preparing the hydrogel as described herein. The present invention also relates to the hydrogel as described herein for use as a cell culture substrate for triaxial mechanical manipulation of cells. The present invention also relates to the cell culture substrate as described herein for use in culturing cells. The present invention also relates to the hydrogel for use as a seed germination substrate.
[0007] BACKGROUND ART
[0008] Hydrogels are commonly used hydrophilic polymers in various applications due to its water retention ability. As such, it possesses similar properties to natural tissues, such as flexibility and stiffness. These properties of hydrogels can be further manipulated by both physical and chemical means, allowing it to transit between gel-like and liquid states with ease. Physical means of manipulating hydrogels include the variation of light intensity, pressure, temperature and solvent composition, while the chemical means of manipulation include the use of chelation reagents and varying solute concentrations. As such, there is a heightened interest for hydrogel-based materials with these desirable properties to be used for agriculture, pharmaceutical and cell culture applications. Cell growth has been known to respond to mechanical stimulus and recently, there is a growing interest to investigate the effects of stretch application on cells indirectly by manipulating the microenvironment around them. One value proposition for stretch application of cells pertains to the cell culture market. Cell culturingbased companies are rapidly developing and the inputs and consumables alone already account for approximately $35 billion annually, amongst which include cultured meat companies which are presently under fast industrialization. Advantageously, cultured meat has the potential to alleviate the greenhouse effect due to anthropological livestock production while supplementing the world food supply. In most cases, a substrate material is provided for culturing cells, which is capable of spatiotemporal control in two or three axes. However, many of the technologies pertaining to spatiotemporal manipulation of cells culture involve magnetically labelling the cell which is undesirable as this may cause cytotoxic and non-physiological effects. Further, the primary upstream bottlenecks faced by the industry include the high cost from use of expensive growth factors and serum in media, and significant cell mortality during cell growth in bioreactors.
[0009] Relatedly, such mechanical manipulations may also be applicable in the agriculture industry, in particular, the use of physical methods over chemical methods to increase plant production in addressing global food production. Some physical methods include the application of magnetic fields (magneto-priming) and radiation treatment (e.g., infrared, gamma and X-rays). While magneto-priming remains the most eco-friendly and cost-effective method, the mechanistic pathway is still not well understood as it remains a challenge to replicate the seed microenvironment with environmental factors, such as humidity, temperature and light, with a magnetic field.
[0010] There is thus a need to provide a substrate that overcomes, or at least ameliorates, one or more of the disadvantages described above.
[0011] SUMMARY
[0012] In one aspect, the present disclosure refers to a hydrogel comprising a functionalised graphene oxide.
[0013] Advantageously, the hydrogel, acting as a substrate, is able to mechanically manipulate cells without cytotoxic and non-physiological effects, and still able to provide good imaging. Still advantageously, the hydrogel is able to replicate seed germination microenvironments with paramagnetic manipulation.
[0014] In another aspect, the present disclosure refers to a method of preparing a hydrogel comprising the steps of: a) oxidising graphite to graphene oxide; b) functionali ing the graphene oxide of step a) with a crosslinker; and c) forming a hydrogel from a mixture of a liquid medium, the functionalized graphene oxide (GOC) of step b), an alginate solution, a hydrophilic agent, an additive and a crosslinking agent. Advantageously, the method of preparing the hydrogel may avoid the use of dangerous and corrosive / explosive chemical precursors currently used in the art.
[0015] In one example, where the liquid medium is a cell media, the hydrogel comprising a functionalised graphene oxide is a cell culture substrate.
[0016] In another example, where the liquid medium is water, the hydrogel comprising a functionalized graphene oxide is a seed germination substrate.
[0017] In another aspect, the present disclosure refers to a cell culture substrate comprising the hydrogel as described herein for use in culturing cells.
[0018] In another aspect, the present disclosure refers to a cell culture substrate comprising the hydrogel as described herein for use in triaxial manipulation of the cell.
[0019] In another aspect, the present disclosure refers to use of the hydrogel as described herein in the preparation of a cell culture substrate for culturing cells.
[0020] In another aspect, the present disclosure refers to use of the hydrogel as described herein in the preparation of a cell culture substrate for triaxial manipulation of the cells.
[0021] Advantageously, the cell culture substrate as described herein has paramagnetic property for mechanical stretching, the ability to sustain cultivation of living cell and still able to act as a reservoir for containment of growth media to sustain the survival of cells.
[0022] Further advantageously, the cell culture substrate as described herein allows for capture and maintenance of cell culture medium and provides triaxial mechanical manipulation of the cell via paramagnetic manipulation of the microenvironment within the hydrogel. The paramagnetic manipulation of the microenvironment within the biologically inert hydrogel can be controlled by manipulation of magnetic fields, which allows for high spatiotemporal resolution of the cell without cytotoxic effects, thus improving cell and tissue growth. The functionalized graphene oxide provides both mechanical strength and the paramagnetic manipulation to the cell culture substrate.
[0023] Further advantageously, the cell culture substrate as described herein allows for the transmission of light, allowing for imaging of the cell during mechanical manipulation, providing valuable insight into cell behaviour and growth for research and development. Further advantageously, the cell culture substrate of the present disclosure complements the upstream process of cultured meat value chain by removing the hassle of cell culturing for the cultured meat players and enhancing the growth and proliferative capacity of their proprietary cellular materials with significantly reduced usage of serum and growth factors in cell culturing media to produce cultured meat. This may lead to significant cost cutting on maintenance and culturing of cultured meat cells.
[0024] In another aspect, the present disclosure refers to a seed germination substrate comprising the hydrogel as described herein for use in germinating seed.
[0025] In another aspect, the present disclosure refers to use of the hydrogel as described herein in the preparation of a seed germination substrate for germinating seeds.
[0026] Advantageously, the seed germination substrate provides a good platform to study the magnetic effect on seed germination by replicating the microenvironment of the seed with localised paramagnetic manipulation. Moreover, solvent retention capability of the hydrogel provides the necessary moist environment which aids in the speeding up of seed germination. With a crosslinked matrix, newly sprouted seedlings have the necessary anchorage which promotes further development and prevent drowning of the seedling.
[0027] DEFINITIONS
[0028] The following words and terms used herein shall have the meaning indicated:
[0029] Unless specified otherwise, the terms “comprising” and “comprise”, and grammatical variants thereof, are intended to represent “open” or “inclusive” language such that they include recited elements but also permit inclusion of additional, unrecited elements.
[0030] As used herein, the term “about”, in the context of concentrations of components of the formulations, typically means + / - 5% of the stated value, more typically + / - 4% of the stated value, more typically + / - 3% of the stated value, more typically, + / - 2% of the stated value, even more typically + / - 1% of the stated value, and even more typically + / - 0.5% of the stated value.
[0031] Throughout this disclosure, certain embodiments may be disclosed in a range format. It should be understood that the description in range format is merely for convenience and brevity and should not be construed as an inflexible limitation on the scope of the disclosed ranges. Accordingly, the description of a range should be considered to have specifically disclosed all the possible sub-ranges as well as individual numerical values within that range. For example, description of a range such as from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6 etc., as well as individual numbers within that range, for example, 1, 2, 3, 4, 5, and 6. This applies regardless of the breadth of the range.
[0032] Certain embodiments may also be described broadly and generically herein. Each of the narrower species and subgeneric groupings falling within the generic disclosure also form part of the disclosure. This includes the generic description of the embodiments with a proviso or negative limitation removing any subject matter from the genus, regardless of whether or not the excised material is specifically recited herein.
[0033] DETAILED DESCRIPTION OF OPTIONAL EMBODIMENTS
[0034] Exemplary, non-limiting embodiments of a hydrogel comprising a functionalized graphene oxide will now be disclosed.
[0035] The hydrogel may be formed from a hydrogel precursor solution which is a mixture of a liquid medium, a functionalized graphene oxide, an alginate solution, a hydrophilic agent, an additive and a crosslinking agent.
[0036] The graphene oxide may be functionalized by a crosslinkcr to form the functionalized graphene oxide (GOC), wherein the crosslinker is selected from the group consisting of methyltrimethoxy silane, methyltriethoxy silane, dimethyldimethoxy silane, dimethyldiethyoxysilane, tetramethoxysilane, tetraethoxysilane, vinyltriacetoxysilane, vinyltricthoxysilanc, N-(3-dimcthylaminopropyl)-N'-cthylcarbodiimidc hydrochloride, N- hydroxysuccinimide, 2-aminoethyl methacrylate hydrochloride and any combinations thereof. The crosslinker may be vinyltriethoxysilane.
[0037] The functionalized graphene oxide may be weakly ferromagnetic or known as paramagnetic. The functionalized graphene oxide may be intrinsically weakly ferromagnetic, that is, the ferromagnetism is due to the functionalized graphene oxide and not due to any magnetic materials added to the functionalized graphene oxide. The weak ferromagnetism may be characterized by an unsaturated magnetic hysteresis loop measured by magnetometry techniques. The magnetometry' techniques include, but arc not limited to, vibrating sample magnetometry (VSM), magneto-optical Kerr effect (MOKE), high frequency electron paramagnetic or ferromagnetic resonance (ESR / FMR)), synchrotron magnetometry and superconducting quantum interference device (SQUID).
[0038] The ferromagnetism of the functionalized graphene oxide stems from the paramagnetic nature of the functionalized graphene oxide. The magnetic property of the functionalized graphene oxide is due to the dispersion of pi electrons and sp3hybridised carbon molecules as the pi electrons are able to move freely and align in the direction of the magnetic field. This in turn increases the magnetic moment within the functionalized graphene oxide. The paramagnetic property of the functionalized graphene oxide is described by the Curie-Weiss law, whereby above a critical temperature, ferromagnetic materials become paramagnetic as the thermal energy is sufficient to overcome the position of the magnetic moments.
[0039] The liquid medium may be selected from the group consisting of water, saline, buffer solutions, cell media and any mixture thereof. Where the liquid medium is water, the hydrogel may be termed as a seed germination substrate, whereby the seed germination substrate comprises the functionalised graphene oxide. The seed germination substrate may be in the form of the hydrogel comprising the functionalised graphene oxide. Where the liquid medium is cell media, the hydrogel may be termed as a cell culture substrate, whereby the cell culture substrate comprises the functionalised graphene oxide. The cell culture substrate may be in the form of the hydrogel comprising the functionalised graphene oxide.
[0040] The alginate solution may be selected from the group consisting of alginic acid, sodium alginate, potassium alginate, ammonium alginate and propylene glycol alginate. The alginate solution may be sodium alginate.
[0041] Advantageously, the functionalised graphene oxide provides improved crosslinking with alginate, resulting in a higher Young’s modulus. This aids in increasing the stiffness of the hydrogel. When the hydrogel is used as a seed germination substrate, the improved stiffness of the hydrogel allows for better propagation of mechanical forces to the external parts of seedlings placed in the hydrogel which in turn induce faster maturation and greater growth of the seedlings in terms of size.
[0042] The Young’s modulus of the hydrogel with the functionalised graphene oxide may be in the range of about 800 Pa to about 1 000 Pa, about 900 Pa to about 1 000 Pa or about 800 Pa to about 900 Pa as measured by nanoindentation (assuming that the Young’s modulus is proportional to the indentation hardness). This is in comparison to conventional hydrogel without the functionalised graphene oxide where the Young’s modulus may be in the range of about 500 Pa to about 700 Pa, about 600 Pa to about 700 Pa or about 500 Pa to about 600 Pa as measured by nanoindentation. The Young’s modulus of the hydrogel with the functionalised graphene oxide may be adjusted according to the concentration of functionalised graphene oxide used, with higher concentrations leading to increased Young’s modulus.
[0043] With the increased Young’s modulus, and given that Young’s modulus is defined as the ratio of tensile stress to tensile strain, propagation of force via hydrogel to cells / tissue would be enhanced. Henceforth, any forms / means of stretching on elastomer substrate can better propagate mechanical forces via hydrogel to the cells / tissue sandwiched within the hydrogel.
[0044] The hydrophilic agent may be selected from the group consisting of hyaluronic acid, sodium acetylated hyaluronate and sodium hyaluronate. The hydrophilic agent may be sodium hyaluronate.
[0045] The sodium hyaluronate acts as a water retention reagent in the hydrogel due to its highly anionic nature. Advantageously, sodium hyaluronate is able to cross-polymerise, affording better water retention capabilities to the hydrogel.
[0046] The additive may be selected from the group consisting of collagen, fibronectin and a combination thereof.
[0047] The crosslinking agent may be metal chloride salts, wherein the metal may be selected from the group consisting of calcium (Ca), strontium (Sr), barium (Ba) and zinc (Zn). The crosslinking agent may be calcium chloride (CaCh).
[0048] Tn the functionalized graphene oxide, C-N bonds are present (which are absent in reduced graphene oxide (rGO)). The functionalized graphene oxide may act as a crosslinker to covalently crosslink with the additive and / or hydrophilic agent when forming the hydrogel. With the hydrogel’s crosslinking agents and use of functionalised graphene oxide, the physical property of the hydrogel can be modulated to not only be manipulablc by magnetism, but can also better transmit mechanical forces through the hydrogel to induce mechanotransduction in the various systems (such as cell, tissue or seed systems). Hence, the use of functionalised graphene oxide differs from existing prior art which adds rGO into hydrogel for magnetic property only, as the use of functionalised graphene oxide goes one step further to capitalise on the additional crosslinking feature of the functionalised graphene oxide. Exemplary, non-limiting embodiments of a method of preparing a hydrogel will now be disclosed.
[0049] The method may comprise the steps of: a) oxidising graphite to graphene oxide; b) functionalizing the graphene oxide of step a) with a crosslinker; and c) forming a hydrogel from a mixture of a liquid medium, the functionalized graphene oxide (GOC) of step b), an alginate solution, a hydrophilic agent, an additive and a crosslinking agent.
[0050] The method may be regarded as a modified Hummer’s method to form the functionalised graphene oxide.
[0051] Advantageously, the method of preparing the cell culture substrate as described herein avoids the use of dangerous and corrosive / explosive chemical precursors currently used in the art.
[0052] The graphite may be natural graphite flakes.
[0053] The oxidising step in step a) may further comprise the steps of: ai) mixing the graphite with an acid and at least one oxidising agent to form a solution; and aii) stirring the solution of step ai) for a duration at a temperature to form the graphene oxide.
[0054] The acid may be selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid and combinations thereof. The acid may be sulfuric acid.
[0055] The oxidising agent may be selected from the group consisting of potassium permanganate, hydrogen peroxide, potassium chlorate and mixtures thereof.
[0056] The mixing step ai) may be carried out using a magnetic stirrer and stirred at a rotation speed in the range of about 200 rotations per minute to about 800 rotations per minute, about 400 rotations per minute to about 800 rotations per minute, about 600 rotations per minute to about 800 rotations per minute, about 200 rotations per minute to about 600 rotations per minute or about 200 rotations per minute to about 400 rotations per minute. The mixing may be carried out at a temperature of below about 15 °C, or in the range of about 0 °C to about 15 °C, about 5 °C to about 15 °C or about 10 °C to about 15 °C for a duration of about 1 hour to about 4 hours, about 2 hour to about 4 hours or about 2 hours to 3 hours or about 2 hour.
[0057] The stirring step aii) may be conducted at a first temperature in the range of about 15 °C to about 55 °C, about 25 °C to about 45 °C, about 30 °C to about 40 °C or about 35 °C for a duration of about 1 hour to 6 hours, about 2 hours to about 6 hours, about 3 hours to about 6 hours, about 4 hours to about 6 hours, about 2 to 4 hours or about 3 to about 4 hours. The temperature of the stirring step aii) may be increased to a second temperature in the range of about 90°C to about 100°C, and about 95 °C to about 100 °C for a duration of about 10 minutes to about 30 minutes, about 10 minutes to about 20 minutes. The temperature of the stirring step aii) may be reduced to a third temperature in the range of about 20 °C to about 30 °C, and about 25 °C to about 30 °C, for a duration of about 1 hour to 6 hours, about 2 hours to about 6 hours, about 3 hours to about 6 hours, about 4 hours to about 6 hours, about 2 to 4 hours or about 3 to about 4 hours.
[0058] The stirring step aii) may further comprise before obtaining the graphene oxide, the step of drying a resulting gel-like mixture comprising the graphene oxide. The drying step may be conducted at a temperature in the range of about 60°C to about 70°C, and about 65 °C to about 70 °C for a duration of about 1 hour to about 6 hours, about 2 hours to about 6 hours, about 3 hours to about 6 hours, about 4 hours to about 6 hours, about 2 to 4 hours or about 3 to about 4 hours. The graphene oxide may be recovered from the resulting gel-like mixture via centrifugation.
[0059] The centrifugation may be carried out at a speed of about 10 000 rotations per minute to about 50 000 rotations per minute, about 20 000 rotations per minute to about 50 000 rotations per minute, about 30 000 to about 50 000 rotations per minute, about 40 000 rotations per minute to about 50 000 rotations per minute, about 10 000 rotations per minute to about 40 000 rotations per minute, about 10000 rotations per minute to about 30 000 rotations per minute or about 10 000 rotations per minute to about 20 000 rotations per minute.
[0060] The recovered graphene oxide may be dried in an oven at a temperature range of about 70 °C to about 100 °C, about 80 °C to about 100 °C, about 90 °C to about 100 °C, about 70 °C to about 90 °C or about 70 °C to about 80 °C for a duration of about 12 hours to about 48 hours, about 24 hours to about 48 hours or about 12 hours to about 24 hours.
[0061] The functionalising step in step b) may further comprise the steps of: bi) dispersing the graphene oxide in a solvent comprising a crosslinker to form a solution; and bii) heating the solution of step bi) at a temperature for a duration.
[0062] The solvent used in step bi) may be a polar solvent. The polar solvent may be deionised water.
[0063] The graphene oxide may be dispersed in the solution at a concentration in the range of 10 mg / mL to about 100 mg / mL, about 20 mg / mL to about 100 mg / mL, about 40 mg / mL to about 100 mg / mL, about 60 mg / mL to about 100 mg / mL, about 80 mg / mL to about 100 mg / mL, about 10 mg / mL to about 80 mg / mL, about 10 mg / mL to about 60 mg / mL, about 10 mg / mL to about 40 mg / mL or about 10 mg / mL to about 20 mg / mL.
[0064] The crosslinker may be selected from the group consisting of methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethyoxysilane, tetramethoxy silane, tertraethoxysilane, vinyltriacetoxysilane, vinyltriethoxy silane and any combinations thereof. The crosslinker may be vinyltriethoxysilane.
[0065] The solution containing the dispersed graphene oxide from step bi) may further comprise an acid.
[0066] The acid may be selected from the group consisting of nitric acid, hydrochloric acid, sulfuric acid and combinations thereof. The acid may be hydrochloric acid.
[0067] The temperature of the heating step bii) may be in a range of about 50 °C to about 100 °C, about 60 °C to about 100 °C, about 70 °C to about 100 °C, about 80 °C to about 100 °C, about 90 °C to about 100 °C, about 50 °C to about 90 °C, about 50 °C to about 80 °C, about 50 °C to about 70 °C or about 50 °C to about 60 °C. The duration of the heating step bii) may be in a range of about 5 hours to about 10 hours, about 6 hours to about 10 hours, about 7 hours to about 10 hours, about 8 hours to about 10 hours, about 9 hours to about 10 hours, about 5 hours to about 9 hours, about 5 hours to about 8 hours, about 5 hours to about 7 hours or about 5 hours to about 6 hours.
[0068] The functionalized graphene oxide may be recovered via centrifugation.
[0069] The recovered functionalized graphene oxide may be dried in an oven at a temperature range of about 70 °C to about 100 °C, about 80 °C to about 100 °C, about 90 °C to about 100 °C, about 70 °C to about 90 °C or about 70 °C to about 80 °C for a duration of about 12 hours to about 48 hours, about 24 hours to about 48 hours or about 12 hours to about 24 hours. The forming step c) may further comprise the steps of: ci) providing a hydrogel precursor solution comprising the mixture of the liquid medium, the functionalized graphene oxide (GOC) of step b), the alginate solution, the hydrophilic agent, the additive and the crosslinking agent; and cii) setting the hydrogel precursor solution to form the hydrogel.
[0070] The liquid medium in providing step ci) may be selected from the group consisting of water, saline, buffer solutions, cell media and any mixture thereof. The liquid medium may be water. Where the liquid medium is water, the method of preparing the hydrogel may be deemed as a method of preparing a seed germination substrate, whereby the seed germination substrate comprises the functionalised graphene oxide. The seed germination substrate may be in the form of the hydrogel comprising the functionalised graphene oxide. The liquid medium may be cell media. Where the liquid medium is cell media, the method of preparing the hydrogel may be deemed as a method of preparing a cell culture substrate, whereby the cell culture substrate comprises the functionalised graphene oxide. The cell culture substrate may be in the form of the hydrogel comprising the functionalised graphene oxide.
[0071] The providing step in step ci) may further comprise the step of dispersing the functionalized graphene oxide in the liquid medium at a concentration in the range of about 1 mg / mL to about 4 mg / mL, about 2 mg / mL to about 4 mg / mL, about 3 mg / mL to about 4 mg / mL, about 1 mg / mL to about 3 mg / mL or about 1 mg / mL to about 2 mg / mL.
[0072] Where the liquid medium is the cell media, the cell media may be selected from the group consisting of natural cell media or synthetic cell media. The cell media may be selected from the group consisting of Minimum Essential Medium Eagle - alpha modification (Alpha MEM) with or without nucleosides, Dulbecco’s Modified Eagle’s Medium / Nutrient Elam’s Mixture F-12 (DMEM / F-12), Iscove’s Modified Dulbecco’s Medium (IMDM), Minimum Essential Medium Eagle (MEM) with Earle’s salts and non-essential amino acids (NEAA) McCoy’s 5 A medium and RPMI 1640 medium. The cell media may be Dulbecco’s Modified Eagle Medium (DMEM) or any other suitable cell culture media known in the art.
[0073] The cell media comprising the functionalized graphene oxide may be dispersed by sonication at a temperature in the range of about 30 °C to about 50 °C, about 40 °C to about 50 °C or about 30 °C to about 40 °C for a duration of about 30 minutes to about 120 minutes, about 60 minutes to about 120 minutes, about 90 minutes to about 120 minutes, about 30 minutes to about 90 minutes or about 30 minutes to about 60 minutes.
[0074] The sonicated cell media solution comprising the dispersed functionalized graphene oxide may be mixed with the alginate solution and the hydrophilic agent, wherein the solution may be stirred at a temperature in the range of about 1 °C to about 10 °C, about 2 °C to about 10 °C, about 4 °C to about 10 °C, about 6 °C to about 10 °C, about 8 °C to about 10 °C, about 1 °C to about 8 °C, about 1 °C to about 6 °C, about 1 °C to about 4 °C or about 1 °C to about 2 °C for a duration of about 12 hours to about 48 hours, about 24 hours to about 48 hours, about 36 hours to about 48 hours, about 12 hours to about 36 hours or about 12 hours to about 24 hours. The mixture may be stirred at 4 °C for a duration of 24 hours.
[0075] The alginate may be selected from the group consisting of alginic acid, sodium alginate, potassium alginate, ammonium alginate and propylene glycol alginate. The alginate may be sodium alginate.
[0076] The hydrophilic agent may be selected from the group consisting of hyaluronic acid, sodium acetylated hyaluronate and sodium hyaluronate. The hydrophilic agent may be sodium hyaluronate.
[0077] The additive may be collagen, fibronectin or a combination thereof.
[0078] The concentration of collagen may be in the range of about 2 mg / mL to about 10 mg / mL, about 4 mg / mL to about 10 mg / mL, about 6 mg / mL to about 10 mg / mL, about 8 mg / mL to about 10 mg / mL, about 2 mg / mL to about 8 mg / mL, about 2 mg / mL to about 6 mg / mL or about 2 mg / mL to about 4 mg / mL. The concentration of collagen may be 4 mg / mL.
[0079] The mixture comprising the liquid media, functionalized graphene oxide, alginate solution, hydrophilic agent and additive may be adjusted to a pH in the range of about pH 7 to about pH 8, about pH 7.2 to about pH 8, about pH 7.4 to about pH 8, about PH 7.6 to about pH 8, about pH 7.8 to about pH 8, about pH 7 to about pH 7.8, about pH 7 to about pH 7.6, about pH 7 to about pH 7.4 or about pH 7 to about pH 7.2. The pH may be pH 7.4.
[0080] The pH may be adjusted via the addition of a base selected from the group consisting of sodium hydroxide, potassium hydroxide or mixtures thereof. The base may by sodium hydroxide. A crosslinking agent may then be added to the pH-adjusted mixture comprising the liquid media, functionalized graphene oxide, alginate solution, hydrophilic agent and additive to form the hydrogel precursor solution.
[0081] The crosslinking agent may be metal chloride salts, wherein the metal may be selected from the group consisting of calcium (Ca), strontium (Sr), barium (Ba), and zinc (Zn). The crosslinking agent may by calcium chloride (CaCh).
[0082] The functionalised graphene oxide may also act as a crosslinker to covalently crosslink the additive and / or the hydrophilic agent.
[0083] The setting step cii) may further comprise setting the hydrogel precursor solution comprising the liquid media, functionalized graphene oxide, alginate solution, hydrophilic agent, additive and crosslinking agent via incubation in a carbon dioxide (CO2) incubator. In one example, the setting of the hydrogel precursor solution is gelation.
[0084] The incubation may be carried out at a temperature in the range of about 35 °C to about 40 °C, about 37 to about 40 °C or about 35 °C to about 37 °C for a duration in a range of about 10 minutes to about 20 minutes, about 15 minutes to about 20 minutes or about 10 minutes to about 15 minutes. The temperature may be 37 °C and the duration may be 15 minutes.
[0085] The amount of CO2 in the incubator may be in the range of about 1% to about 10%, about 2% to about 10%, about 4% to about 10%, about 6% to about 10%, about 8% to about 10%, about 1% to about 8%, about 1% to about 6%, about 1% to about 4% or about 1% to about 2%. The amount of CO2 may be 5%.
[0086] Exemplary, non-limiting embodiments of a cell culture substrate in the form of a hydrogel as described herein for use in culturing cells will now be disclosed.
[0087] The cell culture substrate for use in culturing cells may be subjected to triaxial manipulation of the cells. The triaxial manipulation of the cells may involve physically inducing mechanical forces through the cell culture substrate in the form of the hydrogel. During the culturing of the cells, the cells may be grown sandwiched between an elastomer and the cell culture substrate in the form of the hydrogel or may be grown sandwiched between two layers of the cell culture substrate in the form of the hydrogel. Mechanical forces were then physically induced through the cell culture substrate in the form of the hydrogel. Advantageously, when the hydrogel is used as the cell culture substrate, the inventors have found that cell density growth is greater than when compared to cells grown in the absence of the hydrogel cell culture substrate. This growth is increased further when the cells were sandwiched between two layers of the hydrogel cell culture substrate. The elastomer used during the culturing of the cells may comprise of an elastomeric material. The elastomeric material may not be particularly limited and in one example, can be silicone rubber. Where the elastomer is used for culturing cells, the elastomer may not be toxic to cells and may be biocompatible. Therefore, a suitable elastomer may be one that can be used to culture cells.
[0088] The cell culture substrate for use in culturing cells may be further subjected to mechanically stimulation of the hydrogel to drive differentiation of cells. The mechanical stimulation may be in the form of inducing strain on the hydrogel. As an example, cells (such as H9C2 myoblast cells) were seeded on the cell culture substrate (hydrogel), and when mechanical stimulation in the form of inducing strain was applied to the cell culture substrate (hydrogel), the cells (such as H9C2 myoblast cells) were able to undergo differentiation into another phenotype (such as cardiomyocytes). Advantageously, when the cells that are seeded or cultured on or within the hydrogel substrate are subjected to mechanical stimulation, the use of the hydrogel substrate along with the mechanical stimulation allow the cells to undergo differentiation, as compared to using a non-hydrogel substrate where the same mechanical stimulation on the non-hydrogcl substrate was insufficient to drive differentiation of cells.
[0089] The manipulation of the cells may be conducted in a controllable magnetic field. Advantageously, the inventors have found that cells grown on the hydrogel cell culture substrate, in the presence of mechanical stretching due to the induced magnetic field, showed translocation of mechanosensitive transcription co-activator protein (such as mGFP-YAP) into the nuclei of cells in response to mechanical forces. This shows that mechanical force is able to propagate from external source through the hydrogel cell culture substrate to the cells.
[0090] Further advantageously, the cell culture substrate as described herein allows for the transmission of light, allowing for imaging of the cell during mechanical manipulation, providing valuable insight into cell behaviour and growth for research and development.
[0091] The magnetic field may be controlled using neodymium magnets, a magnetic field generator or any combination thereof.
[0092] The cells may be adherent cells. The adherent cells may be selected from the group consisting of MDCK, HeLA, MCF7, H9C2, C2C12 and MEF cells. The cells may comprise specialized cell types selected from the group consisting of primary cells, secondary cells and stem cells.
[0093] The cell culture substrate in the form of a hydrogel may be further placed in a containment unit capable of ferromagnetic manipulation. Advantageously, the containment unit acts as a capture reservoir should the hydrogel rupture under extreme deformation stresses (e.g., above 130% of its original dimensions). The containment unit is then able to contain the liquid medium and continue to exert ferromagnetic manipulation on the cells. Advantageously, the cell culture substrate as described herein has paramagnetic property for mechanical stretching, the ability to sustain cultivation of living cell and still able to act as a reservoir for containment of growth media to sustain the survival of cells.
[0094] The cells may be embedded within the cell culture substrate (hydrogel). During culturing of the cells, cells may be embedded within the volumetric hydrogel. As an example, the cells may be embedded by mixing cells suspended in the cell media into the alginate solution prior to the addition of the functionalized graphene oxide, the hydrophilic agent, the additive and the crosslinking agent. As an example, when the hydrogel is used as the cell culturing substrate, the embedded cultured cells may be isolated from the hydrogel using a chelating agent via chelation method known in the ail. Advantageously, the cells isolated from the cell culture substrate arc still able to proliferate and remain viable. The chelating agents may be selected from the group consisting of ethylenediaminetetraacetic acid (EDTA), ethylenebis(oxyethylenenitrilo)tetraacetic acid (EGTA), 1,2-cyclohexylenedinitrilotetraacetic acid (CDTA), diethylenetriaminepentaacetic acid (DTPA), salt of citrate and combination thereof. The chelating agents may be ethylenediaminetetraacetic acid (EDTA) or sodium citrate (NaC).
[0095] Advantageously, the hydrogel may significantly enhance cell proliferation, cell viability, and allows ease of use of dye-based fluorescent probes to visualize the cells in comparison with commercially available hydrogels. Further advantageously, the cell culture substrate complements the upstream processing of the cultured meat value chain by removing the hassle of cell culturing for the cultured meat players and enhancing the growth and proliferative capacity of their proprietary cellular- materials with significantly reduced usage of serum and growth factors in cell culturing media to produce cultured meat. This may lead to significant cost cutting on maintenance and culturing of cultured meat cells. Exemplary, non-limiting embodiments of use of the hydrogel as described herein in the preparation of a cell culture substrate for culturing cells will now be disclosed. The cell culture substrate may be prepared by the method as described above.
[0096] Exemplary, non-limiting embodiments of use of the hydrogel as described herein in the preparation of a cell culture substrate for triaxial manipulation of the cells will now be disclosed. The cell culture substrate may be prepared by the method as described above.
[0097] Exemplary, non-limiting embodiments of a seed germination substrate in the form of a hydrogel as described herein for use in seed germination will now be disclosed.
[0098] The seeds that can be planted in the seed germination substrate are not particularly limited and can include any plant seeds. Exemplary seeds may be seeds from Vigna radiata (mung beans), Ocimum bascilicum (basil), and Arundina graminifolia (bamboo orchid).
[0099] When germinating the seeds, the seeds may be placed in the hydrogel as described herein and where needed, be further placed in the containment unit capable of ferromagnetic manipulation as mentioned above. During the germination phase, the time taken for the seeds to germinate (rupture of seed coat and presence of radicle) can be recorded. For germinated seeds, the effect of the hydrogel on growth and development of seedling to young plant (vs control which was normal soil) can be measured by observing the following characteristics after a fixed number of days of cultivation: (1) density of roots; (2) length of roots; (3) lengths of major and minor axes of foliage; (4) length and diameter of hypocotyl; (5) length and diameter of epicotyl; (6) length of stem; and (7) dry mass (after oven treatment for total removal of water content). Hence, the seed germination substrate allows for the monitoring of the germination process.
[0100] Advantageously, the seed germination substrate provides a good platform to study the magnetic effect on seed germination by replicating the microenvironment of the seed with localised paramagnetic manipulation. Moreover, solvent retention capability of the hydrogel provides the necessary moist environment which aids in the speeding up of seed germination. With a crosslinked matrix, newly sprouted seedlings have the necessary anchorage which promotes further development and prevent drowning of the seedling.
[0101] When the seedlings are grown in the seed germination substrate in a magnetic environment, the magnetism may aid in increasing the rate of germination of the seeds. This is in addition to the requirement of water for speeding up germination. Exemplary, non-limiting embodiments of use of the hydrogel as described herein in the preparation of a seed germination substrate for germinating seeds will now be disclosed. The seed germination substrate may be prepared by the method as described above.
[0102] BRIEF DESCRIPTION OF THE DRAWINGS
[0103] The accompanying drawings illustrate a disclosed embodiment and serve to explain the principles of the disclosed embodiment. It is to be understood, however, that the drawings are designed for purposes of illustration only, and not as a definition of the limits of the invention.
[0104] Fig. l
[0105] Fig. 1 shows a box plot with error bar s comparing the number of roots in germinated seedling between a control hydrogel substrate without magnetism, a hydrogel substrate with only bottom magnetism, and a hydrogel substrate with both bottom and side magnetism.
[0106] Fig. 2
[0107] Fig. 2 shows a box plot with error bars comparing the root thickness factor (mm3) in germinated seedling between a control hydrogel substrate without magnetism, a hydrogel substrate with only bottom magnetism, and a hydrogel substrate with both bottom and side magnetism.
[0108] Fig. 3
[0109] Fig. 3 shows a box plot with error bars comparing the foliage area factor (mm2) in germinated seedling between a control hydrogel substrate without magnetism, a hydrogel substrate with only bottom magnetism, and a hydrogel substrate with both bottom and side magnetism.
[0110] Fig. 4
[0111] Fig. 4 shows an illustration of cells seeded on elastomer only (without hydrogel), cells seeded between an elastomer and hydrogel (Composite E-C-H), or cells seeded between two layers of hydrogels on an elastomer (Composite E-H-C-H).
[0112] Fig. 5
[0113] Fig. 5 shows microscopic images comparing the growth of cells on elastomer without hydrogel, two sets of composite E-C-H (Al and A2), and two sets of composite E-H-C-H (Bl and B2). Cells are stably expressing mGFP-YAP which is a mechanosensitive transcription co-activator protein that translocate into the nuclei of cells in response to mechanical forces. Scale bar is at 10 pm. Fig. 6
[0114] Fig. 6 shows a chart comparing the cell density (mm-2) of the cells grown on elastomer without hydrogel (control), two sets of composite E-C-H (Al and A2), and two sets of composite E-H- C-H (B 1 and B 2) from day 1 to day 5. It can be observed that cells can grow much better within the composites E-C-H (Al and A2) and E-H-C-H (B1 and B2) than control.
[0115] Fig. 7
[0116] Fig. 7 shows microscopic images comparing the growth of cells on two sets of composite E-C- H (Al and A2) and two sets of composite E-H-C-H (B 1 and B2). Al and B 1 are used as control without any mechanical stretching induced on the hydrogel. Cells in A2 and B2 arc subjected to mechanical stretching and cells shown with arrows displayed nuclear translocation of mGFP-YAP. Scale bar is at 10 pm.
[0117] Fig. 8
[0118] Fig. 8 shows a box plot with error bars comparing the nuclear / cytoplasmic ratio of mGFP-YAP intensities of cells in composite E-C-H (Al and A2, n=20 each) and of cells in composite E- H-C-H (Bl and B2, n=20 each). For both composites, cells strained under mechanical force experienced greater degree of nuclear translocation of mGFP-YAP (For ****, Mann-Whitney Test was used and a value of p=6.8 x 108was obtained).
[0119] Fig. 9
[0120] Fig. 9 shows fluorescent images of cells tagged with Cell Tracker membrane marker to locate position of cells at different z-axial heights (HEK293T - human embryonic kidney epithelial cells; C2C12 - mouse skeletal muscle cell line).
[0121] Fig. 10A
[0122] Fig. 10A shows an image of hydrogel treated with equivalents of EDTA, where the equivalents of EDTA could not depolymerize the hydrogel.
[0123] Fig. 10B
[0124] Fig. 10B shows an image of hydrogel treated with salts of citrate (NaC), where the salts of citrate fully depolymerize the hydrogel.
[0125] Fig. 11
[0126] Fig. 11 shows a plot of 100,000 cells seeded on Day 0 and after the chelation treatment with Na-Citrate and EDTA, cells were counted again the following day (Day 1). Error bars are shown as ± 1 standard deviation. Total number of cells obtained from both chelation treatments were comparably similar at an average of around 200,000 to 250,000 cells. Fig. 12
[0127] Fig. 12 shows a plot of post-treated cells seeded onto brand new dishes at around 20,000 and allowed to grow up to Day 4. Cells treated with equivalents of EDTA were able to increase considerably to an average of 330,000 while cells treated with salt of citrate could only grow to an average number of 210,000 cells. Error bars are shown as ± 1 standard deviation.
[0128] Fig. 13
[0129] Fig. 13 shows a plot of at Day 4 post-treatment, cell viability was measured, and cells treated with equivalents of EDTA showed around double the viability (-60%) as compared to cells treated with salts of citrate (-30%). Error bars arc shown as ± 1 standard deviation.
[0130] Fig. 14
[0131] Fig. 14 shows a collection of phase and fluorescent images of H9C2 cells subjected to mechanical stimulation only (top row) and both 3D hydrogel and mechanical stimulation (bottom row). The H9C2 cells were stained with cardiac troponin T tagged with green fluorescent protein (GFP-cTnT). Top row shows that absence of hydrogel and mechanical stimulation, H9C2 cells did not undergo differentiation. Bottom row shows that with hydrogel and mechanical stimulation, H9C2 cells were able to undergo differentiation as indicated by detection of green fluorescence signal.
[0132] Fig. 15
[0133] Fig. 15 shows a collection of transmitted-light images and fluorescent images of cells grown on plastic (control), Matrigel, hydrogel only and hydrogel crosslinked with graphene oxide. The box with diagonal line across represents that it was not possible to fluorescently probe the cells that were grown on Matrigel.
[0134] Fig. 16
[0135] Fig. 16 shows a graph plot of total cell count of cells retrieved from the plastic culture well (Control), Matrigel, Hydrogel and Hydrogel + GO on Day 0 based on cell seeding density and Day 2, Day 4, Day 6 and Day 8 of cell cultivation using chelator EDTA. Initial cell seeding density was 0.125 x 105. Interval plots plotted to illustrate the mean number (horizontal line) and error bars represented ± 1 standard deviation (SD).
[0136] Fig. 17
[0137] Fig. 17 shows a graph plot of total cell count of cells retrieved from Matrigel, Hydrogel and Hydrogel + GO on Day 0 based on cell seeding density and Day 2, Day 4, Day 6 and Day 8 of cell cultivation using chelator sodium citrate (Na-Citrate). Initial cell seeding density was 0.125 x 10’. Interval plots plotted to illustrate the mean number (horizontal line) and error bars represented ± 1 standard deviation (SD).
[0138] Fig. 18
[0139] Fig. 18 shows a graph plot of viability of cells retrieved from the plastic culture well (Control), Matrigel, Hydrogel and Hydrogel + GO on Day 0 based on cell seeding density and Day 2, Day 4, Day 6 and Day 8 of cell cultivation using chelator EDTA were measured using the Luna II automated cell counter. Initial cell seeding density was 0.125 x 105. Interval plots plotted to illustrate the mean number (horizontal line) and error bars represented ± 1 standard deviation (SD).
[0140] Fig. 19
[0141] Fig. 19 shows a graph plot of viability of cells retrieved from the Matrigel, Hydrogel and Hydrogel + GO on Day 0 based on cell seeding density and Day 2, Day 4, Day 6 and Day 8 of cell cultivation using chelator sodium citrate (Na-Citrate), measured using the Luna II automated cell counter. Initial cell seeding density was 0.125 x 105. Interval plots plotted to illustrate the mean number (horizontal line) and error bars represented ± 1 standard deviation (SD).
[0142] Fig. 20
[0143] Fig. 20 shows a box plot of live cell count of cells retrieved from the plastic culture well (Control), Matrigel, Hydrogel and Hydrogel + GO on Day 0 based on cell seeding density and Day, Day, Day 6 and Day 8 of cell cultivation using chelators EDTA and sodium citrate (Na- Citrate). Initial cell seeding density was 0.125 x 105. Interval plots plotted to illustrate the mean number (bar) and error bars represented ± 1 standard deviation (SD).
[0144] EXAMPLES
[0145] Non-limiting examples of the invention will be further described in greater detail by reference to specific examples, which should not be construed as in any way limiting the scope of the invention.
[0146] Example 1: Method of preparing 3D magnetized cell culture substrate
[0147] Prepar ation of graphene oxide (GO)
[0148] Herein, the cell culture substrate was prepared by first oxidising graphite flakes into graphene oxide. A beaker containing 25 mL of sulfuric acid (obtained from Acros Organics B.V.B.A, Belgium) and a stir bar was placed in an ice bath and mixed at 600 rpm and below 15°C in corrosive fume hood. While stirring, 1 g of natural graphite flakes (obtained from Sigma Aldrich Pte Ltd, Singapore) was added slowly into the mixing solution, followed by 3 g of potassium permanganate (obtained from Sigma Aldrich Pte Ltd, Singapore). The mixing of oxidising agent (potassium permanganate) and graphite flakes was carried out below 15°C, as the reaction is highly exothermic and generated heat may induce damage to the glassware. When the solution had turned dark green, 184 mL of Milli-Q water was added dropwise to the mixture and the mixture was allowed to stir for about 2 hours and subsequently the ice bath was removed, and the mixture was allowed to mix at around 35 °C for another 2 hours. Next, the mixture was kept in a reflux system at 98°C for 10 minutes before reducing the temperature to 30°C for 10 minutes, and lastly reducing the temperature to 25 °C for 2 hours. Subsequently, 40 mL of hydrogen peroxide (obtained from Thermo Scientific Chemicals, Netherlands) was added to the stirring mixture dropwise. The resulting mixture was poured equally into two beakers containing 200 mL of Milli-Q water each and the mixture in both beakers were stirred continuously for 1 hour before incubating them at room temperature for 3 to 4 hours. The Milli- Q water was then discarded, and the resulting mixture was washed by centrifugation with 10% hydrochloric acid (HC1) and Milli-Q water repeatedly. The resulting gel-like mixture was vacuum dried at 60°C for more than 6 hours. The resulting mixture was then centrifugated in 15 mL Falcon tubes at 10 000 rpm for 20 minutes in a centrifuge (obtained from Eppendorf, Singapore). The graphene oxide was collected and washed three times, using 50 mL of hydrochloric acid (obtained from Sigma Aldrich Pte Ltd, Singapore) each time. The washed graphene oxide was then dried in an oven at 90 °C for 24 hours.
[0149] Preparation of functionalised graphene oxide crosslinkcr (GOC)
[0150] 50 mg of the dried graphene oxide (GO) was then dispersed in 100 mL of deionised water in a beaker and sonicated at 40 °C for 90 minutes. Subsequently, 1 mL of vinyltriethoxysilane crosslinker (obtained from Sigma Aldrich Pte Ltd, Singapore) and 0.50 mL of hydrochloric acid were added into the mixture and heated at 75 °C for 6 hours. The functionalized graphene oxide crosslinker (GOC) was then centrifugated at 600 rpm for 2 minutes. The collected GOC was then washed with deionised water and centrifugated again to collect the washed GOC. The washing step was repeated at least two times. The final wash of the GOC was then collected and dried in at oven at 90 °C for 24 hours. Preparation of 3D cell culture substrate
[0151] 50 mg of the dried GOC was dispersed in 40 tnL of cell media (obtained from Life Technologies Holdings Pte Ltd, Singapore) in a beaker and sonicated 40 °C for 90 minutes. Subsequently, 0.8 g of sodium alginate (obtained from Sigma Aldrich Pte Ltd, Singapore) and 0.16 g of sodium hyaluronate (obtained from Sigma Aldrich Pte Ltd, Singapore) were dissolved in the solution comprising the functionalized graphene oxide and stirred at 4 °C for 24 hours. The solution was then mixed with 0.08 g (4 mg / mL) of collagen solution (obtained from Life Technologies Holdings Pte Ltd, Singapore) and the pH was adjusted to about pH 7.4 by addition of 1 M aqueous sodium hydroxide solution (obtained from 1st Base, Singapore). The final solution was then crosslinked with the addition of 50 mM of calcium chloride solution (obtained from Sigma Aldrich Pte Ltd, Singapore) and gelation was achieved by incubating the final solution at 37 °C for 15 minutes in 5% CO2 incubator (obtained from Analytik Jena GmbH, Germany). The 3D cell culture substrate was obtained after the gelation.
[0152] Example 2: Effect of magnetism on seed germination
[0153] To compare the effects of magnetism on seed germination, a control hydrogel substrate was prepared as described in Example 1 with the omission of the functionalised graphene oxide. Subsequently, two more sets of hydrogels with functionalised graphene oxide were prepared as described in Example 1. 50 seeds of each type ( Vigua radiata and Ocimum basilicum, obtained from Horti Flora Singapore and Australia, respectively) were embedded on the surface of each set of control and sample hydrogels (Day 0). The control set (CTRL) had no magnetic field applied. The first sample set (M-BTM) had a magnetic field applied using a neodymium magnet placed only at the bottom of the hydrogel substrate about 1 cm away, subjecting the seeds to a magnetic field perpendicular to the hydrogel surface. The second sample set (M- BOTH) had a magnetic field applied using neodymium magnets placed on the sides and bottom of the hydrogel substrate about 1 cm away each side, subjecting the seed to a magnetic field which is both perpendicular and parallel to the hydrogel surface. The seeds were observed for germination 24 hours post-sowing (Day 1). The seeds were then left to grow for the next 96 hours (Days 2 to 5) under conditions of 25 °C at 70% humidity under short wavelength ultraviolet light before being harvested for analysis.
[0154] The number of roots for the control, first sample and second sample were manually counted with the eye and hand. As seen from Fig. 1, the M-BOTH sample with magnetism applied to both side and bottom showed the highest maximum number of roots and a much higher median number of roots over the CTRL sample and marginally higher median over the M-BTM sample.
[0155] The thickness of the roots was measured with a micrometre screw gauge (293-344 external micrometre, range 0 mm to 25 mm, obtained from Mitutoyo Kanagawa, Japan). As seen from Fig. 2, the M-BTM sample with magnetic field applied to only the bottom showed the thickest roots obtained, while the M-BOTH sample showed higher median values over the CTRL and M-BTM sample with a smaller spread (smaller interquartile range).
[0156] The area of the foliage was calculated by the product of the minor and major axes across the foliage measured using a stainless-steel ruler (obtained from Vogel, Germany) As seen from Fig. 3, both the CTRL and M-BTM sample showed the largest foliage area with M-BTM having the highest median value. It is to be noted that the CTRL sample displayed a larger spread than the M-BTM and M-BOTH samples. While the M-BOTH sample has slightly lower foliage area, it is more consistent as it has the smallest spread (lowest interquartile range).
[0157] Example 3: Characterization of hydroael (cell culture substrate) for use in cell culturinn
[0158] Biocompatibility for use in cell culturing
[0159] To determine if the hydrogel (cell culture substrate) as prepared according to Example 1 is biocompatible for use in cell culturing, two different types of composites namely Composite E-C-H (Elastomcr-Ccll-Hydrogcl) and Composite E-H-C-H (Elastomcr-Hydrogcl-Ccll- Hydrogel) were prepared (Fig. 4). The elastomer was prepared by mixing Part A and Part B of liquid silicone rubber (SilpuranTM 6000 / 05, obtained from WACKERTM Silicones, Michigan, United States of America) in a 1 :1 w / w ratio. The mixture was mixed thoroughly and degassed for about 15 minutes before casting into the desired mould and baked at about 165 °C for about 5 minutes in an oven to form the elastomer.
[0160] MDCK cells stably expressing mGFP-YAP (about 200,000 cells on each substrate obtained from Mcchano biology Institute, National University of Singapore) were cither sandwiched between the elastomer substrate and hydrogel, or between two layers of hydrogel as illustrated in Fig. 4. As seen from Fig. 5, all the cell cultures (MDCK cells stably expressing mGFP-YAP obtained from Mechanobiology Institute, National University of Singapore) (grown with or without hydrogel) were stably expressing mGFP-YAP which is a mechanosensitive transcription co-activator protein that translocates into the nuclei of cells in response to mechanical forces. Therefore, the MDCK cells in the cell cultures (grown with or without hydrogel) were able to grow comparably well to confluency under both composite systems as compared to control (without hydrogel).
[0161] The cell density of the cell cultures was monitored using microscope imaging (EVOS m5000 Imaging System, obtained from Thermo Fisher Scientific, Massachusetts, United States of America) and fluorescent images of mGFP-YAP expressed in the MDCK cells were excited by 488nm laser line and detected at 510nm). As seen from Fig. 6, when propagation of mechanical forces was physically induced through the hydrogel, greater cell density growth for both composite systems (with hydrogel) was observed as compared to cell culture grown only on the elastomer substrate. The cell density was obtained by selecting a random region on the tissue and imaged on 40x. The image was subsequently captured onto a window of 1268.17 pm by 951.13 pm and the cells were counted based on their phase images. The cell density was computed by the number of cells per square millimetre of tissue area. Comparing between the two composite systems, it can be observed that the cell density growth is greater for Composite E-H-C-H than in Composite E-C-H up to 5 days after seeding of cells.
[0162] Hydrogel (cell culture substrate) promoting cell proliferation and viability
[0163] Three types of cells (mouse embryonic fibroblast (obtained from Mechano biology Institute, National University of Singapore), HEK293T (obtained from Mechanobiology Institute, National University of Singapore), and C2C12 skeletal muscle cells (obtained from Mechanobiology Institute, National University of Singapore)) were embedded within the hydrogel crosslinked with graphene oxide (GO) crosslinker (cell culture substrate). The cells were embedded by mixing the cells suspended in the cell media into the alginate solution prior to the addition of the functionalized graphene oxide, the hydrophilic agent, the additive and the crosslinking agent. About 500pL of hydrogel embedded with each cell type is used for the following procedures.
[0164] As shown in Fig. 9, cells were embedded within the volumetric hydrogel with images taken at different z-heights from the microscope lens. The results show that cells were able to grow throughout the volume of the hydrogel.
[0165] After confirming that cells can grow within the 3D hydrogel (cell culture substrate), the cells may be isolated from the hydrogel through chelation by using two main methods - one by detaching the cells only without affecting the polymerization of the hydrogel, and the other method by depolymerizing the hydrogel and then obtaining the cells from the liquified hydrogel mixture. First, media flooding the hydrogel was aspirated using a vacuum pump attached to a aspiration pipette via a tubing. The hydrogel was then washed and rinsed with Dulbecco's Phosphate Buffered Saline (DPBS) (obtained from Life Technologies Holdings Pte Ltd, Singapore) thrice. Then, the chelating agent was added to submerge the hydrogel and incubated in a 37°C, 5% CCh incubator for 15 minutes. Lastly, cells suspended in DPBS were transferred to a brand new 15mL falcon tube for collection.
[0166] Two chelating agents, ethylenediaminetetraacetic acid (EDTA) (obtained from Sigma Aldrich Pte Ltd, Singapore) and sodium citrate (NaC) (obtained from Sigma Aldrich Pte Ltd, Singapore) were used. It was observed that the chelating agents such as ethylenediaminetetraacetic acid (EDTA), ethylenebis(oxyethylenenitrilo)tetraacetic acid (EGTA), 1,2-cyclohcxylcncdinitrilotctraacctic acid (CDTA), dicthylcnctriamincpcntaacctic acid (DTPA) (Fig. 10 A), and salts of citrate (Fig. 10B) were able to detach the cells from the hydrogel (cell culture substrate) either by depolymerizing the hydrogel with NaC or by detaching the cells without affecting the polymerization of the hydrogel by adding equivalents of EDTA.
[0167] To validate if the methods mentioned above to either detach the cells or depolymerize the hydrogel, or both, would affect the cells, the cells that were embedded within the 3D hydrogel were counted. As shown in Fig. 11, both hydrogels were seeded with 100,000 cells on Day 0, and the following day, the methods as shown in Figs. 10A and 10B were carried out. A high- throughput cell counting device (LUNA-II™ Automated Cell Counter) was used to count the number of cells obtained. The total number of cells obtained through both chelation methods were comparably similar' at an average of around 200,000 to 250,000 cells. Next, these isolated / extracted cells were re-seeded onto brand new dishes to see if the cells are healthy, and able to carry out proliferation as per normal.
[0168] The cells were allowed to recover after the chelation treatments on brand new dishes and were allowed to proliferate up to Day 4. As shown in Fig. 12, cells treated with equivalents of EDTA were able to increase considerably to an average of 330,000 while cells treated with salt of citrate could only grow to an average number of 210,000 cells. As shown in Fig. 13, at Day 4 post-treatment, cell viability was measured, and cells treated with equivalents of EDTA showed around double the viability (-60%) as compared to cells treated with salts of citrate (-30%). From Fig. 12 and Fig. 13, it was shown that despite seeding similar' number of cells at 20,000 on Day 0, cells treated with equivalents of EDTA were able to grow to greater numbers and better viability as compared to cells treated with salts of citrate.
[0169] With knowledge of these two methods of obtaining cells from the hydrogel, it is possible to tailor the mode of obtaining cells based on the specific needs required (e.g. obtaining cells loosely held within the hydrogel using equivalents of EDTA treatment versus obtaining sticky cells or intact spheroid or intact tissues within the hydrogel using salts of citrate treatment). ing cell differentiation
[0170] H9C2 myoblast cells were seeded within the 3D hydrogel by mixing with the alginate solution before gelation with extracellular matrix proteins such as collagen and fibronectin, additive linkers and GO crosslinker. Upon gelation, the cells were cultivated in the 37°C, 5% CO2 incubator for 18 to 24 hours before the hydrogel was mechanically strained using electromagnetic means.
[0171] To understand if the hydrogel could aid in driving differentiation, H9C2 myoblast cells (obtained from Mechanobiology Institute, National University of Singapore) were seeded on 3D hydrogel and stimulated mechanically by inducing strain on the 3D hydrogel. H9C2 myoblast cells were able to undergo differentiation into cardiomyocytes as demarcated by the detection of cTnT, one of the two key components of the force generation machinery in cardiomyocytcs (bottom row of Fig. 14). Mechanical stimulation, but absence of the 3D hydrogel, was insufficient to drive differentiation of H9C2 myoblast cells into cardiomyocytes as shown in the top row of Fig. 14. This result suggests a strong contribution of the 3D hydrogel system to the differentiation process in the absence of necessary differentiation factor all-trans- retinoic acid. Up to this point, the 3D composite hydrogel has shown capabilities in promoting cell proliferation, maintaining cell viability, and promoting differentiation.
[0172] The Young’s modulus of the hydrogel (defined as the ratio of tensile stress to tensile strain) is about 700 Pa without the addition of the functionalised graphene oxide. Upon crosslinking the functionalised graphene oxide with hydrogel in a 1 :4 w / w ratio, the Young’s module was increased to about 950 Pa, as probed by nanoindentation (nanoindentation tester NHT3 obtained from Anton Paar, Singapore). Depending on the concentration of the functionalised graphene oxide used, the Young’s modulus may be adjusted accordingly, with higher concentrations leading to higher Young’s modulus. Advantageously, the increased Young’s modulus of the hydrogel indicates a stiffer gel which can better propagate the mechanical forces to the cells and tissues.
[0173] The propagation of force through the hydrogel was induced by placing permanent neodymium magnet at a distance of about 13 to 17 mm away from the hydrogel composites to provide mechanical stretching in a magnetic field. The electromagnetic field strength was between 44.04 mT to 99.72 mT, wherein a shorter distance of the magnets away from the hydrogel corresponds to a higher electromagnetic field strength.
[0174] To understand if the hydrogel (cell culture substrate) prepared according to Example 1 possesses suitable mechanical properties to propagate force to the MDCK cells stably expressing mGFP-YAP (about 200,000 cells on each substrate obtained from Mcchanobiology Institute, National University of Singapore) cultured within the composite systems according to Example 3, one set of each composite was subjected as control and another set of each composite was subjected as experimental group. The control without any mechanical stretching was labelled as Al (Composite E-C-H) and B 1 (Composite E-H-C-H). The experimental group strained under mechanical stretching was labelled as A2 (Composite E-C-H) and B2 (Composite E-H-C-H). As shown in Fig. 7, subpopulation of cells (as shown by the arrows) in composite systems A2 and B2 showed nuclear translocation of mGFP-YAP in response to strain under mechanical stretching. To further analyse this phenomenon quantitatively, the mGFP-YAP intensities was measured using imageJ, an image processing software (National Institutes of Health, Bethesda, United States of America), within nuclei and cytoplasmic regions of cells of interest. As shown in Fig. 8, cells from both composite systems (A2 and B2) strained under mechanical force experienced significantly greater degree of nuclear translocation of mGFP-YAP as compared to the controls without mechanical stretching (Al and Bl). These results illustrated that mechanical force could propagate from external source through the hydrogel (cell culture substrate) to the cells. Therefore, the mechanotransduction process was observed in composites A2 and B2.
[0175] Comparative Example 1 - Comparison of cell proliferation and viability capabilities of the hydrogel (cell culture substrate) with 2D plastic and commercialized Matrigel
[0176] To determine if the cell proliferation and viability capabilities were due to the the hydrogel only or due to the hydrogel with presence of the graphene oxide, more detailed probing of the effects on cell viability and proliferation was carried out in further comparison with the commercially available hydrogel and the 2D plastic.
[0177] Cell proliferation test
[0178] To probe if the cells could grow viably and proliferate at a greater rate within the hydrogel, mouse embryonic fibroblast (MEF) cells obtained from Mechanobiology Institute, National University of Singapore) were seeded on 2D plastic, and 3D gels consisting of commercialized Matrigel (obtained from Coming, Singapore), hydrogel only (Hydrogel only) (prepared according to Example 1), and hydrogel crosslinked with graphene oxide (Hydrogel + GO) (prepared according to Example 1) (Fig. 15). Given that the matrices of the hydrogels may make it hard to visualize MEF cells within the 3D gels, fluorescent probes (Celltracker fluorescent probes) were applied into the media to allow tracking of the location of the cells embedded within the 3D matrices of the 3D gels. Based on the experiment conducted, it was not possible to fluorescently probe the cells that were seeded on the commercialized Matrigel. However, the hydrogel allowed ease of probing the cells with fluorescent markers. This gave the hydrogel an advantage over the commercial Matrigel in terms of the ease of use of fluorescent probes, which is a widespread practice in research and development laboratories. As shown in Fig. 15, the number of cells was higher for all four conditions when compared between Day 2 and Day 8 of culturing. In summary, the hydrogel has similar 3D cell culturing capability compared to that of commercial Matrigel.
[0179] To understand which system and / or conditions can enhance proliferation, the total cell count within each system / condition on Day 2, Day 4, Day 6, and Day 8 of cell cultivation was obtained.
[0180] Based on the earlier results in Example 3, it was shown that cells obtained using the EDTA treatment were more viable than the Na-Citrate treatment. Therefore, total cell count of cells were obtained from the 2D plastic culture well (Control), and from the 3D gels (Matrigel, Hydrogel, and Hydrogel + GO) on Day 0 based on cell seeding density. Day 2, Day 4, Day 6, and Day 8 of cell cultivation using chelator EDTA. As shown in Fig. 16, the total number of cells obtained from the Hydrogel + GO group was significantly greater as compared to the other groups between Day 4 and Day 8. On the other hand, the total number of cells obtained from the Hydrogel + GO group using the Na-Citrate treatment was significantly greater as compared to the other groups, but only between Day 6 and Day 8 (Fig. 17). However, total number of cells obtained from the hydrogel without crosslinkcr GO was about twice for EDTA treatment than Na-Citrate treatment between Day 4 and Day 8 (Fig. 16 and Fig. 17). The total number of cells on 2D plastic well reached a plateau of around 2 x 105cells due to the limited space of the 2D surface, such that the cells halted proliferating under the influence of contact inhibition leading to cell growth arrest (Fig. 16). However, it was found that the Matrigel system (which is typically used to grow suspended cells or induce differentiation) did not support pronounced cell proliferation, leading to very humble increment of cell numbers even up to Day 8 of cultivation (Fig. 16 and Fig. 17).
[0181] It has been shown that the hydrogel can significantly increase cell number by Day 4 of culturing. Hence, the hydrogel has another commercial advantage over commercial Matrigel in the hydrogel-extracellular matrix (ECM) market.
[0182] Cell viability test
[0183] Given that the hydrogel with GO could improve the total cell count, cell viability test was then conducted to compare between 2D plastic culture well (Control), and the 3D gels (Matrigel, Hydrogel, and Hydrogel + GO). The results show that the hydrogel with GO gave good cell viability comparable to that of cells cultured on 2D plastic well surface (Control) detached using the EDTA treatment between Day 2 and Day 6 (Fig. 18). However, the composite hydrogel with GO viability dropped on Day 8 (Fig. 18). Without GO, hydrogel alone influenced the cell viability as shown in Fig. 18, and Matrigel provided nominal cell viability as compared to both 2D plastic well surface (Control) and composite hydrogel with GO groups. When the cell detachment treatment was switched to Na-Citrate, cell viability of cells cultured in all three 3D gel systems became compromised (Fig. 19).
[0184] In summary, the 3D hydrogel with graphene oxide crosslinker is able to support cell viability comparable to that of cells on 2D plastic well. It is also notable that EDTA cell detachment treatment is less harsh than Na-Citrate cell detachment treatment.
[0185] To emphasize the superiority of the hydrogel to other platforms, the live cell count of MEF cells for 2D plastic well (Control), commercial Matrigel, Hydrogel only without GO crosslinker (Hydrogel only), and Hydrogel with GO crosslinker (Hydrogel + GO) was measured and compared. By comparing the live cell count on Day 0 (initially seeding of cell density onto the various systems) and on Day 8, it was found that the number of live cells obtained from the Hydrogel + GO system were at least 10-folds as compared to other systems (Control, Matrigel, Hydrogel only) when cells on Day 8 were retrieved using the EDTA cell detachment treatment (Fig. 20). Despite being a harsher cell detachment treatment, the live cell counts for cells obtained from Hydrogel + GO system were at least 6-folds as compared to Hydrogel only system.
[0186] In summary, this finding further substantiates the hydrogel with GO crosslinker’s superiority over commercial Matrigel and highlight the importance of the GO crosslinker on its influence on enhancing cell proliferation and supporting cell viability up to Day 8 of cell cultivation.
[0187] Overall, the 3D hydrogel with graphene oxide crosslinker is superior to commercial Matrigel in terms of enhancing cell proliferation, cell viability, and ease of use of dye-based fluorescent probes to visualize compartments and parts of the cells embedded within the 3D gel system. Cells obtained from the 3D composite hydrogel either by depolymerization or by detaching of cells from intact hydrogel remained proliferative and viability.
[0188] INDUSTRIAL APPLICABILITY
[0189] The disclosed hydrogel may be used in cell culturing or seed germination as a cell culture substrate or a seed germination substrate. This is applicable to industries such as cultured meat, food, pharmaceutical, agriculture, medical and life sciences.
[0190] It will be apparent that various other modifications and adaptations of the invention will be apparent to the person skilled in the art after reading the foregoing disclosure without departing from the spirit and scope of the invention and it is intended that all such modifications and adaptations come within the scope of the appended claims.
Claims
Claims1. A hydrogel comprising a functionalised graphene oxide.
2. The hydrogel of claim 1 , wherein the graphene oxide is functionalized by a crosslinkcr.
3. The hydrogel of claim 1 or 2, wherein the crosslinker is selected from the group consisting of methyltrimethoxy silane, methyltriethoxysilane, dimethyldimethoxy silane, dimethyldiethyoxysilane, tetramethoxysilane, tetraethoxysilane, vinyltriacetoxysilane, vinyltriethoxysilane and any combinations thereof.
4. The hydrogel of any one of claims 1 to 3, wherein the functionalised graphene oxide is paramagnetic.
5. The hydrogel of any one of claim 1 to 4, wherein the hydrogel has a Young’s modulus in the range of about 800 Pa to about 1 000 Pa.
6. A method of preparing a hydrogel comprising the steps of: a) oxidising graphite to graphene oxide; b) functionalising the graphene oxide of step a) with a crosslinker; and c) forming a hydrogel from a mixture of a liquid medium, the functionalized graphene oxide (GOC) of step b), an alginate solution, a hydrophilic agent, an additive and a crosslinking agent.
7. The method of claim 6, wherein the crosslinker is selected from the group consisting of me thy Itrimcthoxy silane, mcthyltricthoxysilanc, dimcthyldimcthoxy silane, dimethyldiethyoxysilane, tetramethoxysilane, tetraethoxysilane, vinyltriacetoxysilane, vinyltriethoxysilane, N-(3-dimcthylaminopropyl)-N'-cthylcarbodiimidc hydrochloride, N- hydroxysuccinimide, 2-aminoethyl methacrylate hydrochloride and any combinations thereof.
8. The method of claim 6 or 7, wherein the functionalising step b) further comprises the steps of: bi) dispersing the graphene oxide in a solvent comprising the crosslinker to form a solution; and bii) heating the solution of step bi) at a temperature for a duration.
9. The method of claim 8, wherein the solution in step bi) further comprises an acid.
10. The method of claim 8 or 9, wherein the solvent in step bi) is a polar solvent.
11. The method of any one of claims 8 to 10, wherein the temperature in the heating step bii) is in a range of about 50 °C to about 100 °C and the duration is in a range of about 5 hours to about 10 hours.
12. The method of any one of claims 6 to 11, wherein the forming step c) further comprises the steps of: ci) providing a hydrogel precursor solution comprising the mixture of the liquid medium, the functionalized graphene oxide (GOC) of step b), the alginate solution, the hydrophilic agent, the additive and the crosslinking agent; and cii) setting the hydrogel precursor solution to form the hydrogel.
13. The method of claim 12, wherein the setting step is via incubation in a carbon dioxide incubator.
14. The method of any one of claims 6 to 13, wherein the alginate in the alginate solution is selected from the group consisting of alginic acid, sodium alginate, potassium alginate, ammonium alginate and propylene glycol alginate.
15. The method of any one of claims 6 to 14, wherein the hydrophilic agent is selected from the group consisting of hyaluronic acid, sodium acetylated hyaluronate, sodium hyaluronate and any combinations thereof.
16. The method of any one of claims 6 to 15, wherein the additive is selected from the group consisting of collagen, fibronectin and a combination thereof.
17. The method of any one of claims 6 to 16, wherein the crosslinking agent is a metal chloride salt.
18. The method of any one of claims 6 to 17, wherein the liquid medium is selected from the group consisting of water, saline, buffer solutions, cell media and any mixtures thereof.
19. The method of any one of claims 6 to 18, wherein the liquid medium is a cell media and the hydrogel is a cell culture substrate.
20. The method of any one of claims 6 to 18, wherein the liquid medium is water and the hydrogel is a seed germination substrate.
21. A cell culture substrate comprising the hydrogel of any one of claims 1 to 5 for use in culturing cell.
22. Use of the hydrogel of any one of claims 1 to 5 in the preparation of a cell culture substrate for culturing cells.
23. Use of the hydrogel of any one of claims 1 to 5 in the preparation of a cell culture substrate for triaxial manipulation of the cells.
24. A seed germination substrate comprising the hydrogel of any one of claims 1 to 5 for use in germinating seeds.
25. Use of the hydrogel of any one of claims 1 to 5 in the preparation of a seed germination substrate for germinating seeds.
Citation Information
Cited By
Systems and methods for compartmentalizing and analyzing cells
US12797849B2