Method for extracting lithium from brine by means of electrochemical adsorption, and use thereof
By combining electrochemical adsorption technology in brine and centripetal stirring, the problems of low lithium extraction efficiency and high energy consumption of lithium resources are solved, efficient and environmentally friendly lithium ion recovery is achieved, and the rapidly growing market demand is met.
Patent Information
- Application Number
- PCT/CN2023/093381
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-14
AI Technical Summary
The existing lithium resource extraction methods have problems such as long time to extract lithium, low efficiency, complex methods and high energy consumption. Especially in the recycling of lithium resources in China's salt lakes, it is difficult to meet the rapidly growing market demand.
The method of electrochemical adsorption and extraction of lithium in brine is adopted. The lithium ion adsorbent is added to the brine and the centripetal stirring technology is used to enrich lithium ions around the electrode. Combined with chemical adsorption, the lithium extraction efficiency is improved, and the cost is reduced by recycling the electrode materials. .
It significantly shortens the lithium extraction time, improves the lithium ion recovery efficiency, the lithium ion recovery rate is higher than 99%, and greatly reduces energy consumption and the use of chemical raw materials, which meets the requirements of energy conservation and environmental protection policies.
Smart Images

Figure CN2023093381_14112024_PF_FP_ABST
Abstract
Description
A method for extracting lithium from brine by electrochemical adsorption and its application Technical Field
[0001] The present disclosure belongs to the field of lithium resource extraction, for example, a method for extracting lithium from brine by electrochemical adsorption and its application. Background Art
[0002] With the rapid development of new energy vehicles, electronic devices, and energy storage technologies, lithium's application in new energy materials has garnered significant attention. It has been hailed as the "energy metal of the 21st century" and the "white oil." Global lithium resources are primarily found in salt lake brines and ores. Of the currently proven lithium resources, salt lake brines account for 58%, and lithium concentrates for 26%. According to the USGS, as of 2021, global proven lithium reserves amounted to approximately 89 million tons, primarily concentrated in Bolivia, Argentina, Chile, the United States, Australia, and China. China's proven lithium reserves (metal equivalent) are approximately 5.34 million tons, accounting for 6% of global reserves, primarily in Qinghai, Tibet, Hubei, and Sichuan. Salt lake resources account for approximately 82% of the country's total reserves, while ore resources contribute approximately 18%. With the rapid development of the new energy vehicle industry, demand for lithium resources is increasing. However, due to environmental, transportation, and technological constraints, domestic lithium ore and salt lake extraction in China struggle to meet market demand. At present, the extraction of lithium resources is still mainly based on primary lithium ore. How to accelerate the development and recovery of secondary lithium resources from lithium-containing solutions has become the key to the healthy, sustainable and rapid development of the lithium salt industry.
[0003] In order to adapt to and develop a process suitable for China's salt lakes, many domestic research institutions and salt lake companies have invested in the field of lithium extraction from salt lakes for many years, and have explored and developed a variety of routes such as precipitation, adsorption, membrane, extraction and electrochemical methods, making up for the shortcomings of China's natural salt lakes through technological innovation. Generally, the precipitation process is complex and costly, and is not suitable for treating raw liquids containing a large amount of Mg. 2+ and Ca 2+ Lithium-containing solutions of alkaline earth metals such as chlorinated metals. Solvent extraction and ion exchange adsorption have been popular research methods in recent years. However, issues such as severe dissolution loss, expensive ion membranes, and the need for regular cleaning in ion exchange adsorption still need improvement. Solvent extraction also faces urgent challenges, including the emulsification of FeCl3, recycling of extractants and hydrochloric acid, and equipment selection and maintenance.
[0004] CN1724372A discloses a method for producing lithium carbonate, magnesium oxide, and hydrochloric acid from high-magnesium, lithium-containing brine. The process involves spray drying, calcination, water washing, evaporation concentration, and precipitation to produce the lithium carbonate product. The method utilizes temperatures as high as 1200°C to calcine the lithium-magnesium brine, causing it to decompose into magnesium oxide and simultaneously recovering the lithium carbonate.
[0005] CN101654741A discloses a method for separating and recovering lithium and cobalt from lithium-ion batteries. Specifically, a method is disclosed in which a sample treated with lithium magnesium manganese oxide after acid washing is used as a lithium ion adsorbent for the lithium-containing filtrate after acid dissolution of waste lithium-ion batteries. The sample is combined with an immersed ultrafiltration membrane element to allow lithium ions to be embedded in the lattice gaps of the ion sieve to reach the maximum adsorption amount. Finally, the adsorbent is eluted with an acid solution to achieve the purpose of recovering lithium.
[0006] The above-disclosed lithium recovery processing method has a relatively complicated recovery process, and the equipment is easily corroded by acidic gases or liquids, which can easily cause environmental pollution and has high energy consumption.
[0007] Therefore, it is urgent to provide a clean and efficient lithium resource recovery process, minimize energy consumption in the lithium resource recovery process, and reduce the emission of related chemical raw materials or auxiliary materials, so that the recovery of lithium resources complies with current energy-saving and environmental protection policies.
[0008] Summary of the Invention
[0009] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0010] The present invention provides a method for extracting lithium from brine by electrochemical adsorption and its application, which solves the problems of long lithium extraction time, low efficiency, complex method and high energy consumption in related technologies.
[0011] To achieve this purpose, the present disclosure adopts the following technical solutions:
[0012] One of the purposes of the present disclosure is to provide a method for extracting lithium from brine by electrochemical adsorption, the method comprising:
[0013] An electrode containing a lithium-deficient lithium ion carrier is placed in the middle of the brine as a cathode electrode. A lithium ion adsorbent is added to the brine to enrich the lithium ions in the brine. The brine is stirred centripetally and the electrode is energized to obtain an electrode containing a lithium-rich lithium ion carrier.
[0014] The disclosed embodiment uses a lithium ion adsorbent to enrich lithium ions in a brine pool, cleverly utilizes external force to move the lithium ion adsorbent material, and transports the lithium ion adsorbent to the vicinity of the electrode to form a lithium-rich area, thereby greatly shortening the distance from the lithium ions to the electrode, thereby improving the lithium extraction efficiency and greatly saving the lithium extraction time.
[0015] In the embodiment of the present disclosure, centripetal stirring is achieved using a centripetal stirrer. Two stirrers are provided on the centripetal stirrer. The two stirrers are respectively provided on both sides of the cathode electrode. When the centripetal stirrer is turned on, the two stirrers stir in the direction of the electrode, thereby achieving the purpose of enriching the lithium ion adsorbent.
[0016] In the embodiment of the present disclosure, the lithium ion adsorbent added to the brine solution is a physical adsorbent, which can be adsorbed without power. The cathode electrode adopts chemical adsorption. When power is applied, chemical adsorption has a stronger adsorption capacity for lithium ions. Therefore, the lithium ion carrier in the lithium-deficient state after power is applied can better enrich the surrounding lithium ions.
[0017] As an optional technical solution of the embodiment of the present disclosure, the brine includes any one of salt lake brine, underground brine or concentrated seawater, or a combination of at least two of them, wherein typical but non-limiting examples of the combination include: a combination of salt lake brine and underground brine, a combination of underground brine and concentrated seawater, or a combination of salt lake brine and concentrated seawater, etc.
[0018] The concentrations of the elements in the brine solution in the embodiment of the present disclosure include: Li + The concentration range is 0.1-0.3g / L, Mg + The concentration range is 15.0-25.0g / L, K + The concentration range is 0.5-1.0g / L, SO4 2- The concentration range is 20.5-21.0g / L and Cl - The concentration range is 60.0-64.0g / L.
[0019] The Li + The concentration can be 0.1g / L, 0.12g / L, 0.14g / L, 0.16g / L, 0.18g / L, 0.2g / L, 0.22g / L, 0.24g / L, 0.26g / L, 0.28g / L or 0.3g / L, but is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0020] The Mg + The concentration can be 15.0g / L, 16.0g / L, 17.0g / L, 18.0g / L, 19.0g / L, 20.0g / L, 21.0g / L, 22.0g / L, 23.0g / L, 24.0g / L or 25.0g / L, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] The K + The concentration can be 0.5g / L, 0.6g / L, 0.7g / L, 0.8g / L, 0.9g / L or 1.0g / L, but is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0022] The SO4 2-The concentration can be 20.5g / L, 20.6g / L, 20.7g / L, 20.71g / L, 20.8g / L, 20.9g / L or 21.0g / L, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable.
[0023] The Cl - The concentration can be 60.0g / L, 60.5g / L, 61.0g / L, 61.5g / L, 62.0g / L, 62.1g / L, 62.18g / L, 62.2g / L, 62.3g / L, 62.4g / L, 62.5g / L, 62.6g / L, 62.7g / L, 62.8g / L, 62.9g / L or 63.0g / L, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] In one embodiment, the concentrations of the elements in the brine solution include: Li + The concentration of Mg is 0.2g / L, + The concentration of K is 23.0g / L + The concentration range is 0.91g / L, SO4 2+ The concentration range is 20.71 g / L and Cl - The concentration range is 62.18g / L.
[0025] In one embodiment, the lithium ion carrier includes any one of LiMn2O4, LiV3O8 or LiFePO4, or a combination of at least two of them, wherein typical but non-limiting examples of the combination include: a combination of LiMn2O4 and LiV3O8, a combination of LiV3O8 and LiFePO4, or a combination of LiMn2O4 and LiFePO4, etc.
[0026] As an optional technical solution of the embodiment of the present disclosure, the lithium ion adsorbent is a reversibly bound lithium ion adsorbent.
[0027] In one embodiment, the lithium ion adsorbent includes an Al 2 O 3 adsorbent and / or a SiO 2 adsorbent.
[0028] As an optional technical solution of the embodiment of the present disclosure, the enrichment time is 30 to 60 minutes, and the time can be 30 minutes, 35 minutes, 40 minutes, 45 minutes, 55 minutes or 60 minutes, etc., but is not limited to the listed values. Other unlisted values within the numerical range are also applicable.
[0029] In one embodiment, the centripetal stirring speed is 80 to 100 rpm, wherein the speed may be 80 rpm, 85 rpm, 90 rpm, 85 rpm or 100 rpm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0030] In one embodiment, the centripetal stirring time is 20 to 30 minutes, wherein the time can be 20 minutes, 21 minutes, 22 minutes, 23 minutes, 24 minutes, 25 minutes, 26 minutes, 27 minutes, 28 minutes, 29 minutes or 30 minutes, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] In the embodiment of the present disclosure, centripetal stirring gathers the lithium ion adsorbent in the brine toward the central area, and gathers around the electrode to form a lithium ion enrichment area.
[0032] As an optional technical solution in the embodiment of the present disclosure, the power-on voltage is 1 to 1.5V, wherein the voltage can be 1V, 1.1V, 1.2V, 1.3V, 1.4V or 1.5V, etc., but is not limited to the listed values. Other unlisted values within the numerical range are also applicable.
[0033] In one embodiment, the power-on time is 1.5 to 2.5 hours, where the time can be 1.5 hours, 1.6 hours, 1.7 hours, 1.8 hours, 1.9 hours, 2.0 hours, 2.1 hours, 2.2 hours, 2.3 hours, 2.4 hours or 2.5 hours, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] As an optional technical solution of the embodiment of the present disclosure, the power is turned off after the power is turned on, and the brine is stirred to disperse the lithium ions in the brine.
[0035] In the embodiment of the present disclosure, the power-on and power-off operations can be repeated, and the lithium ion carrier material and lithium ion adsorbent material on the electrode can be recycled, with a lifespan of more than 500 to 1,000 times, greatly reducing the recycling cost of lithium resources.
[0036] In the embodiment of the present disclosure, external force is applied to perform centrifugal stirring to disperse the lithium ion carriers.
[0037] As an optional technical solution of the embodiment of the present disclosure, the electrode containing the lithium-rich lithium ion carrier serves as the anode electrode.
[0038] In the embodiment of the present disclosure, a lithium-rich lithium ion carrier electrode is placed in a solution to be used for collecting lithium ions, so that the electrode is oxidized to release lithium ions, and the electrode is converted to a lithium-poor state before entering the next cycle.
[0039] As an optional technical solution of the embodiment of the present disclosure, the anode electrode is placed in a NaCl solution.
[0040] As an optional technical solution of the embodiment of the present disclosure, the method includes:
[0041] A lithium-deficient lithium ion carrier is placed in the middle of the brine as a cathode electrode, a lithium ion adsorbent is added to the brine, the brine is centripetally stirred at a speed of 80 to 100 rpm / min for 20 to 30 minutes, and the electrode is energized at a voltage of 1 to 1.5 V for 1.5 to 2.5 hours to obtain a lithium-rich lithium ion carrier.
[0042] The second object of the present disclosure is to provide an application of the method as described in the first object, which is applied to the field of lithium resource extraction.
[0043] The present disclosure has the following beneficial effects:
[0044] Related technologies use direct electrochemical lithium extraction methods. Usually, the lithium extraction process produces a lot of impurity cations, and the lithium extraction efficiency is low. In the present disclosure, two adsorbents are used to extract lithium together. The lithium ion adsorbent acts as a lithium ion carrier to transport lithium ions to the vicinity of the electrode while filtering out some cationic impurities, making the lithium ion concentration around the electrode higher. After further power is applied to extract lithium, the concentration of cationic impurities (such as magnesium ions) will be greatly reduced. At the same time, the method of electrochemical adsorption of lithium extraction in brine disclosed in the present disclosure has a high lithium extraction efficiency, greatly saving the time of lithium extraction, and the lithium ion recovery rate is higher than 99%.
[0045] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of the present disclosure, they are used to explain the technical solution of this article and do not constitute a limitation to the technical solution of this article.
[0047] FIG1 is a schematic diagram of the method for extracting lithium from brine in Examples 1-2 of the present disclosure. DETAILED DESCRIPTION
[0048] The technical solution of the present disclosure is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present disclosure and should not be regarded as specific limitations of the present disclosure.
[0049] Example 1
[0050] This embodiment provides a method for extracting lithium from brine as shown in FIG1 , the method comprising:
[0051] (1) 0.5 liters of brine solution (Mg) to be recovered is introduced into the cathode area of the electrolytic cell. 2+ The concentration is 20g / L, Li + The concentration is 0.2 g / L), and the same amount of NaCl solution is introduced into the anode area to electrolytically delithiate the electrode sheet containing the LiMn2O4 lithium ion carrier to a lithium-deficient state. The electrode sheet is then inserted into the middle position of the cathode area, and Al2O3 adsorbent is added to the brine to evenly distribute it in the brine pool to enrich the lithium ions in the brine pool for 30 minutes.
[0052] (2) A centrifugal stirring is performed at the bottom of the brine pool in the cathode area using a stirrer at a stirring speed of 80 rpm / min for 10 minutes, so that the lithium-enriched manganese oxide lithium ion sieve moves to the central area and gathers around the electrode to form a lithium ion enrichment area;
[0053] (3) The electrode is energized at a voltage of 1.2 V for 2 h. Under electrochemical action, the electrode adsorbs lithium ions in the enriched area and regenerates a lithium-poor manganese oxide lithium ion sieve;
[0054] (4) Then, the power is turned off and the stirrer is switched to centrifugal stirring mode to disperse the manganese oxide lithium ion sieve, and steps (1) and (2) are repeated;
[0055] (5) The lithium-rich electrode is replaced in the anode area, and the cathode area is still replaced with the lithium-poor electrode. Power is applied at a voltage of 1.2 V. The electrodes in the anode and cathode areas work simultaneously, so that the lithium-rich electrode is oxidized under the anode current, releasing lithium ions and converting to a lithium-poor state. The lithium-poor electrode absorbs lithium ions at the cathode, and this cycle is repeated 20 times.
[0056] (6) The collected lithium-containing solution after removing the precipitate was mixed with Na2CO3 powder and heated to 60°C to make Li + The lithium ion recovery rate was calculated based on the precipitation of Li2CO3 crystals. The magnesium ion concentration in the brine after multiple cycles was also tested according to HJ776-2015 "Determination of 32 Elements in Water Quality - Inductively Coupled Plasma Emission Spectrometry."
[0057] Example 2
[0058] This embodiment provides a method for extracting lithium from brine as shown in FIG1 , the method comprising:
[0059] (1) 0.5 liters of brine solution (Mg) to be recovered is introduced into the cathode area of the electrolytic cell. 2+ The concentration is 20g / L, Li +The concentration is 0.2 g / L), an electrode sheet containing a LiV3O8 lithium ion carrier is electrolytically delithiated to a lithium-deficient state, and then the electrode sheet is inserted into the middle of the cathode area containing brine in the electrolytic cell, and a SiO2 adsorbent is added to the brine to uniformly distribute it in the brine pool to enrich the lithium ions in the brine pool for 60 minutes;
[0060] (2) Centrifugal stirring was performed at the bottom of the brine pool in the cathode region using a stirrer at a stirring speed of 100 rpm / min for 8 minutes, so that the lithium-enriched vanadium oxide lithium ion sieve moved to the central region and gathered around the electrode, forming a lithium ion enrichment region;
[0061] (3) The electrodes are energized at a voltage of 1.2 V for 2 h. Under electrochemical action, the electrodes adsorb lithium ions in the enriched area and regenerate a lithium-poor vanadium oxide lithium ion sieve.
[0062] (4) Then, the power is turned off and the stirrer is switched to centrifugal stirring mode to disperse the vanadium oxide lithium ion sieve, and steps (1) and (2) are repeated;
[0063] (5) The lithium-rich electrode is replaced in the anode area, and the cathode area is still replaced with the lithium-poor electrode. Power is applied at a voltage of 1.2 V. The electrodes in the anode and cathode areas work simultaneously, so that the lithium-rich electrode is oxidized under the anode current, releasing lithium ions and converting to a lithium-poor state. The lithium-poor electrode absorbs lithium ions at the cathode, and this cycle is repeated 20 times.
[0064] (6) The collected lithium-containing solution after removing the precipitate was mixed with Na2CO3 powder and heated to 60°C to make Li + The recovery rate of lithium ions is calculated by the precipitation of Li2CO3 crystals. The concentration of magnesium ions in the brine after multiple cycles is tested according to HJ776-2015 "Determination of 32 elements in water quality - Inductively coupled plasma emission spectrometry" to calculate the magnesium ion concentration in the brine solution.
[0065] Example 3
[0066] In this embodiment, except that the time for the lithium ion adsorbent to enrich lithium ions in step (1) is replaced with 20 minutes, other conditions are the same as those in Example 1.
[0067] Example 4
[0068] In this embodiment, except that the time for enriching lithium ions with the lithium ion adsorbent in step (1) is replaced with 80 min, other conditions are the same as those in Example 1.
[0069] Comparative Example 1
[0070] Compared with Example 1, this comparative example does not add a reversibly bound lithium ion adsorbent and does not apply an external force.
[0071] (1) 0.5 liters of brine solution (Mg) to be recovered is introduced into the cathode area of the electrolytic cell. 2+ The concentration is 20g / L, Li + The concentration is 0.2 g / L), the electrode sheet containing the LiMn2O4 lithium ion carrier is electrolytically delithiated to a lithium-deficient state, and then the electrode sheet is inserted into the middle of the cathode area containing brine in the electrolytic cell;
[0072] (2) The electrodes are energized at a voltage of 1.2 V for 2 h, and the electrodes adsorb lithium ions under electrochemical action;
[0073] (3) The lithium-rich electrode is replaced in the anode area, and the cathode area is still replaced with a lithium-poor electrode. Power is applied at a voltage of 1.2 V. The electrodes in the anode and cathode areas work simultaneously, so that the lithium-rich electrode is oxidized under the anode current, releasing lithium ions and converting to a lithium-poor state. The lithium-poor electrode absorbs lithium ions at the cathode, and this cycle is repeated 20 times.
[0074] (4) The collected lithium-containing solution after removing the precipitate was mixed with Na2CO3 powder and heated to 60°C to make Li + The recovery rate of lithium ions was calculated based on the precipitation of Li2CO3 crystals.
[0075] Comparative Example 2
[0076] Compared with Example 1, this comparative example uses a lithium ion adsorbent to directly enrich lithium ions.
[0077] (1) 0.5 liters of brine solution (Mg) to be recovered is introduced into the cathode area of the electrolytic cell. 2+ The concentration is 20g / L, Li + The concentration is 0.2g / L), and Al2O3 adsorbent is added to the brine to make it evenly distributed in the brine pool, enriching the lithium ions in the brine pool;
[0078] (2) placing the lithium ion sieve enriched with lithium ions in (1) in a solution to be collected lithium ions, adding hydrogen peroxide as an oxidizing agent, causing the lithium ion sieve to undergo an oxidation reaction to release lithium ions, and repeating this cycle 20 times;
[0079] (3) The collected lithium-containing solution after removing the precipitate was mixed with Na2CO3 powder and heated to 60°C to make Li + The recovery rate of lithium ions was calculated based on the precipitation of Li2CO3 crystals.
[0080] The lithium ion recovery rates after 20 lithium extraction cycles in Examples 1-4 and Comparative Examples 1-2 are shown in Table 1.
[0081] Table 1
[0082] As shown in Table 1, by comparing Example 1 with Examples 3-4, it can be seen that when the adsorbent is added to the solution and the lithium ions in the brine pool are enriched before centripetal stirring, the lithium ion enrichment time is too short, and the lithium ion recovery rate decreases. If the enrichment time is too long, the lithium ion recovery rate will not be improved.
[0083] By comparing Example 1 with Comparative Examples 1-2, it can be seen that the lithium ion recovery rate of the lithium extraction method disclosed in the present invention is greatly improved after 20 lithium extraction cycles.
[0084] The embodiment has a certain positive effect on the removal of magnesium ion impurities in the lithium extraction process compared with the comparative example.
Claims
1. A method for extracting lithium from brine by electrochemical adsorption, the method comprising: An electrode containing a lithium-deficient lithium ion carrier is placed in the middle of the brine as a cathode electrode, a lithium ion adsorbent is added to the brine to enrich the lithium ions in the brine, the brine is stirred centripetally and the electrode is energized to obtain an electrode containing a lithium-rich lithium ion carrier.
2. The method according to claim 1, wherein: The brine includes any one of salt lake brine, underground brine or concentrated seawater, or a combination of at least two of them.
3. The method according to claim 1 or 2, wherein: The lithium ion carrier includes any one of LiMn2O4, LiV3O8 or LiFePO4 or a combination of at least two thereof.
4. The method according to any one of claims 1 to 3, wherein: The lithium ion adsorbent is a reversibly bound lithium ion adsorbent.
5. The method according to any one of claims 1 to 4, wherein: The lithium ion adsorbent includes an Al2O3 adsorbent and / or a SiO2 adsorbent.
6. The method according to any one of claims 1 to 5, wherein: The enrichment time is 30 to 60 minutes.
7. The method according to any one of claims 1 to 6, wherein: The speed of the centripetal stirring is 80-100 rpm.
8. The method according to any one of claims 1 to 7, wherein: The time of the centripetal stirring is 20 to 30 minutes.
9. The method according to any one of claims 1 to 8, wherein: The voltage of the power supply is 1 to 1.5V.
10. The method according to claim 9, wherein: The power-on time is 1.5 to 2.5 hours.
11. The method according to any one of claims 1 to 10, wherein: After the power is turned on, the power is turned off and the brine is stirred.
12. The method according to any one of claims 1 to 11, wherein: The electrode containing the lithium-rich lithium ion carrier is used as the anode electrode.
13. The method according to claim 12, wherein: The anode electrode is placed in a NaCl solution.
14. The method according to any one of claims 1 to 13, wherein: The method comprises: A lithium-deficient lithium ion carrier is placed in the middle of the brine as a cathode electrode, a lithium ion adsorbent is added to the brine, the brine is stirred centripetally at a speed of 80 to 100 rpm / min for 20 to 30 minutes, and the electrode is energized at a voltage of 1 to 1.5 V for 1.5 to 2.5 hours to obtain a lithium-rich lithium ion carrier.
15. An application of the method for extracting lithium by electrochemical adsorption in brine as described in any one of claims 1 to 14, wherein the method is applied in the field of lithium resource extraction.
Citation Information
Patent Citations
Method for recovering lithium resource from lithium-ion-containing solution by using lithium ion carrier
CN104577243A
Method for extracting lithium from salt lake brine through adsorbents
CN111826524A
Method for recovering lithium and electrode used therefor
JP2013011003A
Apparatus for forming solder layer on terminal of circuit board
KR102445477B1
Process for producing lithium concentrate from brine or seawater
US20040074774A1