The bioactivate titanium coating process for orthopedics and dental implants

The bioactive titanium coating process using rhSLPI protein enhances osseointegration and bone growth in orthopedic and dental implants, addressing the challenges of existing coatings by promoting cell adhesion and reducing inflammation, thereby improving treatment outcomes for orthopedic and dental implant procedures.

WO2024225986A1PCT designated stage expired Publication Date: 2024-10-31CHIANG MAI UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/TH2023/050021
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2023-08-15
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Current orthopedic and dental implants face challenges in osseointegration and bone regeneration, particularly in elderly or diabetic patients, due to insufficient bone mass, and existing coatings may have negative side effects or immune responses, with no effective biological coatings that reduce inflammation and promote bone growth.

Method used

A bioactive titanium coating process using recombinant human secretory leukocyte protease inhibitor (rhSLPI) protein, which is applied to titanium surfaces to enhance osseointegration, stimulate bone growth, and reduce inflammation, by preparing the titanium surfaces, diluting the rhSLPI protein in phosphate buffered saline, and incubating at specific temperatures to promote cell adhesion and bone regeneration.

Benefits of technology

The rhSLPI coating significantly increases bone cell adhesion and growth, reduces inflammation, and promotes wound healing without toxicity, improving the efficiency and quality of orthopedic and dental implant treatments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure TH2023050021_31102024_PF_FP_ABST
    Figure TH2023050021_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The bioactive titanium coating process for orthopedics and dental implants comprises a series of steps: Prepare a titanium material by sterilization and then prepare a recombinant human secretory leukocyte protease inhibitor (rhSLPI) protein. Use the prepared rhSLPI protein to coat the titanium material, and then rinse the coated titanium with phosphate buffered saline to remove any protein that failed to adhere to the material. Then add human bone cells so that they adhere to the coated material under the effect of the rhSLPI protein. The proliferation and adhesion of the bone cells will thus become more efficient as the protein stimulates the expression of the molecules in their ability to adhere to the bone cell, while controlling the stimulated development of embryonic bone cells. It is thus capable of stimulating bone growth as well as dental root growth.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] THE BIOACTIVE TITANIUM COATING PROCESS FOR ORTHOPEDICS AND DENTAL IMPLANTS

[0002] Field of the Invention

[0003] The scientific fields related to the bioactive titanium coating process for orthopedics and dental implants

[0004] Background of the Invention

[0005] The world population has entered an ageing society, where the number of people over 60 is 10% higher than the total global population. Elderly health care is therefore an important issue, and the government is obligated to provide support for medical care. It is reported that the cause of death and illness among the elderly is accidents, and 70% are caused by falls in people over 75 years old. The most common problem after a fall is a bone fracture, which possibly leads to death or disability in the elderly. Bone fracture in the elderly is also caused by osteoporosis, which is a bone disease developed throughout the body when there is a decrease in bone mass and bone strength, increasing the risk of bone fracture. A bone fracture can be treated with a splint to prevent movement of the broken bone or by an internal fixation using metal or titanium alloy orthopedic fixation implants. These require a high cost of treatment.

[0006] In addition, for those with dental problems, dental implant treatment has been greatly helpful and popular in the past decade as it significantly helps with dental restoration and favorable appearance, which improves the patient’s quality of life and reduces dental anxiety. Dental implants are likewise made from titanium alloy. Nonetheless, bone regeneration with sufficient bone mass for the use of dental implants, especially in the elderly or diabetic patients who have bone deterioration, essentially requires osseointegration on metal implants. Accordingly, a process that stimulates or increases the efficiency of osseointegration would increase treatment efficiency. The improvement of the surface of medical materials or medical titanium alloys for the purpose of enhancing osseointegration is thus challenging and constantly needed.

[0007] Several current studies interested in the development of a titanium contact surface to enhance its functional efficiency in orthopedics and dental implants by increasing osseointegration and adhesion between bones and implants. Currently, there are many implant materials with various contact surfaces available on the market, but those coating agents are synthetic chemicals that might have negative impact or side effects. Trending research and innovation are targeting the study of coatings that are biological substances obtained from the human body since they do not cause a problem concerning immune responses, and have only a few side effects. The coating of implants with hyaluronic acid is an example of such a study. However, there are no reports of coating agents that are biological substances obtained from the human body and provide other beneficial effects e.g., reducing inflammation, stimulating embryonic bone cells to develop into calcium-accumulating bones, promoting wound healing, or reducing inflammation.

[0008] As per a patent database search, some prior inventions relating to orthopedic and dental implant coatings were found, such as the following:

[0009] The bones cited above have resulted in the development of processes for coating implanted bones or in the replacement of bones with various kinds of polymers, for instance, coatings with bioactive substances, as in the following examples:

[0010] An international patent, publication number W02015187110A3, describes a coating of orthopedic and dental implant surfaces with hydroxyl apatite (HA) obtained from eggshells comprising these steps: preparing calcium- Ethylenediaminetetraacetic acid (Ca-EDTA) with egg shell powder together with treatment with acetic acid and EDTA; adjusting the pH of the solution to 13 with sodium hydroxide (NaOH); and dipping the orthopedics and dental implants into the solution for coating. The reaction takes place in a 600-watt microwave at a frequency of 2.45 gigahertz (GHz) for a period of 10 minutes and is followed by drying in a vacuum environment.

[0011] A Swedish patent, publication number SE1850520A1, describes the implants or artificial bone used for repairing cartilage and / or bone joints made from titanium and titanium alloy with a wear-resistant layer comprising titanium nitride (TiN). The cartilage contact surface is covered with bio-active substances or with a biological coating in the protein or peptide group, among which are the following examples:

[0012] A Chinese patent, publication number CN203458622U, describes a coating to improve the biocompatibility of the titanium alloy, which requires the innermost layers to be an oxide layer, a transition layer, and a bioactive protein layer. These layers are bio-active from the interior to the exterior and thereby aid the cell's adhesion capacity.

[0013] A Chinese patent, publication number CN105624762B, describes a coating of titanium or titanium alloy with a bio-active composite material. The steps are as follows: conditioning the titanium or titanium alloy surface; then steeping it in an electrolytic solution containing fluorine, with the titanium or titanium alloy as the anode and a platinum plate as the cathode; preparing an electrolyte containing calcium phosphorous and peptide as a primer; and coating the titanium or titanium alloy by using the electro-chemical cell principle.

[0014] A United States patent, publication number US 10426871B2, describes a coating of dental implant surfaces (medical implants) with a bioactive agent stored in a nanotube, which forms a film covering the surface.

[0015] With regard to the prior arts above, bio-active covering agents for use on orthopedics and dental implants have been developed. However, there has been no discovery of any invention that has come into view, referring to the use of the recombinant human secretory leukocyte protease inhibitor (SLPI) protein, which is a protein 11.7 kilodalton in size. The non-glycosylate protein group has found use in the coating of orthopedic and dental implant surfaces. The aforementioned protein was formed and ejected from epithelium and immune cells. It has the important function of inhibiting serine protease, elastase, and cathepsin G from the neutrophils. Previous studies have shown that the recombinant human SLPI protein can promote the differentiation of osteoblasts and mineralization to build bones and increase osseointegration on titanium surfaces. In addition, the recombinant human SLPI protein is potent enough to reduce inflammation, reduce and protect against disease infections, kill and suppress the growth of bacteria and fungus, and reduce viral infections. It is capable of increasing cell division, reducing cell death caused by apoptosis, increasing the healing action of wounds, reducing the formation of free radicals, stimulating the production of antioxidants, and reducing injuries and myocardial ischemia. Researchers have conducted previous in vitro, ex vivo and in vivo experiments, indicating that the recombinant human SLPI protein is a protein that is beneficial towards the inflammation process, and it repairs and regenerates organs or new tissues on a large scale. It is therefore possible that the recombinant human SLPI protein, in addition to stimulating the adhesion, growth, and development of bone cells, also benefits other functioning processes of the body. It is thus a subject of research and development for use as a titanium coating for orthopedics and dental implants. It has been found that by coating titanium with the recombinant human SLPI protein, it is possible to increase human embryonic osseointegration with a statistical significance and with no toxicity to the cells. It was also found that it stimulates the human osteoblast expansion mechanism very efficiently.

[0016] Summary of the Invention

[0017] The process of coating titanium surfaces with bio-active substances for orthopedics and dental implants consists of certain steps. The titanium must be prepared by sterilizing its metallic surfaces. The recombinant human secretory leukocyte protease inhibitor (rhSLPI) must then be prepared from a stock solution with a concentration of 1 milligram / milliliter at a temperature of - 80 degrees Celsius. It can be diluted to a concentration of 0.1-100 micrograms / milliliter with phosphate buffered saline (PBS), which will adjust the pH to 7.4. The material surfaces are to be coated at a temperature ranging from 0 to 10 degrees Celsius. Then apply the rhSLPI protein as a coating for the titanium surfaces so that it floods the surfaces. Cure them at a temperature of 4-6 degrees Celsius for a period of 24 hours. Rinse the coated titanium material with phosphate buffered saline to remove any cells that did not adhere to the material. The purpose of this invention is to innovate a titanium-coating process using bio-active substances for orthopedics and dental implants by means of the recombinant human secretory leukocyte protease inhibitor (rhSLPI). The rhSLPI will make bone cell distribution and adhesion more efficient, stimulate the presence of molecules adhering to the surfaces of bone cells, and control the stimulated development of osteoblasts. It stimulates bone growth and dental root growth. It increases cell division, promotes the healing of wounds, reduces infections and inflammation, and imparts more quality to bone and dental implants. It leads to further development of products for use in orthopedics and may also function as a dental implant coating. Ultimately, it reduces dependency on foreign imports of medical supplies while increasing the quality of life for the people of Thailand.

[0018] Brief Description of the Drawings

[0019] Figure 1 shows the effect of the concentration levels of the recombinant human secretory leukocyte protease inhibitor (rhSLPI) protein on osseointegration (type hFOB 1.19) by determining a cell count through a cell toxicity-testing method derived from the functional capability of the dehydrogenase enzyme and cofactors in the mitochondria (MTT cell viability assay) and at values of absorbance at a wavelength of 595 nanometers.

[0020] Figure 2 shows the effect of the recombinant human secretory leukocyte protease inhibitor (rhSLPI) protein at concentration levels of 0.1 micrograms / milliliter, 10 micrograms / milliliter and 100 micrograms / milliliter on the survival percentage of the cells.

[0021] Figure 3 shows test results in determining the quantity of the recombinant human secretory leukocyte protease inhibitor (rhSLPI) protein on the surfaces of titanium specimens following a 24-hour coating period by the ELISA method. It was found from the experimental results that after coating the titanium at concentrations of 10 micrograms / milliliter and 100 micrograms / milliliter for a period of 24 hours, rhSLPI could be found on the surfaces of the material.

[0022] Figure 4 shows the adhesion characteristics and distribution of human bone cells (type hFOB 1.19) following a 20-minute period of adhesion to the titanium alloy coated with the rhSLPI protein at concentrations of 10 micrograms / milliliter and 100 micrograms -milliliter, as determined by use of a scanning electron microscope.

[0023] Figure 5 shows the layout of the actin cell-support structure of the human bone cells (type hFOB 1.19) following a 20-minute period of adhesion to the titanium surfaces that had been coated with the rhSLPI protein at concentrations of 10 micrograms / milliliter and 100 micrograms / milliliter by staining with phalloidin-TRITC and monitoring the arrangement of the actin structure with a florescent microscope. Figure 6 shows the results of increasing the number of human bone cells (type hFOB 1.19) on the titanium alloy surfaces that had been coated with the rhSLPI protein at concentrations of 10 micrograms / milliliter and 100 micrograms / milliliter over a 3 -day period and a 5-day period, respectively. The cell count was determined through a test for toxicity in the cells as derived from the functional capability of the dehydrogenase enzyme and cofactors in the mitochondria (MTT cell viability assay). The values of absorbance were determined at a wavelength of 595 nanometers.

[0024] Figure 7 shows the results of increasing the presence of the integrin a-1 gene, which is a molecule on the surface of bone cells that plays an important role in cell adhesion. The results were found by experimenting with human bone cells (type hFOB1.19) that were being nurtured on titanium surfaces that had been coated with the rhSLPI protein at a concentration of 10 micrograms / milliliter for a period of 24 hours. The relative gene presence was first checked and then analyzed through a reverse transcription-quantitative polymerase chain reaction (RT-qPCR).

[0025] Figure 8 shows the results of increasing the presence of the integrin a-2 gene, which is a molecule on the surface of bone cells that plays an important role in cell adhesion. The results were found by experimenting with human bone cells (type hFOB1.19) that were being nurtured on titanium surfaces that had been coated with the rhSLPI protein at a concentration of micrograms / milliliter for a period of 24 hours. The relative gene presence was first checked and then analyzed through a reverse transcription-quantitative polymerase chain reaction (RT-qPCR).

[0026] Figure 9 shows the results of increasing the presence of the integrin a-5 gene, which is a molecule on the surface of bone cells that plays an important role in cell adhesion. The results were found by experimenting with human bone cells (type hFOB1.19) that were being nurtured on titanium surfaces that had been coated with the rhSLPI protein at a concentration of 10 micrograms / milliliter for a period of 24 hours. The relative gene presence was first checked and then analyzed through a reverse transcription-quantitative polymerase chain reaction (RT-qPCR).

[0027] Figure 10 shows the results of increasing the presence of the alkaline phosphatase (ALP) gene, which is a molecule that indicates the development of bone cells. The results were found by experimenting with human bone cells (type hFOB1.19) that were being nurtured on titanium surfaces that had been coated with the rhSLPI protein at a concentration of 10 micrograms / milliliter, both in the normal state and in the induction state for bone cell development, over a period of 7 days. The relative gene presence was first checked and then analyzed through a reverse transcription-quantitative polymerase chain reaction (RT-qPCR).

[0028] Figure 11 shows the results of increasing the presence of the osteocalcin (OCN) gene, which is a molecule that indicates the development of bone cells. The results were found by experimenting with human bone cells (type hFOB1.19) that were being nurtured on titanium surfaces that had been coated with the rhSLPI protein at a concentration of 10 micrograms / milliliter, both in the normal state and in the induction state for bone cell development, over a period of 7 days. The relative gene presence was first checked and then analyzed through a reverse transcription-quantitative polymerase chain reaction (RT-qPCR).

[0029] Figure 12 shows the results of having increased the presence of the RUNX2 gene, which is a molecule that indicates the development of bone cells. The results were found by experimenting with human bone cells (type hFOB1.19) that were being nurtured on titanium surfaces that had been coated with the rhSLPI protein at a concentration of 10 micrograms / milliliter, both in the normal state and in the induction state for bone cell development, over a period of 7 days. The relative gene presence was first checked and then analyzed through a reverse transcription-quantitative polymerase chain reaction (RT-qPCR).

[0030] Detailed Description of the Invention

[0031] The process of coating titanium surfaces with bio-active substances for orthopedics and dental implants consists of the following steps:

[0032] A. Preparing the titanium surfaces by sterilization

[0033] B . Preparing the recombinant human secretory leukocyte protease inhibitor protein

[0034] C . Coating the titanium surfaces with the recombinant human secretory leukocyte protease inhibitor protein

[0035] Each of the steps involved in the coating of the titanium surfaces with the recombinant human secretory leukocyte protease inhibitor protein is described in detail below:

[0036] A. The titanium may be sterilized by any of the following methods: use of an autoclave as a means of disinfection; baking in a hot-air oven; steaming in hot water vapor; use of ethylene oxide or use of hydrogen peroxide gas plasma; any combination of these same methods.

[0037] In the case of baking in a hot-air oven, the specimen shall be baked at a temperature of 160-180 degrees Celsius for a period of 1-2 hours.

[0038] In the case of steaming in hot water vapor, the specimen shall be steamed at a temperature of 100-140 degrees Celsius for a period of 1-30 minutes.

[0039] In the case of using ethylene oxide, the concentration of the ethylene oxide shall be between 700 and 1,200 milligrams / liter, with the temperature set between 40 and 60 degrees Celsius for a period of 3-6 hours.

[0040] B . The recombinant human secretory leukocyte protease inhibitor protein is prepared at a concentration of 0.1-100 micrograms / milliliter from a stock solution with a concentration of 1 milligram / milliliter, which has been stored at -80 degrees Celsius. This solution is then diluted to a concentration of 0.1-100 micrograms / milliliter with phosphate buffered saline (or PBS), which will adjust the pH to 7.4. The material surfaces will then be coated at a temperature of 1-10 degrees Celsius.

[0041] C. The titanium surfaces are coated with the recombinant human secretory leukocyte protease inhibitor protein by putting the recombinant protein prepared in step B into containers with the titanium prepared in step A until the titanium is fully immersed. It is then incubated at a temperature of 4-6 degrees Celsius for a period of 24 hours. The coated titanium is then rinsed with phosphate buffered saline in order to remove any proteins that failed to adhere to the material. When the rinsing is complete, human bone cells are then added so that these cells may cling to the material that has now been coated with the recombinant human secretory leukocyte protease inhibitor protein.

[0042] One other aspect of this process is that the titanium that has been coated with the recombinant human secretory leukocyte protease inhibitor protein will be rinsed with phosphate buffered saline from 1 to 3 times.

[0043] This invention will hereafter be described by citing examples of inventions that can help provide enhanced understanding and greater clarity. In any case, the titanium-coating process based on bio-active substances for orthopedics and dental implants, together with the relevant data that will be cited herewith, are simply examples. They are provided for illustration purposes to foster greater awareness of the invention process. They do not signify the setting of any limitations to the outcome of the invention process of any kind whatsoever.

[0044] Example 1: The coating of titanium material with the bio-active recombinant human secretory leukocyte protease inhibitor protein for orthopedics and dental implants.

[0045] A. Prepare the titanium material by using medical-grade titanium alloy with a thickness of 1 millimeter that has been cut into a circular disc with a diameter of 5 millimeters and sterilized in an autoclave.

[0046] B. Prepare the recombinant human secretory leukocyte protease inhibitor protein at concentrations of 0, 0.1, 1, 10, and 100 micrograms / milliliter in phosphate buffered saline.

[0047] C. Coat the titanium alloy with the recombinant human secretory leukocyte protease inhibitor protein by placing the same recombinant human secretory leukocyte protease inhibitor protein from step B into the vessel containing the titanium material prepared in step A until the titanium is fully immersed. Incubate it at a temperature of 4-6 degrees Celsius for a period of 24 hours. Finally, rinse the coated titanium material with phosphate buffered saline to remove any cells that may unable to adhere to the material surface.

[0048] Example 2: Testing the efficiency of coating titanium with the recombinant human secretory leukocyte protease inhibitor protein on human osseointegration and on the mechanism of adhesion at both the cellular and molecular levels:

[0049] A. Prepare human bone cells (Type hFOB 1.19) by the cultivation of human bone cells in a bacterial medium, which will be an ingredient in the Ham’s F12 medium and the Modified Dulbecco Eagle’s Medium (DMEM) in a 1:1 ratio. It is supplemented by 2.5 millimoles (mM) of L-glutamine and 10% fetal bovine serum. Specimens are cultivated at a temperature of 37 degrees Celsius in a medium of 5% carbon dioxide and 95% air.

[0050] B. Prepare a cell suspension from the human bone cells in step A with a concentration of 1x105cells per milliliter. Adding 200 microliters of the cell suspension into the cavity containing the titanium disc coated with the recombinant human secretory leukocyte protease inhibitor protein, allowing at least 20 minutes to test the cell adhesion. When the time has elapsed, then draw off the cell suspension by suction and remove any cells that failed to adhere to the material by rinsing with phosphate buffered saline three times.

[0051] C. Add 200 microliters of the cell culture, then nurture and incubate for 1 hour, and determine the number of cells that have adhered to the material by adding 200 microliters of 3- (4,5,dimethylthiazolyl-2)-2, 5-diphenyltetrazolium bromide (MTT) assay at a concentration of 0.5 milligrams / milliliter for 2 hours.

[0052] D. Dissolve the formazan crystals with 200 microliters of dimethyl sulfoxide (DMSO) and perform an analytical check by measuring the light absorbance at a wavelength of 595 nanometers. Use the obtained value of absorbance for further analysis. Also, conduct a test for cell toxicity using a cell toxicity-testing method derived from the functional capability of the dehydrogenase enzyme and cofactors in the mitochondria (MTT cell survival assay). Finally, test for the amount of recombinant human secretory leukocyte protease inhibitor protein coating the titanium surfaces by using the ELISA method.

[0053] Example 3: Results of coating the titanium surfaces with the recombinant human secretory leukocyte protease inhibitor protein

[0054] After coating the titanium surfaces with the recombinant human secretory leukocyte protease inhibitor protein at concentration levels of 0, 0.1, 1.0, 10, and 100 micrograms / milliliter in phosphate buffered saline, it was found that using this recombinant protein at concentrations of 10 and 100 micrograms / milliliter could increase the adhesion capacity of the human bone cells with statistical significance (Figure 1), while the same recombinant protein at all concentrations had no toxic effects on the human bone cells (Figure 2). It was possible to find the recombinant protein on titanium surface (Figure 3).

[0055] Example 4: Testing the adhesion and spread of the bone cells on the titanium alloy surfaces that had been coated with the recombinant human secretory leukocyte protease inhibitor protein

[0056] Begin by placing the titanium alloy that has been coated with the recombinant human secretory leukocyte protease inhibitor protein at concentrations of 10 and 100 micrograms / milliliter in phosphate buffered saline. Then add 200 microliters of the cell suspension from the human bone cells at a concentration of IxlO5cells / milliliter into the cavity containing the titanium disc that has been coated with this protein for a period of 20 minutes. Finally, fix the cells with 2.5% glutaraldehyde for 30 minutes and check the adhesion and spread of the bone cells with a scanning electron microscope.

[0057] It was found that coating titanium alloy with the recombinant human secretory leukocyte protease inhibitor protein at concentrations of 10 and 100 micrograms / milliliter could increase the adhesion and spread of cells within 20 minutes following cell attachment (Figure 4).

[0058] Example 5: Studying the shape and inner structure of the cells and the structural arrangement of the actin fibers with a fluorescent microscope

[0059] A. Nurture the human bone cells (hFOB1.19) until they attain a concentration of 80%. Then, subculture the cells in order to make a cell count. Prepare a cell suspension at a concentration of 1x105cells / milliliter.

[0060] B. Add 200 microliters of the cell suspension into the cavity holding the titanium disk coated with the recombinant human secretory leukocyte protease inhibitor protein for periods of 20 minutes and 60 minutes. Finally, suction out the cell suspension and rinse with phosphate buffered saline for three times.

[0061] C. Add 200 microliters of cell-culture medium and then incubate at 37 degrees Celsius in a medium of 5% carbon dioxide and 95% air for a period of 1 hour. Rinse the cells with 2 milliliters of phosphate buffered saline twice.

[0062] D. After rinsing, fix the cells with 2% formaldehyde and 0.05% glutaraldehyde for a period of 30 minutes at room temperature. Then, rinse the cells with 2 milliliters of phosphate buffered saline two additional times. E. Induce cell membrane porosity with 0.5% Tritron X-100 for a period of 20 minutes at room temperature so that the cells become permeabilized. Then, stain them with F-actin with TRITC-conjugated phalloidin (targeting filamentous actin network) at a concentration of 50 micrograms / milliliters. Incubate for 40 minutes in an opaque humidifier chamber. At the end of the 40 minutes, rinse the cells with 2 milliliters of phosphate buffered saline two additional times.

[0063] F. Continue by staining the cell nuclei with 0.1 microgram / milliliter DAPI and incubating for a period of 30 minutes in an opaque humidifier chamber. Then, rinse the cells with 2 milliliters of phosphate buffered saline three times. Place the cover glass with the cells that have been stained onto slides containing 20 microliters of 50% glycerol and coat the cover glass with nail varnish. Then, examine the actin structure under a fluorescent microscope using a TRITC filter with excitation wavelength at 544 nanometers and emission wavelength at 570 nanometers. The actin filaments will show the red color of TRITC fluorophore.

[0064] From the experimental results, it was found that coating the titanium alloy with the recombinant human secretory leukocyte protease inhibitor protein, in addition to its capacity to enhance cell adhesion within a 20-minute period, enhance cell expansion and distribution, as well. It is also a protein that sends a signal promoting further cell growth. From the results of this study, it can be seen that coating materials with the aforementioned coating protein activates the adhesion of the actin-molecule in the vicinity of the cell boundaries, activates cell expansion and spreading (Figure 5).

[0065] Example 6: Testing the effect of coating titanium alloy with the recombinant human secretory leukocyte protease inhibitor protein on the promotion of human bone cell growth

[0066] Coat the titanium alloy with the recombinant human secretory leukocyte protease inhibitor protein at concentrations of 0, 10, and 100 micrograms / milliliter in phosphate buffered saline and add 200 microliters of a cell suspension having a concentration of 1x105cells / milliliter into the cavity containing the titanium disc coated with the aforementioned protein. Incubate the cells for a period of 5 days, and measure the cell growth on days 3 and on days 5 by using the MTT cell viability assay.

[0067] The experimental results found that coating the titanium alloy with the recombinant human secretory leukocyte protease inhibitor protein at concentrations of 10 and 100 micrograms / milliliter could enhance the growth of human bone cells with statistical significance as compared to the results obtained from non-coating the titanium alloy with the aforementioned protein (Figure 6). Example 7: Analytical testing for the presence of cell adhesion molecules and regulatory molecules that control and stimulate differentiation of osteoblasts by a reverse transcription- quantitative polymerase chain reaction (RT-qPCR).

[0068] Adding of 500-microliter of 5xl05cells / milliliter human bone cell suspension into the culture wells containing the titanium disc coated with the recombinant human secretory leukocyte protease inhibitor protein, allowing it to remain for 7 days. At the end of the 7 days, rinse three times with phosphate buffered saline and extract the RNA, convert to cDNA. Finally, measure the purity and concentration of the cDNA present.

[0069] Perform an analytical test for the presence of the integrin-al, integrin-a2 and integrin-a5 genes by applying the reverse transcription-quantitative polymerase chain reaction (RT- qPCR)method. (Use the SYBR Premix Ex Taq Kit in testing the PCR results. There will be GAPDH control genes, which is housekeeping genes, in accordance with 2AACt.)

[0070] Perform an analytical test for the presence of regulatory molecules that control the differentiation of osteoblasts (namely ALP, osteocalcin, and RUNX2) by reverse transcription- quantitative polymerase chain reaction (RT-qPCR)method. (Proceed by using the SYBR Premix Ex Taq Kit in testing the PCR results. There will be GAPDH control genes, which will provide internal control, and also housekeeping genes, in accordance with 2AACt.)

[0071] It was found from the test results that coating the titanium alloy with the recombinant human secretory leukocyte protease inhibitor protein at a concentration of 10 micrograms / milliliter could stimulate the presence of cell adhesion molecules, namely integrin-al, integrin-a2 and integrin-a5, with statistical significance (Figures 7-9).

[0072] It was found from the test results that coating the titanium alloy with the recombinant human secretory leukocyte protease inhibitor protein at a concentration of 10 micrograms / milliliter could stimulate a controlled expression of osteoblast development (namely ALP, osteocalcin, and RUNX2) with statistical significance (Figures 10-12).

[0073] Best Mode of the Invention

[0074] As described in Detailed Description of the Invention

Claims

Claims1. A bioactive titanium coating process for orthopedics and dental implants comprises the following steps:A. Preparation of a titanium material by sterilization of titanium metalB. Preparation of a recombinant human secretory leukocyte protease inhibitor (rhSLPI) protein with a concentration ranging between 0.1 and 100 micrograms / milliliter. It is prepared from a stock solution with a concentration of 1 milligram / milliliter stored at -80 degrees Celsius and diluted to a concentration between 0.1 and 100 micrograms / milliliter with phosphate buffered saline (PBS) at a temperature ranging from 0 to 10 degrees Celsius and adjusted to pH 7.4C. Coating of the titanium material with the rhSLPI proteins. It is done by retrieving the rhSLPI protein that was prepared in step B and pouring it into the container holding the titanium material that was prepared in step A until it is fully immersed. Then incubate it at a temperature of 4-6 degrees Celsius for a period of 24 hours. Rinse the titanium material that has been treated with phosphate buffered saline to remove any proteins that did not adhere to the material. Then, add in the human bone cells, which will adhere to the coated material due to the effect of the rhSLPI protein.

2. The bioactive titanium coating process for orthopedics and dental implants according to claim1, wherein step A, the procedure for sterilizing the titanium metal, is selected from any one of disinfection with an autoclave, baking in a hot-air oven, steaming in hot water vapor, use of ethylene oxide or hydrogen peroxide gas plasma, or combination thereof.

3. The bioactive titanium coating process for orthopedics and dental implants according to claim2, wherein the hot-air-oven baking procedure is done at a temperature of 160-180 degrees Celsius for a period of 1-2 hours.

4. The bioactive titanium coating process for orthopedics and dental implants according to claim 2, wherein the steaming procedure is done at temperature of 100-140 degrees Celsius for a period of 1-30 minutes.

5. The bioactive titanium coating process for orthopedics and dental implants according to claim 2, wherein the use of ethylene oxide is at a concentration of 700-1,200 milligrams per liter and at a temperature of 40-60 degrees Celsius over a period of 3-6 hours.

6. The bioactive titanium coating process for orthopedics and dental implants according to claim 1, wherein step C, the titanium material that has been coated with the rhSLPI proteins is rinsed with phosphate buffered saline from 1 to 3 times.

Citation Information

Patent Citations

  • Medical prosthetic devices and implants having improved biocompatibility

    US20020111694A1

  • Enhanced bonding layers on titanium materials

    US20110093082A1

  • Osseointegrative surgical implant and implant surgical kit

    US20220031429A1