Negative electrode sheet, preparation method therefor, battery cell, battery and electrical apparatus
By using laser etching technology to form a chemically bonded graphene active material layer on the graphite negative electrode material, the problems of increased capacity and structural stability of the graphite negative electrode material are solved, and the rate performance and energy density of the battery are significantly improved.
Patent Information
- Application Number
- PCT/CN2023/129229
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-06
- Filing Date
- 2023-11-02
- Publication Date
- 2024-11-14
AI Technical Summary
The current graphite negative electrode material is difficult to further increase its capacity, and interlayer stacking is prone to occur during the preparation process, poor structural stability, which limits the rate performance and energy density of the battery.
Laser etching technology is used to form a graphene active material layer on the surface of the negative electrode current collector. By mixing the organic carbon source and the organic doping source of doped elements, a chemically bonded doped elements and graphene active material layer are formed to increase the capacity of gram and electrochemical properties.
The structural stability and three-dimensional structure of the graphene active material layer are achieved, the intercalation and removal ability of lithium ions or sodium ions is improved, and the rate performance and energy density of the battery are significantly improved.
Smart Images

Figure CN2023129229_14112024_PF_FP_ABST
Abstract
Description
Negative electrode sheet and preparation method thereof, battery cell, battery and electrical device
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 202310499595.9 filed on May 6, 2023, entitled “Negative electrode sheet and preparation method thereof, battery cell, battery and electrical device,” the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to a negative electrode plate and a preparation method thereof, a battery cell, a battery and an electrical device. Background Art
[0004] Battery cells are widely used due to their reliable performance, pollution-free operation, and zero memory effect. For example, with increasing attention paid to environmental protection and the growing popularity of new energy vehicles, the demand for power battery cells is expected to experience explosive growth.
[0005] As battery applications become increasingly widespread, the requirements for battery performance are becoming increasingly stringent. As an important component of battery cells, the specific capacity of negative electrode active materials still needs to be further improved.
[0006] Summary of the Invention
[0007] The present application provides a negative electrode plate and a preparation method thereof, a battery cell, a battery and an electrical device, which can increase the gram capacity of the negative electrode plate.
[0008] In a first aspect, the present application proposes a method for preparing a negative electrode sheet, comprising:
[0009] providing an organic carbon source solution;
[0010] adding an organic doping source containing a doping element into an organic carbon source solution to form a precursor solution;
[0011] providing a precursor solution onto the surface of the negative electrode current collector and heat-treating the precursor solution to form a precursor film layer;
[0012] A laser source is used to etch the precursor film layer to obtain a graphene active material layer containing doping elements, wherein the doping elements are connected to the carbon elements in the graphene active material layer in a chemically bonded form.
[0013] Therefore, the negative electrode plate obtained by the method according to the embodiment of the present application includes a graphene active material layer. The structure of the graphene active material layer is relatively stable and presents a three-dimensional structure, which is conducive to the embedding or extraction of active ions such as lithium ions and sodium ions, and can improve the rate performance of the battery cell; and because doping elements are introduced into the graphene active material layer, the gram capacity of the negative electrode plate can be improved, and the organic doping source can be laser-etched by the laser source, so that the doping elements in the organic doping source and the carbon elements in the graphene active material layer are chemically bonded, which can further improve the gram capacity of the negative electrode plate.
[0014] In some embodiments, the doping element includes at least one of a first element, a second element, and a third element.
[0015] The first element includes one or more of sulfur, phosphorus, silicon, selenium and tin.
[0016] The second element includes one or more of iron, cobalt, nickel, aluminum and copper.
[0017] The third element includes one or more of boron, germanium, titanium and magnesium.
[0018] Therefore, the first element in the embodiment of the present application has electrochemical activity, and elements with electrochemical activity can increase the energy density of the battery cell. The second element may include an element with conductivity, which can reduce the internal resistance of the electrode and improve the rate performance of the battery cell. The third element may occupy the position of carbon atoms in the graphene, forming electron transfer or electron holes, giving the graphene special semiconductor properties; and the doping element may also create lattice defects, broaden the transmission channels of active ions, improve the wettability of the graphene active material layer, etc., thereby further improving the performance of the negative electrode.
[0019] In some embodiments, the doping element includes sulfur, and the organic doping source includes one or more of thiourea, methionine, thioglycolic acid, 2-mercaptoethanol, thiobenzoic acid, diphenyl sulfoxide, cysteine, and benzenesulfonic acid.
[0020] In some embodiments, the doping element includes phosphorus, and the organic dopant source includes one or more of phosphorous acid, hydrocarbyl phosphinous acid, hydrocarbyl phosphinous acid, phosphite ester, ethyl hypophosphite, and hydrocarbyl phosphite ester.
[0021] In some embodiments, the doping element includes silicon, and the organic doping source includes one or more of trimethylsilanol, triethylsilanol, diphenylmethylsilane, hexamethyldisiloxane, trimethylphenylsilane, and tetraethyl orthosilicate.
[0022] In some embodiments, the doping element includes tin, and the organic doping source includes one or more of monobutyltin, dibutyltin, tributyltin, tributyltin oxide, triphenyltin, and dioctyltin.
[0023] In some embodiments, the doping element includes nickel, and the organic doping source includes one or more of nickel oxalate, nickel oleate, nickel propionate, nickel butyrate, nickel octoate, and nickel lactate.
[0024] In some embodiments, the doping element includes copper, and the organic doping source includes one or more of copper acetate, fatty acid copper, and copper naphthenate.
[0025] In some embodiments, the doping element includes boron, and the organic doping source includes one or more of phenylboric acid, diphenylboric acid, triphenylboron, and trimethoxyboroxane.
[0026] In some embodiments, the doping element includes selenium, and the organic doping source includes one or more of dimethyl selenium and diethyl diselenide.
[0027] In some embodiments, the doping element includes germanium, and the organic doping source includes one or more of tetraethylgermanium, methylgermanium thiol, butylgermanium thiol, and octylgermanium thiol.
[0028] In some embodiments, the doping element includes iron, and the organic doping source includes one or more of ferrous lactate, ferric citrate, and ferric glycinate.
[0029] In some embodiments, the doping element includes cobalt, and the organic doping source includes one or more of cobalt oxalate and cobalt acetate.
[0030] In some embodiments, the doping element includes titanium, and the organic doping source includes one or more of orthotitanate and butyl titanate.
[0031] In some embodiments, the doping element includes aluminum, and the organic doping source includes one or more of triethylaluminum, triisobutylaluminum, and diethylaluminum chloride.
[0032] In some embodiments, the doping element includes magnesium, and the organic doping source includes one or more of magnesium glycinate, magnesium citrate, and magnesium lactate.
[0033] In some embodiments, the mass percentage of the organic dopant source is 0.2 wt % to 20 wt % based on the total mass of the precursor solution. When the mass percentage of the organic dopant source is within the above range, the gram capacity and electrochemical performance of the negative electrode can be further improved.
[0034] In some embodiments, the thickness of the precursor solution is 40 μm to 150 μm. Precursor solutions meeting the above thickness range can increase the occupied space of the active material layer, thereby improving the energy density of the battery cell.
[0035] In some embodiments, the step of heat-treating the precursor solution to form the precursor film layer includes:
[0036] first heat-treating the precursor solution to remove at least a portion of the solvent in the precursor solution and retain the solute in the precursor solution;
[0037] The second heat treatment is performed on the solute in the precursor solution and provides an external force to the solute to form a precursor film layer.
[0038] In some embodiments, the thickness of the precursor film layer is 30 μm to 120 μm. Precursor solutions meeting the above thickness range can increase the occupied space of the active material layer, thereby improving the energy density of the battery cell.
[0039] In some embodiments, the step of providing an organic carbon source solution comprises: dissolving the organic carbon source in a solvent to obtain an organic carbon source solution, wherein the organic carbon source comprises one or more of polyamic acid, polyvinyl pyrrolidone, isobutyl vinyl ether, polyvinyl acetate, cellulose ester compounds, polyenol compounds, polyolefin compounds and polysaccharide compounds.
[0040] In some embodiments, the cellulose ester compound includes one or more of cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate.
[0041] In some embodiments, the polyenol compound includes polyvinyl alcohol and / or polypropylene alcohol.
[0042] In some embodiments, the polyolefin compound includes polypropylene and / or polystyrene.
[0043] In some embodiments, the polysaccharide compound includes one or more of cellulose, chitosan, and chitin.
[0044] In some embodiments, the current collector comprises a metal substrate.
[0045] In some embodiments, the current collector includes an organic polymer layer and a metal layer disposed on at least one surface of the organic polymer layer, wherein the precursor solution is provided to the surface of the metal layer.
[0046] In some embodiments, the laser source includes one or more of a carbon dioxide laser source, a diode laser source, an argon ion laser source, a nitrogen laser source, a red laser source, a blue laser source, and a femtosecond laser source.
[0047] In some embodiments, the laser source comprises a carbon dioxide laser source.
[0048] In some embodiments, the output power of the CO2 laser source is 10 W to 30 W. When the output power of the CO2 laser source is within the above range, at this output power, the doping element in the organic doping source can be chemically bonded to the carbon element in the graphene active material layer.
[0049] In some embodiments, the carbon dioxide laser source satisfies at least one of the following conditions:
[0050] (1) The laser wavelength of the carbon dioxide laser source is 2 μm to 50 μm;
[0051] (2) The pulse width of the CO2 laser source is 10 μs to 30 μs;
[0052] (3) The number of pulses per inch of the carbon dioxide laser source is 800 to 1200;
[0053] (4) The beam radius of the CO2 laser source is 50 μm to 150 μm;
[0054] (5) The scanning speed of the carbon dioxide laser source is 2 cm / s to 5 cm / s;
[0055] (6) Along the thickness direction of the negative electrode current collector, the distance between the carbon dioxide laser source and the precursor film layer is 2 mm to 4 mm;
[0056] (7) The laser intensity range of the precursor film layer facing the carbon dioxide laser source is 10J / cm 2 Up to 30J / cm 2 .
[0057] Therefore, when at least one of the above conditions is met, the embodiments of the present application can further improve the performance of the prepared graphene active material layer, for example, the uniformity of the performance of the entire graphene active material layer can be improved.
[0058] Secondly, the present application proposes a negative electrode plate, which includes a negative electrode current collector and a graphene active material layer. The graphene active material layer is located on at least one surface of the negative electrode current collector. The graphene active material layer is formed by laser etching. The graphene active material layer includes doping elements and carbon elements connected in a chemically bonded form.
[0059] In some embodiments, the mass percentage of the doping element is 0.1 wt % to 10 wt % based on the total mass of the graphene active material layer. When the mass percentage of the doping element is within the above range, the specific capacity and electrochemical performance of the negative electrode can be further improved.
[0060] In some embodiments, the thickness of the graphene active material layer is 30 μm to 120 μm. A graphene active material layer having a thickness within the above range can improve the energy density of a battery cell.
[0061] In some embodiments, the negative electrode sheet uses lithium metal as the counter electrode, and in the charge and discharge curve tested in the range of 0.005V to 2.5V, the charging capacity at 0.005V to 2.5V is 400mAh / g to 480mAh / g; optionally 433mAh / g to 466mAh / g.
[0062] In some embodiments, the graphene active material layer has a porous structure, which is beneficial to the migration of active ions.
[0063] In some embodiments, the pore size of the porous structure is 1 nm to 80 nm. The pores of the porous structure may be nanopores, which can improve the structural strength of the graphene sheet and facilitate the transport of active ions.
[0064] In some embodiments, the graphene active material layer has a porosity of 5% to 30%. When the graphene active material layer has a porosity within the above range, it can increase the tap density of the negative electrode sheet and improve the energy density of the battery cell.
[0065] In some embodiments, the specific surface area of the graphene active material layer is 30 m 2 / g to 500m 2 When the specific surface area of the graphene active material layer is within the above range, the bonding property of the graphene active material layer can be improved, and the tap density of the negative electrode sheet can be increased, thereby increasing the energy density of the battery cell.
[0066] In a third aspect, the present application proposes a battery cell comprising a negative electrode plate as described in any embodiment of the second aspect of the present application.
[0067] In a fourth aspect, the present application proposes a battery comprising the battery cell as described in the third aspect of the present application.
[0068] In a fifth aspect, the present application proposes an electrical device comprising the battery as described in the fourth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.
[0070] FIG1 is a schematic diagram of a process for preparing a negative electrode sheet according to an embodiment of the present application.
[0071] FIG2 is a schematic diagram of a battery cell according to an embodiment of the present application.
[0072] FIG3 is an exploded schematic diagram of the battery cell shown in FIG2 .
[0073] FIG4 is a schematic diagram of a battery module according to an embodiment of the present application.
[0074] FIG5 is a schematic diagram of a battery pack according to an embodiment of the present application.
[0075] FIG6 is an exploded schematic diagram of the battery pack shown in FIG5 .
[0076] FIG7 is a schematic diagram of an electric device including a battery cell according to an embodiment of the present application as a power source.
[0077] FIG8 is an X-ray diffraction (XRD) diagram of the graphene active material layer formed by laser etching in Example 1 of the present application.
[0078] FIG9 is a Raman spectrum diagram of the graphene active material layer formed by laser etching in Example 1 of the present application.
[0079] FIG10 is a transmission electron microscope (TEM) image of the graphene active material layer formed by laser etching in Example 1 of the present application.
[0080] FIG11 is a scanning electron microscope (SEM) image of the graphene active material layer formed by laser etching in Example 1 of the present application.
[0081] FIG12 is an EDX elemental analysis diagram of the graphene active material layer formed by laser etching in Example 1 of the present application.
[0082] FIG13 is a schematic diagram of the charge and discharge curve (100 cycles at 0.1C) of the lithium-ion battery of Example 1 of the present application. DETAILED DESCRIPTION
[0083] Below, with appropriate reference to the accompanying drawings, the embodiments of the negative electrode sheet and its preparation method, battery cell, battery and electrical device of the present application are described in detail. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0084] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0085] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0086] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0087] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0088] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0089] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0090] A battery cell includes a positive electrode sheet, a negative electrode sheet, and a separator. The separator is located between the positive electrode sheet and the negative electrode sheet to isolate the positive electrode sheet from the negative electrode sheet. Active ions migrate between the positive electrode sheet and the negative electrode sheet through the electrolyte, thereby realizing the charging and discharging of the battery cell.
[0091] The negative electrode sheet consists of a negative current collector and a negative active material layer containing the negative electrode active material. The negative electrode active material is typically a graphite-based material. Based on the lithium storage mechanism of LiC6 between graphite layers, its theoretical specific capacity is approximately 372 mAh / g. Furthermore, lithium diffusion between graphite layers also limits its rate performance. With technological advancements, the realized capacity of graphite negative electrodes has gradually approached the theoretical value, leaving limited room for improvement. Consequently, with the increasing demand for battery energy and power performance in the new energy sector, pure graphite-based negative electrode materials are becoming insufficient. Graphene, due to its excellent optical, electrical, and mechanical properties, holds significant application potential in the new energy sector. However, when preparing graphene as the negative electrode active material, its specific capacity is difficult to further increase, and the resulting graphene is prone to interlayer stacking and other issues, resulting in poor structural stability.
[0092] In view of the above problems, an embodiment of the present application proposes a method for preparing a negative electrode plate, wherein an organic carbon source solution and an organic doping source are arranged on the surface of a negative electrode current collector, and the organic carbon source solution and the organic doping source are etched by a laser source to obtain a graphene active material layer bonded to the negative electrode current collector. The structure of the graphene active material layer is relatively stable and presents a three-dimensional structure. The structure is relatively stable, which is conducive to the embedding or extraction of active ions such as lithium ions and sodium ions, and can improve the rate performance of the battery cell; and because the organic doping source is subjected to laser etching by the laser source, the doping elements in the organic doping source and the carbon elements in the graphene active material layer can be chemically bonded, and the doping elements can further improve the gram capacity of the negative electrode plate.
[0093] Preparation method of negative electrode sheet
[0094] In a first aspect, an embodiment of the present application provides a method for preparing a negative electrode sheet, the method comprising:
[0095] Step S100, providing an organic carbon source solution;
[0096] Step S200, adding an organic dopant source containing a doping element into an organic carbon source solution to form a precursor solution;
[0097] Step S300, providing a precursor solution onto the surface of the negative electrode current collector, and heat-treating the precursor solution to form a precursor film layer;
[0098] In step S400 , a laser source is used to etch the precursor film layer to obtain a graphene active material layer containing a doping element, wherein the doping element is chemically bonded to the carbon element in the graphene active material layer.
[0099] The negative electrode plate obtained by the method according to the embodiment of the present application includes a graphene active material layer. The structure of the graphene active material layer is relatively stable and presents a three-dimensional structure, which is conducive to the embedding or extraction of active ions such as lithium ions and sodium ions, and can improve the rate performance of the battery cell; and because doping elements are introduced into the graphene active material layer, the gram capacity of the negative electrode plate can be improved, and the organic doping source can be laser-etched by a laser source so that the doping elements in the organic doping source and the carbon elements in the graphene active material layer are chemically bonded, which can further improve the gram capacity of the negative electrode plate.
[0100] In the embodiments of the present application, chemical bonding refers to the connection between two elements in the form of a chemical bond. The doping element is a non-carbon element, and the introduction of the doping element can further increase the specific capacity of the negative electrode.
[0101] In step S100, the organic carbon source solution includes an organic carbon source and a solvent, and the organic carbon source is dissolved in the solvent to obtain an organic carbon source solution. The organic carbon source is the solute of the organic carbon source solution, and the solvent is a solvent that can dissolve the organic carbon source. In the embodiment of the present application, dissolution means that the solute and the solvent can be mixed to form a uniform phase. When the solute can be dissolved in the solvent, the solubility of the solute in the solvent is generally greater than or equal to 10g; that is, the solubility of the organic carbon source in the solvent is greater than or equal to 10g. Since the solvent dissolves the organic carbon source, the distribution of the organic carbon source in the solvent is more uniform, which is conducive to subsequent uniform film formation. Since the organic carbon source solution only contains the organic carbon source as a solute, it is more conducive to uniform dissolution in the solvent, which is conducive to the formation of a lightweight and thin graphene layer structure. Of course, the organic carbon source solution in the embodiment of the present application may also include other substances that are conducive to film formation.
[0102] Illustratively, the organic carbon source is added to the solvent and stirred for 20 to 60 minutes to obtain an organic carbon source solution.
[0103] In some embodiments, the organic carbon source is an organic compound, which may include an organic high molecular compound (such as a polymer) or an organic low molecular compound (such as a small molecule compound). The organic compound is more conducive to forming a graphene active material layer with uniform performance and thickness on the negative electrode current collector.
[0104] In some embodiments, the organic carbon source includes one or more of polyamic acid, polyvinyl pyrrolidone, isobutyl vinyl ether, polyvinyl acetate, cellulose ester compounds, polyenol compounds, polyolefin compounds, and polysaccharide compounds. Films made from these organic carbon sources are dense, uniform, and have high mechanical strength.
[0105] As some examples, the cellulose ester compound includes one or more of cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate.
[0106] As some examples, the polyenol compound includes polyvinyl alcohol and / or polypropylene alcohol.
[0107] As some examples, the polyolefin-based compound includes polypropylene and / or polystyrene.
[0108] As some examples, the polysaccharide compound includes one or more of cellulose, chitosan, and chitin.
[0109] In the embodiments of the present application, there is no specific limitation on the type of solvent, as long as the solvent can dissolve the corresponding organic compound. In some embodiments, the solvent may include one or more of water, alcohol solvents, ketone solvents, N-methylpyrrolidone, N,N-dimethylformamide, dichloromethane, chloroform, methyl acetate, and acetic acid.
[0110] Illustratively, the organic carbon source solution may include a polyamic acid solution, wherein the solute is polyamic acid and the solvent is N-methylpyrrolidone.
[0111] Illustratively, the organic carbon source solution may include a polypropylene solution, wherein the solute is polypropylene and the solvent is acetone.
[0112] Illustratively, the organic carbon source solution may include a polyvinyl alcohol solution, wherein the solute is polyvinyl alcohol and the solvent is water.
[0113] Illustratively, the organic carbon source solution may include a polypropylene alcohol solution, wherein the solute is polypropylene alcohol and the solvent is ethanol.
[0114] Illustratively, the organic carbon source solution may include a polyvinyl pyrrolidone solution, wherein the solute is polyvinyl pyrrolidone and the solvent is water.
[0115] Illustratively, the organic carbon source solution may include a polystyrene solution, wherein the solute is polystyrene and the solvent is a mixture of N,N-dimethylformamide and chloroform.
[0116] Illustratively, the organic carbon source solution may include an isobutyl vinyl ether solution, wherein the solute is isobutyl vinyl ether and the solvent is diethyl ether.
[0117] Illustratively, the organic carbon source solution may include a cellulose acetate solution, the solute of which is cellulose acetate, and the solvent of which includes at least one of dichloromethane and methyl acetate.
[0118] Illustratively, the organic carbon source solution may include a cellulose acetate butyrate solution, the solute of which is cellulose acetate butyrate, and the solvent of which includes at least one of dichloromethane and methyl acetate.
[0119] Illustratively, the organic carbon source solution may include a cellulose acetate propionate solution, the solute of which is cellulose acetate propionate, and the solvent of which includes at least one of dichloromethane and methyl acetate.
[0120] Illustratively, the organic carbon source solution may include a polyvinyl acetate solution, wherein the solute is polyvinyl acetate and the solvent is ethanol.
[0121] Illustratively, the organic carbon source solution may include a cellulose acetate solution, wherein the solute is cellulose and the solvent is acetic acid.
[0122] Illustratively, the organic carbon source solution may include a chitosan acetate solution, wherein the solute is chitosan and the solvent is acetic acid.
[0123] Illustratively, the organic carbon source solution may include a chitin acetate solution, wherein the solute is chitin and the solvent is acetic acid.
[0124] In step S200 , an organic dopant source is added to an organic carbon source solution and mixed to form a precursor solution.
[0125] By adding an organic dopant source, doping elements can be introduced into the precursor solution, thereby improving the electrochemical properties of the graphene active material layer. The precursor solution can be considered to be a mixture of an organic dopant source and an organic carbon source solution. For example, the organic dopant source can be dissolved or dispersed in the organic carbon source solution, and no chemical reaction between the organic dopant source and the organic carbon source solution is required.
[0126] In some embodiments, the doping element includes at least one of a first element, a second element, and a third element.
[0127] The first element may include an electrochemically active element, which can increase the energy density of the battery cell. For example, the first element may include one or more of sulfur, phosphorus, silicon, selenium, and tin. The material formed after etching the organic dopant source containing the first element may also be electrochemically active.
[0128] The second element can include a conductive element, which can reduce the internal resistance of the electrode and improve the rate performance of the battery cell. For example, the second element can include one or more of iron, cobalt, nickel, aluminum, and copper. The material formed after etching the organic dopant source containing the second element can also be conductive.
[0129] The third element can include one or more of boron, germanium, titanium, and magnesium. These doping elements may occupy carbon atoms in graphene, creating electron transfer or electron holes, giving graphene unique semiconductor properties. The doping elements may also create lattice defects, broaden the transport channels for active ions, and improve the wettability of the graphene active material layer, thereby further enhancing the performance of the negative electrode.
[0130] In some embodiments, the organic dopant source containing sulfur may include one or more of thiourea, methionine, thioglycolic acid, 2-mercaptoethanol, thiobenzoic acid, diphenyl sulfoxide, cysteine, and benzenesulfonic acid.
[0131] In some embodiments, the organic dopant source containing phosphorus may include one or more of phosphorous acid, hydrocarbyl phosphinous acid, hydrocarbyl phosphinous acid, phosphite ester, ethyl hypophosphite, and hydrocarbyl phosphite ester.
[0132] In some embodiments, the organic dopant source containing silicon element may include one or more of trimethylsilanol, triethylsilanol, diphenylmethylsilane, hexamethyldisiloxane, trimethylphenylsilane, and tetraethyl orthosilicate.
[0133] In some embodiments, the organic dopant source containing tin element may include one or more of monobutyltin, dibutyltin, tributyltin, tributyltin oxide, triphenyltin, and dioctyltin.
[0134] In some embodiments, the organic dopant source containing nickel may include one or more of nickel oxalate, nickel oleate, nickel propionate, nickel butyrate, nickel octoate, and nickel lactate.
[0135] In some embodiments, the organic dopant source containing copper element may include one or more of copper acetate, fatty acid copper, and copper naphthenate.
[0136] In some embodiments, the organic dopant source containing the boron element may include one or more of phenylboric acid, diphenylboric acid, triphenylboron, and trimethoxyboroxane.
[0137] In some embodiments, the organic dopant source containing selenium may include one or more of dimethyl selenide and diethyl diselenide.
[0138] In some embodiments, the organic dopant source containing germanium element may include one or more of tetraethylgermanium, methylgermanium thiol, butylgermanium thiol, and octylgermanium thiol.
[0139] In some embodiments, the organic dopant source containing iron may include one or more of ferrous lactate, ferric citrate, and ferric glycinate.
[0140] In some embodiments, the organic dopant source containing cobalt element may include one or more of cobalt oxalate and cobalt acetate.
[0141] In some embodiments, the organic dopant source containing titanium element may include one or more of orthotitanate and butyl titanate.
[0142] In some embodiments, the organic dopant source containing aluminum element may include one or more of triethylaluminum, triisobutylaluminum, and diethylaluminum chloride.
[0143] In some embodiments, the organic dopant source containing magnesium may include one or more of magnesium glycinate, magnesium citrate, and magnesium lactate.
[0144] In some embodiments, the mass percentage of the organic dopant source is 0.2 wt % to 20 wt % based on the total mass of the precursor solution. When the mass percentage of the organic dopant source is within the above range, the gram capacity and electrochemical performance of the negative electrode can be further improved.
[0145] Exemplarily, the mass percentage of the organic dopant source can be 0.2wt%, 0.3wt%, 0.5wt%, 0.8wt%, 1 wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt% or a range consisting of any two of the above values.
[0146] In some embodiments, the mass percentage of the doping element is 0.1 wt % to 10 wt % based on the total mass of the graphene active material layer. When the mass percentage of the doping element is within the above range, the specific capacity and electrochemical performance of the negative electrode can be further improved.
[0147] Exemplarily, the mass percentage of the doping element can be 0.1wt%, 0.2wt%, 0.3wt%, 0.5wt%, 0.8wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt% or a range consisting of any two of the above values.
[0148] In step S300, a precursor solution is provided to the surface of the negative electrode current collector. The precursor solution can be disposed on the surface of the negative electrode current collector by coating or the like. After removing at least part of the solvent in the precursor solution and heat-treating the precursor solution, the precursor solution is prepared into a precursor film layer.
[0149] As shown in FIG1 , the precursor solution may be coated on the surface of the negative electrode current collector by using a doctor blade. Specifically, the specific steps of using a doctor blade coating include:
[0150] Step S310, coating the precursor solution on the surface of the negative electrode current collector;
[0151] Step S320 , adjusting the distance between the scraper and the surface of the negative electrode current collector to adjust the thickness of the precursor solution.
[0152] The precursor solution is applied to the surface of the negative electrode current collector. Due to the fluidity of the precursor solution, the thickness of the precursor solution applied to the surface of the negative electrode current collector tends to be uniform. To further improve the uniformity of the thickness, a portion of the precursor solution can be removed. For example, a scraper is used to remove a portion of the precursor solution. During the removal process, the distance between the scraper and the surface of the negative electrode current collector remains substantially constant along the thickness direction of the negative electrode current collector. The scraper is moved along a first direction to remove a portion of the precursor solution. In an embodiment of the present application, the first direction is perpendicular to the thickness direction of the negative electrode current collector and can be the length direction or the width direction of the negative electrode current collector.
[0153] In some embodiments, the thickness of the precursor solution is 40 μm to 150 μm. Precursor solutions meeting this thickness range can increase the space occupied by the active material layer, thereby increasing the energy density of the battery cell. In this embodiment of the present application, the thickness of the precursor solution is the thickness adjusted by a scraper.
[0154] Illustratively, the thickness of the precursor solution may be 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm, 110 μm, 120 μm, 150 μm, or a range consisting of any two of the above values.
[0155] In some embodiments, the step of heat-treating the precursor solution to form the precursor film layer includes:
[0156] Step S330: first heat-treating the precursor solution to remove at least a portion of the solvent in the precursor solution and retain the solute in the precursor solution;
[0157] In step S340 , the solute in the precursor solution is subjected to a second heat treatment and an external force is applied to the solute to form a precursor film layer.
[0158] The precursor solution undergoes a multi-step heat treatment, for example, including a first heat treatment and a second heat treatment; specifically, the precursor solution undergoes a first heat treatment at a first temperature, which can remove at least part of the solvent in the precursor solution and retain the solute in the precursor solution (the solute includes an organic carbon source and an organic doping source), so that the solute of the precursor solution can initially form a film; in other words, the temperature range of the first temperature should be greater than or equal to the boiling point of the solvent. Exemplarily, the first temperature can be 50°C to 100°C. For example, the precursor solution is placed in a vacuum oven and vacuum-dried at 50°C to 100°C for 2 hours.
[0159] After the precursor solution is subjected to the first heat treatment, the remaining main component is the solute, and the solute is subjected to the second heat treatment at a second temperature, and an external force is provided on the solute of the precursor solution. It can be understood that the solute of the precursor solution is subjected to hot pressing to form a precursor film layer. The temperature range of the second temperature should be greater than or equal to the melting point of the solute of the precursor solution. Exemplarily, the second temperature can be 150°C to 350°C. For example, the solute of the precursor solution is hot pressed into a film at 200°C under a pressure of 0.5MPa to 5.0MPa.
[0160] The embodiment of the present application performs heat treatment on the precursor solution, etc., so that the solvent in the precursor solution gradually evaporates, and the solute in the precursor solution is evenly distributed on the surface of the negative electrode current collector, which is conducive to forming a precursor film layer with uniform thickness on the surface of the negative electrode current collector. The thermal expansion coefficient of the precursor film layer is relatively low, and it is not easy to have pinhole morphology.
[0161] In some embodiments, the thickness of the precursor film layer is 30 μm to 120 μm. When the thickness of the precursor film layer is within the above range, more space can be provided for the active material layer, thereby improving the energy density of the battery cell.
[0162] Exemplarily, the thickness of the precursor film layer can be 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, 75μm, 80μm, 85μm, 90μm, 95μm, 100μm, 110μm, 120μm or a range consisting of any two of the above values.
[0163] The precursor solution according to the embodiment of the present application can be coated on one side or on both sides.
[0164] In some embodiments, a single-sided coating method is used, that is, the precursor solution is provided to one surface of the negative electrode current collector. In other embodiments, a double-sided coating method is used, and the negative electrode current collector includes two surfaces facing each other along its own thickness direction. The precursor solution is provided to one of the two surfaces of the negative electrode current collector, and the precursor solution is heat-treated to form a precursor film layer. The precursor solution is then provided to the other surface of the negative electrode current collector and heat-treated to form a precursor film layer.
[0165] In the embodiment of the present application, the thickness of the precursor film layer refers to the thickness of the precursor film layer on one surface of the negative electrode current collector.
[0166] The method according to the embodiment of the present application is applicable to preparing a positive electrode current collector or a negative electrode current collector.
[0167] In some embodiments, the negative electrode current collector may include a metal substrate, such as a metal foil, or a composite current collector. Copper foil may be used as an example of a metal foil. The composite current collector may include an organic polymer layer and a metal layer disposed on at least one surface of the organic polymer layer. The metal layer may be disposed on one surface of the organic polymer layer, or on both surfaces.
[0168] As an example, the main material of the metal layer may include at least one of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the organic polymer layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE). It should be noted that when a composite current collector is used as the negative electrode current collector, the precursor solution may be disposed on the surface of the metal layer.
[0169] In step S400, a laser source is used to etch the precursor film layer to obtain a graphene active material layer.
[0170] The precursor film undergoes morphological changes under the etching of the high-energy laser spot. The organic carbon source in the precursor film forms a graphene skeleton structure. Because the graphene skeleton structure is derived from the organic carbon source (organic material), its thickness is relatively uniform, which makes the graphene active material layer more uniform and consistent. The graphene active material layer presents a three-dimensional structure with relatively large spacing between graphene sheets, and relatively large space and specific surface area, which is conducive to the transmission of active ions and improves the rate performance of the battery cell.
[0171] Graphene also has excellent conductivity, which can effectively reduce the internal resistance of battery cells, reduce ohmic polarization, and improve the rate performance of battery cells.
[0172] Specifically, graphene is formed by the disordered loose aggregation of carbon atoms with a single-atom thickness. This structure is conducive to the insertion of active ions such as lithium ions, thus making graphene have a high specific capacity; graphene materials have a special structure with a two-dimensional high specific surface area and excellent electron transmission ability, which can reduce the resistance to the movement of lithium ions and thus significantly optimize the reversibility of the battery cell cycle, thus making graphene have a good ion transmission channel; the graphene skeleton structure has high thermal conductivity and structural stability, which can timely evacuate the energy accumulation generated by the battery cell due to long-term operation, thereby alleviating the problem of rising internal temperature of the battery, which is conducive to maintaining the long-term cycle performance of the battery; the interlayer spacing of the graphene material is large, and the sheet scale is much smaller than that of bulk graphite. Such a structure shortens the diffusion distance of lithium ions between graphene sheets, which is more conducive to the rapid insertion and deinsertion of lithium ions, thereby significantly improving the rate performance of lithium-ion batteries.
[0173] The organic doping source and the organic carbon source in the precursor film layer are laser etched at the same time. Under high-energy etching, the doping elements in the organic doping source can be connected to the carbon atoms in a chemically bonded manner, thereby further improving the electrochemical performance of the negative electrode. This preparation method can prevent the graphene sheets from stacking up, thereby improving the first coulombic efficiency, etc.
[0174] In some embodiments, the laser source may include one or more of a carbon dioxide laser source, a diode laser source, an argon ion laser source, a nitrogen laser source, a red laser source, a blue laser source, and a femtosecond laser source. Optionally, the laser source includes a carbon dioxide laser source. The laser source is scanned along a preset path until the entire precursor film layer is scanned. For example, the laser source may be scanned linearly along the length of the negative electrode current collector until the entire precursor film layer is scanned. Of course, the laser source may also be scanned linearly along the width of the negative electrode current collector, etc.
[0175] In some embodiments, the output power of the CO2 laser source is 10 W to 30 W. When the output power of the CO2 laser source is within the above range, at this output power, the doping element in the organic doping source can be chemically bonded to the carbon element in the graphene active material layer.
[0176] Illustratively, the output power of the CO2 laser source may be 10 W, 12 W, 13 W, 14 W, 15 W, 16 W, 18 W, 20 W, 22 W, 23 W, 25 W, 26 W, 28 W, 30 W, or a range consisting of any two of the above values.
[0177] When at least one of the following conditions is met, the embodiments of the present application can further improve the performance of the prepared graphene active material layer, for example, the uniformity of the performance of the entire graphene active material layer can be improved.
[0178] In some embodiments, the wavelength of the carbon dioxide laser source is 2 μm to 50 μm.
[0179] In some embodiments, the pulse width of the carbon dioxide laser source is 10 μs to 30 μs.
[0180] In some embodiments, the CO2 laser source has a pulse count of 800 to 1200 pulses per inch.
[0181] In some embodiments, the beam radius of the CO2 laser source is 50 μm to 150 μm.
[0182] In some embodiments, the scanning speed of the carbon dioxide laser source is 2 cm / s to 5 cm / s.
[0183] In some embodiments, along the thickness direction of the negative electrode current collector, the distance between the carbon dioxide laser source and the precursor film layer is 2 mm to 4 mm.
[0184] In some embodiments, the laser intensity of the precursor film layer facing the carbon dioxide laser source is in the range of 10 J / cm 2 Up to 30J / cm 2 When the laser intensity of the carbon dioxide laser source is within the above range, at this output power, the doping elements in the organic doping source can be linked to the carbon elements in the graphene active material layer in the form of chemical bonding. For example, the laser intensity of the surface of the precursor film layer facing the carbon dioxide laser source is in the range of 10J / cm 2 , 12J / cm 2 , 14J / cm 2 , 15J / cm 2 , 16J / cm 2 , 18J / cm 2 , 20J / cm 2 , 21J / cm 2 , 22J / cm 2 , 23J / cm 2 , 25J / cm 2 , 26J / cm 2 , 27J / cm 2 , 28J / cm 2 , 29J / cm 2 、30J / cm 2 Or a range consisting of any two of the above values.
[0185] The graphene active material layer of the embodiment of the present application does not need to add other conductive agents, thickeners, binders, etc. during the preparation process, which can significantly reduce the internal resistance of the negative electrode plate. In addition, the thickness of the graphene active material layer is easier to adjust and the preparation process is relatively simplified.
[0186] Negative electrode
[0187] In a second aspect, embodiments of the present application further provide a negative electrode sheet. The negative electrode sheet includes a negative electrode current collector and a graphene active material layer. The graphene active material layer is located on at least one surface of the negative electrode current collector. The graphene active material layer is formed by laser etching. The graphene active material layer includes a doping element and a carbon element connected in a chemically bonded form. Of course, the negative electrode sheet can also be prepared by any embodiment of the first aspect of the present application. As an example, the negative electrode current collector has two surfaces that are opposite to each other in its own thickness direction, and the graphene active material layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0188] In some embodiments, the thickness of the graphene active material layer may be 30 μm to 120 μm. When the thickness of the graphene active material layer is within the above range, the energy density of the battery cell can be improved. Exemplarily, the thickness of the graphene active material layer may be 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm, 110 μm, 120 μm or a range consisting of any two of the above values. In an embodiment of the present application, the thickness of the graphene active material layer refers to the thickness of the graphene active material layer on one surface of the negative electrode current collector.
[0189] In some embodiments, the negative electrode sheet uses lithium metal as the counter electrode, and in the charge and discharge curve tested in the range of 0.005V to 2.5V, the charging capacity at 0.005V to 2.5V is 400mAh / g to 480mAh / g; optionally 433mAh / g to 466mAh / g.
[0190] The graphene active material layer can effectively increase its gram capacity by introducing doping elements.
[0191] For example, the gram capacity of the negative electrode sheet can be 400mAh / g, 405mAh / g, 410mAh / g, 418mAh / g, 420mAh / g, 422mAh / g, 425mAh / g, 428mAh / g, 430mAh / g, 432mAh / g, 435mAh / g, 438mAh / g, 439mAh / g, 440mAh / g, 441mAh / g, 442mAh / g, 443mAh / g, 444mAh / g, 445mAh / g, 446mAh / g, 447mAh / g, 448mAh / g, 449mAh / g, 450mAh / g, 451mAh / g, 452mAh / g, 453mAh / g, 454mAh / g, 455mAh / g, 456mAh / g, 457mAh / g, 458mAh / g, 459mAh / g, 460mAh / g, 461mAh / g, 462mAh / g, 463mAh / g, 464mAh / g, 465mAh / g, 466mAh / g, 467mAh / g, 468mAh / g, 469mAh / g, 470mAh / g, 471mAh / g, 472mAh / g, 473mAh / g, 474mAh / g, 475mAh / g, 476mAh / g, 477mAh / g, 478mAh / g, 479mAh / g, 480mAh / g, 481mAh / g, 482mAh / g, 483mAh / g, 484mAh / g, 485 9mAh / g, 450mAh / g, 451mAh / g, mAh / g, 452mAh / g, 453mAh / g, 454mAh / g, 455mAh / g, 456mAh / g, 457mAh / g, 458mAh / g, 459mAh / g, 460mAh / g, 461mAh / g, 462mAh / g, 463mAh / g, 464mAh / g, 465mAh / g, 466mAh / g, 470mAh / g, 472mAh / g, 475mAh / g, 480mAh / g, or a range consisting of any two of the above values.
[0192] In some embodiments, the graphene active material layer is present as a multilayer graphene sheet, each graphene sheet having a porous structure. In the embodiments of the present application, the porous structure includes pores; a pore refers to a recessed structure that is recessed relative to the outer surface of the graphene sheet and recessed into the interior of the graphene active material layer, or is manifested as a through hole that penetrates the graphene sheet. A graphene sheet may have multiple pores, and the multiple pores may be arranged in parallel and / or cross-arranged. The composition of the porous structure includes pore size, pore length, and pore size distribution. The pore size can be micropores, mesopores, or macropores. Micropores refer to pores with a diameter of less than about 2 nanometers. Mesopores refer to pores with a diameter of about 2 nanometers to about 50 nanometers. Macropores refer to pores with a diameter greater than 50 nanometers.
[0193] In an embodiment of the present application, the pores of the porous structure may be nanopores, which, on the one hand, are beneficial to improving the structural strength of the graphene sheet, and on the other hand, are beneficial to the transmission of active ions. Optionally, the pore size of the porous structure is 1 nm to 80 nm. Exemplarily, the pore size of the porous structure may be 1 nm, 2 nm, 5 nm, 8 nm, 10 nm, 12 nm, 15 nm, 18 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 70 nm, 80 nm, or a range consisting of any two of the above values.
[0194] In some embodiments, the graphene active material layer has a porosity of 5% to 30%. When the graphene active material layer has a porosity within this range, it can increase the tap density of the negative electrode sheet and improve the energy density of the battery cell. For example, the graphene active material layer can have a porosity of 5%, 8%, 10%, 12%, 15%, 18%, 20%, 25%, 28%, 30%, or a range consisting of any two of these values.
[0195] In the present application, porosity refers to the ratio of the pore volume within the graphene active material layer to the total volume of the graphene active material layer. Porosity can be measured using the gas displacement method in accordance with GB / T 24586. Porosity W = (L1 - L2) / L1 * 100%, where L1 is the apparent volume of the sample and L2 is the actual volume of the sample.
[0196] In some embodiments, the specific surface area of the graphene active material layer is 30 m 2 / g to 500m 2 When the specific surface area of the graphene active material layer is within the above range, the bonding property of the graphene active material layer can be improved, and the tap density of the negative electrode sheet can be increased, thereby increasing the energy density of the battery cell. For example, the specific surface area of the graphene active material layer can be 30 m 2 / g, 50m 2 / g、80m 2 / g、100m 2 / g, 120m 2 / g, 150m 2 / g, 180m 2 / g, 200m 2 / g, 250m 2 / g, 280m 2 / g、300m 2 / g、320m 2 / g、350m 2 / g、380m 2 / g, 400m 2 / g, 420m 2 / g, 450m 2 / g, 480m 2 / g、500m 2 / g or a range consisting of any two of the above values.
[0197] In the embodiments of the present application, specific surface area is a well-known meaning in the art, and is usually expressed in m 2The unit of pore size is expressed in g and can be tested using methods and instruments known in the art. For example, it can be tested using an inert gas (e.g., nitrogen) adsorption specific surface area analysis method according to GB / T 19587-2017 and calculated using the BET (Brunauer Emmett Teller) method. The nitrogen adsorption specific surface area analysis test can be performed using a Tri-Star 3020 specific surface area pore size analyzer from Micromeritics, USA. The pore size distribution can be analyzed using the BJH (Barrett-Joiner-Halenda) model.
[0198] battery cells
[0199] In a third aspect, the present application provides a battery cell, which includes a positive electrode sheet and a negative electrode sheet.
[0200] In some embodiments, the negative electrode plate is a negative electrode plate prepared as described in any embodiment of the first aspect of the present application or a negative electrode plate according to any embodiment of the second aspect of the present application.
[0201] [Positive electrode]
[0202] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector.
[0203] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is provided on either or both of the two facing surfaces of the positive electrode current collector.
[0204] When the battery cell of the embodiment of the present application is a lithium-ion battery, the positive electrode active material may include, but is not limited to, at least one of a lithium-containing transition metal oxide, a lithium-containing phosphate, and their respective modified compounds. Examples of lithium transition metal oxides may include, but are not limited to, at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds.
[0205] In some embodiments, in order to further improve the energy density of the battery cell, the positive electrode active material for the lithium ion battery may include a general formula of Li a Ni b Co c M d O e A fAt least one of a lithium transition metal oxide and a modified compound thereof. 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M includes at least one of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A includes at least one of N, F, S and Cl.
[0206] As an example, the positive active material for lithium ion batteries may include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM333),LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523),LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622),LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.80 Co 0.15 Al 0.05 At least one of O2, LiFePO4, and LiMnPO4.
[0207] When the battery cell of the present application is a sodium ion battery, the positive electrode active material may include but is not limited to at least one of sodium-containing transition metal oxides, polyanion materials (such as phosphates, fluorophosphates, pyrophosphates, sulfates, etc.), and Prussian blue materials.
[0208] As an example, the positive active material for sodium ion batteries may include NaFeO2, NaCoO2, NaCrO2, NaMnO2, NaNiO2, NaNi 1 / 2 Ti 1 / 2 O2、NaNi 1 / 2 Mn 1 / 2 O2、Na 2 / 3 Fe 1 / 3 Mn 2 / 3 O2、NaNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, NaFePO4, NaMnPO4, NaCoPO4, Prussian blue materials, general formula X p M' q (PO4) r O x Y 3-x At least one of the materials. pM' q (PO4) r O x Y 3-x , 0<p≤4, 0<q≤2, 1≤r≤3, 0≤x≤2, X includes H + 、Li + 、Na + , K + and NH4 + At least one of , M' is a transition metal cation, optionally at least one of V, Ti, Mn, Fe, Co, Ni, Cu and Zn, and Y is a halogen anion, optionally at least one of F, Cl and Br.
[0209] In the embodiment of the present application, the modified compound of each positive electrode active material may be a doping modification and / or surface coating modification of the positive electrode active material.
[0210] In some embodiments, the positive electrode active material layer may further optionally include a positive electrode conductive agent. The present embodiments do not particularly limit the type of positive electrode conductive agent. By way of example, the positive electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the positive electrode conductive agent is ≤5% based on the total mass of the positive electrode active material layer.
[0211] In some embodiments, the positive electrode active material layer may further optionally include a positive electrode binder. The embodiments of the present application do not particularly limit the type of positive electrode binder. As an example, the positive electrode binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin. In some embodiments, based on the total mass of the positive electrode active material layer, the mass percentage of the positive electrode binder is ≤5%.
[0212] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0213] [Electrolytes]
[0214] Battery cells also include an electrolyte, which conducts ions between the positive and negative electrodes. The present embodiments do not specifically limit the type of electrolyte; the electrolyte can be selected based on needs. For example, the electrolyte can be liquid, gel, or solid.
[0215] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0216] When the battery cell of the embodiment of the present application is a lithium ion battery, as an example, the electrolyte salt may include but is not limited to at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0217] When the battery cell of the embodiment of the present application is a sodium ion battery, as an example, the electrolyte salt may include but is not limited to at least one of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bisfluorosulfonyl imide (NaFSI), sodium bistrifluoromethanesulfonyl imide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalatoborate (NaDFOB), sodium dioxalatoborate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorobisoxalatophosphate (NaDFOP) and sodium tetrafluorooxalatophosphate (NaTFOP).
[0218] As an example, the solvent may include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), and diethyl sulfone (ESE).
[0219] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0220] [Isolation film]
[0221] In some embodiments, the battery cell further includes a separator. The embodiments of the present application have no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0222] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0223] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0224] In some embodiments, the battery cell may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0225] In some embodiments, the outer packaging of the battery cell can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the battery cell can also be a soft shell, such as a bag-type soft shell. The soft shell can be made of plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0226] The present invention has no particular restrictions on the shape of the battery cell, which can be cylindrical, square, or any other shape. FIG2 shows a battery cell 5 with a square structure as an example.
[0227] In some embodiments, as shown in FIG3 , the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the separator may be formed into an electrode assembly 52 through a winding process and / or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 may be one or more, which can be adjusted according to demand.
[0228] The preparation methods of the battery cells of the embodiments of the present application are well known. In some embodiments, a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte can be assembled to form a battery cell. As an example, the positive electrode sheet, separator, and negative electrode sheet can be wound and / or laminated to form an electrode assembly. The electrode assembly is then placed in an outer packaging, dried, and then injected with electrolyte. The battery cell is then vacuum packaged, allowed to stand, formed, and shaped to obtain a battery cell.
[0229] In some embodiments of the present application, the battery cells according to the present application can be assembled into a battery module. The battery module can contain multiple battery cells, and the specific number can be adjusted according to the application and capacity of the battery module.
[0230] Figure 4 is a schematic diagram of an example battery module 4. As shown in Figure 4, in the battery module 4, multiple battery cells 5 can be arranged sequentially along the length of the battery module 4. Of course, they can also be arranged in any other manner. The multiple battery cells 5 can further be secured using fasteners. Optionally, the battery module 4 may also include a housing having a storage space, and the multiple battery cells 5 are accommodated in the storage space.
[0231] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0232] Figures 5 and 6 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 5 and 6, the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 covers the lower case 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the battery box.
[0233] The battery according to the embodiment of the present application may include one or more battery cells. When the battery includes a plurality of battery cells, the battery may include a battery module or a battery pack.
[0234] Electrical devices
[0235] A fourth aspect of the embodiments of the present application provides an electrical device, which includes at least one of the battery cells, battery modules, or battery packs of the present application. The battery cells, battery modules, or battery packs can be used as power sources for the electrical device, or as energy storage units for the electrical device. The electrical device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship, a satellite, an energy storage system, etc.
[0236] The electrical device can select battery cells, battery modules or battery packs according to its usage requirements.
[0237] Figure 7 is a schematic diagram of an exemplary electrical device 6. This electrical device 6 can be a pure electric vehicle, hybrid electric vehicle, or plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this electrical device 6, a battery pack or battery module can be used. Another exemplary electrical device can be a mobile phone, tablet computer, or laptop computer. These electrical devices are typically required to be lightweight and thin, and can utilize battery cells as their power source.
[0238] Example
[0239] The following embodiments describe the present disclosure in more detail, and these embodiments are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are by mass, and all reagents used in the embodiments are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the embodiments are commercially available.
[0240] Example 1 Preparation of lithium-ion battery
[0241] 1. Preparation of positive electrode sheet
[0242] The positive electrode active material lithium iron phosphate, the conductive agent Super P, and the binder PVDF are mixed evenly in an appropriate amount of solvent N-methylpyrrolidone (NMP) at a mass ratio of 98:1:1 to obtain a positive electrode slurry; the positive electrode slurry is coated on a 12μm aluminum foil, and the positive electrode sheet is obtained through processes such as drying, cold pressing, slitting, and cutting.
[0243] 2. Preparation of negative electrode sheet
[0244] (1) Preparation of precursor film
[0245] Polyamic acid (PAA) was added to N-methylpyrrolidone (NMP) solvent and stirred for 0.5 hours under magnetic stirring to obtain a polyamic acid solution (the mass percentage of polyamic acid was 12.8 wt %).
[0246] Thiourea was added into the polyamic acid solution to form a precursor solution (the mass percentage of thiourea was 8 wt %).
[0247] The precursor solution was coated onto a 15 μm copper foil using a coating machine. The thickness of the coated precursor solution was adjusted by adjusting the position of the scraper to 100 μm (the position of the scraper to the copper foil surface was 100 μm).
[0248] The precursor solution was placed in a vacuum oven at 80° C. and dried for 2 hours; and then hot pressed at 200° C. and 2 MPa to form a precursor film layer.
[0249] (2) Preparation of graphene active material layer
[0250] A CO2 laser emitter is used to scan and etch the precursor film layer along the length of the copper foil to form the graphene active material layer. The laser wavelength of the CO2 laser emitter is 10.6μm, the pulse width is ≈14μs, the number of pulses per inch is 1000, the output power range is 12W, the beam radius is about 100μm, the scanning speed is 5cm / s, and the laser intensity range of the precursor film surface is 20J / cm 2 , the distance between the laser and the precursor film layer is 3 mm.
[0251] 3. Preparation of electrolyte
[0252] In an environment with a water content of less than 10 ppm, non-aqueous organic solvents ethylene carbonate EC and diethyl carbonate DMC are mixed in a volume ratio of 1:1 to obtain an electrolyte solvent, and then lithium salt lithium hexafluorophosphate and the mixed solvent are mixed to prepare an electrolyte with a lithium salt concentration of 1 mol / L.
[0253] 4. Preparation of lithium-ion batteries
[0254] The positive electrode sheet, polyethylene PE separator, and negative electrode sheet are stacked and wound in sequence to obtain an electrode assembly; the electrode assembly is placed in an outer package, dried, and then injected with electrolyte. After vacuum packaging, standing, formation, shaping and other processes, a lithium-ion battery is obtained.
[0255] Comparative Example 1
[0256] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, the steps for preparing the negative electrode sheet of Comparative Example 1 are as follows:
[0257] Graphene (the negative electrode active material), conductive agent Super P, dispersant sodium carboxymethyl cellulose (CMC), and binder styrene-butadiene rubber (SBR) were mixed uniformly in deionized water to create a negative electrode slurry. The solid components of the negative electrode slurry had a mass ratio of artificial graphite, Super P, CMC, and SBR of 97:1:1:1. The negative electrode slurry was coated onto 15μm copper foil, dried at 85°C, and cold-pressed to produce a negative electrode sheet.
[0258] Comparative Example 2
[0259] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, the steps for preparing the negative electrode sheet of Comparative Example 2 were as follows:
[0260] (1) Preparation of precursor film
[0261] Polyamic acid (PAA) was added to N-methylpyrrolidone (NMP) solvent and stirred under magnetic stirring for 0.5 hours to obtain a polyamic acid solution (the mass percentage of polyamic acid was 12.8 wt %), which was used as a precursor solution.
[0262] The precursor solution was coated onto a 15 μm copper foil using a coating machine. The thickness of the coated precursor solution was adjusted by adjusting the position of the scraper to 100 μm (the position of the scraper to the copper foil surface was 100 μm).
[0263] The precursor solution was placed in a vacuum oven at 80° C. and dried for 2 hours; and then hot pressed at 200° C. and 2 MPa to form a precursor film layer.
[0264] (2) Preparation of graphene active material layer
[0265] A CO2 laser emitter is used to scan and etch the precursor film layer into the graphene active material layer along the length of the copper foil. The laser wavelength of the CO2 laser emitter is 10.6μm, the pulse width is ≈14μs, the number of pulses per inch is 1000, the output power range is 12W, the beam radius is about 100μm, the scanning speed is 5cm / s, and the laser intensity range on the copper foil surface is 20J / cm 2 , the distance between the laser and the precursor film layer is 3 mm.
[0266] Example 2
[0267] A lithium-ion battery was prepared using a method similar to that of Example 1. The difference from Example 1 was that the types of the organic carbon source solutions were adjusted in Examples 2-1 to 2-12.
[0268] Example 2-1 uses a polypropylene solution. Example 2-2 uses a polyvinyl alcohol solution. Example 2-3 uses a polyvinyl pyrrolidone solution. Example 2-4 uses a polystyrene solution. Example 2-5 uses an isobutyl vinyl ether solution. Example 2-6 uses a polyvinyl acetate solution. Example 2-7 uses a cellulose acetate solution. Example 2-8 uses a chitosan acetate solution. Example 2-9 uses a chitin acetate solution. Example 2-10 uses cellulose acetate. Example 2-11 uses cellulose acetate butyrate. Example 2-12 uses cellulose acetate propionate.
[0269] Example 3
[0270] A lithium-ion battery was prepared using a method similar to that of Example 1. The difference from Example 1 was that the types of organic doping sources were adjusted in Examples 3-1 to 3-13.
[0271] Example 4
[0272] Lithium-ion batteries were prepared using a method similar to that of Example 1. The difference from Example 1 was that the content of the organic doping source was adjusted in Examples 4-1 to 4-6.
[0273] Example 5
[0274] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, the thickness of the graphene active material layer was adjusted in Examples 5-1 to 5-3.
[0275] The relevant parameters of the embodiments and comparative examples are shown in Table 1 and Table 2.
[0276] Test section
[0277] 1. Detection of graphene active material layer thickness
[0278] The negative electrode piece was taken, and a scanning electron microscope (SEM) was used to scan the cross section of the negative electrode piece to measure the thickness of the graphene active material layer.
[0279] 2. Negative electrode sheet resistance detection
[0280] Cut small 10mm diameter discs from the left, center, and right sides of the negative electrode. Turn on the indicator light on the Yuanneng Technology electrode resistance meter and place them in the appropriate positions on the "probe" of the film resistance meter. Click the "Start" button and wait for the reading to stabilize before reading. Test each disc in two locations. Calculate the average of the six measurements to obtain the film resistance of that electrode.
[0281] 3. Gram capacity test of negative electrode
[0282] Take the above-mentioned negative electrode sheet and form a counter electrode with a metal lithium sheet. Use polyethylene (PE) film as an isolation membrane, drip a few drops of the same electrolyte as the above-mentioned battery cell, and assemble it into a CR2430 button battery in an argon-protected glove box.
[0283] After the resulting button cell was allowed to rest for 12 hours, it was discharged at a constant current of 0.1C at 25°C to 0.005V, and the discharge capacity was recorded. It was then charged at a constant current of 0.1C to 2.5V, and the charge capacity was recorded. The ratio of the charge capacity to the mass of the negative electrode active material is the initial gram capacity of the negative electrode active material.
[0284] 4. Lithium-ion battery capacity retention rate detection
[0285] The button-type battery cells were charged and discharged at a constant current of 0.33C in the range of 0.005-2.5V at 25°C. The capacity retention after 500 cycles was calculated, with the initial discharge capacity as 100%. Capacity retention after 500 cycles (%) = 500th cycle discharge capacity / initial discharge capacity × 100%.
[0286] Test results
[0287] The test results are shown in Table 1 and Table 2.
[0288] Table 1
[0289] Table 2
[0290] In Table 1 and Table 2,
[0291] The mass percentage of the organic doping source is calculated based on the total mass of the precursor solution;
[0292] The mass percentage of the doping element is calculated based on the total mass of the graphene active material layer.
[0293] It can be seen from Table 1 and Table 2 that Comparative Examples 1 and 2 directly use graphene as the main material of the active material layer. Compared with Comparative Examples 1 and 2, the embodiment of the present application also introduces doping elements into the graphene active material layer, which can increase the gram capacity of the negative electrode sheet, and the organic doping source can be chemically bonded to the carbon element in the graphene active material layer under the laser etching action of the laser source. The doping elements can further increase the gram capacity of the negative electrode sheet.
[0294] Therefore, the embodiments of the present application can improve the electrochemical performance of the negative electrode sheet by doping different elements, thereby further enhancing the performance of the battery cell. In particular, when the doping element is etched into a highly conductive material, such as doping with conductive elements such as iron, nickel, and cobalt, the resistance of the negative electrode sheet can be significantly reduced, improving its overall conductivity and facilitating improved capacity retention of the battery cell.
[0295] By doping elements with high capacity or electrochemical activity, such as silicon, phosphorus and other elements, they can contribute to the capacity and increase the gram capacity of the negative electrode.
[0296] As shown in Figures 8 to 12, the XRD pattern of Example 1 shown in Figure 8 shows that the graphene active material layer has two standard peaks (002) and (100), and the peak at (200) is wider and has a lower angle than that of the graphite crystal, indicating that the degree of order between the graphene active material layers is reduced and the interlayer spacing is increased;
[0297] The Raman graph shift of Example 1 shown in Figure 9 shows D peak, G peak and 2D peak unique to few-layer graphene, and ID / IG=1.35, indicating that the obtained laser-etched graphene has more defect structures, which is conducive to combining with the negative electrode current collector.
[0298] Figure 10 shows a transmission electron microscope image of the graphene active material layer in Example 1; Figure 11 is a scanning electron microscope (SEM) image of the graphene active material layer formed by laser etching in Example 1 of this application. In Figure 11, the area corresponding to 15 μm is the copper foil area, and the area corresponding to 100 μm is the graphene active material layer. The graphene active material layer is dense and uniform, with a three-dimensional structure and a large specific surface area.
[0299] Figure 12 is an EDX elemental analysis of the graphene active material layer formed by laser etching in Example 1 of the present application, from which it can be seen that the mass percentage of the graphene active material layer is 91.1wt%, and the sulfur content is about 5.16wt%.
[0300] FIG13 shows the charge-discharge curve of the lithium-ion battery of Example 1 after 100 cycles at 0.1C. It can be seen that the cycle performance of the lithium-ion battery is relatively good and the capacity decay is relatively slow.
[0301] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions, and modifications may be made to the embodiments without departing from the spirit, principles, and scope of the present application.
Claims
1. A method for preparing a negative electrode sheet, include: providing an organic carbon source solution; adding an organic doping source containing a doping element into the organic carbon source solution to form a precursor solution; Providing the precursor solution onto the surface of the negative electrode current collector, and heat-treating the precursor solution to form a precursor film layer; The precursor film layer is etched by a laser source to obtain a graphene active material layer containing the doping element, wherein the doping element is connected to the carbon element in the graphene active material layer in a chemically bonded form.
2. The preparation method according to claim 1, in, The doping element includes at least one of a first element, a second element, and a third element; The first element includes one or more of sulfur, phosphorus, silicon, selenium and tin; The second element includes one or more of iron, cobalt, nickel, aluminum and copper; The third element includes one or more of boron, germanium, titanium and magnesium.
3. The preparation method according to claim 1 or 2, in, The doping element includes sulfur, and the organic doping source includes one or more of thiourea, methionine, thioglycolic acid, 2-mercaptoethanol, thiobenzoic acid, diphenyl sulfoxide, cysteine and benzenesulfonic acid; and / or The doping element includes phosphorus, and the organic doping source includes one or more of phosphorous acid, hydrocarbyl phosphite, hydrocarbyl phosphite, phosphite ester, ethyl hypophosphite and hydrocarbyl phosphite ester; and / or The doping element includes silicon, and the organic doping source includes one or more of trimethylsilanol, triethylsilanol, diphenylmethylsilane, hexamethyldisiloxane, trimethylphenylsilane and tetraethyl orthosilicate; and / or The doping element includes tin, and the organic doping source includes one or more of monobutyltin, dibutyltin, tributyltin, tributyltin oxide, triphenyltin, and dioctyltin; and / or The doping element includes nickel, and the organic doping source includes one or more of nickel oxalate, nickel oleate, nickel propionate, nickel butyrate, nickel octanoate, and nickel lactate; and / or The doping element includes copper, and the organic doping source includes one or more of copper acetate, fatty acid copper, and copper naphthenate; and / or The doping element includes boron, and the organic doping source includes one or more of phenylboric acid, diphenylboric acid, triphenylboron, and trimethoxyboroxane; and / or The doping element includes selenium, and the organic doping source includes one or more of dimethyl selenium and diethyl diselenide; and / or The doping element includes germanium, and the organic doping source includes one or more of tetraethyl germanium, methyl germanium thiol, butyl germanium thiol, and octyl germanium thiol; and / or The doping element includes iron, and the organic doping source includes one or more of ferrous lactate, ferric citrate, and ferric glycinate; and / or The doping element includes cobalt, and the organic doping source includes one or more of cobalt oxalate and cobalt acetate; and / or The doping element includes titanium, and the organic doping source includes one or more of orthotitanate and butyl titanate; and / or The doping element includes aluminum, and the organic doping source includes one or more of triethylaluminum, triisobutylaluminum, and diethylaluminum chloride; and / or The doping element includes magnesium, and the organic doping source includes one or more of magnesium glycinate, magnesium citrate, and magnesium lactate.
4. The preparation method according to any one of claims 1 to 3, in, Based on the total mass of the precursor solution, the mass percentage of the organic doping source is 0.2 wt % to 20 wt %.
5. The preparation method according to any one of claims 1 to 4, in, The thickness of the precursor solution is 40 μm to 150 μm.
6. The preparation method according to any one of claims 1 to 5, in, The step of heat treating the precursor solution to form a precursor film layer comprises: first heat-treating the precursor solution to remove at least a portion of the solvent in the precursor solution and retain the solute in the precursor solution; The second heat treatment treats the solute in the precursor solution and provides an external force to the solute to form a precursor film layer.
7. The preparation method according to any one of claims 1 to 6, in, The thickness of the precursor film layer is 30 μm to 120 μm.
8. The preparation method according to any one of claims 1 to 7, in, The step of providing an organic carbon source solution comprises: dissolving an organic carbon source in a solvent to obtain the organic carbon source solution, wherein the organic carbon source comprises one or more of polyamic acid, polyvinyl pyrrolidone, isobutyl vinyl ether, polyvinyl acetate, cellulose ester compounds, polyenol compounds, polyolefin compounds and polysaccharide compounds.
9. The preparation method according to claim 8, in, The cellulose ester compound includes one or more of cellulose acetate, cellulose acetate butyrate and cellulose acetate propionate; and / or The polyenol compound comprises polyvinyl alcohol and / or polypropylene alcohol; and / or The polyolefin compound comprises polypropylene and / or polystyrene; and / or The polysaccharide compound includes one or more of cellulose, chitosan and chitin.
10. The preparation method according to any one of claims 1 to 9, in, The current collector comprises a metal substrate; or The current collector includes an organic polymer layer and a metal layer disposed on at least one surface of the organic polymer layer, wherein the precursor solution is provided to the surface of the metal layer.
11. The preparation method according to any one of claims 1 to 10, in, The laser source includes one or more of a carbon dioxide laser source, a diode laser source, an argon ion laser source, a nitrogen laser source, a red laser source, a blue laser source and a femtosecond laser source.
12. The preparation method according to claim 11, in, The output power of the carbon dioxide laser source is 10W to 30W.
13. A negative electrode plate, comprising a negative electrode current collector and a graphene active material layer, wherein the graphene active material layer is located on at least one surface of the negative electrode current collector, the graphene active material layer is formed by etching with a laser source, and the graphene active material layer comprises doping elements and carbon elements connected in a chemically bonded form.
14. The negative electrode sheet according to claim 13, in, Based on the total mass of the graphene active material layer, the mass percentage of the doping element is 0.1 wt % to 10 wt %.
15. The negative electrode sheet according to claim 13 or 14, in, The thickness of the graphene active material layer is 30 μm to 120 μm; and / or The negative electrode plate uses lithium metal as the counter electrode, and in the charge and discharge curves tested in the range of 0.005V to 2.5V, the charge capacity in the range of 0.005V to 2.5V is 400mAh / g to 480mAh / g.
16. The negative electrode sheet according to any one of claims 13 to 15, in, The graphene active material layer has a porous structure. The pore size of the pore structure is 1 nm to 80 nm; and / or The porosity of the graphene active material layer is 5% to 30%; and / or The specific surface area of the graphene active material layer is 30 m 2 / g to 500m 2 / g.
17. A battery cell comprising the negative electrode sheet according to any one of claims 13 to 16.
18. A battery comprising the battery cell according to claim 17.
19. An electrical device comprising the battery as claimed in claim 18.
Citation Information
Patent Citations
Metal monatomic modified graphene material, lithium-sulfur battery modified diaphragm, preparation method of lithium-sulfur battery modified diaphragm and lithium-sulfur battery
CN115611269A
Negative pole piece, preparation method of negative pole piece, battery monomer, battery and power utilization device
CN116247166A
Negative electrode carbon material for lithium secondary battery, negative electrode for lithium battery, and lithium secondary battery
JP2014199746A
Cited By
Biomass-based hard carbon negative electrode material, preparation method thereof and sodium ion battery
CN119591083A