Battery jelly roll, method for manufacturing battery jelly roll, and secondary battery
By setting a stress-relieving layer between the electrode sheets of a lithium battery and using a mixture of ethylene carbonate, polyvinylidene fluoride, and modified polyacrylic acid, the problems of electrode sheet expansion and wrinkling were solved, achieving low-cost performance improvement of lithium batteries.
Patent Information
- Application Number
- PCT/CN2024/077708
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-08
- Filing Date
- 2024-02-20
- Publication Date
- 2024-11-14
AI Technical Summary
During the charging and discharging process, the electrode plates of existing lithium batteries are prone to expansion or wrinkling, which leads to reduced cycle performance and safety, and the existing methods increase production costs.
A stress-relief layer is provided between the electrode plates of a lithium battery, using ethylene carbonate and/or a mixture of polyvinylidene fluoride and modified polyacrylic acid as materials, to provide deformation space and avoid electrode wrinkling and deformation.
This effectively avoids wrinkles and deformation of the electrode sheets, reduces production costs, and improves the cycle performance and safety of lithium batteries.
Smart Images

Figure CN2024077708_14112024_PF_FP_ABST
Abstract
Description
Battery core, method for manufacturing battery core, and secondary battery Technical Field
[0001] The present application mainly relates to the field of battery technology, and specifically to a battery roll core, a method for manufacturing a battery roll core, and a secondary battery. Background Art
[0002] Since the commercialization of lithium batteries, they have been widely used in 3C digital products and power batteries.
[0003] The core of a lithium battery is the core, consisting of the positive and negative electrodes, as well as the separator. Currently, the core of lithium batteries is primarily wound. During subsequent battery processing, the electrodes swell due to electrolyte immersion and battery charging and discharging. This can cause the electrodes to swell or wrinkle, leading to adverse phenomena such as lithium deposition within the electrodes. This can reduce the battery's cycling performance and safety.
[0004] In order to solve the problem of electrode expansion and wrinkling, the relevant technology uses adhesives to bond the diaphragm and the electrode to prevent the electrode from deforming. However, the use of adhesives will increase the production cost of lithium batteries.
[0005] Therefore, how to solve the problem of electrode deformation and wrinkling at low cost is an urgent issue to be solved.
[0006] Summary of the Invention
[0007] The technical problem to be solved by the present application is to provide a battery core, a method for manufacturing a battery core, and a secondary battery, which can solve the problems of electrode deformation and wrinkling at a low cost.
[0008] The technical solution adopted by this application to solve the above-mentioned technical problems is a battery core, which includes a positive electrode sheet, a negative electrode sheet, and a separator, wherein the separator is located between the positive electrode sheet and the negative electrode sheet. The battery core also includes a stress relief layer located between the positive electrode sheet and the negative electrode sheet.
[0009] In one embodiment of the present application, the material of the stress release layer includes a mixture of ethylene carbonate and / or polyvinylidene fluoride and modified polyacrylic acid.
[0010] In one embodiment of the present application, the battery roll core has a corner area, and the stress release layer is located between the negative electrode sheet and the positive electrode sheet in the corner area.
[0011] In one embodiment of the present application, the width of the stress release layer located in the corner area increases as the number of layers of electrode sheets wound around the battery roll core increases.
[0012] In one embodiment of the present application, the thickness of the stress release layer is 1 μm to 30 μm.
[0013] In one embodiment of the present application, the stress release layer is located between the positive electrode plate and the separator, and / or between the negative electrode plate and the separator.
[0014] In order to solve the above-mentioned technical problems, the present application also proposes a method for manufacturing a battery roll core, wherein the battery roll core includes a positive electrode sheet, a negative electrode sheet and a separator, and the separator is located between the positive electrode sheet and the negative electrode sheet. The method includes forming a stress release layer between the positive electrode sheet and the negative electrode sheet, wherein the material of the stress release layer includes a mixture of ethylene carbonate and / or polyvinylidene fluoride and modified polyacrylic acid.
[0015] In one embodiment of the present application, the battery roll core has a corner area, and the stress release layer is formed between the negative electrode sheet and the positive electrode sheet in the corner area.
[0016] In one embodiment of the present application, the width of the stress release layer located in the corner area increases as the number of layers of electrode sheets wound around the battery roll core increases.
[0017] In one embodiment of the present application, the thickness of the stress release layer is 1 μm to 30 μm.
[0018] To solve the above technical problems, the present application further proposes a secondary battery, comprising a battery core and a shell as described above, wherein the battery core is accommodated in the shell.
[0019] The battery core, battery core manufacturing method, and secondary battery disclosed herein provide a stress relief layer between the electrode plates. This stress relief layer provides space for deformation of the electrode plates, thereby preventing wrinkles in the electrode plates and battery deformation. Furthermore, the method of providing a stress relief layer between the electrode plates disclosed herein offers the advantage of low cost.
[0020] Summary of the Figures
[0021] In order to make the above-mentioned objects, features and advantages of the present application more clearly understood, the specific embodiments of the present application are described in detail below with reference to the accompanying drawings, wherein:
[0022] FIG1 is a perspective schematic diagram of a battery roll core according to an embodiment of the present application;
[0023] FIG2 is a schematic top view of an unfolded electrode sheet in a battery roll according to an embodiment of the present application;
[0024] FIG3 is an exemplary flow chart of a method for manufacturing a battery roll core according to an embodiment of the present application.
[0025] Reference Signs Battery roll core 100 Electrode sheet 130 Corner area 110 Stress release layer 140 Flat area 120 Center line 141
[0026] Preferred embodiments of the present invention
[0027] In order to make the above-mentioned objects, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below with reference to the accompanying drawings.
[0028] In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application may also be implemented in other ways different from those described herein. Therefore, the present application is not limited to the specific embodiments disclosed below.
[0029] As used in this application and the claims, unless the context clearly indicates otherwise, the words "a," "an," "an," and / or "the" are not intended to refer to the singular but may include the plural. Generally speaking, the terms "comprises" and "include" only indicate the inclusion of the steps and elements specifically identified, and these steps and elements do not constitute an exclusive list. A method or apparatus may also include other steps or elements.
[0030] Furthermore, it should be noted that the use of terms such as "first" and "second" to define components is solely for the purpose of distinguishing the corresponding components. Unless otherwise stated, these terms have no special meaning and therefore should not be construed as limiting the scope of protection of this application. Furthermore, while the terms used in this application are selected from commonly known and commonly used terms, some terms mentioned in this specification may have been selected by the applicant at his or her discretion, and their detailed meanings are explained in the relevant sections of this description. Furthermore, this application should be understood not only by the actual terms used, but also by the meaning implied by each term.
[0031] Flowcharts are used in this application to illustrate the operations performed by systems according to embodiments of the present application. It should be understood that the preceding or following operations are not necessarily performed in exact order. Instead, the various steps may be processed in reverse order or simultaneously. Furthermore, other operations may be added to these processes, or one or more operations may be removed from these processes.
[0032] Next, the battery core, the manufacturing method of the battery core, and the secondary battery of the present application are described through specific embodiments.
[0033] FIG1 is a perspective schematic diagram of a battery roll core according to an embodiment, and FIG2 is a top view schematic diagram of the unfolded electrode pole pieces in the battery roll core according to an embodiment. Referring to FIG1 , the battery roll core 100 includes a corner region 110 and a flat region 120, and the corner region 110 is located at both ends of the flat region 120 along a first direction D1. FIG2 shows a top view schematic diagram of the unfolded electrode pole pieces in the battery roll core. The electrode pole piece 130 in FIG2 can represent a positive pole piece or a negative pole piece. As shown in FIG2 , the electrode pole piece 130 can be regarded as a top view schematic diagram of the unfolded battery roll core 100 in FIG1 ; the battery roll core 100 can also be regarded as being wound by the positive pole piece and the negative pole piece as shown in FIG2 , and a separator located between the positive pole piece and the negative pole piece.
[0034] The positive electrode sheet can be made of aluminum foil, such as porous aluminum foil or etched aluminum foil. The negative electrode sheet can be made of copper foil. The positive and negative electrode sheets are coated with positive and negative active materials, respectively. A separator can be used to separate the positive and negative electrode sheets to prevent contact and short circuits. The separator can be made of polypropylene (PP) or polyethylene (PE).
[0035] The battery roll core of the present application also includes a stress release layer, which is located between the positive electrode sheet and the negative electrode sheet in the battery roll core. Referring to Figure 2, the electrode sheet 130 extends along the first direction D1, and the size in the first direction D1 is L1, and the size in the second direction D2 is W1. The stress release layer 140 is coated on one surface of the electrode sheet 130 at a preset distance d1 along the first direction D1. The preset distance satisfies that when the electrode sheet 130 is wound into the battery roll core 100 as shown in Figure 1, the stress release layer 140 is located between the negative electrode sheet and the positive electrode sheet in the corner area 110. In some other embodiments, the stress release layer can also be coated on both sides of the electrode sheet, not limited to one side in the above embodiment.
[0036] With reference to FIG1 , the corner area 110 can be approximately regarded as a half cylinder, and as the number of layers of electrode sheets wound by the battery roll core increases, the radius of the cylinder gradually increases. In conjunction with FIG2 , the width W2 of the stress release layer 140 along the first direction D1 increases as the number of layers of electrode sheets wound by the battery roll core increases, thereby ensuring that the area of the stress release layer 140 can cover the positive and negative electrode sheets located in the corner area 110 and adjacent thereto. Specifically, with reference to FIG2 , assuming that the electrode sheet 130 is wound along the first direction D1 starting from the left end, as the winding proceeds, the radius of the corner area formed also gradually increases, and correspondingly, the width of the stress release layer 140 from left to back along the first direction D1 gradually increases.
[0037] As shown in Figure 2 , the predetermined distance refers to the distance along the first direction D1 between the centerlines 141 of two adjacent stress release layers 140 . When the electrode sheet 130 is wound into the battery roll 100 , the centerline 141 can be considered the axis of the cylinder.
[0038] In one embodiment, the thickness of the stress release layer located in the corner area is 2μm to 10μm, for example, it can be 2μm, 4μm, 6μm, 8μm or 10μm. The thickness of the stress release layer can be set according to the thickness of the electrode plate, the specifications of the battery made of the battery core, and the degree of expansion of the electrode plate. For example, when the degree of expansion of the electrode plate is more serious, the thickness of the stress release layer can be increased accordingly, which helps to alleviate the deformation of the electrode plate. This will be explained in detail later.
[0039] In the battery coil, the positive electrode sheet, the separator, and the negative electrode sheet are arranged adjacent to each other in sequence. The stress release layer between the positive electrode sheet and the negative electrode sheet can be located between the positive electrode sheet and the separator adjacent to the positive electrode sheet, that is, the positive electrode sheet, the stress release layer, and the separator are adjacent to each other. In this case, the stress release layer can be coated on the positive electrode sheet; the stress release layer can also be located between the negative electrode sheet and the separator adjacent to the negative electrode sheet, that is, the negative electrode sheet, the stress release layer, and the separator are adjacent to each other in sequence. In this case, the stress release layer can be coated on the negative electrode sheet; the stress release layer can also be located between the negative electrode sheet and the separator adjacent to the negative electrode sheet, and between the separator adjacent to the negative electrode sheet and the positive electrode sheet adjacent to the separator, that is, the negative electrode sheet, the stress release layer, the separator, the stress release layer, and the positive electrode sheet are adjacent to each other. In this case, both the negative electrode sheet and the positive electrode sheet are coated with the stress release layer.
[0040] In the embodiment of FIG2 , the stress relief layer is provided only between the electrode pads in the corner region. In other embodiments, the stress relief layer may coat the entire surface of the electrode pads, and the thickness of the stress relief layer may be any value between 1 μm and 30 μm. In other embodiments, based on FIG2 , the stress relief layer may be applied to a portion of the region between adjacent stress relief layers along the first direction D1.
[0041] The material of the stress release layer in the above-mentioned embodiment of the present application is selected from a mixture of ethylene carbonate (EC) and / or polyvinylidene difluoride (PVDF) and modified polyacrylic acid. In detail, the stress release layer of the present application can be ethylene carbonate, or a mixture of polyvinylidene difluoride and modified polyacrylic acid, or a mixture of ethylene carbonate, polyvinylidene fluoride and modified polyacrylic acid. It should be understood that the materials contained in the stress release layer are not limited to the aforementioned materials. For example, it can also contain auxiliary materials.
[0042] Ethylene carbonate can be dissolved in the electrolyte. Thanks to the fact that ethylene carbonate is one of the components of the electrolyte, the ethylene carbonate dissolved in the electrolyte in the stress release layer will not affect the chemical and physical properties of the electrode liquid. After the ethylene carbonate in the stress release layer dissolves, a space appears at its original position. This space can be used to alleviate the deformation of the electrode plates, avoid wrinkles on the electrode plates or expansion of the battery core. Specifically, the embodiment in Figure 1 is used for illustration. During the use of the battery, the electrode plates (positive plates and / or negative plates) in the corner area 110 are expanded and deformed. After the electrode plates are expanded and deformed, an extrusion force is generated between each other. The extrusion force is transmitted to the flat area 120, thereby causing the electrode plates in the flat area to wrinkle or expand outward. In the present application, ethylene carbonate is set between the electrode plates in the corner area 110 as a stress buffer layer, and the space generated after the ethylene carbonate is dissolved is used to buffer the deformation of the electrode plates, thereby avoiding the electrode plates at the corner 110 from squeezing the electrode plates in the flat area 120.
[0043] Similarly, the hardness of polyvinylidene fluoride and / or modified polyacrylic acid used as a stress buffer layer decreases after being soaked in electrolyte, making it easy to deform under external force. Therefore, when the electrode plate expands and deforms, the electrode plate creates a space that can accommodate the deformed electrode plate by squeezing the polyvinylidene fluoride and / or modified polyacrylic acid, thereby preventing the electrode plate from squeezing the electrode plate in the flat area. It should be understood that the stress buffer layer provided between the electrode plates in the flat area also has the same function as described above. I will not elaborate on this here.
[0044] In addition, compared with the related art method of setting a high-cost adhesive between the electrode plate and the adjacent diaphragm to prevent the electrode plate from deforming, the method of setting a stress buffer layer between the electrode plates in the present application has the advantage of low cost while solving the problem of electrode plate deformation.
[0045] Another aspect of the present application is a method for manufacturing a battery roll core. The battery roll core includes a positive electrode sheet, a negative electrode sheet, and a separator, with the separator being located between the positive electrode sheet and the negative electrode sheet. FIG3 is an exemplary flow chart of a method for manufacturing a battery roll core according to an embodiment. Referring to FIG3 , the manufacturing method according to this embodiment includes the following steps:
[0046] Step S210: providing a positive electrode sheet, a negative electrode sheet and a separator;
[0047] Step S220: forming a stress release layer between the positive electrode sheet and the negative electrode sheet, wherein the material of the stress release layer includes a mixture of ethylene carbonate and / or polyvinylidene fluoride and modified polyacrylic acid.
[0048] The above steps S210 and S220 are described in detail below.
[0049] In step S210, a positive electrode sheet, a negative electrode sheet and a separator are provided, the positive electrode sheet, the separator and the negative electrode sheet are stacked in sequence, and the stacked positive electrode sheet, the separator and the negative electrode sheet are wound into a battery core by winding.
[0050] In step S220, before winding the positive electrode sheet, the separator and the negative electrode sheet, a stress release layer is formed between the positive electrode sheet and the negative electrode sheet, and the material of the stress release layer is selected from a mixture of ethylene carbonate and / or polyvinylidene fluoride and modified polyacrylic acid. Referring to Figure 1, in some embodiments, the battery roll core 100 has a corner area 110, and the stress release layer is formed between the negative electrode sheet and the positive electrode sheet in the corner area 110. Specifically, the stress release layer can be formed between the positive electrode sheet and the separator, or between the negative electrode sheet and the separator, or in the form of a stack of positive electrode sheet, stress release layer, separator, stress release layer and negative electrode sheet in sequence. The stress release layer can be formed between the electrode sheet and the adjacent separator by coating on the electrode sheet, or can be formed between the electrode sheet and the adjacent separator by forming a separate film layer independent of the electrode sheet.
[0051] In some embodiments, the thickness of the stress relief layer ranges from 1 μm to 30 μm. The thickness of the stress relief layer can be determined based on the thickness of the electrode sheet, the specifications of the battery made from the battery core, and the degree of expansion of the electrode sheet. For example, if the degree of expansion of the electrode sheet is severe, the thickness of the stress relief layer can be increased accordingly to help alleviate deformation of the electrode sheet.
[0052] For a clearer understanding of the battery core and the method for manufacturing the battery core of the present application, three examples and two comparative examples are given below.
[0053] Example 1:
[0054] Step 1: Prepare a positive electrode sheet coated with a stress release layer.
[0055] LiFePO4, conductive carbon black, and polyvinylidene fluoride were dispersed in N-methylpyrrolidone to form a positive electrode active material slurry. The percentages of LiFePO4, conductive carbon black, and polyvinylidene fluoride in the total weight of the three ingredients were 96.5%, 1.6%, and 1.9%, respectively. The positive electrode active material slurry was coated on both surfaces of a 13μm thick aluminum foil and then dried at 90°C for 10 minutes. The surface density of the dried coating layer was 33.2mg / cm 2 The dried aluminum foil is rolled and then die-cut into positive electrode sheets with tabs.
[0056] As shown in Figure 2 , the dimension L1 of the positive electrode sheet along the first direction D1 is 10879 mm, and the dimension W1 along the second direction D2 is 164.5 mm. Based on these dimensions, the position of the centerline 141 of the corner area is calculated. A stress relief layer 140 with a width W2 of 12 mm is applied around centerline 141. The material of stress relief layer 140 is ethylene carbonate, and the thickness of the applied ethylene carbonate is 8 μm. It should be understood that in Example 1, the width of stress relief layer 140 does not increase with the number of electrode sheet layers wound around the battery core. This does not constitute a limitation on the width of the stress relief layer in this application; it is merely one example.
[0057] Step 2: Prepare the negative electrode.
[0058] Graphite, conductive carbon black, hydroxymethyl cellulose, and styrene-butadiene rubber are dispersed in deionized water to form a negative electrode active material slurry. The percentages of graphite, conductive carbon black, hydroxymethyl cellulose, and styrene-butadiene rubber in the total weight of the four ingredients are 96%, 0.8%, 1.2%, and 2%, respectively. The negative electrode active material slurry is coated on both surfaces of a copper foil (the thickness of the copper foil is 8 μm) and then dried at 60°C for 10 minutes. The double-sided coating surface density after drying is 16.0 mg / cm2; the dried copper foil is rolled and die-cut into negative electrode tabs. As shown in Figure 2, the dimension L1 of the negative electrode tab along the first direction D1 is 11215 mm, and the dimension W1 along the second direction D2 is 168.5 mm.
[0059] Step 3: Prepare secondary lithium battery
[0060] The positive electrode sheet, negative electrode sheet and polypropylene separator coated with the stress release layer were respectively wound into a battery core; then hot pressed at 90°C and 2MPa for 180min; then the battery core was encapsulated in an aluminum shell, and the encapsulated aluminum shell was baked; LiPF6 was dissolved in ethylene carbonate (EC): propylene carbonate (PC): ethyl methyl carbonate (Ethylene carbonate, EC) at a concentration of 1mol / L. A non-aqueous electrolyte was formed in a mixed solvent of vinyl carbonate (EMC) = 35:5:60 (mass ratio), and 2.5% vinylene carbonate was added as a film-forming additive; the above electrolyte was injected into the above aluminum shell at an amount of 4.5 g / Ah and sealed; after standing for 24 hours, it was formed at a temperature of 45°C; a constant current charge was performed at a charging current of 1.0C to 3.65V, and a constant voltage charge was performed at a charging voltage of 3.65V to a current of 0.05C; and a discharge current of 1.0C to 2.5V was obtained to obtain the initial discharge capacity C0, and the AC internal resistance was recorded.
[0061] The battery roll core can also be encapsulated in a steel shell, an aluminum-plastic film or a plastic shell, not limited to the aforementioned aluminum shell. The non-aqueous electrolyte is composed of a non-aqueous organic solvent and a lithium salt. The non-aqueous organic solvent can be selected from one or more of a carbonate-based solvent, an ether-based solvent and a ketone-based solvent. In particular, the non-aqueous organic solvent can be an aprotic organic solvent, such as propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate and ethyl propionate, etc. Lithium salts are materials that are easily soluble in non-aqueous solvents, including but not limited to LiCl, LiBr, LiI, LiClO4, LiBF4, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, and (CF38O2)2NLi.
[0062] Step 4: Disassemble the Battery
[0063] The battery obtained in step 3 was charged to 3.65V at a constant current of 1.0C, and then charged to a current of 0.05C at a constant voltage of 3.65V. The charged electrode plates were disassembled and inspected for black and purple spots and wrinkles.
[0064] Example 2:
[0065] The difference between the second embodiment and the first embodiment is that the material of the stress release layer in the second embodiment is a mixture of polyvinylidene fluoride and modified polyacrylic acid.
[0066] Similar to the first embodiment, after charging the battery, the charged electrode plates are disassembled and observed to see if there are any black or purple spots or wrinkles.
[0067] Example 3:
[0068] The difference between the third embodiment and the first embodiment is that in the third embodiment, the stress release layer is coated on the negative electrode plate.
[0069] Similar to the first embodiment, after charging the battery, the charged electrode plates are disassembled and observed to see if there are any black or purple spots or wrinkles.
[0070] Comparative Example 1:
[0071] The difference between Comparative Example 1 and Example 1 is that the stress buffer layer is not coated on the positive electrode plate in Comparative Example 1. As in Example 1, after charging, the battery is disassembled and the charged electrode plate is inspected for black and purple spots and wrinkles.
[0072] Comparative Example 2:
[0073] Comparative Example 2 differs from Example 1 in that, instead of applying a stress buffer layer to the positive electrode, a mixture of polyvinylidene fluoride and modified polyacrylic acid is coated on one side of the separator. As with Example 1, the battery in Comparative Example 2 was charged and disassembled to inspect the electrode plates for dark purple spots and wrinkles.
[0074] Table 1 shows the observation results after disassembly of the batteries in Examples 1 to 2. Table 1 provides the following conclusions: As previously explained, stress buffer layers were provided between the electrode plates in Examples 1, 2, 3, and 2, and the disassembly results in Table 1 indicate that none of the batteries in Examples 1, 2, 3, and 2 exhibited dark purple spots or wrinkles. However, in 2, 3, which did not have a stress buffer layer between the electrode plates, dark purple spots and severe wrinkles appeared on the electrode plates.
[0075] Black-purple spots refer to dark purple streaks caused by insufficient lithium insertion in the battery due to wrinkles in the electrode plates. These spots can cause some of the active materials in the battery to become ineffective, and this failure can lead to a reduction in battery capacity. As shown in Table 1, the initial capacity of the battery in Comparative Example 2 was 152.8 Ah, which is lower than the initial capacity of the batteries in the other examples and comparative examples.
[0076] The above-mentioned embodiments and comparative examples and the corresponding disassembly results show that the provision of a stress buffer layer between the electrode plates in the present application can prevent wrinkles in the electrode plates.
[0077] Table 1 Disassembly results of batteries in Example 1 to Comparative Example 2
[0078] Another aspect of the present application is a secondary battery. The secondary battery comprises: a battery core as described above and a housing, wherein the battery core is housed within the housing. The battery core employed in the secondary battery has a stress buffer layer disposed between the electrode plates. The stress buffer layer prevents wrinkling of the electrode plates and swelling of the secondary battery.
[0079] The basic concepts have been described above. It will be apparent to those skilled in the art that the above disclosures are merely examples and do not limit the present application. Although not explicitly stated herein, those skilled in the art may make various modifications, improvements, and revisions to the present application. Such modifications, improvements, and revisions are suggested in the present application and remain within the spirit and scope of the exemplary embodiments of the present application.
[0080] At the same time, this application uses specific terms to describe the embodiments of this application. For example, "one embodiment," "an embodiment," and / or "some embodiments" refer to a certain feature, structure, or characteristic related to at least one embodiment of this application. Therefore, it should be emphasized and noted that "one embodiment," "an embodiment," or "an alternative embodiment" mentioned twice or multiple times in different locations in this specification does not necessarily refer to the same embodiment. In addition, certain features, structures, or characteristics in one or more embodiments of this application may be appropriately combined.
[0081] In some embodiments, numbers are used to describe the quantity of components and attributes. It should be understood that such numbers used in the description of the embodiments are modified by the modifiers "about", "approximately" or "substantially" in some examples. Unless otherwise stated, "about", "approximately" or "substantially" indicate that the numbers are allowed to vary by ±20%. Accordingly, in some embodiments, the numerical parameters used in the description and claims are approximate values, which may change according to the required features of individual embodiments. In some embodiments, the numerical parameters should take into account the specified significant digits and adopt the general method of retaining digits. Although the numerical domains and parameters used to confirm the breadth of their range in some embodiments of the present application are approximate values, in specific embodiments, the settings of such numerical values are as accurate as possible within the feasible range.
Claims
1. A battery roll core, comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is located between the positive electrode sheet and the negative electrode sheet, characterized in that: Also includes: A stress release layer is located between the positive electrode sheet and the negative electrode sheet.
2. The battery roll core according to claim 1, characterized in that: The material of the stress release layer includes a mixture of ethylene carbonate and / or polyvinylidene fluoride and modified polyacrylic acid.
3. The battery roll core according to claim 1, characterized in that: The battery roll core has a corner area, and the stress release layer is located between the negative electrode sheet and the positive electrode sheet in the corner area.
4. The battery roll core according to claim 3, characterized in that: The width of the stress release layer located in the corner area increases as the number of layers of electrode sheets wound around the battery winding core increases.
5. The battery roll core according to claim 1, characterized in that: The thickness of the stress release layer is 1 μm to 30 μm.
6. The battery roll core according to claim 1, characterized in that: The stress release layer is located between the positive electrode plate and the separator, and / or between the negative electrode plate and the separator.
7. A method for manufacturing a battery core, the battery core comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is located between the positive electrode sheet and the negative electrode sheet, characterized in that: A stress release layer is formed between the positive electrode plate and the negative electrode plate, wherein the material of the stress release layer includes a mixture of ethylene carbonate and / or polyvinylidene fluoride and modified polyacrylic acid.
8. The manufacturing method according to claim 7, characterized in that: The battery roll core has a corner area, and the stress release layer is formed between the negative electrode sheet and the positive electrode sheet in the corner area.
9. The manufacturing method according to claim 8, characterized in that: The width of the stress release layer located in the corner area increases as the number of layers of electrode sheets wound around the battery winding core increases.
10. The manufacturing method according to claim 7, characterized in that: The thickness of the stress release layer is 1 μm to 30 μm.
11. A secondary battery, characterized in that: include: The battery roll core and the housing according to any one of claims 1 to 6, wherein the battery roll core is accommodated in the housing.
Citation Information
Patent Citations
Non-aqueous secondary battery and electrodes for use in same
CN102349186A
Reeling electrical core, preparation technology and lithium ion battery
CN110380136A
Winding battery diaphragm, winding battery and vehicle
CN115117557A
Battery winding core, manufacturing method of battery winding core and secondary battery
CN116487730A
Flexible packaging lithium ion battery with winding structure
CN202585643U