Negative electrode sheet, secondary battery and electrical apparatus

By using graphite negative electrode active material with a smaller specific surface area in the negative electrode sheet, the reaction site of the negative electrode surface destroying the SEI film is reduced, and the problem of poor high-temperature cycling performance and storage performance in lithium manganese iron phosphate system secondary batteries is solved. Achieve more stable battery performance.

WO2024230273A1PCT designated stage expired Publication Date: 2024-11-14CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2024/078372
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2024-02-23
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

In secondary batteries with lithium manganese iron phosphate system, carbon-based negative electrode material leads to deterioration of high-temperature cycling and storage performance, mainly due to the side reaction on the surface of the positive electrode sheet, the destruction of the negative electrode SEI film.

Method used

By using a first graphite negative electrode active material with a smaller specific surface area in the negative electrode sheet, the BET specific surface area of ​​the negative electrode layer is reduced, and the effective site of the negative electrode surface destroying the SEI film reaction is reduced, thereby improving the stability of the SEI film and the battery Cycling performance and storage performance.

Benefits of technology

It effectively improves the high-temperature circulation and storage performance of lithium manganese iron phosphate system secondary batteries, while maintaining the charging capacity, avoiding premature damage to the negative electrode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024078372_14112024_PF_FP_ABST
    Figure CN2024078372_14112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a negative electrode sheet, a secondary battery, and an electrical apparatus. The negative electrode sheet comprises a current collector and a negative electrode film layer arranged on at least one side of the current collector, the negative electrode film layer comprising one or more active substance layers; a negative electrode active material in the negative electrode film layer comprises a first graphite negative electrode active material, the BET specific surface area of the first graphite negative electrode active material being A, the BET specific surface area of the negative electrode active material in the negative electrode film layer being B, and A≤B, or the BET specific surface area of a material forming the negative electrode film layer being B', and A<B'.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode sheet, secondary battery and electrical device

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application No. 202310521970.5, filed on May 10, 2023, entitled “Negative electrode sheet, secondary battery and electrical device,” the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application relates to the field of battery technology, and in particular to a negative electrode plate, a secondary battery, and an electrical device. Background Art

[0004] A lithium secondary battery is composed of a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, a separator, and an electrolyte, and is a secondary battery that realizes charging and discharging by the insertion and deintercalation of lithium ions.

[0005] Lithium metal was primarily used as negative electrode material for lithium secondary batteries in the early days. However, as charge and discharge progress, growth of lithium atoms on the surface of metallic lithium causes damage to the separator, and thus carbon-based materials have been primarily used in recent years.

[0006] Carbon-based anode materials are generally either artificial graphite or natural graphite. Natural graphite is formed from natural graphite ore through natural processes and requires initial purification, shaping, and modification to obtain a graphite anode material that meets the requirements for use. Artificial graphite, on the other hand, requires a high-temperature process exceeding 2500°C to graphitize the soft carbon material, resulting in a graphite anode material with superior surface properties and improved cycle stability. However, the use of carbon-based anode materials in lithium iron manganese phosphate secondary batteries significantly deteriorates their high-temperature cycling and storage performance.

[0007] Summary of the Invention

[0008] The present application provides a negative electrode plate, a secondary battery and an electrical device, which improves the high-temperature cycle problem of a secondary battery of a lithium manganese iron phosphate system while maintaining excellent dynamic performance by utilizing the negative electrode plate.

[0009] In a first aspect, the present application provides a negative electrode plate, comprising a current collector and a negative electrode film layer arranged on at least one side of the current collector, wherein the negative electrode film layer comprises one or more active material layers, the negative electrode active material in the negative electrode film layer comprises a first graphite negative electrode active material, the BET specific surface area of ​​the first graphite negative electrode active material is A, the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer is B, A≤B, or the BET specific surface area of ​​the material forming the negative electrode film layer is B', A<B'.

[0010] A<B or A≤B' in the present application indicates that a first graphite negative electrode active material with a smaller specific surface area is used in the negative electrode film layer to reduce the specific surface area of ​​the negative electrode film layer as a whole, that is, the negative electrode plate of the present application reduces the BET specific surface area of ​​the negative electrode active material of the negative electrode film layer by adopting a first graphite negative electrode active material with a lower BET specific surface area, thereby reducing the effective sites on the negative electrode surface where the SEI film destruction reaction occurs, thereby ensuring the stability of the negative electrode SEI film and improving the cycle performance and storage performance of the battery.

[0011] In any embodiment of the first aspect of the present application, the BET specific surface area of ​​the first graphite negative electrode active material is 0.5 m 2 / g≤A≤1.3m 2 / g; optionally, 0.8m 2 / g≤A≤1.22m 2 When the BET specific surface area of ​​the first graphite negative electrode active material is within the above range, the effective specific surface area of ​​the surface active material layer of the corresponding negative electrode sheet is smaller, thereby more effectively reducing side reactions on the negative electrode surface and improving the long-term stability of the SEI film. By improving the long-term stability of the SEI film, the cycling performance and storage performance of the battery cell can be fully improved, while maintaining a high recharge capacity.

[0012] In any embodiment of the first aspect of the present application, the BET specific surface area of ​​the material forming the negative electrode film layer is 0.55 m 2 / g≤B'≤1.85m 2 / g, optionally 0.89m 2 / g≤B'≤1.42m 2 / g; or the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer is 0.5m 2 / g≤B≤1.8m 2 / g, optionally 0.82m 2 / g≤B≤1.38m 2 / g. This can further reduce the effective sites on the negative electrode surface where the SEI film is destroyed, further improve the stability of the negative electrode SEI film, and thus improve the cycle performance of the battery.

[0013] In any embodiment of the first aspect of the present application, the negative electrode film layer further includes a second graphite negative electrode active material, the BET specific surface area of ​​the second graphite negative electrode active material is C, and A<C, optionally, B<C; optionally, 1.3m 2 / g≤C≤1.95m 2 / g, further optionally, 1.5m 2 / g≤C≤1.81m 2 / g. The second graphite negative electrode active material with a larger BET specific surface area has a correspondingly smaller particle size, thereby improving the charging capacity of the negative electrode film layer. By further defining the BET specific surface area of ​​the second graphite negative electrode active material, the charging capacity of the negative electrode film layer can be maximized while the BET specific surface area of ​​the negative electrode active material can be controlled as much as possible.

[0014] In any embodiment of the first aspect of the present application, the negative electrode film layer includes multiple active material layers, and the first graphite negative electrode active material is arranged in the same active material layer or in different active material layers.

[0015] In any embodiment of the first aspect of the present application, the negative electrode film layer includes multiple active material layers, the active material layer located on the surface is defined as the surface active material layer, the active material layer between the surface active material layer and the current collector is defined as the inner active material layer, the BET specific surface area of ​​the negative electrode active material of the surface active material layer is D, and the BET specific surface area of ​​the negative electrode active material of the inner active material layer is E; optionally, A≤D<B<E; optionally, 0.5m 2 / g≤D≤1.22m 2 / g, optionally 0.82m 2 / g≤D≤1.22m 2 / g, and / or 0.82m 2 / g≤E≤1.81m 2 / g, optionally 0.82m 2 / g≤E≤1.52m 2 / g. This more effectively limits the reaction sites of the negative electrode active material, reduces the probability of SEI film damage, and at the same time maximizes the overall charging capacity of the negative electrode film layer.

[0016] In any embodiment of the first aspect of the present application, the above-mentioned negative electrode film layer includes multiple active material layers, the active material layer located on the surface is defined as the surface active material layer, the active material layer between the surface active material layer and the current collector is defined as the inner active material layer, the BET specific surface area of ​​the material forming the surface active material layer is D', and the BET specific surface area of ​​the material forming the inner active material layer is E'; optionally, D'<B'<E'; optionally, 0.59m 2 / g≤D'≤1.77m 2 / g, further optionally 0.89m 2 / g≤D'≤1.59m 2 / g, and / or 0.59m 2 / g≤E'≤1.87m 2 / g, further optionally 0.89m 2 / g≤E'≤1.87m 2 / g. The BET specific surface area of ​​the material forming the surface active material layer is small, so the reaction sites for the SEI film destruction reaction are reduced; the BET specific surface area of ​​the material of the inner active material layer is relatively large, which is beneficial to improving the charging capacity of the negative electrode.

[0017] In any embodiment of the first aspect of the present application, the mass content of the first graphite negative electrode active material in the surface active material layer is 10% to 98%; and / or the mass content of the second graphite negative electrode active material in the inner active material layer is 10% to 98%. This allows full utilization of the first graphite negative electrode active material to reduce reactive sites that damage the SEI film, and allows the second graphite negative electrode active material to fully improve the charging capacity of the negative electrode sheet.

[0018] In any embodiment of the first aspect of the present application, the inner active material layer may be a single layer structure or a multilayer structure. When it is a multilayer structure, those skilled in the art can set the composition of each layer according to its performance requirements.

[0019] The second aspect of the present application provides a negative electrode plate, comprising a current collector and a negative electrode film layer arranged on at least one side of the current collector, wherein the negative electrode film layer is a single layer, and the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer is 0.5 m 2 / g≤B≤1.8m 2 / g, optionally 0.82m 2 / g≤B≤1.38m 2 / g, or the BET specific surface area of ​​the material forming the negative electrode film layer is 0.55m 2 / g≤B'≤1.85m 2 / g, optionally 0.89m 2 / g≤B'≤1.42m 2 The negative electrode film layer or negative electrode active material of the negative electrode plate of the second aspect of the present application has a smaller BET specific surface area, thereby reducing the effective sites on the negative electrode surface for the reaction that destroys the SEI film, thereby ensuring the stability of the negative electrode SEI film and improving the cycle performance and storage performance of the battery.

[0020] In any embodiment of the second aspect of the present application, the negative electrode active material in the negative electrode film layer includes a first graphite negative electrode active material and optionally a second graphite negative electrode active material. The BET specific surface area of ​​the first graphite negative electrode active material is 0.5 m 2 / g≤A≤1.3m 2 / g; optionally, 0.8m 2 / g≤A≤1.22m 2When the BET specific surface area of ​​the first graphite negative electrode active material is within the above range, the corresponding effective specific surface area of ​​the negative electrode active material is smaller, thereby more effectively reducing side reactions on the negative electrode surface and maintaining the long-term stability of the SEI film. Maintaining the long-term stability of the SEI film can significantly improve the cycling performance and storage performance of the battery cell, while maintaining a high recharge capacity.

[0021] In any embodiment of the second aspect of the present application, the negative electrode active material in the negative electrode film layer includes a second graphite negative electrode active material having a BET specific surface area of ​​C, and A<C, B<C; optionally, 1.3m 2 / g≤C≤1.95m 2 / g, further optionally, 1.5m 2 / g≤C≤1.81m 2 / g. The second graphite negative electrode active material with a larger BET specific surface area has a correspondingly smaller particle size, thereby improving the chargeability of the negative electrode film layer. By further defining the BET specific surface area of ​​the second graphite negative electrode active material, the chargeability of the negative electrode film layer can be maximized while the total BET specific surface area of ​​the negative electrode active material can be minimized.

[0022] A third aspect of the present application provides a negative electrode sheet, comprising a current collector and a negative electrode film layer disposed on at least one side of the current collector, wherein the negative electrode film layer comprises a plurality of active material layers, the active material layer located on the surface is defined as a surface active material layer, the active material layer between the surface active material layer and the current collector is defined as an inner active material layer, the BET specific surface area of ​​the negative electrode active material of the surface active material layer is D', and the BET specific surface area of ​​the negative electrode active material of the inner active material layer is E; optionally, D<E; optionally, 0.5m 2 / g≤D≤1.22m 2 / g, optionally 0.82m 2 / g≤D≤1.22m 2 / g, and / or 0.82m 2 / g≤E≤1.81m 2 / g, optionally 0.82m 2 / g≤E≤1.52m 2 / g; or the BET specific surface area of ​​the material forming the surface active material layer is D', and the BET specific surface area of ​​the material forming the inner active material layer is E'; optionally, D'<E'; optionally, 0.59m 2 / g≤D'≤1.77m 2 / g, further optionally 0.89m 2 / g≤D'≤1.59m 2 / g, and / or 0.59m 2 / g≤E'≤1.87m2 / g, further optionally 0.89m 2 / g≤E'≤1.87m 2 / g.

[0023] The negative electrode plate of the third aspect of the present application reduces the effective sites on the negative electrode surface where the SEI film destruction reaction occurs by reducing the BET specific surface area of ​​the negative electrode active material on the surface of the negative electrode film layer or reducing the BET specific surface area of ​​the active material layer on the surface of the negative electrode film layer, thereby ensuring the stability of the negative electrode SEI film and improving the cycle performance and storage performance of the battery.

[0024] In any embodiment of the third aspect of the present application, the negative electrode active material in the negative electrode film layer includes a first graphite negative electrode active material, the BET specific surface area of ​​the first graphite negative electrode active material is A, the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer is B, and A≤D≤B≤E. The first graphite negative electrode active material with a smaller specific surface area is used in the negative electrode film layer to reduce the BET specific surface area of ​​the negative electrode active material and the BET specific surface area of ​​the surface active material layer, thereby more reliably reducing the effective sites on the negative electrode surface where reactions that damage the SEI film occur.

[0025] In any embodiment of the third aspect of the present application, the BET specific surface area of ​​the first graphite negative electrode active material is 0.5 m 2 / g≤A≤1.3m 2 / g; optionally, 0.8m 2 / g≤A≤1.22m 2 When the BET specific surface area of ​​the first graphite negative electrode active material is within the above range, the effective specific surface area of ​​the surface active material layer of the corresponding negative electrode sheet is smaller, thereby more effectively reducing side reactions on the negative electrode surface and maintaining the long-term stability of the SEI film. While maintaining the long-term stability of the SEI film, the cycling and storage performance of the battery cell can be fully improved, while maintaining a high recharge capacity.

[0026] In any embodiment of the third aspect of the present application, the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer is 0.5 m 2 / g≤B≤1.8m 2 / g, optionally 0.82m 2 / g≤B≤1.38m 2 / g. This further reduces the effective sites on the negative electrode surface where the SEI film is destroyed, further improving the stability of the negative electrode SEI film, thereby improving the cycle performance and storage performance of the battery.

[0027] In any embodiment of the third aspect of the present application, the negative electrode film layer further includes a second graphite negative electrode active material, the BET specific surface area of ​​the second graphite negative electrode active material is C, and A<C, B<C; optionally, 1.3m 2 / g≤C≤1.95m 2 / g, further optionally, 1.5m 2 / g≤C≤1.81m 2 / g. The second graphite negative electrode active material with a larger BET specific surface area has a correspondingly smaller particle size, thereby improving the charging capacity of the negative electrode film layer. By further defining the BET specific surface area of ​​the second graphite negative electrode active material, the charging capacity of the negative electrode film layer can be maximized while the BET specific surface area of ​​the negative electrode active material can be controlled as much as possible.

[0028] In any embodiment of the third aspect of the present application, the mass content of the first graphite negative electrode active material in the surface active material layer is 10% to 98%; and / or the mass content of the second graphite negative electrode active material in the inner active material layer is 10% to 98%. This allows full utilization of the first graphite negative electrode active material to reduce reactive sites that damage the SEI film, and allows the second graphite negative electrode active material to fully improve the chargeability of the negative electrode sheet.

[0029] In any embodiment of the first, second, and third aspects of the present application, the mass ratio of the first graphite negative electrode active material to the second graphite negative electrode active material is between 1:9 and 9:1, and optionally between 5:5 and 8:2. Properly increasing the mass ratio of the first graphite negative electrode active material helps reduce the number of active sites for SEI film destruction reactions in the negative electrode sheet, thereby further improving the cycle performance and storage capacity of the battery.

[0030] In any embodiment of the first aspect, the second aspect and the third aspect of the present application, D of the first graphite negative electrode active material v 50 is between 10 μm and 25 μm, and optionally between 15 μm and 22 μm. In some embodiments, the D of the second graphite negative active material is v 50 is between 7 μm and 10 μm, and optionally between 8 μm and 10 μm. The BET specific surface area of ​​the graphite negative electrode active material is further controlled.

[0031] In any embodiment of the first, second and third aspects of the present application, the first graphite negative electrode active material and the second graphite negative electrode active material each independently include any one or more of natural graphite, artificial graphite, graphitized carbon fiber and graphitized mesophase carbon microbeads.

[0032] In any embodiment of the first, second, and third aspects of the present application, the negative electrode plate is a negative electrode plate for a secondary battery, and when the secondary battery is charged, the full battery voltage reaches an upper limit voltage before the potential of the negative electrode in the full battery reaches 0 mV. Optionally, the positive electrode active material of the secondary battery includes a lithium iron manganese phosphate-based positive electrode active material. While improving the cycling performance and storage performance of the secondary battery, its charging capacity is maintained.

[0033] A fourth aspect of the present application provides a secondary battery, the secondary battery comprising a positive electrode sheet and a negative electrode sheet. The negative electrode sheet of the secondary battery of the present application comprises any one of the negative electrode sheets in the above-mentioned embodiments of the present application.

[0034] In any embodiment of the fourth aspect of the present application, the secondary battery of the present application is a secondary battery of a lithium iron manganese phosphate system, and the positive electrode plate includes a positive electrode active material, and the positive electrode active material includes a lithium iron manganese phosphate-based positive electrode active material. Optionally, the lithium iron manganese phosphate-based positive electrode active material includes a doped lithium iron manganese phosphate-based positive electrode active material or a coated lithium iron manganese phosphate-based positive electrode active material. Optionally, the lithium iron manganese phosphate-based positive electrode active material includes Li element, P element, Fe element and M element, and the M element includes Mn and non-Mn elements.

[0035] In any embodiment of the fourth aspect of the present application, the non-Mn element is set to include one or both of a first doping element and a second doping element, the first doping element is manganese doping, and the second doping element is phosphorus doping; optionally, the first doping element includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge; further optionally, the first doping element includes at least two elements selected from the group consisting of Fe, Ti, V, Ni, Co and Mg; optionally, the second doping element includes one or more elements selected from the group consisting of B (boron), S, Si and N. This further improves the composition stability of the positive electrode material and reduces positive electrode side reactions.

[0036] In any embodiment of the fourth aspect of the present application, the above-mentioned lithium iron manganese phosphate system positive electrode active material includes at least one of the following materials: LiMn 1-y Fe y PO4, y is any value in the range of 0.001 to 0.5; Li 1+t Mn 1- c Fe c P 1-z R zO4, t is any value in the range of -0.100 to 0.100, c is any value in the range of 0.001 to 0.500, z is any value in the range of 0.001 to 0.100, and R includes one or more elements selected from B, S, Si and N; Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n , wherein A comprises one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo, and W, E comprises one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, R comprises one or more elements selected from the group consisting of B, S, Si, and N, D comprises one or more elements selected from the group consisting of S, F, Cl, and Br, w is any value within the range of -0.100 to 0.100, m is any value within the range of 0.001 to 0.1, u is any value within the range of 0.001 to 0.500, a is any value within the range of 0.001 to 0.100, n is any value within the range of 0.001 to 0.1, and Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n Doping elements in lithium manganese iron phosphate helps to improve the structural stability of the lithium manganese iron phosphate positive electrode material and the rate performance of the secondary battery having it.

[0037] A fifth aspect of the present application provides an electrical device, which includes a secondary battery. The secondary battery includes any one of the above-mentioned secondary batteries and has better cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.

[0039] FIG1 is a schematic diagram of a secondary battery cell according to an embodiment of the present application.

[0040] FIG. 2 is an exploded view of the secondary battery cell according to the embodiment of the present application shown in FIG. 1 .

[0041] FIG3 is a schematic diagram of a battery module according to an embodiment of the present application.

[0042] FIG4 is a schematic diagram of a battery pack according to an embodiment of the present application.

[0043] FIG. 5 is an exploded view of the battery pack shown in FIG. 4 according to an embodiment of the present application.

[0044] FIG6 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.

[0045] In the drawings, the drawings are not drawn to scale.

[0046] Explanation of reference numerals: 1 battery pack; 2 upper case; 3 lower case; 4 battery module; 5 secondary battery cell; 51 housing; 52 electrode assembly; 53 top cover assembly. DETAILED DESCRIPTION

[0047] The following detailed description of the embodiments of the present application is provided in conjunction with the accompanying drawings and examples. The following detailed description of the embodiments and the accompanying drawings are used to illustrate the principles of the present application, but are not intended to limit the scope of the present application, that is, the present application is not limited to the described embodiments.

[0048] Below, the embodiments of the negative electrode sheet, secondary battery, and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0049] The "ranges" disclosed in this application are defined in the form of lower limits and upper limits, where a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. Ranges defined in this manner can be inclusive or exclusive of the end values ​​and can be combined arbitrarily, i.e., any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60 to 120 and 80 to 110 are listed for a particular parameter, it is understood that ranges of 60 to 110 and 80 to 120 are also contemplated. In addition, if the minimum range values ​​listed are 1 and 2, and if the maximum range values ​​listed are 3, 4, and 5, the following ranges are all contemplated: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4, and 2 to 5. In this application, unless otherwise specified, the numerical range "a to b" is a shorthand representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0050] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0051] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0052] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0053] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0054] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0055] [Negative electrode]

[0056] Graphite is commonly used as the negative electrode in existing lithium-ion batteries. During the charge and discharge process, graphite primarily inserts and extracts lithium ions. In lithium iron manganese phosphate (LIMnPO4)-based secondary batteries (i.e., secondary batteries whose positive electrode active material is LIMNP-based), side reactions continuously occur on the surface of the positive electrode during charge and discharge, as well as during high SOC storage. The resulting free radicals and other substances diffuse with the electrolyte to the negative electrode, continuously damaging the SEI film on the negative electrode surface. Consequently, using this type of negative electrode material in LIMNP-based secondary batteries significantly degrades their high-temperature cycling and storage performance.

[0057] In order to solve this problem, those skilled in the art have found that the root cause of the destruction of the SEI film on the surface of the negative electrode is the side reactions that continue to occur on the surface of the positive electrode. Therefore, they usually try to modify the positive electrode active material, such as by doping elements to improve structural stability or by coating to reduce the occurrence of side reactions, or by improving the electrolyte to reduce side reactions such as adding new additives thereto. However, the above-mentioned improvement route is technically complex and will also have a collateral impact on other battery properties. This application breaks the convention and attempts to improve the negative electrode sheet, reduce the active sites on the negative electrode surface, and thereby slow down the progress of destroying the SEI film on the negative electrode surface. Based on the above attempts and studies, the first embodiment of the present application provides a negative electrode plate, comprising a current collector and a negative electrode film layer arranged on at least one side of the current collector, wherein the negative electrode film layer comprises one or more active material layers, the negative electrode active material of the negative electrode film layer comprises a first graphite negative electrode active material, the BET specific surface area of ​​the first graphite negative electrode active material is A, the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer is B, A≤B, or the BET specific surface area of ​​the material forming the negative electrode film layer is B', A<B'.

[0058] The materials that form the negative electrode film layer include not only the negative electrode active material, but also typically include components such as a conductive agent and a binder. Although the BET specific surface area of ​​the material that forms the negative electrode film layer cannot be completely equal to the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer, there is a clear correlation between the two. Because the negative electrode active material occupies the vast majority of the weight of the negative electrode film layer, when the BET specific surface area of ​​the negative electrode active material is small, the corresponding BET specific surface area of ​​the material that forms the negative electrode film layer is also small. In other words, when the BET specific surface area of ​​the material that forms the negative electrode film layer is small, the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer is also small.

[0059] A<B' or A≤B of the negative electrode plate of the present application indicates that a first graphite negative electrode active material with a smaller specific surface area is used in the negative electrode film layer to reduce the BET specific surface area of ​​the entire negative electrode film layer or the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer. That is, the negative electrode plate of the present application reduces the effective sites on the negative electrode surface where the SEI film destruction reaction occurs by adopting a first graphite negative electrode active material with a lower BET specific surface area, thereby ensuring the stability of the negative electrode SEI film and improving the cycle performance and storage performance of the battery.

[0060] Method for testing the BET specific surface area of ​​the material forming the negative electrode film layer: scrape the negative electrode film layer off the electrode sheet and then test it according to GB / T 19587-2017 / ISO 9277:2010.

[0061] Method for determining the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer: After scraping the negative electrode film layer from the electrode sheet, disperse it in N-methylpyrrolidone, and then separate the solid and liquid and dry it to obtain the negative electrode active material. Refer to GB / T 19587-2017 / ISO 9277:2010 to test the BET specific surface area of ​​the negative electrode active material.

[0062] The above-mentioned negative electrode plate is applied to the lithium iron phosphate battery system and the ternary battery system, which will reduce the charging capacity of the battery cell. However, when the above-mentioned negative electrode plate is applied to the secondary battery of the lithium iron manganese phosphate system, it can not only effectively improve the high-temperature cycle performance and storage performance of the secondary battery of the lithium iron manganese phosphate system, but also will not affect the charging capacity of the battery cell, so that the secondary battery of the lithium iron manganese phosphate system maintains excellent dynamic performance.

[0063] The applicant is not clear about the mechanism that produces the above-mentioned difference. It is speculated that the charging capacity of lithium iron phosphate and ternary systems is often limited by the negative electrode. This is because the potential of the negative electrode in the full battery reaches 0mV before the full battery voltage reaches the upper limit voltage during charging. In secondary batteries based on lithium iron manganese phosphate systems, due to the large polarization of the lithium iron manganese phosphate-based positive electrode material, the charging capacity of the battery cell in the high SOC region is limited by the positive electrode rather than the negative electrode. Therefore, before the negative electrode reaches 0mV, the secondary battery has already reached the upper limit voltage. Therefore, using a graphite negative electrode active material with a smaller BET specific surface area in the negative electrode plate of a secondary battery based on lithium iron manganese phosphate system does not deteriorate the battery's charging capacity.

[0064] The negative electrode plate can include a negative electrode film layer arranged on one side of the current collector, or it can include negative electrode film layers arranged on both sides of the current collector. When negative electrode film layers are arranged on both sides of the current collector, the two negative electrode film layers are arranged independently of each other. The schemes in the following embodiments of this application can be applied to the negative electrode film layer on either side.

[0065] In some embodiments of the present application, the above 0.5m 2 / g≤A≤1.3m 2 / g, for example, 0.5m 2 / g, 0.53m 2 / g, 0.8m 2 / g, 0.82m 2 / g、1m 2 / g, 1.03m 2 / g, 1.5m 2 / g or 1.3m 2 / g; optionally, 0.8m 2 / g ≤A≤1.22m 2 When the BET specific surface area of ​​the first graphite negative electrode active material is within the above range, the effective specific surface area of ​​the surface active material layer of the corresponding negative electrode sheet is smaller, which can more effectively reduce side reactions on the negative electrode surface and improve the long-term stability of the SEI film. By improving the long-term stability of the SEI film, the cycling performance and storage performance of the battery cell can be fully improved, while maintaining a high recharge capacity.

[0066] In some embodiments of the present application, the BET specific surface area of ​​the material forming the negative electrode film layer is 0.55 m 2 / g≤B'≤1.85m 2 / g, for example 0.55m 2 / g, 0.59m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.89m 2 / g, 1.0m2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.25m 2 / g, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g, 1.8m 2 / g or 1.85m 2 / g, optionally 0.89m 2 / g≤B'≤1.42m 2 By controlling the above specific surface area, the effective sites on the negative electrode surface where the SEI film is destroyed are reduced, thereby improving the stability of the negative electrode SEI film and thus improving the cycle performance of the battery.

[0067] In some embodiments of the present application, the BET specific surface area of ​​the negative electrode active material of the negative electrode film layer is 0.5 m 2 / g≤B≤1.8m 2 / g, for example, 0.5m 2 / g, 0.52m 2 / g, 0.8m 2 / g, 0.82m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.25m 2 / g, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g or 1.8m 2 / g, optionally 0.82m 2 / g≤B≤1.38m 2 By controlling the above specific surface area, the effective sites on the negative electrode surface where the SEI film is destroyed are reduced, thereby improving the stability of the negative electrode SEI film and thus improving the cycle performance of the battery.

[0068] In some embodiments of the present application, the negative electrode film layer further includes a second graphite negative electrode active material, the BET specific surface area of ​​the second graphite negative electrode active material is C, and A<C, optionally, B<C; optionally, 1.3m 2 / g≤C≤1.95m 2 / g, for example, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g, 1.8m 2 / g, 1.85m 2 / g, 1.9m 2 / g or 1.95m 2 / g, further optionally, 1.5m 2 / g≤C≤1.81m 2 / g. The second graphite negative electrode active material with a larger BET specific surface area has a correspondingly smaller particle size, thereby improving the charging capacity of the negative electrode film layer. By further defining the BET specific surface area of ​​the second graphite negative electrode active material, the charging capacity of the negative electrode film layer can be maximized while the BET specific surface area of ​​the negative electrode active material can be controlled as much as possible.

[0069] Graphite negative electrode active materials having two different BET specific surface areas are selected and mixed to form the first graphite negative electrode active material and the second graphite negative electrode active material in some embodiments of the present application, so that the BET specific surface areas of the first graphite negative electrode active material and the second graphite negative electrode active material can be adjusted more flexibly.

[0070] The negative electrode film layer of the present application includes a layer of active material layer or multiple layers of active material layer. When there is a layer of active material layer, the negative electrode active material of the active material layer is a first graphite negative electrode active material, in which case A=B; or the active material layer is a combination of a first graphite negative electrode active material and a second graphite negative electrode active material, or also includes other negative electrode active materials, in which case A<B.

[0071] In some embodiments, the negative electrode film layer includes multiple active material layers, and the first graphite negative electrode active material is disposed in the same active material layer or in different active material layers. Taking the negative electrode film layer on one side as an example, for example, the negative electrode active material of the active material layer close to the current collector is a mixture of the first graphite negative electrode active material and the second graphite negative electrode active material, and the negative electrode active material of the active material layer located above it is the first graphite negative electrode active material or the second graphite negative electrode active material; or the negative electrode active material of the active material layer close to the current collector is the first graphite negative electrode active material or the second graphite negative electrode active material, and the negative electrode active material of the active material layer located above it is a mixture of the first graphite negative electrode active material and the second graphite negative electrode active material; or both active material layers contain the first graphite negative electrode active material and the second graphite negative electrode active material, in which case the ratios of the two can be set to different to form different active material layers. When the first graphite negative electrode active material and the second graphite negative electrode active material are both included in the same active material layer, there is no special restriction on the ratio of the two.

[0072] Since the reaction to the destruction of the negative electrode SEI film usually starts from the surface of the negative electrode film layer, in order to further limit the occurrence of the reaction to the destruction of the SEI film, the effective specific surface area of ​​the surface of the negative electrode film layer is further controlled. In some embodiments, the negative electrode film layer includes a multilayer active material layer, the active material layer located on the surface is defined as the surface active material layer, the active material layer between the surface active material layer and the current collector is defined as the inner active material layer, the BET specific surface area of ​​the negative electrode active material in the surface active material layer is D, and the BET specific surface area of ​​the negative electrode active material in the inner active material layer is E; optionally, A≤D<B<E; optionally, 0.5m 2 / g≤D≤1.22m 2 / g, for example, 0.5m 2 / g, 0.55m 2 / g, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.89m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g or 1.22m 2 / g, optionally 0.82m 2 / g≤D≤1.22m 2 / g, and / or 0.82m 2 / g≤E≤1.81m 2 / g, for example, 0.82m 2 / g, 0.9m 2 / g, 0.95m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.25m 2 / g, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.45m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g or 1.8m 2 / g, optionally 0.82m 2 / g≤E≤1.52m 2 / g. This effectively increases the probability of limiting the occurrence of SEI film destruction reactions and at the same time maximizes the overall charging capacity of the negative electrode film layer.

[0073] Method for determining the BET specific surface area of ​​the negative electrode active material of the surface active material layer and the BET specific surface area of ​​the negative electrode active material of the inner active material layer:

[0074] The surface active material layer and the inner active material layer were scraped off from the electrode in sequence, dispersed in N-methylpyrrolidone, and then solid-liquid separated and dried to obtain the negative electrode active material. The BET specific surface area of ​​each was tested with reference to GB / T 19587-2017 / ISO9277:2010.

[0075] In some embodiments, the negative electrode film layer includes multiple active material layers, the active material layer located on the surface is defined as the surface active material layer, the active material layer between the surface active material layer and the current collector is defined as the inner active material layer, the BET specific surface area of ​​the material forming the surface active material layer is D', and the BET specific surface area of ​​the material forming the inner active material layer is E'; optionally, D'<B'<E'; optionally, 0.59m 2 / g≤D'≤1.77m 2 / g, for example, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.82m 2 / g, 0.9m 2 / g, 0.95m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.25m 2 / g, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.45m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g or 1.77m 2 / g, further optionally 0.89m 2 / g≤D'≤1.59m 2 / g, and / or 0.59m 2 / g≤E'≤1.87m 2 / g, for example, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.82m 2 / g, 0.9m 2 / g, 0.95m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.25m 2 / g, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.45m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g, 1.77m 2 / g, 1.8m 2 / g, 1.85m 2 / g or 1.87m 2 / g, further optionally 0.89m 2 / g≤E'≤1.87m 2 / g. The BET specific surface area of ​​the material forming the surface active material layer is small, so the reaction sites for the SEI film destruction reaction are reduced; the BET specific surface area of ​​the material of the inner active material layer is relatively large, which is beneficial to improving the charging capacity of the negative electrode.

[0076] In some embodiments, the active material in the surface active material layer is composed of the first graphite negative electrode active material or the first graphite negative electrode active material and the second graphite negative electrode active material. In some embodiments, the thickness of the surface active material layer is set to 40 μm to 120 μm.

[0077] In some embodiments, to maximize the overall performance of the battery, the mass content of the first graphite negative electrode active material in the surface active material layer is 10% to 98%; and / or the mass content of the second graphite negative electrode active material in the inner active material layer is 10% to 98%. This fully utilizes the first graphite negative electrode active material to reduce the reactive sites that damage the SEI film, and utilizes the second graphite negative electrode active material to fully improve the charging capacity of the negative electrode sheet. To further maximize the above effects, in some embodiments, the mass content of the first graphite negative electrode active material in the surface active material layer is 50% to 98%; the mass content of the second graphite negative electrode active material in the inner active material layer is 50% to 98%.

[0078] In some embodiments, the inner active material layer may be a single layer structure or a multilayer structure. When it is a multilayer structure, those skilled in the art can set the composition of each layer according to its performance requirements.

[0079] In order to solve the above technical problems, the second embodiment of the present application provides a negative electrode sheet, including a current collector and a negative electrode film layer arranged on at least one side of the current collector, wherein the negative electrode film layer is a single layer, and the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer is 0.5m 2 / g≤B≤1.8m 2 / g, for example, 0.5m 2 / g, 0.52m 2 / g, 0.8m 2 / g, 0.82m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.25m 2 / g, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g or 1.8m 2 / g, optionally 0.82m 2 / g≤B≤1.38m 2 / g, or the BET specific surface area of ​​the material forming the negative electrode film layer is 0.55m 2 / g≤B'≤1.85m 2 / g, for example 0.55m 2 / g, 0.59m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.89m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.25m 2 / g, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g, 1.8m 2 / g or 1.85m 2 / g, optionally 0.89m 2 / g≤B'≤1.42m 2 / g.

[0080] Based on the same principle as above, the negative electrode film layer or the negative electrode active material of the negative electrode plate respectively has the above-mentioned smaller BET specific surface area, thereby reducing the effective sites on the negative electrode surface where the SEI film destruction reaction occurs, thereby ensuring the stability of the negative electrode SEI film and improving the cycle performance and storage performance of the battery.

[0081] In some embodiments, the negative electrode active material in the negative electrode film layer includes a first graphite negative electrode active material and optionally a second graphite negative electrode active material. The BET specific surface area of ​​the first graphite negative electrode active material is 0.5 m 2 / g≤A≤1.3m 2 / g; optionally, 0.8m 2 / g≤A≤1.22m 2 When the BET specific surface area of ​​the first graphite negative electrode active material is within the above range, the corresponding effective specific surface area of ​​the negative electrode active material is smaller, thereby more effectively reducing side reactions on the negative electrode surface and maintaining the long-term stability of the SEI film. Maintaining the long-term stability of the SEI film can significantly improve the cycling performance and storage performance of the battery cell, while maintaining a high recharge capacity.

[0082] In some embodiments, the negative electrode active material in the negative electrode film layer includes a second graphite negative electrode active material having a BET specific surface area of ​​C, and A<C, B<C; optionally, 1.3 m 2 / g≤C≤1.95m 2 / g, for example, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g, 1.8m 2 / g, 1.85m 2 / g, 1.9m 2 / g or 1.95m 2 / g, further optionally, 1.5m 2 / g≤C≤1.81m 2 / g. The second graphite negative electrode active material with a larger BET specific surface area has a correspondingly smaller particle size, thereby improving the chargeability of the negative electrode film layer. By further defining the BET specific surface area of ​​the second graphite negative electrode active material, the chargeability of the negative electrode film layer can be maximized while the total BET specific surface area of ​​the negative electrode active material can be minimized.

[0083] In order to solve the above technical problems, the third embodiment of the present application provides a negative electrode plate, including a current collector and a negative electrode film layer arranged on at least one side of the current collector, wherein the negative electrode film layer includes a plurality of active material layers, the active material layer located on the surface is defined as the surface active material layer, the active material layer between the surface active material layer and the current collector is defined as the inner active material layer, the BET specific surface area of ​​the negative electrode active material of the surface active material layer is D, and the BET specific surface area of ​​the negative electrode active material of the inner active material layer is E; optionally, D<E; optionally, 0.5m 2 / g≤D≤1.22m 2 / g, for example, 0.5m 2 / g, 0.55m 2 / g, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.89m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g or 1.22m 2 / g, optionally 0.82m 2 / g≤D≤1.22m2 / g, and / or 0.82m 2 / g≤E≤1.81m 2 / g, for example, 0.82m 2 / g, 0.9m 2 / g, 0.95m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.25m 2 / g, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.45m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g or 1.8m 2 / g, optionally 0.82m 2 / g≤E≤1.52m 2 / g; or the BET specific surface area of ​​the material forming the surface active material layer is D', and the BET specific surface area of ​​the material forming the inner active material layer is E'; optionally, D'<E'; optionally, 0.59m 2 / g≤D'≤1.77m 2 / g, for example 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.82m 2 / g, 0.9m 2 / g, 0.95m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.25m 2 / g, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.45m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g or 1.77m 2 / g, further optionally 0.89m2 / g≤D'≤1.59m 2 / g, and / or 0.59m 2 / g≤E'≤1.87m 2 / g, for example 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.82m 2 / g, 0.9m 2 / g, 0.95m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.25m 2 / g, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.45m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g, 1.77m 2 / g, 1.8m 2 / g, 1.85m 2 / g or 1.87m 2 / g, further optionally 0.89m 2 / g≤E'≤1.87m 2 / g.

[0084] The above-mentioned negative electrode plate reduces the BET specific surface area of ​​the negative electrode active material on the surface of the negative electrode film layer or reduces the BET specific surface area of ​​the active material layer on the surface of the negative electrode film layer, thereby reducing the effective sites on the negative electrode surface where the SEI film destruction reaction occurs, thereby ensuring the stability of the negative electrode SEI film and improving the cycle performance and storage performance of the battery.

[0085] In some embodiments, the negative electrode active material in the negative electrode film layer includes a first graphite negative electrode active material, the first graphite negative electrode active material has a BET specific surface area of ​​A, and the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer is B, where A≤D≤B≤E. The use of the first graphite negative electrode active material with a smaller specific surface area in the negative electrode film layer reduces the BET specific surface area of ​​the negative electrode active material and the BET specific surface area of ​​the surface active material layer, thereby more reliably reducing the effective sites on the negative electrode surface where reactions that damage the SEI film occur. Alternatively, the first graphite negative electrode material may be disposed at least in the surface active material layer to better control the BET specific surface area of ​​the negative electrode active material in the surface active material layer, achieving A≤D.

[0086] In some embodiments, the BET specific surface area of ​​the first graphite negative electrode active material is 0.5 m 2 / g≤A≤1.3m 2 / g, for example, 0.5m 2 / g, 0.53m 2 / g, 0.8m 2 / g, 0.82m 2 / g、1m 2 / g, 1.03m 2 / g, 1.5m 2 / g or 1.3m 2 / g; optionally, 0.8m 2 / g≤A≤1.22m 2 When the BET specific surface area of ​​the first graphite negative electrode active material is within the above range, the effective specific surface area of ​​the surface active material layer of the corresponding negative electrode sheet is smaller, thereby more effectively reducing side reactions on the negative electrode surface and maintaining the long-term stability of the SEI film. While maintaining the long-term stability of the SEI film, the cycling and storage performance of the battery cell can be fully improved, while maintaining a high recharge capacity.

[0087] In some embodiments, the BET specific surface area of ​​the negative electrode active material in the negative electrode film is 0.5 m 2 / g≤B≤1.8m 2 / g, for example, 0.5m 2 / g, 0.52m 2 / g, 0.8m 2 / g, 0.82m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.25m 2 / g, 1.3m 2 / g, 1.35m2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6 m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g or 1.8m 2 / g, optionally 0.82m 2 / g≤B≤1.38m 2 / g. This further reduces the effective sites on the negative electrode surface where the SEI film is destroyed, further improving the stability of the negative electrode SEI film, thereby improving the cycle performance and storage performance of the battery.

[0088] In some embodiments, the negative electrode film layer further comprises a second graphite negative electrode active material, the BET specific surface area of ​​the second graphite negative electrode active material is C, and A<C, B<C; optionally, 1.3m 2 / g≤C≤1.95m 2 / g, for example, 1.3m 2 / g, 1.35m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.65m 2 / g, 1.7m 2 / g, 1.75m 2 / g, 1.8m 2 / g, 1.85m 2 / g, 1.9m 2 / g or 1.95m 2 / g, further optionally, 1.5m 2 / g≤C≤1.81m 2 / g. The second graphite negative electrode active material with a larger BET specific surface area has a correspondingly smaller particle size, thereby improving the charging capacity of the negative electrode film layer. By further defining the BET specific surface area of ​​the second graphite negative electrode active material, the charging capacity of the negative electrode film layer can be maximized while the BET specific surface area of ​​the negative electrode active material can be controlled as much as possible.

[0089] The second graphite negative electrode active material can be mixed with the first graphite negative electrode active material and disposed together in the surface active material layer, or it can be disposed only in the inner active material layer. In some embodiments, the mass content of the first graphite negative electrode active material in the surface active material layer is 10% to 98%; and / or the mass content of the second graphite negative electrode active material in the inner active material layer is 10% to 98%. This fully utilizes the first graphite negative electrode active material to reduce the reactive sites that damage the SEI film, and utilizes the second graphite negative electrode active material to fully improve the charging capacity of the negative electrode sheet. To further enhance the above effects, in some embodiments, the mass content of the first graphite negative electrode active material in the surface active material layer is 50% to 98%, and the mass content of the second graphite negative electrode active material in the inner active material layer is 50% to 98%.

[0090] The first graphite negative electrode active material and the second graphite negative electrode active material have different masses, and the resulting mixture has different BET specific surface areas, and thus the corresponding active site areas are also different. In some embodiments, the mass ratio of the first graphite negative electrode active material to the second graphite negative electrode active material is between 1:9 and 9:1, and optionally between 5:5 and 8:2. Appropriately increasing the mass ratio of the first graphite negative electrode active material is beneficial to reducing the number of active sites, thereby further improving the cycle performance and storage capacity of the battery.

[0091] In some embodiments, the D of the first graphite negative electrode active material is v 50 is between 10 μm and 25 μm, and optionally between 15 μm and 22 μm. In some embodiments, the D of the second graphite negative active material is v 50 is between 7 μm and 10 μm, and optionally between 8 μm and 10 μm. The BET specific surface area of ​​the graphite negative electrode active material is further controlled.

[0092] The sources of the graphite negative electrode active materials used in the present application are not particularly limited. In some embodiments, the first graphite negative electrode active material and the second graphite negative electrode active material independently include any one or more of the group consisting of natural graphite, artificial graphite, graphitized carbon fiber and graphitized mesophase carbon microbeads.

[0093] In some embodiments, the above-mentioned negative electrode plate is a negative electrode plate for a secondary battery. When the secondary battery is charged, the full battery voltage reaches the upper limit voltage before the potential of the anode in the full battery reaches 0mv. Optionally, the positive electrode active material of the secondary battery includes a lithium iron manganese phosphate-based positive electrode active material, thereby improving the cycle performance and storage performance of the secondary battery while maintaining its charging capacity unaffected.

[0094] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0095] In some embodiments, the negative electrode active material in the negative electrode film layer may also include silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0096] In some embodiments, the negative electrode film layer may further include a binder. For example, the binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0097] In some embodiments, the negative electrode film layer may further include a conductive agent. For example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0098] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0099] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0100] [Secondary battery]

[0101] Secondary batteries, also known as rechargeable batteries or storage batteries, are batteries that can be recharged to activate the active materials after discharge and continue to be used.

[0102] Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte. During the battery's charge and discharge process, active ions (such as lithium ions) are embedded and released back and forth between the positive and negative electrode sheets. The separator is set between the positive and negative electrode sheets, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The electrolyte between the positive and negative electrode sheets mainly plays the role of conducting active ions.

[0103] The negative electrode sheet of the secondary battery of the present application includes any one of the negative electrode sheets in the above-mentioned embodiments of the present application.

[0104] The positive electrode sheet generally includes a positive electrode current collector and a positive electrode film layer disposed on at least one side of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.

[0105] As an example, the positive electrode current collector has two opposite sides in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite sides of the positive electrode current collector.

[0106] In some embodiments, the secondary battery of the present application is a lithium manganese iron phosphate system secondary battery, the positive electrode plate includes a positive electrode active material, the positive electrode active material includes a lithium manganese iron phosphate system positive electrode active material, and M includes Mn and non-Mn elements.

[0107] In some embodiments, to further improve the cycle performance of the secondary battery, the non-Mn element is set to include one or both of a first doping element and a second doping element, the first doping element is manganese doping, and the second doping element is phosphorus doping; optionally, the first doping element includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge; further optionally, the first doping element includes at least two elements selected from the group consisting of Fe, Ti, V, Ni, Co, and Mg; optionally, the second doping element includes one or more elements selected from the group consisting of B (boron), S, Si, and N. This further improves the compositional stability of the positive electrode material and reduces positive electrode side reactions.

[0108] In some embodiments, the above-mentioned lithium iron manganese phosphate system positive electrode active material includes but is not limited to a doped lithium iron manganese phosphate system positive electrode active material and a coated lithium iron manganese phosphate system positive electrode active material. In some embodiments, the lithium iron manganese phosphate system positive electrode active material includes at least one of the following materials:

[0109] LiMn 1-y Fe y PO4,y is any value in the range of 0.001 to 0.5;

[0110] Li 1+t Mn 1-c Fe c P 1-z R z O4, t is any value in the range of -0.100 to 0.100, c is any value in the range of 0.001 to 0.500, z is any value in the range of 0.001 to 0.100, and R includes one or more elements selected from B, S, Si and N;

[0111] Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n , wherein A comprises one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo, and W, E comprises one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, R comprises one or more elements selected from the group consisting of B, S, Si, and N, D comprises one or more elements selected from the group consisting of S, F, Cl, and Br, w is any value within the range of -0.100 to 0.100, m is any value within the range of 0.001 to 0.1, u is any value within the range of 0.001 to 0.500, a is any value within the range of 0.001 to 0.100, n is any value within the range of 0.001 to 0.1, and Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n Doping elements in lithium manganese iron phosphate helps to improve the structural stability of the lithium manganese iron phosphate positive electrode material and the rate performance of the secondary battery having it.

[0112] Doping element A at the manganese position of lithium manganese phosphate helps reduce the lattice change rate of lithium manganese phosphate during lithium insertion and extraction, improving the structural stability of the lithium manganese phosphate cathode material, significantly reducing manganese dissolution and reducing oxygen activity on the particle surface. Doping element R at the phosphorus position helps change the difficulty of the Mn-O bond length change, thereby reducing the lithium ion migration barrier, promoting lithium ion migration, and improving the rate performance of the secondary battery.

[0113] Doping at the P and O sites also affects the Mn dissolution and kinetic properties of antisite defects. Therefore, doping reduces the concentration of antisite defects in the material, improves the kinetic properties and gram capacity of the material, and can also change the morphology of the particles, thereby increasing the compaction density. In summary, by doping specific elements at the Li, Mn, P and O sites of the compound LiMnPO4 at specific amounts at the same time, significantly improved rate performance can be obtained, while significantly reducing the dissolution of Mn and Mn-site doping elements, obtaining significantly improved cycle performance and / or high temperature stability, and the gram capacity and compaction density of the material can also be improved.

[0114] The M in the cathode material LiMPO4 designed in this scheme may include Mn and Fe elements. As a possible implementation method, LiMPO4 may be a compound LiMn 1-y Fe y PO4.

[0115] For example, the compound LiMn 0.50 Fe 0.50 The preparation method of PO4 includes:

[0116] Step S1: preparing Fe-doped manganese oxalate.

[0117] 574.7g of manganese carbonate and 579.3g of ferrous carbonate were added to a mixer and thoroughly mixed for 6 hours. The resulting mixture was then transferred to a reactor, and 5L of deionized water and 1260.6g of oxalic acid dihydrate were added. The mixture was heated to 80°C and stirred at 500 rpm for 6 hours, mixing until the reaction terminated and no bubbles were generated, resulting in an Fe-doped manganese oxalate suspension. The suspension was then filtered, dried at 120°C, and sand-milled to obtain ferromanganese oxalate particles with a particle size of 100nm.

[0118] Step S2: Preparation of LiMn 0.50 Fe 0.50 PO4.

[0119] Take the manganese oxalate iron (C2O4Mn 0.50 Fe 0.50 1791.4 g of 1,000 g of 1,000 g of 1,000 g of 1,000 g of 1,000 g of 2,000 g of 1,000 g of 1,000 g of 2,000 g of 1,000 g of 1,000 g of 4,000 g of 1,000 g of 2,000 g of 1 ...1,000 g of 2,000 g of 1,000 g of 1,000 g of 2,000 g of 1,000 g of 1,000 g of 2,000 g of 1,000 g of 1,000 g of 2,000 g of 1,000 g of 1,000 g of 1,000 g of 2,000 g of 1,000 g of 1,000 g of 1,000 g of 1,000

[0120] The positive electrode active material may be a material having the chemical formula Li 1+tMn 1-c Fe c P 1-z R z O4 compound, wherein t is any value in the range of -0.100 to 0.100, c is any value in the range of 0.001 to 0.500, z is any value in the range of 0.001 to 0.100, and R includes one or more elements selected from B (boron), S, Si and N. Wherein, the values ​​of t, c and z satisfy the following conditions: the entire compound remains electrically neutral. The ratio of c to 1-c is 1:10 to 1:1, and can be optionally 1:4 to 1:1. Here c represents the sum of the stoichiometric numbers of the Mn-site doping element Fe. In some embodiments, the ratio of z to 1-z is 1:9 to 1:999, and can be optionally 1:499 to 1:249. Here z represents the sum of the stoichiometric numbers of the P-site doping element R.

[0121] Compound Li 1+t Mn 1-c Fe c P 1-z R z The preparation method of O4 may include the following steps:

[0122] (1) dissolving a manganese source, an iron source, and an acid in a solvent and stirring to generate a suspension of a manganese salt doped with elemental Fe, filtering the suspension and drying the filter cake to obtain a manganese salt doped with elemental Fe; (2) adding a lithium source, a phosphorus source, a source of elemental R, a solvent, and the manganese salt doped with elemental Fe obtained in step (1) into a reaction vessel, grinding and mixing to obtain a slurry; (3) transferring the slurry obtained in step (2) to a spray drying device for spray drying and granulation to obtain particles; (4) sintering the particles obtained in step (3) to obtain a positive electrode active material.

[0123] In any embodiment, the manganese source can be a manganese-containing substance known in the art that can be used to prepare lithium manganese phosphate, such as a manganese source selected from one or a combination of elemental manganese, manganese dioxide, manganese phosphate, manganese oxalate, and manganese carbonate. The iron source is selected from at least one of elemental iron, oxides, phosphates, oxalates, carbonates, and sulfates. The acid is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, and organic acids such as oxalic acid, and can be, for example, oxalic acid. The source of element R is selected from at least one of sulfates, borates, nitrates, and silicates of element R.

[0124] For example, the compound Li 1.001 Mn 0.999 Fe 0.001 P 0.999 Si 0.001 The preparation method of O4 includes:

[0125] Step S1: preparing Fe-doped manganese oxalate.

[0126] 1148.2g of manganese carbonate and 1.2g of ferrous carbonate were added to a mixer and thoroughly mixed for 6 hours. The resulting mixture was then transferred to a reactor, and 5L of deionized water and 1260.6g of oxalic acid dihydrate were added. The mixture was heated to 80°C and stirred at 500 rpm for 6 hours, mixing until the reaction terminated and no bubbles were generated, resulting in an Fe-doped manganese oxalate suspension. The suspension was then filtered, dried at 120°C, and sand-milled to obtain ferromanganese oxalate particles with a particle size of 100nm.

[0127] Step S2: Preparation of Li 1.001 Mn 0.999 Fe 0.001 P 0.999 Si 0.001 O4.

[0128] Take the manganese oxalate iron (C2O4Mn 0.999 Fe 0.001 1789.6 g of 2H2O (calculated as 2H2O), 369.8 g of lithium carbonate, 1148.9 g of ammonium dihydrogen phosphate, and 0.8 g of silicic acid were added to 20 L of deionized water, stirred thoroughly, and uniformly mixed at 80°C for 10 hours to obtain a slurry. The slurry was transferred to a spray dryer for spray drying and granulation, and then dried at 250°C to obtain a powder. The powder was sintered in a roller kiln at 700°C for 4 hours in a protective atmosphere (90% nitrogen and 10% hydrogen).

[0129] In other embodiments, the positive electrode active material may be a material having the chemical formula Li 1+w C m Mn 1-u Fe u P 1- a R a O 4-n D n A compound wherein C comprises one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo, and W, R comprises one or more elements selected from B (boron), S, Si, and N, D comprises one or more elements selected from S, F, Cl, and Br, w is any value in the range of -0.100 to 0.100, u is any value in the range of 0.001 to 0.500, a is any value in the range of 0.001 to 0.100, n is any value in the range of 0.001 to 0.1, and m is any value in the range of 0.9 to 1.1. Similarly, the values ​​of w, u, a, and m satisfy the following condition: the entire compound remains electrically neutral.

[0130] Compound Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n The preparation method may include the following steps:

[0131] (1) dissolving a manganese source, an iron source, and an acid in a solvent and stirring to generate a suspension of a manganese salt doped with element E, filtering the suspension and drying the filter cake to obtain a manganese salt doped with element E; (2) adding a lithium source, a phosphorus source, a source of element A, a source of element R, a source of element D, a solvent, and the manganese salt doped with element E obtained in step (1) into a reaction vessel, grinding and mixing to obtain a slurry; (3) transferring the slurry obtained in step (2) to a spray drying device for spray drying and granulation to obtain particles; (4) sintering the particles obtained in step (3) to obtain a positive electrode active material.

[0132] In any embodiment, the source of element A is selected from at least one of a simple substance, oxide, phosphate, oxalate, carbonate and sulfate of element A. The manganese source can be a manganese-containing substance known in the art that can be used to prepare lithium manganese phosphate, for example, the manganese source can be selected from one or a combination of simple manganese, manganese dioxide, manganese phosphate, manganese oxalate and manganese carbonate. The iron source is selected from at least one of a simple substance, oxide, phosphate, oxalate, carbonate and sulfate of iron. The acid is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, an organic acid such as oxalic acid, etc., for example, oxalic acid. The source of element R is selected from at least one of sulfate, borate, nitrate and silicate of element R, and the source of element D is selected from at least one of a simple substance and an ammonium salt of element D.

[0133] The positive electrode active material may contain Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D nAn embodiment of the present invention, wherein the size of w is affected by the valence of E and R and the size of y and z to ensure that the entire system is electrically neutral. If the value of w is too small, the lithium content of the entire system will be reduced, affecting the gram capacity of the material. The u value will limit the total amount of all doping elements. If u is too small, that is, the doping amount is too little, the doping element will not work. If u exceeds 0.5, the Mn content in the system will be low, affecting the voltage platform of the material. The R element is doped in the position of P. Since the PO tetrahedron is relatively stable, and a value that is too large will affect the stability of the material, the a value is limited to 0.001 to 0.100. More specifically, w is any value in the range of -0.100 to 0.100, m is any value in the range of 0.001 to 0.1, u is any value in the range of 0.001 to 0.500, a is any value in the range of 0.001 to 0.100, and n is any value in the range of 0.001 to 0.1. For example, the 1+w is selected from the range of 0.9 to 1.1, for example, 0.97, 0.977, 0.984, 0.988, 0.99, 0.991, 0.992, 0.993, 0.994, 0.995, 0.996, 0.997, 0.998, 1.01, the m is selected from the range of 0.001 to 0.1, for example, 0.001, 0.005, the u is selected from the range of 0.001 to 0.5, for example, 0.001 , 0.005, 0.02, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.34, 0.345, 0.349, 0.35, 0.4, wherein a is selected from the range of 0.001 to 0.1, for example, 0.001, 0.005, 0.08, 0.1, and n is selected from the range of 0.001 to 0.1, for example, 0.001, 0.005, 0.08, 0.1, and the positive electrode active material is electrically neutral.

[0134] Unless otherwise specified, in the above chemical formulas, when a doping site has two or more elements, the above limits on the numerical ranges of w, u, a, m, or n are not only limits on the stoichiometric number of each element as the site, but also limits on the sum of the stoichiometric numbers of the elements as the site. For example, when the chemical formula is Li 1+t Mn 1-c Fe c P 1-z R zFor compounds containing O4, when R is two or more elements R1, R2, ..., Rn, the stoichiometric numbers z1, z2, ..., zn of R1, R2, ..., Rn must each fall within the numerical range specified for z in this application, and the sum of z1, z2, ..., zn must also fall within this numerical range. Similarly, for the case where A is two or more elements, the numerical range of the stoichiometric number of A specified in this application also has the above meaning.

[0135] In some embodiments, the lithium manganese iron phosphate positive electrode active material optionally further includes a coating layer, which is optionally one or more layers of pyrophosphate, phosphate, and carbon. Since the migration barrier of transition metals in pyrophosphate is relatively high (>1eV), the dissolution of transition metals can be effectively suppressed. Phosphate has excellent lithium ion conductivity and can reduce the surface impurity lithium content. The carbon layer can effectively improve the electrical conductivity and desolvation ability of LiMnPO4, and can also act as a "barrier" to further hinder the migration of manganese ions into the electrolyte and reduce the corrosion of the electrolyte to the active material; at the same time, the above-mentioned carbon layer can also optimize the conductive network around the ternary positive electrode material in the mixture, and improve the mixing uniformity of the lithium manganese iron phosphate positive electrode material and the ternary positive electrode material.

[0136] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0137] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0138] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0139] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0140] [Electrolytes]

[0141] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.

[0142] In some embodiments, the electrolyte is liquid and includes an electrolyte salt and a solvent.

[0143] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0144] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0145] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0146] [Isolation film]

[0147] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0148] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0149] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0150] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0151] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0152] The present application has no particular limitation on the shape of the secondary battery, which can be cylindrical, square, or any other shape. For example, FIG1 shows a secondary battery cell 5 with a square structure as an example.

[0153] In some embodiments, referring to Figure 2, the outer packaging may include a shell 51 and a top cover assembly 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the top cover assembly 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery cell 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0154] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0155] Figure 3 shows an example battery module 4. Referring to Figure 3 , within the battery module 4, multiple secondary battery cells 5 may be arranged sequentially along the length of the battery module 4. Of course, they may also be arranged in any other manner. Furthermore, the multiple secondary battery cells 5 may be secured together using fasteners.

[0156] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of secondary battery cells 5 are accommodated in the accommodation space.

[0157] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0158] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 4 and 5 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0159] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0160] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0161] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high charging capacity requirements of the secondary battery, a battery pack or battery module can be used.

[0162] [Example]

[0163] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0164] The parameters and sources of the graphite used are shown in Table 1.

[0165] Table 1

[0166] The negative electrode slurry compositions of the following examples and comparative examples are as follows: graphite: conductive agent: binder is 96.7:1.5:1.8. The composition of graphite in the negative electrode slurry is shown in Table 2. The binder is SBR and the conductive agent is SP.

[0167] Table 2

[0168] Preparation of negative electrode sheet

[0169] Example 1

[0170] The negative electrode slurry 1 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly coated on both sides of the current collector copper foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P1.

[0171] Example 2

[0172] The negative electrode slurry 3 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly applied on both sides of the current collector copper foil, and the rest is the same as in Example 1 to obtain the negative electrode sheet P2.

[0173] Example 3

[0174] Negative electrode slurry 1 and negative electrode slurry 2 were applied on both sides of the copper foil in sequence, with the coating amount of each layer of slurry being 0.010 g / cm 2 Then, it is dried in vacuum at a high temperature of 100-120°C for 14 hours and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P3. Negative electrode slurry 1 forms the inner active material layer, and negative electrode slurry 2 forms the surface active material layer.

[0175] Example 4

[0176] Negative electrode slurry 2 and negative electrode slurry 1 were applied on both sides of the copper foil in sequence, with the coating amount of each layer of slurry being 0.081 g / 1540 mm 2 , the rest is the same as Example 3, and a negative electrode sheet P4 is obtained. Negative electrode slurry 2 forms the inner active material layer, and negative electrode slurry 1 forms the surface active material layer.

[0177] Example 5

[0178] Negative electrode slurry 1 and negative electrode slurry 3 were applied on both sides of the copper foil in sequence, with the coating amount of each layer of slurry being 0.081 g / 1540 mm 2 , the rest is the same as Example 3, and a negative electrode sheet P5 is obtained. Negative electrode slurry 1 forms the inner active material layer, and negative electrode slurry 3 forms the surface active material layer.

[0179] Example 6

[0180] Negative electrode slurry 3 and negative electrode slurry 1 were applied on both sides of the copper foil in sequence, with the coating amount of each layer of slurry being 0.081 g / 1540 mm 2 , the rest is the same as in Example 3, and a negative electrode sheet P6 is obtained. Negative electrode slurry 3 forms the inner active material layer, and negative electrode slurry 1 forms the surface active material layer.

[0181] Example 7

[0182] Negative electrode slurry 2 and negative electrode slurry 3 were applied on both sides of the copper foil in sequence, with the coating amount of each layer of slurry being 0.081 g / 1540 mm 2 , the rest is the same as Example 3, and a negative electrode sheet P7 is obtained. Negative electrode slurry 2 forms the inner active material layer, and negative electrode slurry 3 forms the surface active material layer.

[0183] Example 8

[0184] Negative electrode slurry 3 and negative electrode slurry 2 were applied on both sides of the copper foil in sequence, with the coating amount of each layer of slurry being 0.081 g / 1540 mm 2 , the rest is the same as in Example 3, and a negative electrode sheet P8 is obtained. Negative electrode slurry 3 forms the inner active material layer, and negative electrode slurry 2 forms the surface active material layer.

[0185] Example 9

[0186] The negative electrode slurry 4 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly coated on both sides of the copper foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P9.

[0187] Example 10

[0188] The negative electrode slurry 5 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly coated on both sides of the copper foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P10.

[0189] Example 11

[0190] The negative electrode slurry 6 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly coated on both sides of the copper foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P11.

[0191] Example 12

[0192] The negative electrode slurry 7 was prepared at 0.162 g / 1540 mm2 The coating amount is evenly coated on both sides of the copper foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P12.

[0193] Example 13

[0194] The negative electrode slurry 8 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly coated on both sides of the copper foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P13.

[0195] Example 14

[0196] The negative electrode slurry 9 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly coated on both sides of the copper foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P14.

[0197] Example 15

[0198] The negative electrode slurry 10 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly coated on both sides of the copper foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P15.

[0199] Example 16

[0200] The negative electrode slurry 11 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly coated on both sides of the copper foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P16.

[0201] Example 17

[0202] The negative electrode slurry 12 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly coated on both sides of the copper foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P17.

[0203] Example 18

[0204] The negative electrode slurry 13 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly coated on both sides of the copper foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P18.

[0205] Example 19

[0206] The negative electrode slurry 14 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly coated on both sides of the copper foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P19.

[0207] Comparative Example 1

[0208] The negative electrode slurry 2 was prepared at 0.162 g / 1540 mm 2 The coating amount is evenly coated on both sides of the current collector aluminum foil, vacuum dried at a high temperature of 100-120°C for 14 hours, and compacted by a roller press to form a negative electrode film layer to obtain a negative electrode sheet P20.

[0209] The thickness and compaction density of the obtained negative electrode sheet were tested using the following method:

[0210] Thickness test: The thickness of the electrode after cold pressing was measured by a micrometer to obtain thickness data, which was around 0.133nm;

[0211] Compaction density: 1540mm 2 The negative electrode sheet has a compaction density of 1.65 g / cm2, which is equal to the double-sided coating weight / 1540.25*1000 / thickness of the sheet after cold pressing. 3 about.

[0212] BET specific surface area of ​​the graphite negative electrode active material of the negative electrode film layer: refer to GB / T 19587-2017 / ISO 9277:2010 to test the BET specific surface area of ​​the graphite negative electrode active material.

[0213] BET specific surface area of ​​the material forming the negative electrode film layer: After the negative electrode film layer is scraped off by the scraping method, the BET specific surface area of ​​the graphite negative electrode active material is tested with reference to GB / T 19587-2017 / ISO 9277:2010.

[0214] BET specific surface area of ​​the materials forming the inner active material layer and the surface active material layer: After the inner active material layer and the surface active material layer are scraped off using the scraping method, the BET specific surface area of ​​the graphite negative electrode active material is tested with reference to GB / T 19587-2017 / ISO 9277:2010.

[0215] The results are shown in 3.

[0216] Table 3

[0217] Production of positive electrode sheet 1:

[0218] The active material LiMn 0.6 Fe0.4 PO4, conductive carbon black Super-P, and binder PVDF were mixed thoroughly in an NMP solvent system at a weight ratio of 97:1:2, and then coated on Al foil. The coating weight was controlled to be 360 ​​g / m 2 , drying, cold pressing, slitting, and cutting to obtain the positive electrode sheet 1.

[0219] Production of battery cells

[0220] A PE / PP / PE three-layer porous polymer film is used as the isolation membrane.

[0221] The positive electrode sheet 1, separator, and the prepared negative electrode sheet are wound in sequence, ensuring the separator is positioned between the cathode and anode to provide isolation. The winding process also controls the misalignment between the cathode and cathode, as well as between the separator and the separator. This completes the process to produce a bare cell. Qualified bare cells are welded to the top cover via the tabs, followed by case placement, baking, liquid injection, formation, and capacity measurement. The completed battery is then tested for performance.

[0222] 1) Cyclic performance test

[0223] Under the same conditions, first conduct a charge and discharge test, recording the cell's BOL (Before of Life), or the discharge capacity Cb at the first cycle. Then conduct a cycle life test, testing at 45°C with 1C / 1C cycles, recording the cell's discharge capacity Ce at all times. The ratio of Ce to Cb is the capacity retention rate during the cycle. Testing is terminated when the capacity retention rate is less than or equal to 80%, indicating EOL (End of Life) has been reached.

[0224] 2) Storage performance test

[0225] Under the same conditions, first perform a charge and discharge test, recording the cell's BOL (Before of Life), or the discharge capacity Cb during the first charge and discharge. Then perform a storage life test at 60°C, performing a room-temperature capacity test every 30 days (actual testing is every 20-40 days), recording the cell's discharge capacity Ce at all times. The ratio of Ce to Cb is the capacity retention rate during storage. Testing is stopped when the capacity retention rate is less than or equal to 80%, indicating that the cell has reached EOL (End of Life).

[0226] 3) Charging capacity

[0227] Test method: At 25°C, fully discharge the battery cell at 0.33C current (full discharge voltage is 2.0V), then charge it at 1C constant current to 4.1V and charge it at 4.1V constant voltage to 0.05V cutoff current, and record the total time of constant current charging + constant voltage charging.

[0228] The test results are recorded in Table 4.

[0229] Table 4

[0230] In addition, the active material Li 1.001 Mn 0.999 Fe 0.001 P 0.999 Si 0.001 O4 replaces the active material LiMn of the positive electrode plate 1 0.6 Fe 0.4 PO4, forming the positive electrode plate 2.

[0231] The positive electrode sheet 2 was combined with the negative electrode sheet P1, the negative electrode sheet P2, the negative electrode sheet P3, the negative electrode sheet P4, and the negative electrode sheet P20, respectively, and battery cells were made according to the above method. They were named as Examples 20, 21, 22, 23 and Comparative Example 2, respectively. The cycle performance, storage performance and charging capacity were tested according to the above method, and the test results are recorded in Table 5.

[0232] Table 5

[0233] It can be clearly seen from the experimental results of the cycle and storage performance tests of the embodiments and comparative examples in Tables 4 and 5 above that the cycle and storage of different pole piece structures have different differences. In the secondary battery of the lithium manganese iron phosphate system, as the content of small BET graphite in the negative pole piece increases, the BET specific surface area of ​​the film layer decreases, making the high-temperature cycle and storage improvement of the battery cell more obvious. Mainly in the secondary battery of the lithium manganese iron phosphate system, the effective active sites of the small BET graphite are greatly reduced, thereby greatly reducing the degree of side reactions on the surface of the negative electrode graphite, thereby indirectly improving the life capacity of the battery cell. However, when the BET of the graphite material used is too small, although the cycle and storage performance of the battery can be improved, the charging capacity of the battery will be slightly lost.

[0234] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and components may be substituted with equivalents without departing from the scope of the present application. In particular, the various technical features described in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but encompasses all technical solutions within the scope of the claims.

Claims

1. A negative electrode sheet, comprising a current collector and a negative electrode film layer disposed on at least one side of the current collector, in, The negative electrode film layer includes one or more active material layers, the negative electrode active material in the negative electrode film layer includes a first graphite negative electrode active material, the BET specific surface area of ​​the first graphite negative electrode active material is A, the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer is B, A≤B, or the BET specific surface area of ​​the material forming the negative electrode film layer is B', A<B'.

2. The negative electrode sheet according to claim 1, in, The BET specific surface area of ​​the first graphite negative electrode active material is 0.5 m 2 / g≤A≤1.3m 2 / g; optionally, 0.8m 2 / g≤A≤1.22m 2 / g.

3. The negative electrode sheet according to claim 1 or 2, in, The BET specific surface area of ​​the material forming the negative electrode film layer is 0.55 m 2 / g≤B'≤1.85m 2 / g, optional 0.89m 2 / g≤B'≤1.42m 2 / g; or the BET specific surface area of ​​the negative electrode active material in the negative electrode film layer is 0.5m 2 / g≤B≤1.8m 2 / g, optional 0.82m 2 / g≤B≤1.38m 2 / g.

4. The negative electrode sheet according to any one of claims 1 to 3, in, The negative electrode film layer further comprises a second graphite negative electrode active material, the BET specific surface area of ​​the second graphite negative electrode active material is C, and A<C, optionally, B<C; optionally, 1.3m 2 / g≤C≤1.95m 2 / g, further optionally, 1.5m 2 / g≤C≤1.81m 2 / g.

5. The negative electrode sheet according to any one of claims 1 to 4, in, The negative electrode film layer includes multiple active material layers, and the first graphite negative electrode active material is arranged in the same active material layer or in different active material layers.

6. The negative electrode sheet according to any one of claims 1 to 5, in, The negative electrode film layer includes multiple active material layers, the active material layer located on the surface is defined as a surface active material layer, the active material layer between the surface active material layer and the current collector is defined as an inner active material layer, the BET specific surface area of ​​the negative electrode active material of the surface active material layer is D, and the BET specific surface area of ​​the negative electrode active material of the inner active material layer is E; optionally, A≤D<E<B; optionally, 0.5m 2 / g≤D≤1.22m 2 / g, optional 0.82m 2 / g≤D≤1.22m 2 / g, and / or 0.82m 2 / g≤E≤1.81m 2 / g, optional 0.82m 2 / g≤E≤1.52m 2 / g.

7. The negative electrode sheet according to any one of claims 1 to 5, in, The negative electrode film layer includes multiple active material layers, the active material layer located on the surface is defined as a surface active material layer, the active material layer between the surface active material layer and the current collector is defined as an inner active material layer, the BET specific surface area of ​​the material forming the surface active material layer is D', and the BET specific surface area of ​​the material forming the inner active material layer is E'; optionally, D'<B'<E'; optionally, 0.59m 2 / g≤D'≤1.77m 2 / g, further optionally 0.89m 2 / g≤D'≤1.59m 2 / g, and / or 0.59m 2 / g≤E'≤1.87m 2 / g, further optionally 0.89m 2 / g≤E'≤1.87m 2 / g.

8. The negative electrode sheet according to claim 5, in, The mass content of the first graphite negative electrode active material in the surface active material layer is 10% to 98%; and / or the negative electrode film layer also includes a second graphite negative electrode active material, and the mass content of the second graphite negative electrode active material in the inner active material layer is 10% to 98%.

9. The negative electrode sheet according to any one of claims 4 to 8, in, The mass ratio of the first graphite negative electrode active material to the second graphite negative electrode active material is 1:9 to 9:1, and can be optionally 5:5 to 8:

2.

10. The negative electrode sheet according to any one of claims 1 to 9, in, The D of the first graphite negative electrode active material v 50 is between 10 μm and 25 μm, optionally between 15 μm and 22 μm; and / or the first graphite negative electrode active material includes any one or more of natural graphite, artificial graphite, graphitized carbon fiber and graphitized mesophase carbon microspheres.

11. The negative electrode sheet according to any one of claims 4 to 10, in, The second graphite negative electrode active material D v 50 is between 7 μm and 10 μm, optionally between 8 μm and 10 μm; and / or the second graphite negative electrode active material includes any one or more of natural graphite, artificial graphite, graphitized carbon fiber and graphitized mesophase carbon microspheres.

12. The negative electrode sheet according to any one of claims 1 to 11, in, The negative electrode plate is a negative electrode plate for a secondary battery, and when the secondary battery is charged, the full battery voltage reaches an upper limit voltage before the potential of the negative electrode in the full battery reaches 0mv; optionally, the positive electrode active material of the secondary battery includes a lithium iron manganese phosphate-based positive electrode active material.

13. A secondary battery comprising a positive electrode sheet and a negative electrode sheet, in, The negative electrode sheet comprises the negative electrode sheet according to any one of claims 1 to 12.

14. The secondary battery according to claim 11, in, The positive electrode plate includes a positive electrode active material, and the positive electrode active material includes a lithium iron manganese phosphate-based positive electrode active material. Optionally, the lithium iron manganese phosphate-based positive electrode active material includes a doped lithium iron manganese phosphate-based positive electrode active material or a coated lithium iron manganese phosphate-based positive electrode active material. Optionally, the lithium iron manganese phosphate-based positive electrode active material includes Li element, P element, Fe element and M element, and the M element includes Mn and non-Mn elements.

15. The secondary battery according to claim 14, in, The non-Mn element includes one or both of a first doping element and a second doping element, wherein the first doping element is manganese doping and the second doping element is phosphorus doping; Optionally, the first doping element includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge; further optionally, the first doping element includes at least two elements selected from the group consisting of Fe, Ti, V, Ni, Co and Mg; Optionally, the second doping element includes one or more elements selected from the group consisting of B (boron), S, Si and N.

16. The secondary battery according to claim 14 or 15, in, The lithium iron manganese phosphate system positive electrode active material includes at least one of the following materials: LiMn 1-y Fe y PO 4 , y is any value in the range of 0.001 to 0.5; Li 1+t Mn 1-c Fe c P 1-z R z O 4 , t is any value in the range of -0.100 to 0.100, c is any value in the range of 0.001 to 0.500, z is any value in the range of 0.001 to 0.100, and R includes one or more elements selected from B, S, Si and N; Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n , wherein A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W, E includes one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, R includes one or more elements selected from B, S, Si and N, D includes one or more elements selected from S, F, Cl and Br, w is any value in the range of -0.100 to 0.100, and m is any value in the range of 0.001 to 0.1, u is any value in the range of 0.001 to 0.500, a is any value in the range of 0.001 to 0.100, n is any value in the range of 0.001 to 0.1, and Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n It is electrically neutral.

17. An electrical device comprising a secondary battery, in, The secondary battery includes the secondary battery according to any one of claims 13 to 16.

Citation Information

Patent Citations

  • Multi-layer anode comprising natural graphite and artificial graphite, and lithium secondary battery comprising same

    CN108701816A

  • Secondary battery and method for preparing same, and device including secondary battery

    CN113875047A

  • Secondary battery, production method therefor, and device comprising same

    CN113875048A

  • Negative electrode for secondary battery and secondary battery comprising same

    CN114430022A

  • Negative plate and electrochemical device

    CN115377416A

Cited By

  • Electrode assembly, lithium ion battery and electric equipment

    CN119764330A

  • Battery cell, battery apparatus, and electric device

    WO2026174440A1