Substrate processing method

The substrate processing method uses a sequential etching approach with hydrofluoric acid, TMAH, and ammonium hydroxide solutions to achieve a flat surface profile, addressing the challenge of surface irregularities and ensuring precise thinning of silicon layers for semiconductor manufacturing.

WO2024228338A1PCT designated stage expired Publication Date: 2024-11-07SCREEN HOLDINGS CO LTD

Patent Information

Application Number
PCT/JP2024/015534
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-02
Filing Date
2024-04-19
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Existing substrate processing methods fail to effectively planarize the surface profile of silicon wafers during thinning, leading to irregularities that can damage the underlying layers and affect the precision of semiconductor device manufacturing.

Method used

A substrate processing method involving sequential etching steps with hydrofluoric acid, TMAH, and ammonium hydroxide solutions, where the etching parameters are adjusted to achieve a flat surface profile, including variable settings for the first and second etching steps and scanning parameters to control the liquid landing position, ensuring a composite surface profile with a flatness of 1.5 μm or less.

Benefits of technology

The method achieves precise thinning of silicon layers with a flat surface profile, preventing damage to the etching stop layer and enabling efficient removal of the silicon layer while maintaining the integrity of the silicon germanium layer, thereby enhancing the precision and reliability of semiconductor device manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015534_07112024_PF_FP_ABST
    Figure JP2024015534_07112024_PF_FP_ABST
Patent Text Reader

Abstract

This substrate processing method comprises: a substrate rotation step for rotating a substrate which has a main surface that has been ground or polished for substrate thinning, about a rotation axis perpendicular to the main surface; a first etching step for supplying a first etching solution which contains hydrofluoric acid or nitric acid to the main surface during the substrate rotation step; and a second etching step for supplying a second etching solution which contains tetramethylammonium hydroxide (TMAH) to the main surface, during the substrate rotation step but after the first etching step. A second etching parameter which is applied in the second etching step is adjusted to flatten a first surface profile which occurs at the main surface due to the first etching step.
Need to check novelty before this filing date? Find Prior Art

Description

Substrate processing method Related Applications

[0001] This application claims priority based on Japanese Patent Application No. 2023-75947 filed on May 2, 2023, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a substrate processing method.

[0003] US Pat. No. 5,699,499 discloses a substrate treatment for thinning a silicon wafer with an etchant.

[0004] JP 2012-199408 A

[0005] One embodiment of the present invention provides a substrate processing method that can flatten the surface profile of a main surface of a substrate while thinning the substrate by processing the main surface of the substrate with an etching solution.

[0006] One embodiment of the present invention provides a substrate processing method having the following exemplary features.

[0007] 1. A substrate processing method comprising: a substrate rotation step of rotating a substrate having a main surface that has been ground or polished for substrate thinning around a rotation axis perpendicular to the main surface; a first etching step of supplying a first etching solution containing hydrofluoric acid and nitric acid to the main surface while the substrate rotation step is being performed; and a second etching step of supplying a second etching solution containing TMAH (tetramethylammonium hydroxide) to the main surface after the first etching step while the substrate rotation step is being performed, wherein second etching parameters applied in the second etching step are adjusted to planarize a first surface profile generated on the main surface by the first etching step.

[0008] 2. The substrate processing method according to Item 1, wherein a first etching profile on the main surface in the first etching step is variable by variable setting of a first etching parameter applied in the first etching step, a second etching profile on the main surface in the second etching step is variable by variable setting of the second etching parameter applied in the second etching step, and the first etching parameter and the second etching parameter are adjusted so that a second surface profile generated on the main surface by sequentially performing the first etching step and the second etching step on the substrate has a flatness of a predetermined value or less.

[0009] 3. The substrate processing method according to Item 2, wherein the first etching parameters and the second etching parameters are adjusted so that a composite etching profile obtained by superimposing the first etching profile and the second etching profile has a flatness of a predetermined value or less.

[0010] 4. The substrate processing method according to Item 2, wherein the first etching parameters and the second etching parameters are adjusted so that a composite surface profile obtained by superposing an initial surface profile of the main surface before the first etching step, the first etching profile, and the second etching profile has a flatness of a predetermined value or less.

[0011] 5. The substrate processing method according to any one of Items 2 to 4, wherein the first etching step includes a first scanning step of moving a landing position of the first etching liquid on the main surface such that a distance between the landing position and the rotation axis changes over time, and the first etching parameters include first scanning parameters that define the change in the landing position in the first scanning step.

[0012] 6. The substrate processing method according to any one of Items 1 to 5, wherein the second etching step includes a second scanning step of moving a landing position of the second etching liquid on the main surface such that a distance between the landing position and the axis of rotation changes over time, and the second etching parameters include second scanning parameters that define the change in the landing position in the second scanning step.

[0013] 7. The substrate processing method according to any one of items 1 to 6, wherein a second surface profile of the main surface after the second etching step has a flatness of 1.5 μm or less.

[0014] 8. The substrate processing method according to any one of items 1 to 7, wherein the main surface is a surface on which a silicon layer is exposed.

[0015] 9. The substrate processing method according to item 8, wherein the substrate has a silicon germanium layer and the silicon layer stacked on the silicon germanium layer.

[0016] 10. The substrate processing method according to item 9, further comprising a third etching step of supplying a third etching solution containing ammonium hydroxide to the main surface after the second etching step while the substrate rotation step is being performed.

[0017] 11. The substrate processing method according to Item 10, wherein the thickness of the silicon layer at the end of the second etching step is 4 μm or less (and 2.5 μm or more).

[0018] 12. The substrate processing method according to item 10 or 11, wherein the thickness of the silicon germanium layer before the third etching step is 10 nm or less (and 5 nm or more).

[0019] 13. The substrate processing method according to any one of Items 10 to 12, wherein the concentration of ammonium hydroxide in the third etching solution and the temperature of the third etching solution are set so that the etching rate of the silicon layer in the third etching step is 200 nm / min or more (more preferably 300 nm / min or more) and the etching selectivity of silicon to silicon germanium is 150 or more (more preferably 250 or more).

[0020] The above and other objects, features and advantages of the present invention will become apparent from the following description of the embodiments with reference to the accompanying drawings.

[0021] FIGS. 1A and 1B show an example of a semiconductor device manufacturing process to which a substrate processing method according to an embodiment of the present invention is applied. FIG. 2 shows an example of the configuration of a substrate processing apparatus for performing the precision thinning step of the substrate processing method. FIG. 3 is a block diagram illustrating the electrical configuration of the substrate processing apparatus. FIGS. 4A to 4I show examples of various etching profiles that can be set by adjusting etching parameters. FIG. 5 is a flowchart showing an example of substrate processing in the precision thinning step. FIGS. 6A, 6B, and 6C show the main steps of the substrate processing. FIG. 7A shows an example of an initial surface profile before the start of the first etching step. FIG. 7B shows an example of a surface profile (first surface profile) after the first etching step. FIG. 7C shows an example of a surface profile (second surface profile) after the second etching step. FIG. 8 shows an example of a flow for adjusting etching parameters. FIG. 9 shows another example of a flow for adjusting etching parameters. 10A shows the results of investigating the relationship between the etching selectivity (left vertical axis) and etching rate (right vertical axis) and the ammonium hydroxide concentration (ammonium hydroxide:water) when etching silicon with ammonia water. Fig. 10B shows the results of investigating the relationship between the etching selectivity (left vertical axis) and etching rate (right vertical axis) and the ammonia water temperature when etching silicon with ammonia water with a concentration of ammonium hydroxide:water = 1:20.

[0022] 1A and 1B show an example of a semiconductor device manufacturing process using a substrate processing method according to an embodiment of the present invention. A first silicon wafer W1 includes a silicon layer 100 made of a silicon substrate, an etching stop layer 101, and a silicon active layer 102. The etching stop layer 101 is formed on the surface of the silicon layer 100, and the silicon active layer 102 is formed on the etching stop layer 101. The etching stop layer 101 is, for example, a silicon germanium (SiGe) layer, and the silicon active layer 102 is a silicon epitaxially grown layer epitaxially grown on the etching stop layer 101. Transistors and other devices (not shown) are formed in the silicon active layer 102. A multilayer wiring layer 103 is formed on the silicon active layer 102. The multilayer wiring layer 103 is formed by stacking wiring layers and interlayer insulating layers (neither of which is shown). A buried power rail (BPR) 104 is disposed across the silicon active layer 102 and the multi-layer wiring layer 103 .

[0023] The first silicon wafer W1 is bonded to a second silicon wafer W2 serving as a carrier substrate. More specifically, the exposed surface of the first silicon wafer W1 facing the multilayer wiring layer 103 is bonded to the main surface of the second silicon wafer W2 via an adhesive layer 300, thereby producing a bonded substrate W. The adhesive layer 300 may include, for example, a SiCN layer. The second silicon wafer W2 typically includes a silicon substrate 200 and an insulating layer 201 formed on the surface thereof. Therefore, the bonding surface of the second silicon wafer W2 is typically the surface of the insulating layer 201. Typically, the surface of this insulating layer 201 is bonded to the surface of the multilayer wiring layer 103 of the first silicon wafer W1 via the adhesive layer 300.

[0024] In the bonded substrate W thus obtained, the exposed main surface of the first silicon wafer W1 is the main surface to be processed, and this main surface is subjected to a thinning process to thin the substrate W. The thinning process is, in short, a process for removing the silicon layer 100 (silicon substrate) of the first silicon wafer W1 to expose the etching stop layer 101. That is, the target of the thinning process is the silicon layer 100 (silicon substrate). After this thinning process, the etching stop layer 101 is removed, leaving the silicon active layer 102. The second silicon wafer W2 is used, for example, to construct a power delivery network (PDN) on the side opposite the silicon active layer 102 (back side).

[0025] The thinning process includes a high-speed thinning stage and a precision thinning stage. The high-speed thinning stage includes a grinding stage and, if necessary, a polishing stage. The grinding stage is a stage in which a silicon layer 100 (silicon substrate) having a thickness of, for example, about 775 μm is thinned to a thickness of about 50 μm by grinding with a grinder. The polishing stage is a stage in which the main surface roughened by the grinding stage is polished, typically by CMP (chemical mechanical polishing). By the polishing stage, for example, the silicon layer 100 is thinned from a thickness of about 50 μm to a thickness of about 49 μm. The remaining 49 to 50 μm thick (hereinafter referred to as about 50 μm thick) of the silicon layer 100 is removed by the precision thinning stage.

[0026] The precision thinning step includes a first etching process in which a first etching solution containing hydrofluoric acid and nitric acid (typically, a hydrofluoric-nitric acid aqueous solution) is supplied to the main surface of the processing target, and then a second etching process in which a second etching solution containing TMAH (tetramethylammonium hydroxide) (typically, a TMAH aqueous solution) is supplied to the main surface of the processing target. In this embodiment, the precision thinning step further includes a third etching process in which a third etching solution containing ammonium hydroxide (typically, ammonia water) is supplied to the main surface of the processing target after the second etching process.

[0027] In the first etching step, the silicon layer 100 (silicon substrate) is thinned from a thickness of about 50 μm to a thickness of about 10 μm. The first etching step is a high-speed wet etching step with a relatively high etching rate.

[0028] The second etching step, which is performed after the first etching step, is a slow wet etching step with a lower etching rate than the first etching step. In the second etching step, the silicon layer 100 is thinned, for example, from a thickness of about 10 μm to a thickness of about 3 μm. The thickness of the silicon layer 100 at the end of the second etching step is preferably 4 μm or less (and 2.5 μm or more).

[0029] The third etching step, which is performed after the second etching step, is a step of removing the remaining silicon layer 100 having a thickness of about 3 μm, and typically involves removing not only the silicon layer 100 but also a portion of the thickness of the surface layer of the etching stop layer 101, so that all the material of the silicon layer 100 thereon is removed while leaving the etching stop layer 101. For example, if the initial thickness of the etching stop layer 101 is about 10 nm, a portion of the surface layer having a thickness of about 5 nm may be removed.

[0030] It is preferable that the silicon germanium layer constituting the etching stop layer 101 has as little germanium as possible and as thin a film thickness as possible. 0.75 Ge 0.25 The etching stop layer 101 can be formed of a silicon germanium layer. This allows the lattice constant of the silicon layer 100 to be inherited by the silicon active layer 102 via the silicon germanium layer, and also suppresses crystal defects (dislocations) caused by stress relaxation in the silicon germanium layer. Therefore, the thickness of the etching stop layer 101 is preferably 10 nm or less.

[0031] On the other hand, because the germanium composition is low, the etching selectivity of the silicon layer 100 relative to the etching stop layer 101 cannot be made very high in the third etching step (etching with ammonia water). Therefore, etching of the etching stop layer 101 inevitably occurs. Therefore, it is preferable that the etching stop layer 101 has a layer thickness of 5 nm or more.

[0032] If the surface profile of the main surface has large irregularities when the third etching step is started, there is a risk that the third etching solution will penetrate the thin etching stop layer 101, which is about 5 nm to 10 nm thick, during the third etching step, and damage the silicon active layer 102. Therefore, the surface profile of the silicon layer 100 must be sufficiently flattened after the thinning step up to the second etching step is completed.

[0033] 2 shows an example of the configuration of a substrate processing apparatus 1 for performing the precision thinning step. This substrate processing apparatus 1 includes a spin chuck 2 that holds and rotates a substrate W, a processing liquid supply unit 5 that supplies a processing liquid to a main surface (the main surface to be processed) of the substrate W held on the spin chuck 2, and a controller 6 that controls the spin chuck 2 and the processing liquid supply unit 5. The processing liquid supply unit 5 includes a first etching liquid supply unit 51, a second etching liquid supply unit 52, and a third etching liquid supply unit 53 that supply a first etching liquid, a second etching liquid, and a third etching liquid, respectively, to the main surface of the substrate W held on the spin chuck 2. This substrate processing apparatus 1 further includes a thickness sensor 7 that detects the height of the surface of the substrate W to thereby detect the thickness of the layer to be processed.

[0034] The spin chuck 2 includes a rotary holder 3 that holds the substrate W to be processed (the bonded substrate described above) in a horizontal position with its main surface facing upward and is rotatable about a rotation axis A1 perpendicular (i.e., plumb) to the main surface, and a spin motor 4 that rotates the rotary holder 3 about the rotation axis A1. The rotary holder 3 preferably has the form of a vacuum chuck that holds the lower surface of the substrate W by suction. However, the rotary holder 3 may also have the form of a mechanical chuck that has holding pins that abut against the peripheral edge surface of the substrate W. The rotation / stop and rotation speed of the spin motor 4 are controlled by a controller 6.

[0035] The first etching liquid supply unit 51 includes a first nozzle 10 that discharges a processing liquid toward the main surface (upper surface) of the substrate W held by the spin chuck 2, a first processing liquid pipe 11 connected to the first nozzle 10, a first etching liquid pipe 12 that supplies a first etching liquid to the first processing liquid pipe 11, a first rinse liquid pipe 13 that supplies a rinse liquid to the first processing liquid pipe 11, and a first nozzle movement unit 14 that moves the first nozzle 10. A first processing liquid valve 15 consisting of an on-off valve is interposed in the first processing liquid pipe 11. The first etching liquid pipe 12 connects a first etching liquid supply source and the first processing liquid pipe 11 and allows the first etching liquid (e.g., a hydrofluoric nitric acid aqueous solution) supplied from the first etching liquid supply source to the first nozzle 10 to flow. A first etching liquid valve 16 and a first etching liquid flow rate adjustment valve 17 are interposed in the first etching liquid pipe 12. The first etching liquid valve 16 is an on-off valve. When the first etching liquid valve 16 is opened, the first etching liquid is discharged from the first nozzle 10 at a flow rate adjusted by the first etching liquid flow rate adjustment valve 17. The first rinse liquid pipe 13 allows the rinse liquid supplied from a rinse liquid supply source to the first processing liquid pipe 11 to flow. The first rinse liquid pipe 13 is provided with a first rinse liquid flow rate adjustment valve 19 that adjusts the flow rate of the rinse liquid, and a first rinse liquid valve 18 that is an on-off valve. The rinse liquid is typically deionized water. However, other types of rinse liquid, such as carbonated water or electrolyzed water, may also be used.

[0036] The first nozzle movement unit 14 includes a first nozzle holder 14A that holds the first nozzle 10 and a first nozzle drive unit 14B that drives the first nozzle holder 14A to move the first nozzle 10. The first nozzle drive unit 14B includes, for example, a first scan motor M1 as a drive source and a first transmission mechanism T1 that transmits the drive force of the first scan motor M1 to the first nozzle holder 14A. The first nozzle drive unit 14B is configured, for example, to be able to move the first nozzle 10 at least in a direction parallel to the main surface of the substrate W (in this embodiment, the horizontal direction). More essentially, the first nozzle movement unit 14 is configured to move the first nozzle 10 so as to change the distance between the rotation axis A1 and a liquid landing position where the processing liquid discharged from the first nozzle 10 lands on the main surface of the substrate W. More specifically, the liquid landing position may move approximately along the radial direction of the rotation of the substrate W centered on the rotation axis A1. While the substrate W is rotated about the rotation axis A1, the landing position of the processing liquid from the first nozzle 10 moves in the direction of the rotation radius, so that the landing position scans the surface of the substrate W. This type of discharge mode of the processing liquid is called "scanning discharge." The processing liquid can also be discharged by keeping the first nozzle 10 stationary at a predetermined position and discharging the processing liquid such that the landing position of the processing liquid on the substrate W is in the direction of the rotation radius. This type of discharge mode of the processing liquid is called "fixed discharge."

[0037] The second etching liquid supply unit 52 includes a second nozzle 20 that discharges a processing liquid toward the main surface (upper surface) of the substrate W held by the spin chuck 2, a second processing liquid pipe 21 connected to the second nozzle 20, a second etching liquid pipe 22 that supplies a second etching liquid to the second processing liquid pipe 21, a second rinse liquid pipe 23 that supplies a rinse liquid to the second processing liquid pipe 21, and a second nozzle moving unit 24 that moves the second nozzle 20. A second processing liquid valve 25 consisting of an on-off valve is interposed in the second processing liquid pipe 21. The second etching liquid pipe 22 connects a second etching liquid supply source and the second processing liquid pipe 21 and allows the second etching liquid (e.g., a TMAH aqueous solution) supplied from the second etching liquid supply source to the second nozzle 20 to flow through the second etching liquid pipe 22. A second etching liquid valve 26 and a second etching liquid flow rate adjustment valve 27 are interposed in the second etching liquid pipe 22. The second etching liquid valve 26 is an on-off valve. When the second etching liquid valve 26 is opened, the second etching liquid is discharged from the second nozzle 20 at a flow rate adjusted by the second etching liquid flow rate adjustment valve 27. The second rinse liquid pipe 23 allows the rinse liquid supplied from the rinse liquid supply source to the second processing liquid pipe 21 to flow. The second rinse liquid pipe 23 is provided with a second rinse liquid flow rate adjustment valve 29 that adjusts the flow rate of the rinse liquid, and a second rinse liquid valve 28 that is an on-off valve.

[0038] The second nozzle movement unit 24 includes a second nozzle holder 24A that holds the second nozzle 20 and a second nozzle drive unit 24B that drives the second nozzle holder 24A to move the second nozzle 20. The second nozzle drive unit 24B includes, for example, a second scan motor M2 as a drive source and a second transmission mechanism T2 that transmits the drive force of the second scan motor M2 to the second nozzle holder 24A. The second nozzle drive unit 24B is configured, for example, to be able to move the second nozzle 20 at least in a direction parallel to the main surface of the substrate W (the horizontal direction in this embodiment). More essentially, the second nozzle movement unit 24 is configured to move the second nozzle 20 so that the distance between the rotation axis A1 and a liquid landing position where the processing liquid discharged from the second nozzle 20 lands on the main surface of the substrate W changes. More specifically, the liquid landing position may move approximately along the radial direction of the rotation of the substrate W centered on the rotation axis A1. While the substrate W is rotated about the rotation axis A1, the landing position of the processing liquid from the second nozzle 20 moves in the direction of the rotation radius, so that the landing position scans the surface of the substrate W. Therefore, the second nozzle 20 also allows for scanning discharge and fixed discharge.

[0039] The third etching liquid supply unit 53 includes a third nozzle 30 that discharges a processing liquid toward the main surface (upper surface) of the substrate W held by the spin chuck 2, a third processing liquid pipe 31 connected to the third nozzle 30, a third etching liquid pipe 32 that supplies a third etching liquid to the third processing liquid pipe 31, a third rinse liquid pipe 33 that supplies a rinse liquid to the third processing liquid pipe 31, and a third nozzle moving unit 34 that moves the third nozzle 30. A third processing liquid valve 35 consisting of an on-off valve is interposed in the third processing liquid pipe 31. The third etching liquid pipe 32 connects a third etching liquid supply source and the third processing liquid pipe 31 and allows the third etching liquid (e.g., ammonia water) supplied from the third etching liquid supply source to the third nozzle 30 to flow through the third etching liquid pipe 32. A third etching liquid valve 36 and a third etching liquid flow rate adjustment valve 37 are interposed in the third etching liquid pipe 32. The third etching liquid valve 36 is an on-off valve. When the third etching liquid valve 36 is opened, the third etching liquid is discharged from the third nozzle 30 at a flow rate adjusted by the third etching liquid flow rate adjustment valve 37. The third rinse liquid pipe 33 allows the rinse liquid supplied from the rinse liquid supply source to the third processing liquid pipe 31 to flow. The third rinse liquid pipe 33 is provided with a third rinse liquid flow rate adjustment valve 39 that adjusts the flow rate of the rinse liquid, and a third rinse liquid valve 38 that is an on-off valve.

[0040] The third nozzle movement unit 34 includes a third nozzle holder 34A that holds the third nozzle 30 and a third nozzle drive unit 34B that drives the third nozzle holder 34A to move the third nozzle 30. The third nozzle drive unit 34B includes, for example, a third scan motor M3 as a drive source and a third transmission mechanism T3 that transmits the drive force of the third scan motor M3 to the third nozzle holder 34A. The third nozzle drive unit 34B is configured, for example, to be able to move the third nozzle 30 at least in a direction parallel to the main surface of the substrate W (in this embodiment, the horizontal direction). More essentially, the third nozzle movement unit 34 is configured to move the third nozzle 30 so as to change the distance between the rotation axis A1 and a liquid landing position where the processing liquid discharged from the third nozzle 30 lands on the main surface of the substrate W. More specifically, the liquid landing position may move approximately along the radial direction of the rotation of the substrate W centered on the rotation axis A1. While the substrate W is rotated about the rotation axis A1, the landing position of the processing liquid from the third nozzle 30 moves in the direction of the rotation radius, so that the landing position scans the surface of the substrate W. Therefore, the third nozzle 30 also allows for scanning discharge and fixed discharge.

[0041] The thickness sensor 7 is held by a sensor holder 45. The sensor holder 45 is driven by a sensor drive unit 46, thereby moving the thickness sensor 7 along the rotation radius direction of the substrate W. As a result, the detection position of the thickness sensor 7 moves in the rotation radius direction of the substrate W. Therefore, the relationship between the detection position of the thickness sensor 7 and the detection value of the thickness sensor 7 represents the surface profile of the substrate W. Therefore, the thickness sensor 7, the sensor drive unit 46, etc. form a surface profile monitor unit that monitors the surface profile. The sensor drive unit 46 typically includes a fourth scan motor M4 and a fourth transmission mechanism T4 that transmits the driving force of the fourth scan motor M4 to the sensor holder 45.

[0042] 3 is a block diagram illustrating the electrical configuration of the substrate processing apparatus 1. The controller 6 includes a processor 61 and a memory 62. The processor 61 executes a program stored in the memory 62 to control various components of the substrate processing apparatus 1 and control processing of substrates W. Specifically, the controller 6 controls the drive / stop and rotation speeds of the spin motor 4, the first scan motor M1, the second scan motor M2, the third scan motor M3, and the fourth scan motor M4. The controller 6 also controls the opening and closing of the first processing liquid valve 15, the first etching liquid valve 16, the first rinse liquid valve 18, the second processing liquid valve 25, the second etching liquid valve 26, the second rinse liquid valve 28, the third processing liquid valve 35, the third etching liquid valve 36, and the third rinse liquid valve 38. Furthermore, the controller 6 may be configured to control the apertures (i.e., flow rates) of the first etchant flow control valve 17, the first rinse liquid flow control valve 19, the second etchant flow control valve 27, the second rinse liquid flow control valve 29, the third etchant flow control valve 37, and the third rinse liquid flow control valve 39. An output signal from the thickness sensor 7 is also input to the controller 6. An input device 66 and a display device 65 that provide a man-machine interface are also connected to the controller 6. A user can input various commands to the controller 6 and check the status of the substrate processing apparatus 1 by using the input device 66 and the display device 65.

[0043] The controller 6 further includes an auxiliary storage device 63, which is a large-capacity storage device. Recipes that define substrate processing conditions can be registered in the auxiliary storage device 63. In addition, various parameter groups for etching processing, i.e., etching parameters, can be set and registered in the auxiliary storage device 63. Specifically, first etching parameters for the first etching step, second etching parameters for the second etching step, and third etching parameters for the third etching step can be set and registered.

[0044] The etching parameters include parameters relating to the discharge conditions, the concentration of the etching liquid, the temperature of the etching liquid, etc. The parameters relating to the discharge conditions may include parameters defining the discharge flow rate of the etching liquid, parameters defining the discharge timing of the etching liquid, parameters relating to the movement speed of the nozzle (in other words, the movement speed of the liquid landing position), parameters relating to the rotation speed of the substrate W, etc. For example, the parameters relating to the discharge conditions may be in the form of a table that defines one or more of the movement speed of the nozzle, the discharge flow rate of the etching liquid, and the substrate rotation speed relative to the position of the nozzle in the rotation radius direction (in other words, the liquid landing position).

[0045] By adjusting these etching parameters, it is possible to adjust the etching profile, which is the relationship between the amount of etching (etching depth) and the position on the main surface of the substrate W in the radial direction of rotation (the distance from the rotation axis A1).

[0046] The term "etching profile" as used herein refers to the surface profile of the main surface of the substrate W after etching when the main surface of the substrate W is completely flat. More specifically, the etching profile represents the relationship between the etching depth and the position in the radial direction of rotation on the substrate main surface. The surface profile refers to the relationship between the height of the main surface of the substrate W and the position in the radial direction of rotation on the main surface of the substrate W. In reality, the main surface of the substrate W is not completely flat when starting substrate processing in the precision thinning stage. Therefore, the surface profile after etching has a shape obtained by superimposing the etching profile on the surface profile before etching.

[0047] Hereinafter, the surface profile before the start of the first etching step will be referred to as the "initial surface profile." Furthermore, the surface profile after the end of the first etching step and before the start of the second etching step will be referred to as the "first surface profile." Furthermore, the surface profile after the end of the second etching step and before the start of the third etching step will be referred to as the "second surface profile." Furthermore, the etching profile in the first etching step will be referred to as the "first etching profile." The first etching profile is the difference between the first surface profile and the initial surface profile. Similarly, the etching profile in the second etching step will be referred to as the "second etching profile." The second etching profile is the difference between the second surface profile and the first surface profile.

[0048] In the first etching step, for example, a scan discharge of the first etching liquid is performed. That is, the first etching step includes a first scanning step in which the landing position of the first etching liquid on the main surface of the substrate is moved so that the distance between the landing position and the rotation axis A1 changes over time. In this case, the first etching parameters include first scanning parameters that define the change in the landing position in the first scanning step. The first scanning parameters are typically in the form of a table that defines the position of the first nozzle 10 in the rotation radius direction over time. By variably setting the first scanning parameters, the first etching profile can be adjusted to various shapes.

[0049] Similarly, in the second etching step, for example, scanning discharge of the second etching liquid is performed. That is, the second etching step includes a second scanning step in which the landing position of the second etching liquid on the main surface of the substrate is moved so that the distance between the landing position and the rotation axis A1 changes over time. In this case, the second etching parameters include second scanning parameters that define the change in the landing position in the second scanning step. The second scanning parameters typically have the form of a table that defines the position of the second nozzle 20 in the rotation radius direction over time. By variably setting the second scanning parameters, the second etching profile can be adjusted to various shapes.

[0050] 4A to 4I show examples of various etching profiles that can be set by adjusting etching parameters when a hydrofluoric nitric acid solution is used as the first etching solution. Similarly, various etching profiles can be set for the second etching solution.

[0051] By appropriately setting the etching parameters, it is possible to set an etching profile that is as flat as possible. In addition, by setting the etching parameters (especially the scan parameters), it is possible to intentionally set the peaks of the etching profile (regions where the etching rate is relatively low and the etching depth is shallow) and the valleys of the etching profile (regions where the etching rate is relatively high and the etching depth is deep) at any rotation radius position.

[0052] The achievable amplitude of the etching profile depends on the etching rate of the etching solution used. The amplitude of the etching profile can be increased with an etching solution having a high etching rate, while the achievable amplitude of the etching profile is small with an etching solution having a low etching rate. Conversely, the minimum amplitude of the etching profile achievable with an etching solution having a high etching rate is larger than the minimum amplitude of the etching profile achievable with an etching solution having a low etching rate.

[0053] More specifically, the etching rate of fluoronitric acid, which is an example of the first etching liquid, is higher than the etching rate of a TMAH aqueous solution, which is an example of the second etching liquid. Therefore, the etching profile of the etching process using the first etching liquid generally has a larger amplitude than the etching profile of the etching process using the second etching liquid.

[0054] Fig. 5 is a flow chart showing an example of substrate processing in the precision thinning stage. Figs. 6A, 6B, and 6C are diagrams showing the main steps. The substrate W that has undergone the high-speed thinning stage is transferred to and held by the spin chuck 2 by the substrate transfer robot. The controller 6 then drives the spin motor 4 to rotate the substrate W about the rotation axis A1, thereby starting the substrate rotation process (step S1).

[0055] While the substrate rotation process is being performed, the controller 6 executes a first etching process (step S2; see FIG. 6A ). The first etching process is a process of supplying a first etching liquid containing hydrofluoric acid and nitric acid (typically, a hydrofluoric-nitric acid aqueous solution) to the main surface of the substrate W. In the first etching process, the controller 6 applies first etching parameters preset for the first etching process. Specifically, the controller 6 controls the spin motor 4, the first etching liquid valve 16, the first etching liquid flow rate control valve 17, the first scan motor M1, and the like in accordance with the first etching parameters. The controller 6 then opens the first processing liquid valve 15 to discharge the first etching liquid from the first nozzle 10 onto the main surface of the substrate W. Typically, the first etching liquid is supplied to the main surface of the substrate W by scan discharge from the first nozzle 10 (first scan process), and the main surface of the substrate W is etched by the first etching liquid. As a result, the main surface of the substrate W is etched in accordance with a first etching profile corresponding to the first etching parameters.

[0056] After the first etching step is completed, the controller 6 closes the first etching liquid valve 16 to stop the supply of the first etching liquid, and then performs a first rinsing step while continuing the substrate rotation step (step S3). The first rinsing step is a process in which a rinse liquid is supplied to the main surface of the substrate W to replace the first etching liquid on the main surface of the substrate W with the rinse liquid and rinse it off the substrate W. Specifically, the controller 6 controls the spin motor 4, the first rinse liquid valve 18, the first rinse liquid flow rate adjustment valve 19, the first scan motor M1, and the like. This causes the rinse liquid to be ejected from the first nozzle 10 onto the main surface of the substrate W. The ejection in this case may be a fixed ejection in which the landing position of the rinse liquid is fixed near the rotation axis A1, or a scanning ejection. After the rinsing process has been performed for a predetermined time, the controller 6 closes the first rinse liquid valve 18 and the first processing liquid valve 15 to complete the first rinsing step.

[0057] Next, while the substrate rotation process is being performed, the controller 6 performs a second etching process (step S4; see FIG. 6B ). The second etching process is a process of supplying a second etching liquid containing TMAH (typically, a TMAH aqueous solution) to the main surface of the substrate W. In the second etching process, the controller 6 applies second etching parameters preset for the second etching process. Specifically, the controller 6 controls the spin motor 4, the second etching liquid valve 26, the second etching liquid flow rate control valve 27, the second scan motor M2, and the like in accordance with the second etching parameters. The controller 6 then opens the second processing liquid valve 25 to discharge the second etching liquid from the second nozzle 20 onto the main surface of the substrate W. Typically, the second etching liquid is supplied to the main surface of the substrate W by scan discharge from the second nozzle 20 (second scan process), and the main surface of the substrate W is etched by the second etching liquid. As a result, the main surface of the substrate W is etched in accordance with a second etching profile corresponding to the second etching parameters.

[0058] Upon completion of the second etching step, the controller 6 closes the second etching liquid valve 26 to stop the supply of the second etching liquid, and then performs a second rinsing step while continuing the substrate rotation step (step S5). The second rinsing step is a process in which a rinse liquid is supplied to the main surface of the substrate W to replace the second etching liquid on the main surface of the substrate W with the rinse liquid and rinse it off the substrate W. Specifically, the controller 6 controls the spin motor 4, the second rinse liquid valve 28, the second rinse liquid flow rate adjustment valve 29, the second scan motor M2, and the like. This causes the rinse liquid to be ejected from the second nozzle 20 onto the main surface of the substrate W. The ejection in this case may be a fixed ejection in which the landing position of the rinse liquid is fixed near the rotation axis A1, or a scanning ejection. After the rinsing process has been performed for a predetermined time, the controller 6 closes the second rinse liquid valve 28 and the second processing liquid valve 25 to complete the second rinsing step.

[0059] Next, while the substrate rotation process is being performed, the controller 6 performs a third etching process (step S6; see FIG. 6C ). The third etching process is a process of supplying a second etching liquid (typically, ammonia water) containing ammonium hydroxide to the main surface of the substrate W. In the third etching process, the controller 6 applies third etching parameters preset for the third etching process. Specifically, the controller 6 controls the spin motor 4, the third etching liquid valve 36, the third etching liquid flow rate adjustment valve 37, the third scan motor M3, and the like in accordance with the third etching parameters. The controller 6 then opens the third processing liquid valve 35 to discharge the third etching liquid from the third nozzle 30 onto the main surface of the substrate W. As a result, typically, the third etching liquid is supplied to the main surface of the substrate W by scan discharge from the third nozzle 30 (third scan process), and the main surface of the substrate W is etched by the third etching liquid.

[0060] After the third etching step is completed, the controller 6 closes the third etching liquid valve 36 to stop the supply of the third etching liquid, and then performs a third rinsing step while continuing the substrate rotation step (step S7). The third rinsing step is a process in which a rinse liquid is supplied to the main surface of the substrate W to replace the third etching liquid on the main surface of the substrate W with the rinse liquid and rinse it off the substrate W. Specifically, the controller 6 controls the spin motor 4, the third rinse liquid valve 38, the third rinse liquid flow rate adjustment valve 39, the third scan motor M3, and the like. This causes the rinse liquid to be ejected from the third nozzle 30 onto the main surface of the substrate W. The ejection in this case may be a fixed ejection in which the landing position of the rinse liquid is fixed near the rotation axis A1, or a scanning ejection. After the rinsing process has been performed for a predetermined time, the controller 6 closes the third rinse liquid valve 38 and the third processing liquid valve 35 to complete the third rinsing step.

[0061] Thereafter, the controller 6 performs a drying process (step S8) to remove the liquid on the substrate W and dry the substrate W. The drying process is typically a spin dry process in which the rotation speed of the spin chuck 2 is accelerated to a drying rotation speed.

[0062] After the drying step is completed, the controller 6 stops the rotation of the spin chuck 2, thereby completing the substrate rotation step (step S9). Thereafter, the processed substrate W is unloaded by the substrate transport robot.

[0063] 7A shows an example of a surface profile of the main surface of the substrate W after the high-speed thinning step, i.e., an initial surface profile before the start of the first etching step. The horizontal axis represents the radial position of rotation (distance from the rotation axis A1), and the vertical axis represents the thickness of the silicon layer 100 to be removed. Since there is some variation in the circumferential position around the rotation axis A1, the surface profile has a band-like shape rather than a linear shape. Here, the target layer thickness in the high-speed thinning step is set to 49 μm.

[0064] 7B shows an example of a surface profile (first surface profile) after the first etching step using a fluoronitric acid aqueous solution (first etching solution). The first surface profile is a superposition of the initial profile and the first etching profile. In other words, the difference between the first surface profile and the initial surface profile is the first etching profile.

[0065] 7C shows an example of a surface profile (second surface profile) after the second etching step using a TMAH aqueous solution (second etching solution). The second surface profile is a superposition of the first surface profile and the second etching profile. In other words, the difference between the second surface profile and the first surface profile is the second etching profile. The second surface profile is a superposition of the initial surface profile, the first etching profile, and the second etching profile.

[0066] In this embodiment, the etching conditions of the first etching step (first etching parameters) and the etching conditions of the second etching step (second etching parameters) are set so as to make the second surface profile as flat as possible. More specifically, the first etching parameters (particularly the first scan parameters) and the second etching parameters (particularly the second scan parameters) are adjusted and set so that the second surface profile is flatter than the first surface profile. The first etching profile is adjusted by adjusting the first etching parameters, and the second etching profile is adjusted by adjusting the second etching parameters. Adjusting the first etching parameters can be rephrased as adjusting the first etching profile, and adjusting the second etching parameters can be rephrased as adjusting the second etching profile.

[0067] As described above, the etching rate of the fluoronitric acid aqueous solution (first etching solution) is relatively high, and therefore the first etching profile has a relatively large amplitude. Therefore, it is difficult for the first surface profile (see FIG. 7B ) to achieve the desired level of flatness. On the other hand, the etching rate of the TMAH aqueous solution (second etching solution) is relatively low, and therefore the second etching profile can have a small amplitude. On the other hand, the second etching profile cannot have a large amplitude. Therefore, the general shape of the second surface profile is determined by the first etching process.

[0068] Therefore, if the first etching step is performed by setting the first etching parameters so that the first surface profile is the flattest, and then the second etching step is performed, it is believed that the second surface profile will have good flatness. However, research by the present inventors has discovered that this process, which is considered to be reasonable, does not necessarily ultimately achieve the best (flattest) second surface profile. More specifically, the combination of the first etching parameters that result in the flattest first surface profile and the second etching parameters that result in the flattest second surface profile for the first etching parameters is not necessarily an optimal solution.

[0069] Therefore, the inventors considered adjusting the first surface profile (i.e., adjusting the first etching profile) based on a second etching profile that can be realized by adjusting the second etching parameters, thereby obtaining a second surface profile with high flatness. They then discovered that, rather than individually setting the conditions for the first etching step and the second etching step and adjusting them so as to obtain the flattest possible surface profile in each step, it is possible to set first etching conditions that do not necessarily result in the flattest first surface profile, while adjusting the first etching conditions and second etching conditions so as to obtain the flattest second surface profile.

[0070] FIG. 8 shows an example of the flow of adjusting the etching parameters.

[0071] A plurality of variations of first etching parameters (parameter group) for the first etching step are prepared (step S11). Then, a first etching profile is obtained by actual measurement or simulation when the first etching step is performed on the main surface of the substrate W that has undergone the high-speed thinning stage using each variation of the first etching parameters (step S12). When the first etching profile is obtained by actual measurement, the first etching profile can be obtained by measuring the first surface profile and the surface profile of the main surface of the substrate W before the first etching step (initial surface profile) using the thickness sensor 7 and calculating the difference between them.

[0072] Furthermore, multiple sets of variations of the second etching parameters (parameter group) for the second etching step are prepared (step S13). Then, a second etching profile obtained by actual measurement or simulation when the second etching step is performed on the main surface of the substrate W using each variation of the second etching parameters (step S14). When the second etching profile is obtained by actual measurement, the second etching profile can be obtained by measuring the second surface profile and the surface profile of the main surface of the substrate W before the second etching step using the thickness sensor 7 and calculating the difference between them. In this case, the substrate W is preferably a substrate W that has undergone the first etching step, but may also be a substrate W that has undergone a high-speed thinning stage but not the first etching step.

[0073] Next, the first etching profile and the second etching profile are superimposed to generate a composite etching profile (step S15). The composite etching profile is generated for all combinations of a plurality of first etching profiles obtained from a plurality of variations of the first etching parameter and a plurality of second etching profiles obtained from a plurality of variations of the second etching parameter.

[0074] From the plurality of composite etching profiles thus created, a composite etching profile that is flattest over the entire substrate W is selected (step S16). At this time, a composite etching profile having a flatness of a predetermined value (e.g., 1.5 μm) or less is selected. A combination of the first etching parameters and the second etching parameters corresponding to the selected composite etching profile is determined as the etching parameters to be applied to the substrate processing (step S17).

[0075] When the initial surface profile has sufficient flatness, the composite etching profile has a flatness of a predetermined value or less, and accordingly, the main surface of the substrate W after the second etching step can have a flatness of a predetermined value (e.g., 1.5 μm) or less. Therefore, by applying the first etching parameters and second etching parameters determined as described above to the first etching step and the second etching step, respectively, the main surface of the substrate W after the second etching step can have a flatness of a predetermined value or less.

[0076] 9 shows another example of the flow of adjusting etching parameters, in which the same steps as those in FIG. 8 are denoted by the same reference numerals.

[0077] In this example, the initial surface profile is superimposed on the multiple composite etching profiles obtained in step S15 to obtain multiple composite surface profiles corresponding to the second surface profile (step S21). Then, the flattest composite surface profile across the entire substrate is selected (step S22). At this time, the composite surface profile with a flatness of a predetermined value (e.g., 1.5 μm) or less is selected. The combination of the first etching parameters and the second etching parameters corresponding to the composite etching profile obtained when the selected composite surface profile is obtained is determined as the etching parameters to be applied to the substrate processing (step S23). When the flatness of the initial surface profile is insufficient, the surface profile after the second etching step can be optimized by determining the etching parameters based on the flatness of the composite surface profile.

[0078] The composite surface profile is a surface profile obtained by superimposing the first etching profile and the second etching profile on the initial surface profile, and corresponds to the second surface profile as described above. Therefore, the first etching parameters and the second etching parameters are determined so that the composite surface profile has a flatness of a predetermined value (e.g., 1.5 μm) or less. By applying the first etching parameters and the second etching parameters determined in this manner to the first etching step and the second etching step, respectively, the main surface of the substrate W after the second etching step can have a flatness of a predetermined value (e.g., 1.5 μm) or less.

[0079] One of the etching parameters that has a significant effect on the etching profile is the scan parameter. As described above, the first etching parameter includes the first scan parameter, and the second etching parameter includes the second scan parameter. The scan parameter is a parameter that defines the change in the landing position over time in the scanning process. That is, the scan parameter defines the change in the landing position over time. More specifically, the scan parameter defines the change in the position of the moving nozzle over time. By appropriately adjusting the combination of the first scan parameter and the second scan parameter, the surface profile of the main surface of the substrate W after the second etching process can have a flatness of a predetermined value (e.g., 1.5 μm) or less.

[0080] 10A and 10B are diagrams illustrating an example of the characteristics of the third etching step. The purpose of the third etching step is to remove all of the silicon layer 100 remaining on the etching stop layer 101, which is a silicon germanium layer, without penetrating the etching stop layer 101. To achieve this, the etching selectivity of silicon relative to silicon germanium is preferably as high as possible, for example, preferably 150 or more, and more preferably 250 or more. Furthermore, to shorten the processing time, the etching rate of the silicon layer 100 is preferably as high as possible, for example, preferably 200 nm / min or more, and more preferably 300 nm / min or more.

[0081] FIG. 10A shows the case where silicon is selectively etched using ammonia water, which is an example of the third etching solution, and shows the results of etching using ammonium hydroxide (NH 4 The graph shows the results of investigating the relationship between the etching selectivity (left vertical axis) and etching rate (right vertical axis) with respect to the concentration of ammonium hydroxide (OH) (ammonium hydroxide:water). The horizontal axis represents the proportion of water when the proportion of ammonium hydroxide is set to 1. The etching selectivity is 0.75 Ge 0.25 This figure shows the ratio of the etching rate of Si to the etching rate of ammonium hydroxide (the same applies to Figure 10B, which will be explained next). The temperature of the ammonia water was 70°C. In the figure, the etching selectivity is represented by "○" and the etching rate by "●". The etching rate increases as the concentration increases. On the other hand, the etching selectivity shows an increasing tendency with increasing concentration up to approximately 1:30 ammonium hydroxide:water, remains almost unchanged in the ammonium hydroxide:water ratio range from 30 to 20, and tends to decrease in the concentration range above 1:20 ammonium hydroxide:water.

[0082] FIG. 10B shows the results of investigating the relationship between the etching selectivity (left vertical axis) and etching rate (right vertical axis) versus the temperature of ammonia water when selectively etching silicon using ammonia water with a concentration of ammonium hydroxide:water = 1:20. The horizontal axis represents the temperature of the ammonia water. As in FIG. 10A, the etching selectivity is represented by "○" and the etching rate by "●". The etching rate increases with increasing temperature. Meanwhile, the etching selectivity tends to decrease up to 50°C, then increases at temperatures above 50°C, reaches a maximum near 60°C, and then decreases again at temperatures above 60°C.

[0083] Therefore, for example, by using ammonia water at 60° C. with ammonium hydroxide:water=1:20 as the third etching solution, an etching rate of 300 nm / min or more and an etching selectivity of 250 or more can be achieved.

[0084] In this way, by performing the third etching step using ammonia water with an appropriately set concentration and temperature as the third etching solution, it is possible to remove all of the silicon layer 100 remaining on the etching stop layer 101 while suppressing film loss in the etching stop layer 101 made of a silicon germanium layer. For example, the film loss in the etching stop layer 101 can be kept to 5 nm or less.

[0085] Although the embodiment of the present invention has been described above, the present invention can be embodied in other forms.

[0086] For example, in the above-described embodiments, the high-speed thinning step has been mainly described as including a grinding step and a polishing step, but the polishing step may be omitted.

[0087] The precision thinning step may also include a dry etching step prior to the first etching step.

[0088] Although the embodiments of the present invention have been described in detail, these are merely examples used to clarify the technical contents of the present invention, and the present invention should not be construed as being limited to these examples, and the scope of the present invention is limited only by the appended claims.

[0089] 1: Substrate processing apparatus 2: Spin chuck 3: Rotary holder 4: Spin motor 5: Processing liquid supply unit 6: Controller 7: Thickness sensor 10: First nozzle 11: First processing liquid pipe 12: First etching liquid pipe 13: First rinse liquid pipe 14: First nozzle moving unit 15: First processing liquid valve 16: First etching liquid valve 18: First rinse liquid valve 20: Second nozzle 21: Second processing liquid pipe 22: Second etching liquid pipe 23: Second rinse liquid pipe 24: Second nozzle moving unit 25: Second processing liquid valve 26: Second etching liquid valve 28: Second rinse liquid valve 30: Third nozzle 31: Third processing liquid pipe 32: Third etching liquid pipe 33: Third rinse liquid pipe 34: Third nozzle moving unit 35: Third processing liquid valve 36: Third etching liquid valve 38: Third rinse liquid valve 45: Sensor holder 46: Sensor driving unit 51: First etching liquid supply unit 52: Second etching liquid supply unit 53: Third etching liquid supply unit 61: Processor 62: Memory 63: Auxiliary storage device 65: Display device 66: Input device 100: Silicon layer 101: Etching stop layer 102: Silicon active layer 103: Multilayer wiring layer 104: Embedded power rail 200: Silicon substrate 201: Insulating layer 300: Adhesion layer A1: Rotation axis M1: First scan motor M2: Second scan motor M3: Third scan motor M4: Fourth scan motor W: Substrate (bonded substrate) W1: First silicon wafer W2: Second silicon wafer

Claims

1. A substrate processing method comprising: a substrate rotation step of rotating a substrate having a main surface that has been ground or polished for substrate thinning, about a rotation axis perpendicular to the main surface; a first etching step of supplying a first etching solution containing hydrofluoric acid and nitric acid to the main surface while the substrate rotation step is being performed; and a second etching step of supplying a second etching solution containing TMAH (tetramethylammonium hydroxide) to the main surface after the first etching step while the substrate rotation step is being performed, wherein second etching parameters applied in the second etching step are adjusted so as to planarize a first surface profile generated on the main surface by the first etching step.

2. A substrate processing method as described in claim 1, wherein a first etching profile for the main surface by the first etching process is variable by variable setting of a first etching parameter applied in the first etching process, a second etching profile for the main surface by the second etching process is variable by variable setting of the second etching parameter applied in the second etching process, and the first etching parameter and the second etching parameter are adjusted so that a second surface profile generated on the main surface by sequentially performing the first etching process and the second etching process on the substrate has a flatness of a predetermined value or less.

3. The substrate processing method according to claim 2, wherein the first etching parameters and the second etching parameters are adjusted so that a composite etching profile obtained by superimposing the first etching profile and the second etching profile has a flatness of a predetermined value or less.

4. A substrate processing method as described in claim 2, wherein the first etching parameters and the second etching parameters are adjusted so that a composite surface profile obtained by superposing an initial surface profile of the main surface before the first etching step, the first etching profile and the second etching profile has a flatness of a predetermined value or less.

5. A substrate processing method as claimed in any one of claims 2 to 4, wherein the first etching step includes a first scanning step of moving a landing position of the first etching liquid on the main surface such that a distance between the landing position and the axis of rotation changes over time, and the first etching parameters include first scanning parameters that define the change in the landing position in the first scanning step.

6. A substrate processing method according to any one of claims 1 to 5, wherein the second etching step includes a second scanning step of moving a landing position of the second etching liquid on the main surface such that a distance between the landing position and the axis of rotation changes over time, and the second etching parameters include second scanning parameters that define the change in the landing position in the second scanning step.

7. The substrate processing method according to claim 1, wherein a second surface profile of the main surface after the second etching step has a flatness of 1.5 μm or less.

8. The substrate processing method according to any one of claims 1 to 7, wherein the main surface is a surface on which a silicon layer is exposed.

9. The substrate processing method according to claim 8, wherein the substrate has a silicon germanium layer and the silicon layer laminated on the silicon germanium layer.

10. The substrate processing method according to claim 9, further comprising a third etching step of supplying a third etching solution containing ammonium hydroxide to the main surface after the second etching step and while the substrate rotation step is being performed.

11. The substrate processing method according to claim 10, wherein the thickness of the silicon layer at the end of the second etching step is 4 μm or less.

12. The substrate processing method according to claim 10, wherein the silicon germanium layer has a thickness of 10 nm or less before the third etching step.

13. A substrate processing method according to any one of claims 10 to 12, wherein the concentration of ammonium hydroxide in the third etching solution and the temperature of the third etching solution are set so that the etching rate of the silicon layer in the third etching step is 200 nm / min or more and the etching selectivity ratio of silicon to silicon germanium is 150 or more.

Citation Information

Patent Citations

  • Substrate processing device

    JP2012199408A

  • Sputtering target material and manufacturing method of the same

    JP2023075947A

  • Etch stop layer system

    JP2003536273A

  • Stress-free etching process with dynamic liquid meniscus

    JP2007520079A

  • Substrate processing method and substrate processing device

    JP2018147908A

Cited By

  • Computer program, information processing method, substrate processing method, information processing device, and substrate processing device

    WO2025249219A1