Laminated cell having dual composite layers

By using tunneling junction and conductive layers as double composite layers in the laminated battery, the parasitic absorption and process damage caused by transparent conductive oxides in the prior art are solved, the filling factor and conversion efficiency are improved, and the cost is reduced.

WO2024230363A1PCT designated stage expired Publication Date: 2024-11-14LONGI GREEN ENERGY TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/085318
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-05
Filing Date
2024-04-01
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

When using transparent conductive oxides as composite layers, existing stacked batteries have serious problems of parasitic absorption and process damage, resulting in lower conversion efficiency and filling factors and higher cost.

Method used

The double composite layer structure is adopted, including a tunnel junction and a conductive layer as the composite layer, and the bottom battery is protected by the barrier effect of the tunnel junction, the conductive layer reduces parasitic absorption, and forms chemical bonds with the conductive layer through the self-assembly hole transport layer and the conductive layer. Improve charge transfer efficiency.

Benefits of technology

The filling factor and conversion efficiency of the stacked battery are improved, the open circuit voltage loss is reduced, the leakage is reduced, and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024085318_14112024_PF_FP_ABST
    Figure CN2024085318_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of solar cells. Particularly disclosed is a laminated cell having dual composite layers. The laminated cell having dual composite layers comprises a bottom cell, a tunnel junction, a conductive layer, a first carrier transport layer, a perovskite absorption layer, a second carrier transport layer, a tin dioxide layer and a transparent electrode layer which are sequentially laminated, wherein the electricity conduction types of the first carrier transport layer and the second carrier transport layer are opposite.
Need to check novelty before this filing date? Find Prior Art

Description

Laminated battery with double composite layers

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 5, 2023, with application number 202310496033.9 and invention name “Laminated battery with double composite layer”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the technical field of solar cells, and in particular to a stacked cell with a double composite layer. Background Art

[0003] Monocrystalline silicon solar cells occupy the vast majority of the photovoltaic market due to their high conversion efficiency and low cost. Currently, the world's highest conversion efficiency of monocrystalline silicon solar cells is 26.81%, created by Longi's heterojunction technology, which is very close to the theoretical efficiency of 29.4%. An effective way to break through the theoretical limit is to develop tandem cell technology, that is, stacking absorption layers with different band gaps together to reduce heat loss. Simulations show that tandem cells at both ends of the surface can achieve a theoretical efficiency of 43%. Perovskite has become the preferred top cell material in tandem cells due to its easy processing, low cost, and easy band gap adjustment. Recently, the Helmholtz Zentrum Berlin (HZB) in Germany created a conversion efficiency of 32.5%.

[0004] The structure of a two-terminal perovskite / silicon tandem cell consists of a perovskite top cell and a silicon base cell, with a composite layer connecting the top and bottom cells. The composite layer serves as a link between the top and bottom cells and requires high transmittance, good chemical stability, simple processing, and suitable energy level matching for efficient electron / hole recombination while maintaining low resistance to achieve current matching. This is crucial to the performance of the perovskite / silicon tandem cell device.

[0005] Summary of the Invention

[0006] The purpose of the present application is to provide a stacked battery with double composite layers.

[0007] Specifically, this application involves the following aspects:

[0008] A stacked battery with a double composite layer includes a bottom battery, a tunnel junction, a conductive layer, a first carrier transport layer, a perovskite absorption layer, a second carrier transport layer, a tin dioxide layer and a transparent electrode layer stacked in sequence, wherein the first carrier transport layer and the second carrier transport layer have opposite conductivity types.

[0009] Optionally, the tunnel junction structure is selected from one or more of a hydrogen-doped n-type microcrystalline silicon stacked with a hydrogen-doped p-type microcrystalline silicon structure, an oxygen-doped n-type amorphous silicon stacked with an oxygen-doped p-type amorphous silicon structure, and a microcrystalline silicon stacked with a silicon oxide structure.

[0010] Optionally, the thickness of the tunnel junction is 0.5 nm to 50 nm.

[0011] Optionally, the conductivity of the conductive layer is greater than 1000 S / m.

[0012] Optionally, the transmittance of the conductive layer in the light wave range of 300nm to 1200nm is greater than 80%.

[0013] Optionally, the work function of the conductive layer is 4.5 eV to 5.4 eV.

[0014] Optionally, the carrier concentration of the conductive layer is 1.5×10 15 cm -3 to 4.5×10 20 cm -3 .

[0015] Optionally, the material of the conductive layer is selected from one or more of indium tin oxide, indium zinc oxide, indium tungsten oxide, indium oxide, zinc aluminum oxide, zinc gallium oxide, zinc oxide, antimony tin oxide, fluorine tin oxide, tin oxide, and titanium dioxide.

[0016] Optionally, the conductive layer has a thickness of 0.5 nm to 20 nm.

[0017] Optionally, the first carrier transport layer is a hole transport layer, and the material of the first carrier transport layer includes a material that can form a chemical bond with the material of the conductive layer.

[0018] Optionally, the material of the first carrier transport layer is selected from one of [4-(9H-carbazole-9-yl)butyl]phosphonic acid (4PACz), [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz), [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), and [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz).

[0019] Optionally, the stacked cell further includes metal electrodes respectively arranged on the bottom cell and the transparent electrode layer on a side away from the perovskite absorption layer.

[0020] Optionally, the bottom cell is selected from one or more of a heterogeneous crystalline silicon cell, a tunneling oxide layer passivated contact solar cell, a passivated emitter and back cell, a back contact cell, and a tin-lead perovskite.

[0021] This application utilizes a tunnel junction and a conductive layer deposited on the tunnel junction as a dual composite layer, facilitating lateral charge collection and improving the fill factor of the stacked battery. The conductive layer reduces parasitic absorption, increases the stacked battery current, and improves the contact resistance between the top cell's charge transfer layer and the tunnel junction, thereby increasing the stacked battery's fill factor. The tunnel junction acts as a barrier during the fabrication of the conductive layer, protecting the bottom cell from process damage and improving the stacked battery's open-circuit voltage.

[0022] Furthermore, a hole transport layer with self-assembly capability is used, which can be anchored to the conductive layer through chemical bonds, and can well cover the battery surface, especially the battery surface with a velvet structure, thereby reducing leakage.

[0023] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present application or related technologies, the following is a brief introduction to the drawings required for use in the embodiments or related technical descriptions. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0025] FIG1 is a schematic diagram of a stacked battery of the present application.

[0026] Reference numerals:

[0027] 1- bottom cell, 2- tunnel junction, 3- conductive layer, 4- first carrier transport layer, 5- perovskite absorption layer, 6- second carrier transport layer, 7- tin dioxide layer, 8- transparent electrode layer, 9- metal electrode. Specific embodiments

[0028] To make the purpose, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0029] At present, without losing the precursor of electrical and optical properties, it is required to realize the recombination of carriers extracted from the battery with opposite carriers extracted from the perovskite battery. One way is to choose transparent conductive oxide as the composite layer, such as indium tin oxide (ITO). In 2016, Steve Albrecht et al. of the Berlin Helmholtz Center (HZB) in Berlin, Germany reported that the titanium ore / silicon tandem battery used ITO as the middle composite layer and matched it with low-temperature tin dioxide, achieving a conversion efficiency of 18%. Among them, the open circuit voltage reached 1.78V and the short circuit current was 14.0mA / cm 2 , fill factor 79.5% (DOI:10.1039 / c5ee02965a). In 2017, Kevin A.Bush et al. from Stanford University in the United States also reported a titanium ore / silicon tandem cell with a conversion efficiency of 23.6% using ITO as the composite layer, with an open circuit voltage of 1.65V and a short circuit current of 18.1mA / cm 2 , fill factor 79.0% (DOI:10.1038 / nenergy.2017.9). The second is to select microcrystalline silicon tunnel junction (nc-Si (n + ) / nc-Si(p + )) as a composite layer. In 2018, Florent Sahli and others from the Swiss Federal Institute of Technology in Lausanne were inspired by the III-V group tandem cells and used microcrystalline silicon as a composite layer to achieve a conversion efficiency of 25% for titanium ore / silicon tandem cells. At the same time, thanks to the weak lateral conductivity of microcrystalline silicon, at 12cm 2 A conversion efficiency of 18% was achieved over a large area (DOI:10.1039 / c5ee02965a).

[0030] Transparent conductive oxides are mostly prepared by magnetron sputtering, which causes serious damage to silicon bottom cells, especially those that are extremely sensitive to heterojunction silicon cells. At the same time, commonly used transparent conductive materials such as ITO have serious parasitic absorption after 800nm, which limits the short-circuit current of the stacked cells. In addition, as a precious metal, indium is expensive. In high-efficiency stacked cells, perovskite top cells often use organic materials as hole transport layers, such as 2,2',7,7'-tetrakis(di-p-tolylamino)spiro-9,9'- Difluorene (spiro-TTB), poly [bis (4-phenyl) (2,4,6-trimethylphenyl) amine] (PTAA), [4- (3,6-dimethyl-9H-carbazol-9-yl) butyl] phosphonic acid (Me-4PACz), [2- (3,6-dimethoxy-9H-carbazol-9-yl) ethyl] phosphonic acid (MeO-2PACz), [2- (9H-carbazol-9-yl) ethyl] phosphonic acid (2PACz), etc., while organic materials and microcrystalline silicon tunneling junction (nc-Si (n + ) / nc-Si(p +)) There is a serious open-circuit voltage loss between them. For example, the open-circuit voltages of 1.79V reported by the Swiss Federal University of Technology in Lausanne in 2018 and 1.91V reported in 2022 are both lower than the open-circuit voltage of the ITO composite layer under the same band gap. In addition, due to the weak lateral conductivity of the tunnel junction itself, it is impossible to efficiently collect and transmit charges, resulting in a lower fill factor.

[0031] To address the above issues, the present application provides a stacked battery with a double composite layer. As shown in Figure 1, the stacked battery of the present application includes a bottom battery 1, a tunneling junction 2, a conductive layer 3, a first carrier transport layer 4, a perovskite absorption layer 5, a second carrier transport layer 6, a tin dioxide layer 7, and a transparent electrode layer 8, which are stacked in sequence. The first carrier transport layer 4 and the second carrier transport layer 6 have opposite conductivity types. That is, if the first carrier transport layer 4 is a hole transport layer, the second carrier transport layer 6 is an electron transport layer; if the first carrier transport layer 4 is an electron transport layer, the second carrier transport layer 6 is a hole transport layer.

[0032] In a specific embodiment, the structure of the tunnel junction 2 is selected from a structure of hydrogen-doped n-type microcrystalline silicon stacked with hydrogen-doped p-type microcrystalline silicon (nc-Si:H(n + ) / nc-Si:H(p + )), oxygen-doped n-type amorphous silicon stacked with oxygen-doped p-type amorphous silicon structure (a-Si:H(n + ) / a-Si:H(p + )), and microcrystalline silicon stacked silicon oxide structure (nc-Si:H(n + ) / SiO2) or more.

[0033] In the preparation process, when the tunnel junction 2 is deposited on the n-side of the bottom cell 1, n-type microcrystalline silicon / amorphous silicon is deposited first, and then p-type microcrystalline silicon / amorphous silicon is deposited thereon; when the tunnel junction 2 is deposited on the p-side of the bottom cell 1, p-type microcrystalline silicon / amorphous silicon is deposited first, and then n-type microcrystalline silicon / amorphous silicon is deposited thereon.

[0034] In a specific embodiment, the thickness of the tunnel junction 2 is 0.5 nm to 50 nm, for example, it can be 0.5 nm, 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, 30 nm, 31 nm, 32 nm, 33 nm, 34 nm, 35 nm, 36 nm, 37 nm, 38 nm, 39 nm, 40 nm, 41 nm, 42 nm, 43 nm, 44 nm, 45 nm, 46 nm, 47 nm, 48 nm, 49 nm, 50 nm, and any ranges therebetween.

[0035] In a specific embodiment, the thickness of the tunnel junction 2 is 5 nm to 15 nm.

[0036] The conductive layer 3 is a metal oxide layer, and its material can be selected from one or more of indium tin oxide (ITO), indium zinc oxide (IZO), indium tungsten oxide (IWO), indium oxide (ln2O3), zinc aluminum oxide (AZO), zinc gallium oxide (GZO), zinc oxide (ZnO2), antimony tin oxide (ATO), fluorine tin oxide (FTO), tin oxide (SnO2), and titanium dioxide (TiO2).

[0037] In a specific embodiment, the electrical conductivity of the conductive layer 3 is greater than 1000 S / m, for example, 1001 S / m, 1100 S / m, 1200 S / m, 1300 S / m, 1400 S / m, 1500 S / m, 1600 S / m, 1700 S / m, 1800 S / m, 1900 S / m, 2000 S / m, and any range therebetween.

[0038] In a specific embodiment, the transmittance of the conductive layer 3 in the wavelength range of 300 nm to 1200 nm is greater than 80%, for example, it can be 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, and any range therebetween.

[0039] In a specific embodiment, the work function of the conductive layer 3 is 4.5 eV to 5.4 eV, for example, 4.5 eV, 4.6 eV, 4.7 eV, 4.8 eV, 4.9 eV, 5 eV, 5.1 eV, 5.2 eV, 5.3 eV, 5.4 eV, and any range therebetween.

[0040] In a specific embodiment, the carrier concentration of the conductive layer 3 is 1.5×10 15 cm -3 to 4.5×10 20 cm -3 For example, it can be 1.5×10 15 cm -3 , 2×10 15 cm -3 , 5×10 15 cm -3 , 1×10 16 cm -3 , 2×10 16 cm -3 , 5×10 16 cm -3 , 1×10 17 cm -3 , 2×10 17 cm -3 , 5×10 17 cm -3 , 1×10 18 cm -3 , 2×10 18 cm -3 , 5×10 18 cm -3 , 1×10 19 cm -3 , 2×10 19 cm -3 , 5×10 19 cm -3 , 1×10 20 cm -3 , 2×10 20 cm -3 , 4.5×10 20 cm -3 , and any ranges between these values.

[0041] Among them, the conductivity, work function, carrier concentration, conductivity and carrier concentration of the conductive layer can be tested using a Hall effect tester, and the work function can be tested using ultraviolet photoelectron spectroscopy.

[0042] In a specific embodiment, the thickness of the conductive layer 3 is 0.5 nm to 20 nm, for example, 0.5 nm, 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, and any range therebetween.

[0043] In a specific embodiment, the thickness of the conductive layer 3 is 1 nm to 10 nm.

[0044] When preparing the conductive layer 3, those skilled in the art will appreciate that different processes can be selected depending on the type of bottom cell 1. For example, when the bottom cell 1 is a silicon heterojunction cell, the conductive layer 3 can be deposited using methods such as PVD, ALD, and spin coating, with the deposition temperature being less than 250°C. Alternatively, the temperature can be less than 190°C. When the bottom cell 1 is a passivated emitter and back cell, or a tunneling oxide layer passivated contact solar cell, the deposition temperature can be higher than 190°C.

[0045] The tunnel junction 2 and conductive layer 3 of the present application serve together as a composite layer of the stacked battery, facilitating lateral charge collection and improving the stacked battery's fill factor. The conductive layer 3 can reduce parasitic absorption, increase the stacked battery's current, improve the contact resistance between the top cell's charge transfer layer and the tunnel junction 2, and increase the stacked battery's fill factor. The tunnel junction 2 acts as a barrier during the preparation of the conductive layer 3, protecting the bottom cell 1 from process damage and improving the stacked battery's open-circuit voltage.

[0046] The first carrier transport layer 4 may be an electron transport layer or a hole transport layer.

[0047] In a specific embodiment, the first carrier transport layer 4 is a hole transport layer with self-assembly capability, and the material of the first carrier transport layer 4 includes a material capable of forming a chemical bond with the material of the conductive layer 3. For example, it may include a phosphonate functional group, a sulfate functional group, or a carboxylate functional group. The material of the first carrier transport layer 4 may be various single-molecule self-assembly materials known in the art. For example, [4-(9H-carbazole-9-yl)butyl]phosphonic acid (4PACz), [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz), [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz), etc. The hole transport layer with self-assembly ability can be anchored to the conductive layer 3 through chemical bonds, so that the battery surface can be well covered, especially the battery surface with a velvet structure, to reduce leakage.

[0048] The band gap of the bottom cell 1 is in the range of 0.6 eV to 1.4 eV, and can be various types of bottom cells known in the art, such as n-type heterojunction silicon cell (HIT), p-type heterojunction silicon cell (HIT), n-type tunneling oxide passivated contact solar cell (Topcon), p-type tunneling oxide passivated contact solar cell (Topcon), n-type passivated emitter and back cell (PERC), p-type passivated emitter and back cell (PERC), back contact cell (BC), tin-lead perovskite cell, etc.

[0049] The band gap of the perovskite absorption layer 5 is 1.5 eV to 2.0 eV, and may be various types of perovskite top cells known in the art.

[0050] The stacked cell further includes metal electrodes 9 respectively arranged on the bottom cell 1 and the transparent electrode layer 8 on a side away from the perovskite absorption layer 5 .

[0051] The second carrier transport layer 6 , the tin dioxide layer 7 , the transparent electrode layer 8 and the metal electrode can be prepared based on techniques known in the art.

[0052] In a specific embodiment, the stacked cell comprises a bottom cell 1, a tunnel junction 2, a conductive layer 3, a first carrier transport layer 4, a perovskite absorption layer 5, a second carrier transport layer 6, a tin dioxide layer 7 and a transparent electrode layer 8 stacked in sequence, and a metal electrode 9 disposed on the side of the bottom cell 1 and the transparent electrode layer 8 away from the perovskite absorption layer 5. The structure of the tunnel junction 2 is selected from a hydrogen-doped n-type microcrystalline silicon stacked with a hydrogen-doped p-type microcrystalline silicon structure (nc-Si:H(n + ) / nc-Si:H(p + )), oxygen-doped n-type amorphous silicon stacked with oxygen-doped p-type amorphous silicon structure (a-Si:H(n + ) / a-Si:H(p + )), and microcrystalline silicon stacked silicon oxide structure (nc-Si:H(n + ) / SiO2); the thickness of tunnel junction 2 is 0.5 nm to 50 nm. The material of conductive layer 3 is selected from one or more of indium tin oxide (ITO), indium zinc oxide (IZO), indium tungsten oxide (IWO), indium oxide (ln2O3), aluminum zinc oxide (AZO), zinc gallium oxide (GZO), zinc oxide (ZnO2), antimony tin oxide (ATO), fluorine tin oxide (FTO), tin oxide (SnO2), and titanium dioxide (TiO2); the thickness of conductive layer 3 is 0.5 nm to 20 nm.

[0053] In a specific embodiment, the stacked battery includes a bottom battery 1, a tunnel junction 2, a conductive layer 3, a first carrier transport layer 4, a perovskite absorption layer 5, a second carrier transport layer 6, a tin dioxide layer 7 and a transparent electrode layer 8 stacked in sequence, and a metal electrode 9 arranged on the side of the bottom battery 1 and the transparent electrode layer 8 away from the perovskite absorption layer 5. Among them, the first carrier transport layer 4 is a hole transport layer, and the second carrier transport layer 6 is an electron transport layer. The material of the first carrier transport layer is selected from [4-(9H-carbazol-9-yl)butyl]phosphonic acid (4PACz). The structure of the tunnel junction 2 is selected from hydrogen-doped n-type microcrystalline silicon stacked with hydrogen-doped p-type microcrystalline silicon structure (nc-Si:H(n + ) / nc-Si:H(p + )), oxygen-doped n-type amorphous silicon stacked with oxygen-doped p-type amorphous silicon structure (a-Si:H(n + ) / a-Si:H(p + )), and microcrystalline silicon stacked silicon oxide structure (nc-Si:H(n + ) / SiO2). The thickness of tunnel junction 2 is 5 nm to 15 nm. The material of conductive layer 3 is selected from one or more of indium tin oxide (ITO), indium zinc oxide (IZO), indium tungsten oxide (IWO), indium oxide (ln2O3), aluminum zinc oxide (AZO), zinc gallium oxide (GZO), zinc oxide (ZnO2), antimony tin oxide (ATO), fluorine tin oxide (FTO), tin oxide (SnO2), and titanium dioxide (TiO2). The thickness of conductive layer 3 is 1 nm to 10 nm.

[0054] Example 1

[0055] As shown in Figure 1, the stacked battery includes a bottom battery 1, a tunnel junction 2, a conductive layer 3, a first carrier transport layer 4, a perovskite absorption layer 5, a second carrier transport layer 6, a tin dioxide layer 7 and a transparent electrode layer 8 stacked in sequence, and a metal electrode 9 arranged on the side of the bottom battery 1 and the transparent electrode layer 8 away from the perovskite absorption layer 5, wherein the first carrier transport layer 4 is a hole transport layer and the second carrier transport layer 6 is an electron transport layer.

[0056] The method for preparing the stacked battery of this embodiment is as follows:

[0057] Step 1: Provide an n-type heterogeneous crystalline silicon cell as a bottom cell, as a substrate, excluding the n-side ITO layer and the front and back electrodes.

[0058] Step 2: Deposit hydrogen-doped n-type microcrystalline silicon on the n-side of the bottom cell, and then deposit hydrogen-doped p-type microcrystalline silicon to form a tunnel junction structure, both using PECVD deposition, with a total thickness of 10nm.

[0059] Step 3: Deposit an ITO layer on the tunnel junction using PVD with a thickness of 5 nm, and anneal at 190° C. for 30 min after deposition.

[0060] Step 4: Deposit [4-(9H-carbazol-9-yl)butyl]phosphonic acid (4PACz) as the hole transport layer of the top cell on the ITO layer with a concentration of 1 mg / ml and anneal at 100°C for 10 min to remove residual solvent. The thickness is 3 nm.

[0061] Step 5: Deposit a wide bandgap perovskite layer on the hole transport layer. The composition of the perovskite layer is Cs 0.5 FA 0.8 MA 0.15 Pb(I 0.77 Br 0.23 )3, the band gap is 1.66eV, and its thickness is 1μm.

[0062] Step 6: Depositing C on the perovskite layer 60 As the electron transport layer, its thickness is 20nm and it is placed between the perovskite layer and the C 60 A thin layer of LiF with a thickness of 1 nm is doped in between to passivate the defects of the perovskite layer.

[0063] Step 7: ALD is used to deposit tin dioxide on the electron transport layer as a buffer layer during magnetron sputtering to prevent damage to the perovskite layer when sputtering ITO. The thickness is 15nm, and then PVD is used to deposit a 100nm ITO transparent electrode.

[0064] Step 8: Deposit silver on the front and back sides as electrodes for the stacked cell, thus forming a complete perovskite / crystalline silicon stacked cell.

[0065] Example 2-Example 5

[0066] The tandem cells of Examples 2 to 5 differ from the tandem cell of Example 1 only in the thickness of the tunnel junction. Specifically, the thickness of the tunnel junction in Example 2 is 3 nm, the thickness of the tunnel junction in Example 3 is 8 nm, the thickness of the tunnel junction in Example 4 is 15 nm, and the thickness of the tunnel junction in Example 5 is 20 nm.

[0067] Example 6

[0068] The only difference between the stacked cell of Example 6 and the stacked cell of Example 1 is the structure of the tunnel junction, wherein the tunnel junction in Example 6 is a-Si:H(n+) / a-Si:H(p+).

[0069] Example 7-Example 9

[0070] The laminated cells of Examples 7-9 differ from the laminated cell of Example 1 only in the thickness of the transparent conductive film, i.e., the conductive layer. The thickness of the conductive layer in Example 7 is 3 nm, the thickness of the conductive layer in Example 8 is 1 nm, and the thickness of the conductive layer in Example 9 is 12 nm.

[0071] Example 10-Example 12

[0072] The laminated cells of Examples 10 to 12 differ from the laminated cell of Example 1 only in the conductive layer material. The conductive layer in Example 10 is made of IZO, the conductive layer in Example 11 is made of In2O3, and the conductive layer in Example 12 is made of ZnO.

[0073] Example 13-Example 19

[0074] The tandem cells of Examples 13 to 19 differ from the tandem cell of Example 1 only in the bottom cell. The bottom cell of Example 13 is a p-type HIT cell, the bottom cell of Example 14 is an n-type Topton cell, the bottom cell of Example 15 is a p-type Topton cell, the bottom cell of Example 16 is an n-type PERC cell, the bottom cell of Example 17 is a p-type PERC cell, the bottom cell of Example 18 is a p-type HIT cell, and the bottom cell of Example 19 is a tin-lead perovskite cell.

[0075] Comparative Example 1

[0076] The laminated battery of Comparative Example 1 differs from the laminated battery of Example 1 only in that it does not have a conductive layer.

[0077] Comparative Example 2

[0078] The difference between the stacked battery of Comparative Example 2 and the stacked battery of Example 1 is that there is no tunneling junction layer, and the thickness of the conductive layer is 20 nm.

[0079] The parameters of the above embodiments and comparative examples, as well as the performance of the obtained stacked batteries are shown in Table 1.

[0080] Table 1 shows the parameters of each embodiment and comparative example and the performance of the stacked battery

[0081] The device embodiments described above are merely illustrative. The units described as separate components may or may not be physically separate, and the components shown as units may or may not be physical units, i.e., they may be located in one location or distributed across multiple network units. Some or all of the modules may be selected based on actual needs to achieve the objectives of the present embodiment. Persons of ordinary skill in the art will be able to understand and implement the present invention without inventive effort.

[0082] References herein to "one embodiment," "an embodiment," or "one or more embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment of the present application. Furthermore, please note that examples of the phrase "in one embodiment" herein do not necessarily all refer to the same embodiment. In the description provided herein, numerous specific details are described. However, it is understood that embodiments of the present application may be practiced without these specific details. In some instances, well-known methods, structures, and techniques are not shown in detail so as not to obscure the understanding of this description.

[0083] In the claims, any reference signs placed between brackets shall not be construed as limiting the claim. The word "comprising" does not exclude the presence of elements or steps not listed in the claim. The word "a" or "an" preceding an element does not exclude the presence of a plurality of such elements. The present application may be implemented by means of hardware comprising several different elements and by means of a suitably programmed computer. In a unit claim enumerating several means, several of these means may be embodied by one and the same item of hardware. The use of the words first, second, and third etc. does not indicate any order. These words may be interpreted as names.

[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A stacked battery with a double composite layer, comprising a bottom battery, a tunnel junction, a conductive layer, a first carrier transport layer, a perovskite absorption layer, a second carrier transport layer, a tin dioxide layer and a transparent electrode layer stacked in sequence, in, The first carrier transport layer and the second carrier transport layer have opposite conductivity types.

2. The laminated battery according to claim 1, in, The structure of the tunnel junction is selected from one or more of a hydrogen-doped n-type microcrystalline silicon stacked with a hydrogen-doped p-type microcrystalline silicon structure, an oxygen-doped n-type amorphous silicon stacked with an oxygen-doped p-type amorphous silicon structure, and a microcrystalline silicon stacked with a silicon oxide structure.

3. The laminated battery according to claim 1 or 2, in, The thickness of the tunnel junction is 0.5 nm to 50 nm.

4. The laminated battery according to any one of claims 1 to 3, in, The electrical conductivity of the conductive layer is greater than 1000 S / m.

5. The laminated battery according to any one of claims 1 to 4, in, The transmittance of the conductive layer in the light wave range of 300nm to 1200nm is greater than 80%.

6. The laminated battery according to any one of claims 1 to 5, in, The work function of the conductive layer is 4.5 eV to 5.4 eV.

7. The laminated battery according to any one of claims 1 to 6, in, The carrier concentration of the conductive layer is 1.5×10 15 cm -3 Up to 4.5×10 20 cm -3 .

8. The laminated battery according to any one of claims 1 to 7, in, The material of the conductive layer is selected from one or more of indium tin oxide, indium zinc oxide, indium tungsten oxide, indium oxide, zinc aluminum oxide, zinc gallium oxide, zinc oxide, antimony tin oxide, fluorine tin oxide, tin oxide, and titanium dioxide.

9. The laminated battery according to any one of claims 1 to 8, in, The thickness of the conductive layer is 0.5 nm to 20 nm.

10. The laminated battery according to any one of claims 1 to 9, in, The first carrier transport layer is a hole transport layer, and the material of the first carrier transport layer includes a material that can form a chemical bond with the material of the conductive layer.

11. The laminated battery according to claim 10, in, The material of the first carrier transport layer is selected from one of [4-(9H-carbazole-9-yl)butyl]phosphonic acid (4PACz), [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz), [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), and [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz).

12. The laminated battery according to any one of claims 1 to 11, in, The stacked cell further includes metal electrodes respectively arranged on the bottom cell and the transparent electrode layer at a side away from the perovskite absorption layer.

13. The laminated battery according to any one of claims 1 to 12, in, The bottom cell is selected from one or more of a heterogeneous crystalline silicon cell, a tunneling oxide layer passivated contact solar cell, a passivated emitter and back cell, a back contact cell, and a tin-lead perovskite.

Citation Information

Patent Citations

  • Structure design of tunnel junction in Perovskite / silicon heterojunction lamination solar battery

    CN107564989A

  • Method for simultaneously improving open-circuit voltage and stability of full-suede perovskite / crystalline silicon laminated solar cell

    CN114267789A

  • Perovskite-based solar cell

    CN115440891A

  • Laminated battery with double composite layers

    CN116634791A