Electrode assembly and method for manufacturing same
The zigzag electrode assembly addresses the issue of adhesive force differences by using distinct porous coating layers on a porous polymer substrate, ensuring balanced adhesion and preventing bending, thereby improving the safety and stability of electrochemical devices.
Patent Information
- Application Number
- PCT/KR2024/005394
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-02
- Filing Date
- 2024-04-22
- Publication Date
- 2024-11-07
AI Technical Summary
The existing zigzag electrode assembly manufacturing process faces issues with bending due to differences in adhesive forces between the separator and electrodes, leading to potential separation and reduced stiffness in electrochemical devices, which can cause safety concerns and decreased air permeability.
A zigzag electrode assembly is designed with a porous polymer substrate having different structured porous coating layers on each side, where the first porous coating layer has a higher adhesive force with the cathode and the second porous coating layer has a higher adhesive force with the anode, with specific binder and inorganic particle compositions to manage adhesion and prevent bending.
This design reduces the variation in electrode-separator adhesion, enhances the safety and stability of electrochemical devices by minimizing bending and maintaining high air permeability, while maintaining the productivity advantages of the zigzag stacking method.
Smart Images

Figure KR2024005394_07112024_PF_FP_ABST
Abstract
Description
Electrode assembly and method for manufacturing the same
[0001] This application claims priority based on Korean Patent Application No. 10-2023-0057043, filed with the Korean Intellectual Property Office on May 2, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to an electrode assembly including a zigzag-shaped separator and a method for manufacturing the same.
[0003] Electrochemical devices convert chemical energy into electrical energy using electrochemical reactions. Recently, lithium secondary batteries have become widely used due to their high energy density and voltage, long cycle life, and wide range of applications. With the increasing demand for electric vehicles and energy storage devices, development is underway on materials and structures to maximize capacity and energy density.
[0004] A secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, and may be manufactured by housing the electrode assembly in a case together with an electrolyte. Secondary batteries may be classified into pouch-type, cylindrical, square, coin-type, etc. depending on the shape of the case in which the electrode assembly is housed, and may be classified into jelly-roll type, stack type, etc. depending on the manufacturing method or shape of the electrode assembly.
[0005] Recently, a zigzag stacking electrode assembly has been developed, which folds a long sheet-shaped separator in a zigzag shape and alternately places positive and negative electrodes between adjacent folds. For example, a zigzag electrode assembly can be manufactured by tilting or swinging a table on which an elongated sheet-shaped separator is stacked when supplied, or by reciprocating a feed roll that transports the separator to fold the separator in a zigzag shape and place each electrode between the folds. Zigzag stacking has the advantage of being simpler than other types of processes, resulting in superior productivity.
[0006] The separator used in zigzag stacking can be formed by coating a coating slurry on both sides of a porous polymer substrate, and the electrode can be formed by coating an active material slurry on both sides of an electrode current collector. As the separator is bent in a zigzag pattern, multiple positive electrodes and negative electrodes are alternately arranged, and the positive and negative electrodes adhere to opposite sides of the separator. At this time, if there is a difference in the adhesive strength between the separator and the positive electrode and the adhesive strength between the separator and the negative electrode, that is, if the adhesive strength applied to both sides of the separator is different, bending of the electrode assembly may occur during the manufacturing process or the manufactured electrode assembly. For example, if the adhesive strength between the separator and the negative electrode is stronger than the adhesive strength between the separator and the positive electrode, bending of the separator may occur in the direction in which the negative electrode is adhered. Bending of the electrode assembly may cause detachment of the electrode and the separator, or may lead to low stiffness of the electrochemical device, which may cause safety issues. When the heat and pressure applied to the electrode assembly were increased to prevent bending of the electrode assembly, the separator located on the outside of the electrode assembly experienced problems such as reduced air permeability and increased electrical resistance due to excessive compression.
[0007] The present invention aims to provide a zigzag electrode assembly including a separator in which porous coating layers on both sides are formed with different structures in consideration of the types of adjacent electrodes, and a method for manufacturing the same.
[0008] One aspect of the present invention provides an electrode assembly comprising a porous polymer substrate, a first porous coating layer formed on one surface of the porous polymer substrate, and a second porous coating layer formed on the other surface of the porous polymer substrate, a separator bent in a zigzag shape, a cathode disposed between the first porous coating layers, and an anode disposed between the second porous coating layers, wherein the first porous coating layer has greater adhesive strength with the cathode than with the anode.
[0009] The second porous coating layer may have a greater adhesive strength with the anode than with the cathode.
[0010] The adhesive strength between the first porous coating layer and the cathode may be 0.8 to 1.2 times the adhesive strength between the second porous coating layer and the anode.
[0011] The first porous coating layer includes first binder particles and inorganic particles, and the average particle diameter of the first binder particles may be greater than or equal to the average particle diameter of the inorganic particles.
[0012] The first porous coating layer may include the first binder particles and the inorganic particles in a weight ratio of 20:80 to 80:20.
[0013] The second porous coating layer includes second binder particles and inorganic particles, and the average particle diameter of the inorganic particles may be larger than the average particle diameter of the second binder particles.
[0014] The positive electrode includes a positive electrode active material and a positive electrode binder resin, and the second binder particles and the positive electrode binder resin may be fluorinated polymers.
[0015] The thickness of the first porous coating layer may be greater than or equal to the thickness of the second porous coating layer.
[0016] The electrode assembly may have a long side length of 500 to 600 mm.
[0017] The thickness of the electrode assembly may be 8 to 20 mm.
[0018] Another aspect of the present invention provides an electrochemical device including the electrode assembly.
[0019] The above electrochemical device may be a lithium secondary battery.
[0020] The zigzag electrode assembly of the present invention maintains the advantage of excellent productivity, while providing a structure in which bending due to the difference in the adhesive strength of electrodes bonded to both sides of a separator is reduced, thereby improving the safety of an electrochemical device including the electrode assembly.
[0021] Figure 1 is a conceptual diagram showing a structure in which a separator and an electrode are bonded in an electrode assembly according to one specific example of the present invention.
[0022] Figure 2 is a conceptual diagram showing a process for evaluating the degree of bending of a secondary battery in an experimental example of the present invention.
[0023] Hereinafter, each component of the present invention will be described in more detail so that a person having ordinary skill in the art to which the present invention pertains can easily practice it; however, this is only an example, and the scope of the rights of the present invention is not limited by the following contents.
[0024] The term "comprises" as used herein is used to list materials, compositions, devices, and methods useful in the present invention, but is not limited to the listed examples.
[0025] As used herein, the terms "about" and "substantially" are used to mean a range or approximation of a numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly exploiting the disclosure, which includes precise or absolute numerical values provided to aid understanding of the present invention.
[0026] As used herein, “electrochemical device” may refer to a primary battery, a secondary battery, a super capacitor, etc.
[0027]
[0028] One specific example of the present invention provides an electrode assembly comprising a porous polymer substrate, a first porous coating layer formed on one surface of the porous polymer substrate, and a second porous coating layer formed on the other surface of the porous polymer substrate, a separator bent in a zigzag shape, a cathode disposed between the first porous coating layers, and a positive electrode disposed between the second porous coating layers. The first porous coating layer may have an adhesive strength with the negative electrode greater than an adhesive strength with the positive electrode.
[0029] The above separator has a structure in which a first porous coating layer and a second porous coating layer are laminated on both sides of a porous polymer substrate. The first porous coating layer and the second porous coating layer are arranged to face each other with the porous polymer substrate therebetween. Folding the separator in a zigzag shape may mean folding the separator at a predetermined interval. Preferably, the intervals may all be the same. While folding the separator, a plurality of positive electrodes and negative electrodes may be alternately arranged one by one. The negative electrode may be arranged between the first porous coating layers of the separator, and the positive electrode may be arranged between the second porous coating layers of the separator.
[0030] The porous polymer substrate may be a porous membrane having a plurality of pores formed therein, which electrically insulates the positive and negative electrodes to prevent short circuits. For example, when the electrochemical device is a lithium secondary battery, the porous polymer substrate may be an ion-conductive barrier that blocks electrical contact between the positive and negative electrodes while allowing lithium ions to pass through. At least a portion of the pores may form a three-dimensional network that connects the surface and the interior of the porous polymer substrate, and a fluid may pass through the porous polymer substrate through the pores.
[0031] The porous polymer substrate may use a material that is physically and chemically stable with respect to the organic solvent electrolyte. For example, the porous polymer substrate may include, but is not limited to, a resin such as a polyolefin-based resin such as polyethylene, polypropylene, and polybutylene, polyvinyl chloride, polyethylene terephthalate, polycycloolefin, polyethersulfone, polyamide, polyimide, polyimideamide, nylon, polytetrafluoroethylene, and copolymers or mixtures thereof. A polyolefin-based resin may be preferably used. A polyolefin-based resin can be processed into a relatively thin thickness and is easy to apply a coating slurry, making it suitable for the manufacture of an electrochemical device with a higher energy density.
[0032] The porous polymer substrate may have a single-layer or multi-layer structure. The porous polymer substrate may include two or more polymer resin layers having different melting points (Tm), thereby providing a shutdown function in the event of a high-temperature runaway of the battery. For example, the porous polymer substrate may include a polypropylene layer having a relatively high melting point and a polyethylene layer having a relatively low melting point. Preferably, the porous polymer substrate may have a three-layer structure in which polypropylene, polyethylene, and polypropylene are laminated in that order. The polyethylene layer melts when the temperature of the battery rises above a predetermined temperature, thereby shutting down the pores, thereby preventing thermal runaway of the battery.
[0033] The thickness of the porous polymer substrate may be 1 ㎛ or more and 100 ㎛ or less. Specifically, the thickness of the porous polymer substrate may be 10 ㎛ or more and 90 ㎛ or less, 20 ㎛ or more and 80 ㎛ or less, 30 ㎛ or more and 70 ㎛ or less, or 40 ㎛ or more and 60 ㎛ or less. Preferably, the thickness of the polymer substrate may be 1 ㎛ or more and 30 ㎛ or less. More preferably, the thickness of the polymer substrate may be 5 ㎛ or more and 15 ㎛ or less, or 7 ㎛ or more and 13 ㎛ or less. By controlling the thickness of the porous polymer substrate within the above-described range, the volume of the electrochemical device can be minimized while electrically insulating the positive and negative electrodes, thereby increasing the amount of active material included in the electrochemical device.
[0034] The above porous polymer substrate may include pores having an average diameter of 0.01 μm or more and 1 μm or less. Specifically, the size of the pores included in the porous polymer substrate may be 0.01 μm or more and 0.09 μm or less, 0.02 μm or more and 0.08 μm or less, 0.03 μm or more and 0.07 μm or less, or 0.04 μm or more and 0.06 μm or less. Preferably, the size of the pores may be 0.02 μm or more and 0.06 μm or less. By controlling the pore size of the porous polymer substrate within the above-described range, the air permeability and ionic conductivity of the entire manufactured membrane can be controlled.
[0035] The porous polymer substrate may have a permeability of 10 s / 100cc or more and 100 s / 100cc or less. Specifically, the permeability of the porous polymer substrate may be 10 s / 100cc or more and 90 s / 100cc or less, 20 s / 100cc or more and 80 s / 100cc or less, 30 s / 100cc or more and 70 s / 100cc or less, or 40 s / 100cc or more and 60 s / 100cc or less. Preferably, the permeability of the porous polymer substrate may be 50 s / 100cc or more and 70 s / 100cc or less. When the permeability of the porous polymer substrate is within the above-described range, the permeability of the manufactured separator may be provided within a range suitable for securing the output and cycle characteristics of the electrochemical device.
[0036] The above air permeability (s / 100cc) means the time (in seconds) it takes for 100cc of air to pass through a porous polymer substrate or membrane of a predetermined area under a constant pressure. The above air permeability can be measured using an air permeability tester (Gurley densometer) according to ASTM D 726-58, ASTM D726-94 or JIS-P8117. For example, using a 4110N device from Gurley, air at a pressure of 0.304 kPa or air at a pressure of 1.215 kN / m 2100 cc of air under the pressure of water occupies 1 square inch (or 6.54 cm 2 ) can be used to measure the time it takes for 100 cc of air to pass through a 1-square-inch sample under a constant pressure of 4.8 inches of water at room temperature. For example, using the Asahi Seico EG01-55-1MR equipment, the time it takes for 100 cc of air to pass through a 1-square-inch sample can be measured.
[0037] The porous polymer substrate may have a porosity of 10 vol% or more and 60 vol% or less. Specifically, the porosity of the porous polymer substrate may be 15 vol% or more and 55 vol% or less, 20 vol% or more and 50 vol% or less, 25 vol% or more and 45 vol% or less, or 30 vol% or more and 40 vol% or less. Preferably, the porosity of the porous polymer substrate may be 30 vol% or more and 50 vol% or less. When the porosity of the porous polymer substrate is in the above-described range, the ionic conductivity of the manufactured separator can be provided in a range suitable for securing the output and cycle characteristics of the electrochemical device.
[0038] The above porosity refers to the volume ratio of pores to the total volume of the porous polymer substrate. The porosity can be measured by methods known in the art. For example, it can be measured by the BET (Brunauer Emmett Teller) measurement method using nitrogen gas adsorption, the capillary flow porosimetry method, or the water or mercury intrusion method.
[0039] The porous coating layer may encompass a first porous coating layer and a second porous coating layer. The first porous coating layer and the second porous coating layer are each formed on one surface of the porous polymer substrate, and may include a polymer binder and inorganic particles. The polymer binder binds the inorganic particles, adheres the porous coating layer and the porous polymer substrate, and provides adhesive force to the separator to achieve adhesion with the electrode. The polymer binder may be a binder particle having a spherical or oval shape. The first porous coating layer may include first binder particles and inorganic particles, and the second porous coating layer may include second binder particles and inorganic particles. The first binder particles and the second binder particles included in the first porous coating layer and the second porous coating layer are different from each other, and the inorganic particles may be the same or different from each other.
[0040] Specifically, the first binder particles may include an acrylic polymer. The above acrylic polymer is (meth)acrylic acid, (meth)acrylate, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-amyl acrylate, isoamyl acrylate, n-ethylhexyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-amyl methacrylate, isoamyl methacrylate, n-hexyl methacrylate, n-ethylhexyl methacrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, (meth)acrylonitrile butyl (meth)acrylate, It may include, as a repeating unit, one or more monomers selected from the group consisting of 2-ethylhexyl (meth)acrylate, ethyl (meth)acrylate, methyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, n-oxyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate, tetradecyl (meth)acrylate, and pentafluorophenyl acrylate.
[0041] For example, the acrylic polymer may include at least one selected from the group consisting of polyacrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butylacrylate, isobutylacrylate, ethylhexylacrylate, methyl methacrylate, styrene-butadiene rubber, nitrile-butadiene rubber, acrylonitrile-butadiene rubber, and acrylonitrile-butadiene-styrene rubber.
[0042] The average particle diameter (D50) of the first binder particles may be greater than or equal to the average particle diameter of the inorganic particles described below. Here, the inorganic particles mean those included together with the first binder particles in the first porous coating layer. The inorganic particles of the first porous coating layer may have an average particle diameter (D50) of 300 nm to 500 nm, and the first binder particles may have an average particle diameter (D50) of 500 nm to 1000 nm. Specifically, the first binder particles may have an average particle diameter of 550 nm to 950 nm, 600 nm to 900 nm, 650 nm to 850 nm, or 700 nm to 800 nm. Preferably, the first binder particles may have an average particle diameter of 500 nm to 700 nm. The first binder particle, which is an acrylic polymer, may have a greater adhesive strength with the negative electrode than the adhesive strength of the second binder particle with the positive electrode. In the present specific example, by adjusting the average particle diameter of the first binder particle to be greater than the average particle diameter of the inorganic particles within the above-described range, the deviation in electrode-separator adhesive strength between each electrode on both sides of the separator can be reduced, thereby preventing bending of the electrode assembly.
[0043] Specifically, the second binder particles may be a fluorinated polymer. Preferably, the fluorinated polymer may be a polyvinylidene fluoride polymer. For example, the fluorinated polymer binder may be at least one selected from the group consisting of polyvinylidene fluoride, polyhexafluoropropylene, polytetrafluoroethylene, polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyvinylidene fluoride-trichloroethylene (PVDF-TCE), and polyvinylidene fluoride-chlorotrifluoroethylene (PVDF-CTFE), and more specifically, may be a copolymer including polyvinylidene fluoride.
[0044] The average particle diameter (D50) of the second binder particles may be smaller than the average particle diameter of the inorganic particles described below. Here, the inorganic particles mean that they are included together with the second binder particles in the second porous coating layer. The inorganic particles of the second porous coating layer may have an average particle diameter (D50) of more than 300 nm and 500 nm, and the second binder particles may have an average particle diameter (D50) of 100 nm or more and 300 nm or less. Preferably, the second binder particles may have an average particle diameter of 200 nm or more and 300 nm or less. The second binder particles, which are fluorinated polymers, may have an adhesive strength with the positive electrode that is smaller than the adhesive strength of the first binder particles with the negative electrode. In this specific example, by adjusting the average particle diameter of the second binder particles to be less than the average particle diameter of the inorganic particles within the above-described range, the surface area through which the second binder particles can come into contact with the electrode is increased, thereby improving the electrode-separator adhesion with the positive electrode. This reduces the deviation in the electrode-separator adhesion between each electrode on both sides of the separator, thereby preventing the formation of bending in the electrode assembly.
[0045] The above inorganic particles can be used as electrochemically stable particles. The above inorganic particles can be used in the operating voltage range of the electrochemical device (e.g., Li / Li + There is no particular limitation as long as no oxidation and / or reduction reaction occurs at 0 to 5 V as a standard. In particular, when using inorganic particles having a high dielectric constant as inorganic particles, it can contribute to increasing the degree of dissociation of electrolyte salt, such as lithium salt, in the liquid electrolyte, thereby improving the ionic conductivity of the electrolyte. For the reasons described above, it is preferable that the inorganic particles include high-dielectric constant inorganic particles having a dielectric constant of 5 or more, preferably 10 or more. Non-limiting examples of inorganic particles having a dielectric constant of 5 or more include BaTiO3, Pb(Zr,Ti)O3(PZT), b 1-x La x Zr 1-y Ti yO3(PLZT, 0 <x<1, 0<y<1), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3(PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, Al(OH)3, SiC, AlOOH, TiO2 or mixtures thereof.
[0046] In addition, inorganic particles having lithium ion transfer capability, i.e., inorganic particles containing lithium element but having the function of transferring lithium ions without storing lithium, can be used. Non-limiting examples of inorganic particles having lithium ion transfer capability include lithium phosphate (Li3PO4), lithium titanium phosphate (Li). x Ti y (PO4)3, 0 < x <2, 0 < y <3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), 14Li2O-9Al2O3-38TiO2-39P2O5, etc. (LiAlTiP) x O y Series glass (0 <x < 4, 0 < y < 13), 리튬란탄티타네이트(Li x La y TiO3, 0 < x <2, 0 <y <3), Li 3.25 Ge 0.25 P 0.75 Lithium germanium thiophosphate (Li) such as S4 x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitride (Li 3 N ), etc. x N y , 0 < x <4, 0 < y < 2), SiS2 series glass (Li) such as Li3PO4-Li2S-SiS2x Si y S z , 0 < x < 3, 0 <y < 2, 0 < z < 4), LiI-Li2S-P2S5등과 같은 P2S5계열 glass(Li x P y S z , 0 < x < 3, 0< y < 3, 0 < z < 7) or mixtures thereof.
[0047] In addition, as the inorganic particles, inorganic particles having flame retardancy can be used to impart flame retardant properties to the separator or to prevent a rapid increase in temperature inside the electrochemical device. Non-limiting examples of inorganic particles having flame retardancy include Sb2O3, Sb2O4, Sb2O5, SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, Zn2SnO4, ZnSnO3, ZnSn(OH)6, ZrO2, Y2O3, SiO2, Al2O3, AlOOH, Al(OH)3, SiC, TiO2, H3BO3, HBO2, and mixtures thereof.
[0048] The first porous coating layer and the second porous coating layer may include inorganic particles of the same or different types or average particle diameters. For example, the first porous coating layer and the second porous coating layer may include inorganic particles that are the same but have different average particle diameters. Preferably, the first porous coating layer and the second porous coating layer may include the same inorganic particles having an average particle diameter (D50) of 300 nm or more and 500 nm or less. By controlling the average particle diameter of the inorganic particles within the above-described range, the adhesive force between the first porous coating layer and the negative electrode and the adhesive force deviation between the second porous coating layer and the positive electrode can be reduced, thereby preventing bending of the electrode assembly.
[0049] The porous coating layer may contain a polymer binder and inorganic particles in a weight ratio of 20:80 to 80:20. Specifically, the porous coating layer may contain the binder particles and the inorganic particles in a weight ratio of 25:75 to 75:25, 30:70 to 70:30, 35:65 to 65:35, 40:60 to 60:40, or 45:55 to 55:45. By controlling the content of the polymer binder and the inorganic particles within the above-described range, thermal shrinkage of the porous polymer substrate is prevented, thereby preventing electrode short-circuiting due to shrinkage of the separator, and adhesion of the separator to the electrode can be secured. The content ratios of the binder particles and the inorganic particles in the first porous coating layer and the second porous coating layer may be the same as or different from each other. For example, the first porous coating layer may have a higher content of binder particles than the second porous coating layer.
[0050] The porous coating layer may be formed by coating one surface of the porous polymer substrate with a coating slurry containing the binder particles, the inorganic particles, and a dispersion medium. The separator may be manufactured by applying a first coating slurry for forming the first porous coating layer on one surface of the porous polymer substrate, and a second coating slurry for forming the second porous coating layer on the other surface, respectively, and drying to remove the dispersion medium. Preferably, the first coating slurry and the second coating slurry may be applied and dried simultaneously. The porous coating layer may have a porous structure including an interstitial volume in which the inorganic particles are connected by binder particles. The porous coating layer may allow lithium ions to pass therethrough and may be adhered to the porous polymer substrate to prevent thermal shrinkage of the porous polymer substrate.
[0051] The above coating slurry can disperse binder particles and inorganic particles by including a dispersion medium. The coating slurry can be used in which the inorganic particles are uniformly dispersed by adjusting the type or content of the dispersion medium. For example, it can be water.
[0052] The above coating slurry may further include additives such as a dispersant, a surfactant, an antifoaming agent, a flame retardant, and a wetting agent to improve dispersibility and flame retardancy and to improve the uniformity of the porous coating layer formed. For example, the dispersant may include at least one selected from the group consisting of a soluble polyamine, a soluble amine compound, fatty acids, fatty alcohols, sorbitan fatty acid esters, tannic acid, and pyrogallic acid. By using the above-described type of dispersant, the stability of the coating slurry can be improved and the uniformity of the porous coating layer formed with the coating slurry can be secured.
[0053] The additive may be included in an amount of 0 wt% or more and 5 wt% or less based on the total weight of the coating slurry. Specifically, the content of the additive may be included in an amount of 0.01 wt% or more and 4 wt% or less, 0.1 wt% or more and 3 wt% or less, or 1 wt% or more and 2 wt% or less. Preferably, the content of the additive may be 3 wt% or more and 5 wt% or less. By controlling the content of the additive within the above-described range, uniform dispersion and stability of the inorganic particles included in the coating slurry can be achieved.
[0054] The dispersion medium included in the coating slurry may be removed by drying or heating after the porous coating layer is formed. For example, the porous coating layer may contain the dispersion medium in an amount of 5 ppm or less. Preferably, the porous coating layer may be composed of binder particles and inorganic particles. In the process of removing the dispersion medium, a plurality of pores may be formed on the surface and inside of the porous coating layer. The pores may include interstitial volumes formed between inorganic particles, and may have a structure that allows fluid to pass through by forming a three-dimensional network.
[0055] The thickness of the porous coating layer may be 1 ㎛ or more and 15 ㎛ or less. Specifically, the thickness of the porous coating layer may be 2 ㎛ or more and 14 ㎛ or less, 3 ㎛ or more and 13 ㎛ or less, 4 ㎛ or more and 12 ㎛ or less, 5 ㎛ or more and 11 ㎛ or less, 6 ㎛ or more and 10 ㎛ or less, or 7 ㎛ or more and 9 ㎛ or less. By controlling the thickness of the porous coating layer within the above-described range, shrinkage of the porous polymer substrate can be minimized and stable adhesion to the porous polymer substrate can be implemented. Preferably, the thickness of the first porous coating layer may be thicker than the thickness of the second porous coating layer.
[0056] The separator for the electrochemical device may have a permeability of 50 s / 100cc or more and 300 s / 100cc or less. Specifically, the permeability of the separator may be 100 s / 100cc or more and 250 s / 100cc or less, or 150 s / 100cc or more and 200 s / 100cc or less. Preferably, the permeability of the separator may be 100 s / 100cc or more and 150 s / 100cc or less. When the permeability of the separator is within the above-described range, the output, stability, and cycle characteristics of the electrochemical device can be secured.
[0057] The positive electrode and the negative electrode may be coated by applying and drying an electrode active material on both sides of each current collector. The current collector may be a material that is conductive and does not cause a chemical change in the electrochemical device. For example, the current collector for the positive electrode may be, but is not limited to, aluminum, nickel, titanium, sintered carbon, stainless steel; aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.; etc. For example, the current collector for the negative electrode may be, but is not limited to, copper, nickel, titanium, sintered carbon, stainless steel; copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.; etc. The current collector may be in various forms, such as a metal plate, film, foil, net, porous body, foam, etc.
[0058] The positive electrode has a positive electrode current collector and a positive electrode active material layer including a positive electrode active material, a conductive material, and a positive electrode binder resin on both sides of the positive electrode current collector. The positive electrode active material is a layered compound such as lithium manganese oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; chemical formula LiNi 1-x M x Ni-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga and x = 0.01 to 0.3); chemical formula LiMn 1-x M xA lithium manganese composite oxide represented by O2 (wherein, M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (wherein, M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which a part of the Li in the chemical formula is replaced with an alkaline earth metal ion; a disulfide compound; and Fe2(MoO4)3 may include one or a mixture of two or more thereof. Preferably, the positive electrode active material may include one or more transition metals.
[0059] The positive electrode binder resin may be a binder resin commonly used in electrodes of electrochemical devices, but may include a fluorine-based polymer. Specifically, the positive electrode binder resin may be a polyvinyl fluoride-based polymer or a mixture containing the same. Preferably, the positive electrode binder resin may include the same polymer as the second binder particles included in the second porous coating layer. The second porous coating layer and the positive electrode active material layer may include polymers having the same or identical polymer backbones as the second binder particles and the positive electrode binder resin, respectively. The second porous coating layer may exhibit higher adhesive strength with the positive electrode than with the negative electrode.
[0060] The above negative electrode has a negative electrode current collector and a negative electrode active material layer including a negative electrode active material, a conductive material, and a negative electrode binder resin on both sides of the current collector. The negative electrode includes carbon such as lithium metal oxide, non-graphitizable carbon, and graphite carbon as the negative electrode active material; LixFe2O3(0≤x≤1), Li x WO2(0≤x≤1), Si, SiO x (0 <x<2), SiC, Si 합금 등의 실리콘계 재료; Sn x Me 1-x Me' y O z(Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of group 1, 2, and 3 of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8) 등의 금속 복합 산화물; 리튬 금속; 리튬 합금; 주석계 합금; SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, 및 Bi2O5등의 금속 산화물; 폴리아세틸렌 등의 도전성 고분자; Li-Co-Ni 계 재료; 티타늄 산화물 중 선택된 1종 또는 2종 이상의 혼합물을 포함할 수 있다.
[0061] The above-described negative electrode binder resin may be a binder resin commonly used in electrodes of electrochemical devices, but may include an acrylic polymer. Specifically, the negative electrode binder resin may be an acrylic polymer or a mixture containing the same. Preferably, the negative electrode binder resin may include the same polymer as the first binder particles included in the first porous coating layer. The first porous coating layer and the negative electrode active material layer may include polymers having the same or identical polymer backbones as the first binder particles and the negative electrode binder resin, respectively. The first porous coating layer may exhibit higher adhesive strength with the negative electrode than with the positive electrode.
[0062] The conductive material may be one or a mixture of two or more conductive materials selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powders, conductive whiskers, conductive metal oxides, carbon nanotubes, activated carbon, and polyphenylene derivatives. The carbon nanotubes have a graphite sheet in the shape of a cylinder with a nano-sized diameter, and sp 2It has a bonding structure, and exhibits the characteristics of a conductor or a semiconductor depending on the angle and structure at which the graphite plane is rolled. Carbon nanotubes can be classified into single-walled carbon nanotubes (SWCNTs), double-walled carbon nanotubes (DWCNTs), and multi-walled carbon nanotubes (MWCNTs) depending on the number of bonds forming the wall, and these carbon nanotubes can be appropriately selected depending on the use of the dispersion. More specifically, it can be one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more conductive materials among these.
[0063] The electrode assembly of the present specific example can reduce the difference in electrode-separator adhesion between the two sides of the separator by controlling the average particle size of the binder particles included in the porous coating layer in consideration of the type of electrode to be adhered to the porous coating layer in the separator and the adhesive strength thereof. Specifically, the first porous coating layer can have a higher adhesive strength with the cathode than with the anode, and the second porous coating layer can have a higher adhesive strength with the anode than with the cathode. The adhesive strength between the first porous coating layer and the cathode can be higher than the adhesive strength between the second porous coating layer and the anode. By controlling the average particle size of the first binder particles to be greater than the average particle size of the inorganic particles, the contact area between the binder particles and the electrode can be reduced, thereby controlling the adhesive strength between the first porous coating layer and the cathode to a level similar to the adhesive strength between the second porous coating layer and the anode. By adjusting the average particle diameter of the second binder particles to be smaller than the average particle diameter of the inorganic particles, the contact area between the binder particles and the electrode can be increased, thereby adjusting the adhesive strength between the second porous coating layer and the positive electrode to a level similar to the adhesive strength between the first porous coating layer and the negative electrode. This can reduce the difference in adhesive strength between the first porous coating layer and the negative electrode and the second porous coating layer and the positive electrode.
[0064] FIG. 1 is a conceptual diagram showing a structure in which a separator (100) is bonded to an adjacent negative electrode (200) and positive electrode (300) in an electrode assembly according to the above specific example. The separator (100) may include a first porous coating layer (120) formed on both sides of a porous polymer substrate (110) and a second porous coating layer (130) formed on the opposite side. The first porous coating layer (120) may include first binder particles (121) and inorganic particles (122), and the second porous coating layer (130) may include second binder particles (131) and inorganic particles (132). The inorganic particles (122, 132) included in each coating layer may be the same or different, but it will be understood that in the first porous coating layer (120), the first binder particles (121) are used with an average particle diameter larger than the inorganic particles (122), and in the second porous coating layer (130), the second binder particles (131) are used with an average particle diameter smaller than the inorganic particles (132). The adhesive force between one first binder particle (121) and the negative electrode (200) is greater than the adhesive force between one second binder particle (131) and the positive electrode (300), but the second binder particle (131), which is smaller in size than the inorganic particle (132), may have an area exposed to the bonding surface with the positive electrode (300) larger than the area of the first binder particle (121). Accordingly, the adhesive force between the first porous coating layer (120) and the cathode (200) and the adhesive force between the second porous coating layer (130) and the anode (300) can have a smaller deviation.
[0065] For example, the adhesive strength between the first porous coating layer and the cathode may be 0.8 to 1.2 times the adhesive strength between the second porous coating layer and the anode. Specifically, the adhesive strength between the first porous coating layer and the cathode may be 0.85 to 1.15 times, 0.9 to 1.1 times, or 0.95 to 1.05 times the adhesive strength between the second porous coating layer and the anode. Preferably, the two adhesive strengths may be the same. In an electrode assembly in which the electrode-separator adhesive strength on both sides is controlled as described above, bending may not occur or the level of bending may be reduced.
[0066] The electrode assembly as described above has a small deviation in electrode-separator adhesion on both sides based on a portion of the separator, so that even when the size of the electrode assembly increases or the thickness of the electrode assembly increases by stacking multiple electrodes, bending of the separator can be prevented or reduced.
[0067] For example, the electrode assembly may have a rectangular shape having long sides and short sides in a plan view. Specifically, the electrode assembly may have a long side length of 500 mm or more and 600 mm or less, and a short side length of 80 mm or more and 150 mm or less. When the long side length of the electrode assembly is in the above-described range, the tension applied to the separator may increase as the size of the electrode assembly increases, but in the electrode assembly according to the present specific example, bending does not occur or the bending level can be reduced, so that it is excellent in safety and can be stored and used in an electric vehicle.
[0068] For example, the electrode assembly may include a plurality of electrodes and have an overall thickness of 8 mm or more and 20 mm or less. When the thickness of the electrode assembly is within the above-described range, bending may occur as the accumulated deviation in the adhesive force applied to the separator increases. However, in the electrode assembly according to the present specific example, bending may not occur or the bending level may be reduced, so that it has excellent safety and can be stored and used in an electric vehicle.
[0069]
[0070] Another embodiment of the present invention provides an electrochemical device comprising an electrode assembly according to the aforementioned embodiment. The electrochemical device can be manufactured by inserting and sealing one or more electrode assemblies into a case or pouch. Before sealing the case or pouch, an electrolyte may be injected to impregnate the electrode assembly with the electrolyte. The shape of the case or pouch is not limited. For example, the electrochemical device may be a cylindrical, square, coin-shaped, or pouch-shaped lithium secondary battery.
[0071] The above electrolyte is A + B - As a salt with the same structure, A + is Li + , Na + , K + Contains ions composed of alkali metal cations or combinations thereof, such as B - is PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2)2 - , C(CF2SO2)3 -A salt comprising an anion such as or a combination thereof may be dissolved or dissociated in an organic solvent comprising propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma butyrolactone or a mixture thereof.
[0072] The electrochemical device including the electrode assembly may be a lithium secondary battery. The battery may be used as a unit cell, and may be used as a battery module including the unit cell, a battery pack including the battery module, or a device including the battery pack as a power source. The devices may include, but are not limited to, small devices such as computers, mobile phones, and power tools; electric vehicles including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs) that are powered by an electric motor; electric two-wheeled vehicles including electric bicycles (E-bikes) and electric scooters; electric golf carts; and power storage systems.
[0073]
[0074] Another specific example of the present invention provides a method for manufacturing the electrode assembly, comprising the steps of (S10) forming a laminate by folding a separator in a zigzag pattern and alternately arranging positive and negative electrodes therebetween, and (S20) applying heat and pressure to the laminate to manufacture the electrode assembly. In the description of the method for manufacturing the electrode assembly, the same content as the description of the electrode assembly described above is replaced with the description of the preceding specific example.
[0075] The above step (S10) is a step of forming a laminate by alternately arranging positive and negative electrodes between folds formed by zigzag folding a separator. The separator may have a length in the longitudinal direction (or MD direction; Machine Direction) longer than a length in the width direction (or TD direction; Transverse Direction). The separator may be folded in a zigzag manner at a predetermined interval along the MD direction. The arrangement of the positive and negative electrodes may be determined in consideration of the type of binder particles included in the porous coating layer of the separator, and the negative electrode may be arranged between the first porous coating layer having a higher adhesive strength with the negative electrode, and the positive electrode may be arranged between the second porous coating layer. The negative electrode may be used one more than the positive electrode, so that the two electrodes located at the outermost ends of the electrode assembly may both be negative electrodes.
[0076] The separator, the anode, and the cathode may each have a rectangular shape, but is not limited thereto. For example, the separator, the anode, and the cathode may each have a rectangular shape in which the MD direction is longer than the TD direction. The anode and the cathode may be arranged in multiples along the MD direction of the separator, and may be arranged such that the MD direction of the separator and the TD directions of the anode and the cathode are parallel to each other. Preferably, the anode and the cathode may be aligned such that their respective TD direction center lines are aligned.
[0077] The step (S20) above is a step of manufacturing an electrode assembly in which a positive electrode and a separator, and a negative electrode and a separator are bonded by thermocompression bonding the laminate formed in the step (S10). Through the thermocompression bonding, the first porous coating layer of the separator and the active material layer of the negative electrode may be bonded, and the second porous coating layer and the active material layer of the positive electrode may be bonded. The thermocompression bonding may be performed by compressing the top and bottom ends of the laminate using a press device, and may be performed by applying a pressure of 1 to 7 MPa at a temperature of 45 to 80° C. for 1 to 30 seconds to one or more laminates. By controlling the temperature and pressure conditions of the thermocompression bonding within the above-described range, uniform bonding of the separators and electrodes constituting the laminate can be achieved without causing damage to the laminate. The type of the press device is not limited as long as it can bond the separators and electrodes by simultaneously or simultaneously applying heat and pressure to one or both sides of the laminate while maintaining the alignment of the separators and electrodes included in the laminate.
[0078] Preferably, the thermocompression bonding can be divided into two or more steps. The step (S20) may include a first thermocompression bonding in which a pressure of 1 to 6 MPa is applied at 45 to 65°C for 1 to 30 seconds to fix the relative position of the electrode with respect to the separator, and a second thermocompression bonding in which a pressure of 1 to 7 MPa is applied at 50 to 80°C for 1 to 30 seconds to completely bond the separator and the electrodes. The first thermocompression bonding may partially bond the separator and adjacent electrodes to fix the position of the electrode. The second thermocompression bonding may completely bond the separator and the electrodes at the position determined through the first thermocompression bonding to manufacture an electrode assembly. Through the first thermocompression bonding and the second thermocompression bonding, an electrode assembly having excellent alignment compared to a single-step thermocompression bonding and having uniform electrode-separator bonding may be manufactured. By alleviating the thermal compression conditions compared to single-stage thermal compression through the above first thermal compression and the above second thermal compression, damage to the separator can be prevented, thereby achieving excellent production efficiency.
[0079]
[0080] Hereinafter, the present invention will be described in more detail through specific examples and experimental examples. The following examples and experimental examples are intended to illustrate the present invention, and the present invention is not limited by the following examples and experimental examples.
[0081] Example 1
[0082] A first coating slurry was prepared by mixing alumina with an average particle diameter (D50) of 500 nm and SBR (weight average molecular weight: 300,000) with an average particle diameter (D50) of 700 nm in a weight ratio of 80:20 at room temperature and dispersing them in water. A second coating slurry was prepared by mixing alumina with an average particle diameter (D50) of 500 nm and PVdF-HFP (weight average molecular weight: 400,000) with an average particle diameter (D50) of 300 nm in a weight ratio of 80:20 at room temperature and dispersing them in water.
[0083] A first coating slurry and a second coating slurry were simultaneously coated on each side of a polyethylene substrate having a thickness of 9 ㎛ using a slot die and dried to produce a separation membrane (thickness 15 ㎛) having a first porous coating layer (thickness 3 ㎛) and a second porous coating layer (thickness 3 ㎛) formed thereon.
[0084] By folding the separator in a zigzag pattern at intervals of 98.5 mm, 30 and 31 positive electrodes (positive electrode binder resin: PVdF-HFP) each measuring 90 mm × 315 mm and 125 μm thick and 30 and 31 negative electrodes (negative electrode binder resin: SBR) each measuring 95.5 mm × 320 mm and 150 μm thick were prepared, respectively. The separator was folded in a zigzag pattern at intervals of 98.5 mm, and the negative electrode was placed between the first porous coating layers, and the positive electrode was placed between the second porous coating layers, thereby preparing a laminate. The laminate was placed on a press device, and thermo-compression-bonded at 60°C and a pressure of 6 MPa for 1 second, and then thermo-compression-bonded at 70°C and a pressure of 6 MPa for 1 second, thereby manufacturing an electrode assembly (thickness: 9.3 mm) having a shape as shown in FIG. 2.
[0085] The electrode assembly was placed inside the case using a pouch outer material of a laminated sheet of CPP / aluminum / nylon as a case, an ethyl methyl carbonate (EMC) electrolyte containing LiPF6 was injected, and the pouch outer material was heat-sealed to complete the assembly of the secondary battery.
[0086] Afterwards, the secondary battery was subjected to a pre-activation heating press process and an activation process. The heating press process was performed at a temperature of 30°C and a pressure of 3.0 kgf / cm. 2 It was performed for 5 minutes under pressure conditions. The activation process was performed at a temperature of 50℃ and a pressure of 1.0 kgf / cm 2 The secondary battery was charged at 0.5 C under pressure conditions.
[0087] Example 2
[0088] An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that alumina having an average particle diameter (D50) of 300 nm and SBR (weight average molecular weight: 300,000) having an average particle diameter (D50) of 500 nm were used in a weight ratio of 80:20 in the first coating slurry.
[0089] Comparative Example 1
[0090] An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that alumina having an average particle diameter (D50) of 500 nm and SBR (weight average molecular weight: 300,000) having an average particle diameter (D50) of 300 nm were used in a weight ratio of 80:20 in the first coating slurry.
[0091] Comparative Example 2
[0092] An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that alumina having an average particle diameter (D50) of 500 nm and PVdF-HFP (weight average molecular weight: 400,000) having an average particle diameter (D50) of 700 nm were used in a weight ratio of 80:20 in the first coating slurry so that the first porous coating layer manufactured with the first coating slurry was adhered to the negative electrode.
[0093] Comparative Example 3
[0094] An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that alumina having an average particle diameter (D50) of 500 nm and SBR (weight average molecular weight: 300,000) having an average particle diameter (D50) of 300 nm were used in a weight ratio of 80:20 in the second coating slurry.
[0095] Example 3
[0096] An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that an electrode having a negative electrode with a long side of 525 mm and an anode with a long side of 520 mm was used.
[0097] Comparative Example 4
[0098] An electrode assembly and a secondary battery were manufactured in the same manner as in Comparative Example 2, except that an electrode having a long side of the cathode of 525 mm and a long side of the anode of 520 mm was used.
[0099] Comparative Example 5
[0100] An electrode assembly (thickness: 13.6 mm) and a secondary battery were manufactured in the same manner as in Comparative Example 2, except that 44 and 45 positive and negative electrodes were used, respectively.
[0101]
[0102] Experimental example
[0103] Air permeability measurement
[0104] The air permeability of the separator manufactured during the electrode assembly preparation process of the examples and comparative examples was confirmed.
[0105] The air permeability was measured using a Gurley densometer (Gurley, 4110N) when 100 cc of air was displaced through a 28.6 mm diameter, 645 mm area. 2 The time taken to penetrate the membrane was measured.
[0106] Confirming the adhesion of the electrode-separator
[0107] In the electrode assemblies manufactured in the examples and comparative examples, the electrode-separator adhesion was confirmed.
[0108] The adhesive strength when peeling the electrode from the separator while peeling the electrode layer by layer at an angle of 90° and a speed of 200 mm / min at the adhesive surface of the first porous coating layer of the cathode and the separator of each electrode assembly and the adhesive surface of the second porous coating layer of the anode and the separator was measured, and the results are summarized in Tables 1 and 2 below.
[0109] Checking the bending of secondary batteries
[0110] Referring to Fig. 2, a method for evaluating the bending level of a secondary battery is described. The secondary battery (10) including the electrode assembly of the examples and comparative examples that have completed the activation process may have a shape in which one side is concavely bent. As shown in Fig. 2, the secondary battery (10) was placed on a flat surface (G) with the concave side facing upward. A first ruler (A) was placed at both ends of the concave side, and a second ruler (B) was placed in a direction perpendicular to the first ruler (A), and the longest distance (d, mm) between the secondary battery (10) and the first ruler (A) was evaluated as the bending level, which is shown in the table below. The bending level of the secondary battery can be evaluated as good when it is less than 5 mm.
[0111] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 First porous coating layer Inorganic particles (D50) Alumina (500 nm) Alumina (300 nm) Alumina (500 nm) Alumina (500 nm) Alumina (500 nm) Binder particles (D50) SBR (700 nm) SBR (500 nm) SBR (300 nm) PVdF-HFP (700 nm) SBR (700 nm) Second porous coating layer Inorganic particles (D50) Alumina (500 nm) Alumina (500 nm) Alumina (500 nm) Alumina (500 nm) Binder particles (D50) PVdF-HFP (300 nm) PVdF-HFP (300 nm)PVdF-HFP(300 nm)PVdF-HFP(300 nm)SBR(300 nm)Separator air permeability(s / 100cc)1201251201201201201201 First porous coating layer-cathode adhesion(gf / 25mm)35351015352nd porous coating layer-anode adhesion(gf / 25mm)3535353510Bending level(mm)1.51.07.08.08.0
[0112]
[0113] Example 3 Comparative Example 4 Comparative Example 5 First porous coating layer Inorganic particles (D50) Alumina (500 nm) Alumina (500 nm) Alumina (500 nm) Binder particles (D50) SBR (700 nm) PVdF-HFP (700 nm) PVdF-HFP (700 nm) Second porous coating layer Inorganic particles (D50) Alumina (500 nm) Alumina (500 nm) Alumina (500 nm) Binder particles (D50) PVdF-HFP (300 nm) PVdF-HFP (300 nm) PVdF-HFP (300 nm) Total thickness of electrode assembly (mm) 9.5 9.5 13.6 Long side length of electrode assembly (mm) 5 26 5 26 3 21 First porous Coating layer - negative electrode adhesion (gf / 25mm) 351515 Second porous coating layer - positive electrode adhesion (gf / 25mm) 353535 Bending level 1.78.59.0
[0114]
[0115] [Explanation of symbols]
[0116] 100: Separator 110: Porous polymer substrate
[0117] 120: First porous coating layer 121: First binder particle
[0118] 122: Inorganic particles 130: Second porous coating layer
[0119] 131: Second binder particle 132: Inorganic particle
[0120] 200: Cathode 300: Anode
[0121] 10: Secondary batteries
[0122] A: First party B: Second party
Claims
1. A separator comprising a porous polymer substrate, a first porous coating layer formed on one surface of the porous polymer substrate, and a second porous coating layer formed on the other surface of the porous polymer substrate, and bent in a zigzag shape; a cathode disposed between the first porous coating layers; and An electrode assembly including an anode disposed between the second porous coating layers, An electrode assembly, wherein the first porous coating layer has greater adhesive strength with the cathode than with the anode.
2. In paragraph 1, An electrode assembly wherein the second porous coating layer has greater adhesive strength with the anode than with the cathode.
3. In paragraph 1, An electrode assembly, wherein the adhesive strength between the first porous coating layer and the cathode is 0.8 to 1.2 times the adhesive strength between the second porous coating layer and the anode.
4. In paragraph 1, The first porous coating layer comprises first binder particles and inorganic particles, An electrode assembly, wherein the average particle diameter of the first binder particles is greater than or equal to the average particle diameter of the inorganic particles.
5. In paragraph 4, An electrode assembly, wherein the first porous coating layer comprises the first binder particles and the inorganic particles in a weight ratio of 20:80 to 80:
20.
6. In paragraph 1, The second porous coating layer comprises second binder particles and inorganic particles, An electrode assembly, wherein the average particle diameter of the above-mentioned inorganic particles is larger than the average particle diameter of the above-mentioned second binder particles.
7. In paragraph 1, The above positive electrode includes a positive electrode active material and a positive electrode binder resin, An electrode assembly, wherein the second binder particles and the positive electrode binder resin are fluorinated polymers.
8. In paragraph 1, An electrode assembly, wherein the thickness of the first porous coating layer is greater than or equal to the thickness of the second porous coating layer.
9. In paragraph 1, The electrode assembly is an electrode assembly having a long side length of 500 to 600 mm.
10. In paragraph 1, An electrode assembly having a thickness of 8 to 20 mm.
Citation Information
Patent Citations
An electrode assembly and a method of manufacturing the same
KR1020240160356A
Secondary battery separator, secondary battery laminate and wound body including the same, and non-aqueous secondary battery
JP2019192340A
Electrode assembly
KR1020160059688A
Design device using module-type pattern
KR1020230029030A
Stack-type electrode assembly with no deflection of the electrode and manufacturing methods thereof
KR102328527B1
Cited By
Battery monomer, isolating membrane, battery and power utilization device
CN119890559A
Battery cells, separators, batteries, electrical devices
CN119890559B