Back-contact slice battery and preparation method therefor
By depositing semiconductor layers on the back of the silicon wafer during the preparation process and cutting them, combined with plasma processing, the problems of low conversion efficiency and production yield of the slice battery are solved, and efficient preparation of slice back contact battery is achieved, reducing production cost.
Patent Information
- Application Number
- PCT/CN2024/081017
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2024-03-11
- Publication Date
- 2024-11-14
AI Technical Summary
The existing slice batteries have reduced conversion efficiency, low production efficiency and yield after cutting, and increased production costs.
The cutting is carried out after depositing the semiconductor layer on the back of the silicon wafer, and the cutting section is cleaned by plasma treatment, combining laser cutting and atmospheric plasma treatment to reduce cutting damage and residues, and improve production efficiency and yield.
The conversion efficiency and production yield of the slice back contact battery are improved, and the production cost is basically not increased, and the equipment is versatile and preliminary process flow are maintained.
Smart Images

Figure CN2024081017_14112024_PF_FP_ABST
Abstract
Description
A sliced back contact battery and its preparation method
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This disclosure claims priority to application number CN202310525001.7, filed with the Patent Office of China on May 11, 2023, entitled “A sliced back contact battery and its preparation method,” the entire contents of which are incorporated by reference into this disclosure. Technical Field
[0003] The present disclosure belongs to the technical field of sliced batteries, and particularly relates to a sliced back-contact battery and a preparation method thereof. Background Art
[0004] Slicing a battery is to divide a battery cell into several battery cells, thereby reducing the short-circuit current of the battery, thereby reducing the power loss of the battery and its module, and ultimately improving the conversion efficiency of the battery and module.
[0005] Existing cell slicing processes typically complete all production processes before cutting into halves. This results in a cell efficiency typically 0.1%-0.5% lower than the pre-cut efficiency, ultimately impacting cell module efficiency and power generation. The existing cell slicing process also involves splitting the silicon wafer in half at the start of cell production. This reduces production efficiency and yield, potentially reducing production capacity by 50%. Furthermore, existing equipment and tooling require replacement, increasing investment costs.
[0006] CN109545886B discloses a method for preparing half-cell polycrystalline solar cells. The patent mentions that after the cell is manufactured, a passivation treatment is introduced to passivate impurities and defects in the cell, reduce recombination within the silicon wafer, and improve the efficiency of the cell. However, this invisibly increases the number of process steps and production costs, which may lead to an increase in the damage rate or defect rate by 0.5%-1%, that is, a reduction in production yield.
[0007] Therefore, there is an urgent need in the art for a sliced back-contact battery and a preparation method thereof that can ensure battery conversion efficiency and improve production yield while minimizing the increase in production cost.
[0008] Summary of the Invention
[0009] The purpose of the present disclosure is to overcome the above-mentioned defects of the prior art and to provide a sliced back-contact battery and a preparation method thereof. The preparation method of the sliced back-contact battery can ensure the battery conversion efficiency and improve the production yield while minimizing the increase in production costs.
[0010] To achieve the above objectives, in a first aspect, the present disclosure provides a method for preparing a sliced back-contact battery, comprising the following steps:
[0011] S101, depositing a first semiconductor layer on the back side of the silicon wafer;
[0012] S102, continuing to deposit a semiconductor mask layer outside the first semiconductor layer;
[0013] S103, opening a second semiconductor opening region on the back surface obtained in S102 to expose the silicon wafer in a corresponding region;
[0014] S104, cutting the semi-finished product obtained in S103;
[0015] S105, performing plasma treatment on the cross-section of the silicon wafer obtained in S104;
[0016] S106, then cleaning and texturing the semi-finished product obtained in S105;
[0017] S107 , then depositing a second semiconductor layer on the back side of the semi-finished product obtained in S106 .
[0018] In some preferred embodiments of the present disclosure, the cutting in S104 is performed by laser cutting or mechanical cutting.
[0019] More preferably, the laser cutting method includes two-pass cutting, wherein the first cutting pass adopts ultraviolet pulse laser continuous scanning, the laser used is spatially shaped into a flat-top laser spot, and the overlap rate between adjacent spots is between 0-60%, preferably between 10%-50%; the second cutting pass adopts green light pulse laser continuous scanning, the laser used is a circular Gaussian laser, and the overlap rate between adjacent spots is between 30%-60%, preferably between 30%-50%.
[0020] More preferably, the pulse width of the continuous scanning of the ultraviolet pulsed laser in the first cutting pass is 10-30 picoseconds, preferably 15-25 picoseconds, and the light spot formed by the laser used for the first cutting pass on the silicon wafer is square; the pulse width of the continuous scanning of the green light pulsed laser in the second cutting pass is 15-45 nanoseconds, and the light spot formed by the laser used for the second cutting pass on the silicon wafer is circular.
[0021] In some preferred embodiments of the present disclosure, the cutting is performed from the back side or the front side of the semi-finished product in S104.
[0022] In some preferred embodiments of the present disclosure, the plasma treatment in S105 is performed by atmospheric plasma treatment, plate-type plasma-enhanced chemical vapor deposition, or tube-type plasma-enhanced chemical vapor deposition.
[0023] More preferably, the conditions for the atmospheric plasma treatment include: controlling the movement speed of the atmospheric plasma nozzle in the silicon wafer cutting section to be 0.1-3 cm / s, preferably 0.5-2 cm / s, the gas flow rate of the atmospheric plasma jet nozzle to be 5-15 mL / min, preferably 9-15 mL / min, the distance between the jet nozzle and the silicon wafer cutting section to be 10-30 mm, preferably 10-25 mm, the frequency of the radio frequency power supply to be 40 kHz-13.56 MHz, and the area of the plasma formed to be no more than 10 cm 2 The treatment time is 5-40 min, preferably 10-30 min; the gas source of the atmospheric plasma is the atmosphere or an introduced gas containing oxygen and hydrogen, and the introduced gas containing oxygen and hydrogen is doped with 2 volume%-10 volume% oxygen, 2 volume%-10 volume% hydrogen, and an inert gas.
[0024] More preferably, the conditions for the plate-type plasma-enhanced chemical vapor deposition or the tube-type plasma-enhanced chemical vapor deposition independently include: carrying out the deposition under the condition of introducing an oxygen-containing gas, the total amount of oxygen-containing gas introduced is 1000 sccm-10000 sccm, the volume content of O2 and / or N2O in the oxygen-containing gas is 1%-20%, the power supply frequency is controlled to be 40 kHz-13.56 MHz, and the processing time is 5-40 min, preferably 10-30 min.
[0025] In some preferred embodiments of the present disclosure, the first semiconductor layer includes a tunneling oxide layer and a first doped polysilicon layer; the second semiconductor layer includes a second semiconductor passivation layer and a second doped layer, the second semiconductor passivation layer is an intrinsic amorphous silicon layer or a microcrystalline silicon layer; the second doped layer is an amorphous silicon layer or a microcrystalline silicon layer; one of the first doped polysilicon layer and the second doped layer is N-type and the other is P-type.
[0026] In some preferred embodiments of the present disclosure, the preparation method further includes: S100, providing a double-sided polished silicon wafer, and then performing the subsequent S101.
[0027] In some preferred embodiments of the present disclosure, the preparation method further comprises:
[0028] S108, depositing a passivation layer and an anti-reflection layer on the front side of the semi-finished product obtained in S107;
[0029] S109, removing a portion of the second semiconductor layer outside the first semiconductor layer on the back side of the semi-finished product to form a first semiconductor opening region to expose the first semiconductor layer, wherein the first semiconductor opening region and the second semiconductor opening region are arranged alternately;
[0030] S110, depositing a conductive film layer on the back side of the semi-finished product obtained in S109;
[0031] S111, forming an isolation trench on the conductive film layer between the first semiconductor opening region and the second semiconductor opening region;
[0032] S112 , forming metal electrodes at the first semiconductor opening region and the second semiconductor opening region respectively.
[0033] In a second aspect, the present disclosure provides a sliced back-contact battery, which is obtained by the preparation method described in the first aspect. Beneficial effects:
[0034] The present invention performs cutting in the middle of the production process (i.e., after S103), retains the process and equipment configuration of the previous steps, improves production efficiency and maintains the versatility of some original equipment, and is supplemented by plasma treatment. On the one hand, the physical action of plasma is used to sweep away the residual broken silicon powder in the cut section to achieve a cleaning effect, which is conducive to subsequent thorough cleaning. On the other hand, the decomposed oxygen ions are used to oxidize the tip and loose part of the cut section, which is conducive to the subsequent wet chemical corrosion of the tip residue and repair of cutting defects in cleaning, thereby improving the process production yield and battery efficiency, and basically does not increase the production cost. The mechanism of plasma treatment and cleaning and texturing combined to achieve wet chemical corrosion tip residue and repair of cutting defects is: silicon oxide formed by plasma oxidation easily reacts with the cleaning agent (usually acidic chemicals) used for cleaning, and the reaction rate of silicon oxide with the cleaning agent is more than 10 times that of polysilicon with the cleaning agent. Therefore, the tip residue or cutting defect is oxidized by plasma treatment and initially cleaned with its physical action, and then quickly removed with subsequent cleaning (the cleaning agent used includes acidic chemicals), so that the area or edge to be coated is smoother and rounder, reducing the recombination damage of carriers, which is beneficial to the subsequent process.
[0035] In the preferred two-pass cutting scheme disclosed herein, the first pass of cutting can accurately form a small cutting gap, and the second pass of cutting can quickly and safely cut along the above-mentioned small cutting gap, which is more conducive to avoiding damage to the coated layer and expansion of hidden cracks.
[0036] In the preferred embodiment of the present disclosure, atmospheric plasma treatment is employed, enabling localized plasma treatment, more precisely controlling and treating the cut cross-section, while also better protecting the coated first semiconductor layer without affecting subsequent steps. Conventional plate- or tube-type PECVD processes, on the other hand, are unable to achieve localized treatment and cannot precisely treat the cut cross-section, potentially damaging the coated first semiconductor layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.
[0038] FIG1 is a schematic structural diagram of a silicon wafer according to Example 1 of the present disclosure;
[0039] FIG2 is a schematic structural diagram of a second semiconductor opening region formed on the back side of the embodiment 1 of the present disclosure;
[0040] FIG3 is a schematic diagram of the structure of a silicon wafer being cut in half in Example 1 of the present disclosure;
[0041] FIG4 is a schematic structural diagram of forming a first semiconductor opening region in Embodiment 1 of the present disclosure;
[0042] FIG5 is a schematic structural diagram of forming a first semiconductor opening region in Embodiment 1 of the present disclosure;
[0043] FIG6 is a schematic diagram of the structure of the printed grid lines in Example 1 of the present disclosure;
[0044] FIG. 7 is a process flow chart of an embodiment of the present disclosure.
[0045] DESCRIPTION OF REFERENCE NUMERALS 1. silicon wafer, 2. second semiconductor opening region, 3. first semiconductor opening region, 4. isolation trench, 5. first metal electrode, 6. second metal electrode DETAILED DESCRIPTION
[0046] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. Among them, the terms "optional" and "optional" all mean that they may be included or not (or may be present or not).
[0047] In this disclosure, the area close to the silicon wafer is considered as the inside, and the area far from the silicon wafer is considered as the outside.
[0048] In a first aspect, the present disclosure provides a method for preparing a sliced back-contact battery, comprising the following steps:
[0049] S101, depositing a first semiconductor layer on the back side of the silicon wafer;
[0050] S102, continuing to deposit a semiconductor mask layer outside the first semiconductor layer;
[0051] S103, opening a second semiconductor opening region on the back surface obtained in S102 to expose the silicon wafer in a corresponding region;
[0052] S104, cutting the semi-finished product obtained in S103;
[0053] S105, performing plasma treatment on the cross-section of the silicon wafer obtained in S104;
[0054] S106, then cleaning and texturing the semi-finished product obtained in S105;
[0055] S107 , then depositing a second semiconductor layer on the back side of the semi-finished product obtained in S106 .
[0056] It should be noted that the semiconductor mask layer described in S102 of the present disclosure is a conventional material capable of protecting the first semiconductor layer. For example, it may be at least one of silicon nitride, silicon oxynitride, silicon carbide, and an organic protective ink, and is used to protect the first semiconductor layer from corrosion by strong acid and alkali solutions used in cleaning and texturing, or from damage caused by subsequent processes. It is understood that the further deposition of the semiconductor mask layer refers to the deposition of a semiconductor mask layer that completely covers the outer surface of the first semiconductor layer.
[0057] In step S103 of the present disclosure, the second semiconductor opening regions are spaced apart in the first semiconductor layer to facilitate the subsequent formation of two emitters. A person skilled in the art can select a width Wa of the second semiconductor opening regions according to actual needs, for example, Wa can be 300-700 μm.
[0058] In some preferred embodiments of the present disclosure, the cutting in S104 is performed by laser cutting or mechanical cutting.
[0059] More preferably, the laser cutting method includes a two-pass cutting method, wherein the first cutting pass uses continuous scanning of an ultraviolet pulsed laser, the laser used is spatially shaped into a flat-top laser spot, and the overlap rate between adjacent spots is between 0% and 60%, preferably between 10% and 50%; the second cutting pass uses continuous scanning of a green pulsed laser, the laser used is a circular Gaussian laser, and the overlap rate between adjacent spots is between 30% and 60%, preferably between 30% and 50%. In some specific embodiments, the wavelength of the ultraviolet pulsed laser is approximately 355nm, and the wavelength of the green pulsed laser is approximately 532nm.
[0060] It can be understood that the two-pass cutting refers to first performing a first pass of cutting along the line to be cut from beginning to end, and then performing a second pass of cutting along the line to be cut from beginning to end.
[0061] More preferably, the pulse width of the continuous scanning of the ultraviolet pulsed laser in the first cutting pass is 10-30 picoseconds, preferably 15-25 picoseconds, and the light spot formed by the laser used for the first cutting pass on the silicon wafer is square; the pulse width of the continuous scanning of the green light pulsed laser in the second cutting pass is 15-45 nanoseconds, and the light spot formed by the laser used for the second cutting pass on the silicon wafer is circular.
[0062] In the present disclosure, it is understood that the overlap ratio between adjacent light spots refers to the area ratio of the overlapping area to any corresponding light spot area.
[0063] In the preferred embodiment of the two-pass cutting process disclosed herein, the first pass forms a small slit. This, combined with the specific process parameters of the first pass, further reduces the risk of cracks in the laser melt zone propagating and damaging the already coated film. The second pass allows for rapid cutting along the small slit. Combined with the specific process parameters of the second pass, this further facilitates the formation of a rapid longitudinal slit melt zone on the silicon wafer, thereby facilitating rapid cutting of the silicon wafer while minimizing damage to the already coated film. The overlap ratio between adjacent laser spots is a key parameter in the cutting process. Maintaining these overlap ratios within the aforementioned ranges minimizes the spread of cracks in the film surrounding the cutting line. Any small cracks that inevitably occur can be repaired through subsequent plasma treatment, cleaning, and other steps, ensuring that the film layers remain largely intact. Under the same conditions, a high overlap ratio in the first pass can exacerbate the spread of cracks in the surrounding film layers, making subsequent performance restoration relatively difficult. A low overlap ratio requires increased force in the second pass, potentially increasing the risk of fragmentation and film damage.
[0064] The cutting described in the present disclosure can divide the silicon wafer into two equal parts, three equal parts, or any equal parts. The embodiment of the present disclosure adopts the method of dividing the silicon wafer into two equal parts from the middle.
[0065] In some preferred embodiments of the present disclosure, the cutting is performed from the back or front of the semi-finished product in S104. More preferably, the cutting is performed from the front of the semi-finished product.
[0066] In some preferred embodiments of the present disclosure, the plasma treatment in S105 is performed by atmospheric plasma treatment, plate-type plasma-enhanced chemical vapor deposition (PECVD), or tube-type plasma-enhanced chemical vapor deposition (PECVD). More preferably, the plasma treatment is performed by atmospheric plasma treatment because atmospheric plasma treatment can precisely treat the cut cross-section locally, thus preventing damage to the first semiconductor layer; whereas plate-type or tube-type PECVD cannot precisely treat the cut cross-section locally, and thus may damage the coated first semiconductor layer.
[0067] More preferably, the conditions for the atmospheric plasma treatment include: controlling the movement speed of the atmospheric plasma nozzle in the silicon wafer cutting section to be 0.1-3 cm / s, preferably 0.5-2 cm / s, the gas flow rate of the atmospheric plasma jet nozzle to be 5-15 mL / min, preferably 9-15 mL / min, the distance between the jet nozzle and the silicon wafer cutting section to be 10-30 mm, preferably 10-25 mm, the frequency of the radio frequency power supply to be 40 kHz-13.56 MHz, and the area of the plasma formed to be no more than 10 cm 2 The processing time is 5-40 min, preferably 10-30 min.
[0068] In the preferred atmospheric plasma treatment scheme disclosed herein, because the plasma is generated locally, combined with appropriate process parameter control, it can more precisely control and treat the cut cross-section, preventing the already coated first semiconductor layer and the second semiconductor opening area from being damaged by the plasma, leading to performance degradation. The gas flow rate, nozzle movement speed, spacing, and treatment time are all within appropriate ranges, enabling precise control and effective treatment of the cut cross-section while preventing oxidation and damage to the silicon film in non-defective areas. Under the same conditions, during plasma treatment, if the gas flow rate is too high and the treatment time is too long, there is a risk of excessive oxidation of the silicon film in non-defective areas, making subsequent cleaning susceptible to corrosion and damage. If the gas flow rate is too low and the treatment time is too short, the effect of fully oxidizing and removing the tip residue or cutting defects is limited, and subsequent repair results cannot achieve better results.
[0069] Further preferably, the gas source for the atmospheric plasma is the atmosphere or an introduced gas containing oxygen and hydrogen. It is understood that the introduced gas containing oxygen and hydrogen is an additional gas introduced. More preferably, the introduced gas containing oxygen and hydrogen is doped with 2% to 10% by volume of oxygen, 2% to 10% by volume of hydrogen, and an inert gas. Examples of the inert gas include helium and argon.
[0070] More preferably, the conditions for the plate-type plasma-enhanced chemical vapor deposition or the tube-type plasma-enhanced chemical vapor deposition each independently include: being carried out under the condition of introducing an oxygen-containing gas, the total amount of oxygen-containing gas introduced is 1000 sccm-10000 sccm, the volume content of O2 and / or N2O in the oxygen-containing gas (i.e., the total amount of O2 and / or N2O) is 1%-20%, the power supply frequency is controlled to be 40 kHz-13.56 MHz, and the processing time is 5-40 minutes, preferably 10-30 minutes. The oxygen-containing gas is introduced into the plate-type plasma-enhanced chemical vapor deposition or the tube-type plasma-enhanced chemical vapor deposition, which generates oxygen ions that react with the silicon film. The remaining diluent gases in the oxygen-containing gas other than O2 and / or N2O can be inert gases such as nitrogen, argon, and helium.
[0071] The cleaning and texturing in S106 of the present disclosure can further clean and repair the cut cross section and clean and texturize the second semiconductor opening area and the front surface.
[0072] In some preferred embodiments of the present disclosure, the first semiconductor layer includes a tunneling oxide layer and a first doped polysilicon layer; the second semiconductor layer includes a second semiconductor passivation layer and a second doped layer, the second semiconductor passivation layer is an intrinsic amorphous silicon layer or a microcrystalline silicon layer, and the second doped layer is an amorphous silicon layer or a microcrystalline silicon layer; one of the first doped polysilicon layer and the second doped layer is N-type and the other is P-type.
[0073] Those skilled in the art can select the thickness of each layer in the first semiconductor layer and the second semiconductor layer according to actual needs. For example, the thickness of the tunneling oxide layer can be 0.5-2.5 nm, and the thickness of the first doped polysilicon layer can be 50-300 nm; the thickness of the second semiconductor passivation layer can be 3-15 nm, and the thickness of the second doped layer can be 4-30 nm. Those skilled in the art can select the doping concentration of the first doped polysilicon layer and the second doped layer according to actual needs, and will not be further described here.
[0074] The silicon wafer disclosed herein may be a single crystal silicon wafer or a single cast silicon wafer.
[0075] In some preferred embodiments of the present disclosure, the preparation method further includes: S100, providing a double-sided polished silicon wafer, and then performing the subsequent S101.
[0076] In some preferred embodiments of the present disclosure, the preparation method further includes: S108, depositing a passivation layer and an anti-reflection layer on the front surface.
[0077] In some preferred embodiments of the present disclosure, the preparation method further includes: S109, removing a portion of the second semiconductor layer on the back side of the semi-finished product that is outside the first semiconductor layer, forming a first semiconductor opening region to expose the first semiconductor layer, wherein the first semiconductor opening region and the second semiconductor opening region are arranged alternately. The first semiconductor opening region and the second semiconductor opening region are arranged alternately, and are respectively used to form two emitters. The width Wb of the first semiconductor opening region can be, for example, 100-300 μm.
[0078] In some preferred embodiments of the present disclosure, the preparation method further includes: S110, depositing a conductive film layer on the back of the semi-finished product obtained in S109. The conductive film layer is preferably a transparent conductive film, or a composite film layer composed of a transparent conductive film and a metal conductive film. The transparent conductive film can be, for example, zinc-doped, tin-doped, tungsten-doped, titanium-doped or silicon-doped indium oxide, or aluminum-doped, boron-doped or gallium-doped zinc oxide, and the metal conductive film is at least one of metallic aluminum, metallic copper, metallic silver, nickel alloy (such as nickel-copper alloy), and titanium alloy. More preferably, the conductive film layer is a composite film layer of tin-doped indium oxide, metallic copper, and nickel-copper alloy, and the square resistance of the conductive film layer is less than 0.2Ω / □, such as 0.1Ω / □. The present disclosure has no restriction on the thickness ratio of each layer in the composite film layer, as long as the required square resistance is met.
[0079] In some preferred embodiments of the present disclosure, the preparation method further includes: S111, forming an isolation trench in the conductive film layer between the first semiconductor opening region and the second semiconductor opening region. The width Wg of the isolation trench disclosed herein can be, for example, 50-200 μm, primarily to isolate the first semiconductor layer from the second semiconductor layer and reduce the occurrence of short circuits or leakage.
[0080] In some preferred embodiments of the present disclosure, the preparation method further includes: S112, forming metal electrodes at the first semiconductor opening region and the second semiconductor opening region. The process of forming the metal electrodes, for example, involves printing gate lines on the back side to form two metal electrodes at the first semiconductor opening region and the second semiconductor opening region of the silicon wafer.
[0081] In a second aspect, the present disclosure provides a sliced back-contact battery, which is obtained by the preparation method described in the first aspect.
[0082] The present disclosure will be further elaborated below in conjunction with specific embodiments.
[0083] Example 1
[0084] A sliced back contact battery is obtained by the following preparation method:
[0085] S100, as shown in FIG1 and FIG7, providing a double-sided polished silicon wafer 1, where the silicon wafer 1 is a single crystal silicon wafer;
[0086] S101, depositing a first semiconductor layer on the back side of the silicon wafer 1, wherein the first semiconductor layer comprises a tunneling oxide layer and an N-type doped polysilicon layer, wherein the thickness of the tunneling oxide layer is 1 nm, and the thickness of the N-type doped polysilicon layer is 100 nm;
[0087] S102, continuing to deposit a semiconductor mask layer on the first semiconductor layer, wherein the semiconductor mask layer is silicon oxynitride, and the purpose is to protect the first semiconductor from corrosion in a strong acid or alkaline solution or damage caused by subsequent processes;
[0088] S103 , as shown in FIG2 , forming a second semiconductor opening region 2 on the back surface, wherein the width Wa of the second semiconductor opening region 2 is 300 μm.
[0089] S104, as shown in FIG3 , cutting the silicon wafer 1 in half, cutting the silicon wafer 1 from the front side of the silicon wafer 1; this embodiment adopts cutting from the middle of the silicon wafer 1 into two equal parts;
[0090] The silicon wafer 1 is cut using a laser cutting method in a two-pass cutting mode. The first pass utilizes continuous scanning of a pulsed ultraviolet laser with a wavelength of approximately 355 nm and a pulse width of 20 picoseconds. The laser is spatially shaped into a flat-top laser spot with an overlap ratio of approximately 20%. The laser spot formed on the silicon wafer 1 is square. This first-pass cutting mode helps reduce damage to the coating layer caused by the propagation of micro-cracks in the laser melt zone.
[0091] The second pass uses a continuous scanning green pulsed laser with a wavelength of approximately 532 nm and a pulse width of 30 nanoseconds. The laser is a circular Gaussian laser with a spot overlap of approximately 40%. The laser creates a circular spot on silicon wafer 1. Using a green Gaussian laser in the second pass facilitates the rapid formation of a longitudinal molten zone on the bulk silicon, facilitating rapid cutting of silicon wafer 1.
[0092] S105. The cut cross section of the silicon wafer 1 is treated with atmospheric plasma. The atmospheric plasma nozzle moves at a speed of 1 cm / s over the cut cross section of the silicon wafer 1. The atmospheric plasma nozzle has a gas flow rate of 10 mL / min. The frequency of the radio frequency power supply is 320 kHz. The distance between the nozzle and the cut cross section of the silicon wafer 1 is 20 mm. The treatment time is 10 minutes.
[0093] The area of the plasma formed by the atmospheric plasma treatment is no more than 10 cm 2 Because the plasma is generated locally, the cutting surface can be controlled and processed more accurately, avoiding the damage of the coated first semiconductor layer and the laser opening area by the plasma, which will lead to performance degradation.
[0094] The gas source during the atmospheric plasma treatment utilizes components such as oxygen and hydrogen contained in the atmosphere.
[0095] S106 , cleaning and texturing the silicon wafer 1 after atmospheric plasma treatment, further cleaning and repairing the cut surface, and cleaning and texturing the second semiconductor opening region 2 and the front surface.
[0096] S107: Deposit a second semiconductor layer on the second semiconductor opening region 2 and on the surface of the first semiconductor layer. The second semiconductor layer includes a second semiconductor passivation layer and a second doped layer. The second semiconductor passivation layer is an intrinsic amorphous silicon layer with a thickness of 5 nm. The second doped layer is a P-type amorphous silicon layer with a thickness of 10 nm.
[0097] S108 , depositing a passivation layer and an anti-reflection layer on the front side.
[0098] S109, as shown in FIG4, thinly remove the second semiconductor layer above the first semiconductor layer on the back side to form a first semiconductor opening region 3, exposing the first semiconductor layer. The width Wb of the exposed first semiconductor layer is 100 μm. The first semiconductor opening region 3 is spaced apart from the second semiconductor opening region 2.
[0099] S110, depositing a conductive film layer on the back side of the battery, the conductive film layer being a composite film layer of tin-doped indium oxide, metallic copper, and nickel-copper alloy, and the sheet resistance of the conductive film layer being 0.1Ω / □.
[0100] S111. As shown in FIG5 , a gap isolation trench 4 with a width of Wg is formed between the first semiconductor opening region 3 and the second semiconductor opening region 2. The width of Wg is 50 μm, mainly for isolating the two semiconductor layers to reduce short circuit or leakage.
[0101] S112 , as shown in FIG6 , printing gate lines on the back side of the battery, and forming a first metal electrode 5 and a second metal electrode 6 at the first semiconductor opening region 3 and the second semiconductor opening region 2 of the silicon wafer 1 , respectively.
[0102] Example 2
[0103] The method of Example 1 was used, except that tubular PECVD was used for plasma treatment in S105 instead of atmospheric plasma treatment. The PECVD conditions were as follows: the treatment was carried out under the condition of introducing oxygen-containing gas (O2 and nitrogen), the total amount of oxygen-containing gas introduced was 2000sccm, the volume content of O2 in the oxygen-containing gas was 10%, the treatment time was controlled at 20min, and the power supply was 320kHz.
[0104] Example 3
[0105] The method of Example 1 was followed, except that the atmospheric plasma treatment in S105 lasted for 35 min and the area of the plasma formed did not exceed 10 cm 2 .
[0106] Example 4
[0107] The method of Example 1 was followed, except that the gas flow rate of the atmospheric plasma jet in S105 was 5 mL / min, and the area of the plasma formed did not exceed 10 cm 2 .
[0108] Example 5
[0109] The method of Example 1 is followed, except that the speed of the atmospheric plasma nozzle in step S105 is 3 cm / s when processing the silicon wafer cutting section, and the area of the plasma formed does not exceed 10 cm 2 .
[0110] Example 6
[0111] The method of Example 1 is followed, except that the distance between the air jet in S105 and the cut section of the silicon wafer is 30 mm, and the area of the plasma formed does not exceed 10 cm 2 .
[0112] Example 7
[0113] The method of Example 1 is referred to, except that the cutting in S104 adopts a one-pass cutting method (that is, the first-pass cutting is not performed, but the second-pass cutting of Example 1 is performed directly). Specifically, green light pulsed laser continuous scanning is directly adopted, with a wavelength of about 532nm and a pulse width of 30 nanoseconds. The laser is a circular Gaussian laser, and the overlap rate between the light spots is between 40%. The light spot formed on the silicon wafer by the laser is circular.
[0114] Example 8
[0115] The method of Example 1 is referred to, except that the pulse width of the first cutting in S104 is different, specifically 30 picoseconds.
[0116] Example 9
[0117] The method of Example 1 is referred to, except that the overlap rate between adjacent light spots in the first cutting in S104 is 0.
[0118] Example 10
[0119] The method of Example 1 is referred to, except that the overlap rate between adjacent light spots in the first cutting in S104 is 60%.
[0120] Example 11
[0121] The method of Example 1 is referred to, except that the overlap rate between adjacent light spots in the second cutting in S104 is 60%.
[0122] Comparative Example 1
[0123] The method of Example 1 is referred to, except that the atmospheric plasma treatment in S105 is not performed, but S106 is performed directly after S104.
[0124] Comparative Example 2
[0125] The method of Example 1 is referred to, except that the cutting is performed after the battery preparation is completed, that is, the cutting in S104 is performed after S112, and the plasma treatment in S105 is not performed.
[0126] Comparative Example 3
[0127] The method of Example 1 is referred to, except that the cutting and plasma treatment are performed after the battery preparation is completed, that is, the cutting in S104 is performed after S112, and the plasma treatment in S105 is performed after the cutting.
[0128] Test Case
[0129] The cell conversion efficiency of the back-contact cells obtained in the above examples and comparative examples was tested, and the production yield and manufacturing cost of each batch were measured. The results are shown in Table 1. The manufacturing cost is calculated as C = 1 + (1 - P) + (1 - E), where C is the manufacturing cost, P is the production yield, and E is the cell efficiency.
[0130] Table 1
[0131] It can be seen from the above results that, according to the embodiments and comparative examples, compared with the comparative examples, the embodiment scheme of the present disclosure can effectively improve the battery conversion efficiency, while helping to reduce the breakage rate and ensure a high production yield.
[0132] Furthermore, according to Examples 1 and 2 of the present disclosure, it can be seen that the solution of the preferred embodiment 1 of the present disclosure can be used to more centrally deal with residual debris and damage on the cut surface, avoid the spread of hidden cracks in the coated layer, and be more conducive to ensuring the improvement of the conversion efficiency of the half-cell battery after cutting. According to Examples 1 and 3-6 of the present disclosure, it can be seen that the appropriate atmospheric plasma process parameters can be controlled, which is more conducive to ensuring the production yield and battery conversion efficiency of the process, while reducing the cost of process manufacturing. According to Examples 1 and 7-11 of the present disclosure, it can be seen that the use of the preferred cutting scheme is more conducive to improving the production yield and battery conversion efficiency of the process, especially significantly improving the production yield, while reducing the cost of process manufacturing.
[0133] The preferred embodiments of the present disclosure are described in detail above, but the present disclosure is not limited thereto. Within the technical concept of the present disclosure, various simple variations of the technical solution of the present disclosure may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed by the present disclosure and fall within the scope of protection of the present disclosure. Industrial Applicability
[0134] The present invention performs cutting in the middle of the production process (i.e., after S103), retaining the processes and equipment configurations of the previous steps, improving production efficiency and maintaining the versatility of some of the original equipment. At the same time, it is supplemented by plasma treatment. On the one hand, the physical action of the plasma removes the residual broken silicon powder on the cut section, achieving a cleaning effect, which is conducive to subsequent thorough cleaning. On the other hand, the decomposed oxygen ions are used to oxidize the tip and loose parts of the cut section, which is conducive to the subsequent wet chemical etching of the tip residue and repair of cutting defects during cleaning, thereby improving the process production yield and battery efficiency, and basically does not increase the production cost. The overall process has very good industrial application prospects.
Claims
1. A method for preparing a sliced back contact battery, characterized in that: The following steps are involved: S101, depositing a first semiconductor layer on the back side of the silicon wafer; S102, continuing to deposit a semiconductor mask layer outside the first semiconductor layer; S103, opening a second semiconductor opening region on the back surface obtained in S102 to expose the silicon wafer in a corresponding region; S104, cutting the semi-finished product obtained in S103; S105, performing plasma treatment on the cut cross section of the silicon wafer obtained in S104; S106, then cleaning and texturing the semi-finished product obtained in S105; S107 , then depositing a second semiconductor layer on the back side of the semi-finished product obtained in S106 .
2. The preparation method according to claim 1, characterized in that: The cutting in S104 is performed by laser cutting or mechanical cutting.
3. The preparation method according to claim 2, characterized in that: The laser cutting method includes two-pass cutting, in which the first-pass cutting adopts ultraviolet pulse laser continuous scanning, the laser used is spatially shaped into a flat-top laser spot, and the overlap rate between adjacent spots is between 0-60%; the second-pass cutting adopts green light pulse laser continuous scanning, the laser used is a circular Gaussian laser, and the overlap rate between adjacent spots is between 30%-60%.
4. The preparation method according to claim 3, characterized in that: In the first cutting pass, the pulse width of the continuous scanning of the ultraviolet pulse laser is 10-30 picoseconds, and the spot formed by the laser used for the first cutting pass on the silicon wafer is square; in the second cutting pass, the pulse width of the continuous scanning of the green light pulse laser is 15-45 nanoseconds, and the spot formed by the laser used for the second cutting pass on the silicon wafer is circular.
5. The preparation method according to claim 1, characterized in that: In S104, the cutting is performed from the back side or the front side of the semi-finished product.
6. The preparation method according to claim 1, characterized in that: The plasma treatment in S105 is carried out by atmospheric plasma treatment, plate-type plasma enhanced chemical vapor deposition or tube-type plasma enhanced chemical vapor deposition.
7. The preparation method according to claim 6, characterized in that: The conditions of the atmospheric plasma treatment include: controlling the movement speed of the atmospheric plasma nozzle in the silicon wafer cutting section to be 0.1-3 cm / s, the gas flow rate of the atmospheric plasma jet nozzle to be 5-15 mL / min, the distance between the jet nozzle and the silicon wafer cutting section to be 10-30 mm, the frequency of the radio frequency power supply to be 40 kHz-13.56 MHz, and the area of the formed plasma to be no more than 10 cm 2 , the treatment time is 5-40min; the gas source of the atmospheric plasma is the atmosphere or an introduced gas containing oxygen and hydrogen, wherein the introduced gas containing oxygen and hydrogen is doped with 2 volume %-10 volume % oxygen, 2 volume %-10 volume % hydrogen, and an inert gas; and / or The conditions of the plate-type plasma enhanced chemical vapor deposition or the tube-type plasma enhanced chemical vapor deposition independently include: conducting the process under the condition of introducing an oxygen-containing gas, the total amount of the oxygen-containing gas introduced is 1000sccm-10000sccm, the volume content of O2 and / or N2O in the oxygen-containing gas is 1%-20%, the power supply frequency is controlled to be 40kHz-13.56MHz, and the processing time is 5-40min.
8. The preparation method according to claim 1, characterized in that: The first semiconductor layer includes a tunneling oxide layer and a first doped polysilicon layer; the second semiconductor layer includes a second semiconductor passivation layer and a second doped layer, the second semiconductor passivation layer is an intrinsic amorphous silicon layer or a microcrystalline silicon layer, and the second doped layer is an amorphous silicon layer or a microcrystalline silicon layer; one of the first doped polysilicon layer and the second doped layer is N-type and the other is P-type.
9. The preparation method according to claim 1, characterized in that: The preparation method further comprises: S100, providing a double-sided polished silicon wafer, and then performing subsequent S101; and / or S108, depositing a passivation layer and an anti-reflection layer on the front side of the semi-finished product obtained in S107; S109, removing a portion of the second semiconductor layer outside the first semiconductor layer on the back of the semi-finished product, forming a first semiconductor opening region to expose the first semiconductor layer, the first semiconductor opening region and the second semiconductor opening region being arranged alternately; S110, depositing a conductive film layer on the back side of the semi-finished product obtained in S109; S111, opening an isolation trench on the conductive film layer between the first semiconductor opening region and the second semiconductor opening region; S112, forming metal electrodes at the first semiconductor opening region and the second semiconductor opening region respectively.
10. A sliced back contact battery, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Heterojunction cell processing method, sliced heterojunction cell and heterojunction cell assembly
CN113555472A
Silicon wafer cutting method and battery
CN114823317A
Combined passivation back contact battery and preparation method thereof
CN115207137A
Mask-layer-free joint passivation back contact battery and preparation method thereof
CN115312633A
Double-sided tunneling silicon oxide passivated back contact solar cell and preparation method thereof
CN115621333A
Cited By
Method for synchronously realizing lossless cutting and passivation of solar cell
CN121078836A