Process for producing sulfur-carbon composites

The use of an extruder to react sulfur and carbon at elevated temperatures ensures thorough sulfur infiltration into carbon airgel micropores, addressing the inefficiencies of previous methods by enhancing throughput and reducing energy consumption, facilitating the production of high-quality sulfur-carbon composites for applications like metal-sulfur batteries.

WO2024231267A1PCT designated stage expired Publication Date: 2024-11-14DEUTSCHES ZENTRUM FÜR LUFT UND RAUMFAHRT E V
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/062241
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-05
Filing Date
2024-05-03
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Existing methods for producing sulfur-carbon composites, such as gas infiltration, melt infiltration, and grinding infiltration, are time and energy intensive, limit material throughput, and fail to achieve sufficient sulfur infiltration into the micropores of carbon materials, making them economically unfeasible for large-scale production.

Method used

A continuous process using an extruder to react sulfur and carbon at temperatures of 300°C or more, allowing short-chain sulfur molecules to penetrate the micropores of carbon airgel, significantly increasing throughput and reducing energy consumption, while enabling complete pore infiltration.

Benefits of technology

This process allows for the efficient production of sulfur-carbon composites with high sulfur content in micropores, reducing energy requirements and processing time, enabling the production of larger quantities with lower lead times and improved economic viability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024062241_14112024_PF_FP_ABST
    Figure EP2024062241_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a process for producing sulfur-carbon composites, in particular sulfur-carbon aerogel composites, which are produced by way of extrusion at a temperature of at least 300°C.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Process for the production of sulfur-carbon composites

[0002] The invention relates to a process for producing sulfur-carbon composites, in particular sulfur-carbon aerogel composites, which are produced by extrusion.

[0003] In a metal-sulfur battery, sulfur is an electrochemically active material. At room temperature, sulfur is known to exist as crown-shaped cyclooctasulfur (α-S8). At 95.5 °C, orthorhombic sulfur (α-S8) is converted into monoclinic β-sulfur; this melts at 119.6 °C (Meyer B (1976) Elemental sulfur. Chem. Rev. 76: 367. D01 : 10.1021 / cr60301a003). Above 120 °C, sulfur rings of various sizes (Sn, n=5-33) are present in the sulfur melt. At temperatures above 159 °C, the melt viscosity increases dramatically due to radical ring-opening polymerization. Upon further heating, the viscosity decreases again above 243 °C, and short (Sn, n<6) sulfur chains form. The boiling point is 444 °C. In the gaseous state, sulfur molecules exist in the form of S2-8, with the equilibrium shifting toward S2 species with increasing temperatures.In the gaseous state at 600 °C, sulfur exists in the form of S6 (about 58.8%) and about 16.4% in the form of S2 molecules. These short-chain sulfur radicals can deposit in micropores of a carbon material (e.g., activated carbon) and also form covalent bonds with carbon (Korpiel JA, Vidic RD (1997) Effect of Sulfur Impregnation Method on Activated Carbon Uptake of Gas-Phase Mercury; Environmental Science & Technology 31 : 2319. DOI: 10.1021 / es9609260). There are several processes for producing such composites, often referred to as infiltration or impregnation. One method, gas infiltration, usually takes place at 400-600 °C, so that the sulfur is in the gas phase, and takes about two to six hours (Liu W, Vidic RD, Brown TD (1998) Optimization of Sulfur Impregnation Protocol for Fixed-Bed Application of Activated Carbon-Based Sorbents for Gas-Phase Mercury Removal. Environmental Science & Technology 32: 531. D01 : 10.1021 / es970630 ; Nojabaee M, Sievert B, Schwan M, et al. (2021) Ultramicroporous carbon aerogels encapsulating sulfur as the cathode for lithium-sulfur batteries. J. Mater. Chem. A 9: 6508. DOI: 10.1039 / D0TA11332H). With this method, a large portion of the sulfur is also introduced into the micropores. However, the entire process, including heating and cooling phases, can take over 10 hours and is therefore very time- and energy-intensive. Furthermore, the processes established so far can only process very small quantities of sample. Furthermore, the processes are carried out as batch processes. For the processing of large quantities, the effort increases so significantly that the processes are not economically feasible.

[0004] Sulfur-carbon composites can also be produced using melt infiltration. For this, a sulfur-carbon mixture is heated to the melting temperature or higher and held at this temperature for several hours. The following process parameters are known from the literature: T=280 °C, holding time 12 hours (Balakumar K, Kalaiselvi N (2015) High sulfur loaded carbon aerogel cathode for lithium-sulfur batteries. RSC Advances 5: 34008. DOI: 10.1039 / C5RA01436K], T=150-300 °C); (Wei S, Xu S, Agrawral A, et al. (2016) A stable room-temperature sodium-sulfur battery. Nature Communications 7: 11722. DOI: 10.1038 / ncommsll722]) or T=155 °C with holding time 5 hours (Choudhury S, Krüner B, Massuti-Ballester P, et al. (2017) Microporous novolac-derived carbon beads / sulfur hybrid cathode for lithium-sulfur batteries. J. Power Sources 357: 198. DOI: https: / / doi.Org / 10.1016 / j.jpowsour.2017.05.005).Another method for producing sulfur-carbon composites is milling infiltration, in which a sulfur-carbon mixture is milled in a mill (e.g. ball mill) for 15 min at 550 rpm (Häcker J, Danner C, Sievert B, et al. (2020) Investigation of Magnesium-Sulfur Batteries using Electrochemical Impedance Spectroscopy. Electrochim. Acta 338: 135787.

[0005] DOI: https: / / doi.org / 10.1016 / j.electacta.2020.135787) or 30 min at Fedorkova AS, Kazda T, Gavalierova K, Gomez-Romero P, Shembel E (2018) Synthesis and Characterization of Porous Sulfur / MWCNTs Composites with Improved Performance and Safety as Cathodes for Li-S Batteries. Int. J. Electrochem. Sci. 13: 551. DOI: 10.20964 / 2018.01.67. In both melt infiltration and mill infiltration, sulfur is still present in longer chains due to the lower temperatures, so that the micropores can only be infiltrated to a small extent.

[0006] The main disadvantages of producing sulfur-carbon composites by gas infiltration are the small material quantities, the long processing time, and the high energy consumption. While melt infiltration and mill infiltration can be performed with larger quantities and in a shorter time, unlike gas infiltration, they do not achieve sufficient infiltration of the sulfur into the micropores of the carbon.

[0007] DE 10 2014 210 249 A1 discloses the extrusion of sulfur and carbon, in particular conductive carbon black, for the production of a battery cell cathode. This does not involve microporous carbon. The goal of the process is to mix the sulfur and carbon material, not to infiltrate the sulfur into the pores of the porous carbon material.

[0008] In the publication US 2017 / 0 313 844 A1, a corresponding mixture is introduced into an extruder to produce a masterbatch of carbon nanofibers and sulfur. This masterbatch, too, is not microporous carbon. The goal of the process is also to mix the sulfur and the carbon material, not to infiltrate the sulfur into the pores of the porous carbon material.

[0009] EP 2 966 708 B1 also describes a combination of carbon material with sulfur in an extruder. This, too, does not involve microporous carbon. The goal of the process is to mix the sulfur and carbon material with an ion-conductive polymer binder, not to infiltrate the sulfur into the pores of the porous carbon material.

[0010] The above-mentioned processes only describe the mixing and combination of sulfur with carbon.

[0011] The object of the present invention, with regard to the aforementioned prior art, concerns the optimization of the production of sulfur-carbon composites, in particular sulfur-carbon aerogel composites, in particular to significantly increase the material throughput while simultaneously improving the duration and energy consumption, especially the infiltration of sulfur into the micropores of the carbon material. Temperature also plays an important role. To melt the sulfur, as described in previous applications, a temperature of 115 °C is sufficient; therefore, these processes are carried out at temperatures well below 200 °C.

[0012] However, the invention relates to a batch or continuous process for producing a sulfur-carbon composite in which the sulfur is embedded in micropores of the carbon, particularly a carbon aerogel. This is not possible with previously known processes.

[0013] A first embodiment of the present invention therefore relates to a process for producing sulfur-carbon composites by introducing and reacting sulfur and a carbon material at a temperature of 300 °C or more in an extruder.

[0014] To achieve the aforementioned object, the invention provides a process in which an extruder commercially available in the plastics industry is used, thus homogenizing and heating the carbon with sulfur in a continuous process. This scalable process can be operated batchwise or continuously on systems established in the mass production industry, enabling the processing of significantly larger quantities with a significantly reduced throughput time and lower energy consumption. A person skilled in the art can easily adjust the appropriate process parameters, such as temperature, residence time, speed, and L / D ratios, based on their knowledge. At temperatures below 159 °C, the sulfur is present in S8 rings or long-chain molecules, as described above.Only at temperatures of at least 300 °C do short-chain sulfur molecules (S6, S4 and S2) form in sufficient numbers to fully penetrate the small pores of the carbon. This is not possible for the large sulfur molecules at temperatures below 300 °C. Therefore, complete infiltration of the pores (especially micropores) of the carbon cannot occur at these lower temperatures. This can be seen in the TGA curves of samples processed at different temperatures. The lower the temperature at which sulfur is released, i.e. the lower the mass loss visible in the TGA curve, the less energy is required to evaporate sulfur from the carbon. More energy is required to free small pores, especially micropores, of sulfur than for surface sulfur.Therefore, mass loss occurs at significantly higher temperatures than when sulfur is present in large pores and on the surface of the carbon particles. Therefore, after processing the composite in the extruder at 200 °C, two steps are evident in the TGA curve of the resulting material (Fig. 1). The step in the mass loss between 200 °C and 300 °C is caused by the sulfur in large pores or on the surface. The mass loss from around 350 °C is triggered by the sulfur in the smaller pores (particularly micropores). When processed at 350 °C, only one step is visible in the TGA curve. This sample only loses significant mass above 300 °C. This shows that the sulfur is completely present in the pores (particularly micropores), as intended by the process according to the invention.

[0015] In a preferred embodiment of the present invention, the aforementioned process is characterized in that both sulfur and the optionally porous carbon material are introduced separately into the extruder. The mixture formation and reaction thus takes place in the extruder. Alternatively, it is also possible to first produce a homogeneous mixture of sulfur and the carbon material in a first step and then introduce the aforementioned mixture into the extruder in a second step. Here, too, the reaction takes place in the extruder.

[0016] A wide variety of extruders of all sizes are commercially available. According to the invention, a single-screw or twin-screw extruder is used in particular.

[0017] The feed materials used are commercially available sulfur in powder form and the carbon material used is, in particular, a conventional carbon aerogel.

[0018] The material introduced into the extruder preferably undergoes one or more temperature steps. The throughput time in the extruder is preferably set in the range of 0.1 to 10 minutes. If the throughput time is too short, sufficient conversion will not be achieved.

[0019] In a further embodiment of the invention, it is possible to add additional materials in solid form, such as thickeners or binders, conductive additives, or liquid form, such as solvents, in the further course of the process, but also when adding the base materials, in particular after the first temperature treatment steps.

[0020] Preferably, within the meaning of the invention, different nozzle geometries are used in the discharge zone for further processing during the further course of the process. For strand extrusion, round strand die heads with screw-in nozzles or pasta die heads with different diameters can be used. For extrusion coatings, wide slot dies with adjustable coating thicknesses can be used. For more precise temperature control, modular cooling nozzles with independent temperature control of heating and cooling zones can be installed along the die. Extruders without nozzles in the discharge zone can also be used.

[0021] To the knowledge of the inventors, although many processes for infiltrating carbon with sulfur are known, no patent or other publication is known in which an extruder is used to infiltrate the sulfur into the micropores of the carbon material.

[0022] Extruders allow for the batch and, in particular, continuous production of sulfur-carbon composites, something previously impossible with gas or melt infiltration methods. The carbon and sulfur can either be added individually, or a premixed carbon-sulfur mixture is fed into the extruder. This mixture is advanced by the screw(s) in the extruder and passes through a zone where the temperature is increased to at least 300 °C, allowing the sulfur to diffuse into the micropores of the porous carbon (Wu HB, Wei S, Zhang L, Xu R, Hng HH, Lou XW (2013) Embedding Sulfur in MOF-Derived Microporous Carbon Polyhedrons for Lithium-Sulfur Batteries. Chemistry - A European Journal 19: 10804).

[0023] DOI: https: / / doi.org / 10.1002 / chem.201301689). The sulfur-carbon composite is then cooled again. The sample throughput time ranges from a few seconds to minutes, significantly shorter than the times used in previous batch processes of up to more than 10 hours. With this method, throughputs of more than 200 g / h can be achieved; in previous processes, batch sizes were on the gram scale. Since extruders are already established in other industrial applications, the devices are available in a wide variety of scales, allowing for any scaling of the process without great effort.

[0024] To obtain a powder using the process according to the invention, it is possible to actively cool the final section of the extruder to temperatures of 20°C or lower, which embrittles the material and causes it to exit the extruder as a powder. This eliminates the need for a subsequent milling step.

[0025] The process according to the invention can be carried out on single-screw and twin-screw extruders. The skilled person can adjust the appropriate process parameters, such as temperature, residence time, speed, and volumetric ratios.

[0026] The sulfur-carbon, in particular sulfur-carbon aerogel composites obtainable according to the invention can be used, for example, in metal-sulfur batteries or for the adsorption of mercury from aqueous solutions.

[0027] Example:

[0028] Production of sulfur-carbon aerogel composites as an example of a sulfur-carbon composite • 60 g of a carbon aerogel (molar ratios: R / W=0.008, R / C=50 and R / F=0.5, pH=5.65) (Marina Schwan, Lorenz Ratke (DE) (2019); Process for the production of flexible aerogels based on resorcinol-formaldehyde and aerogels obtainable with this process DE 10 2012 218548 Al) was mixed in particular with 40 g of sulfur (20 to 95 wt%) to form a homogeneous mixture.

[0029] Extrusion process

[0030] • The sulfur-carbon aerogel mixture was added to the extruder via a dosing device at a fixed dosing rate of 200 g / h. The material was fed through various temperature ranges in a twin-screw extruder, with temperatures up to 350 °C, and then cooled to 10 °C.

[0031] • The processing time was in the range of 1 to 10 minutes, during which the material was heated up to 350 °C.

[0032] The amount of sulfur in the sulfur-carbon aerogel composite was determined using thermogravimetric analysis (Fig. 1). Fig. 1 shows a thermogravimetric analysis of sulfur-carbon aerogel composites using an extruder compared to gas, melt, and mill infiltration methods.

[0033] The following samples were analyzed:

[0034] • CA10+S Vmicro Gas:

[0035] Gas-infiltrated sample, sulfur quantity adjusted to the volume of the micropores

[0036] • CA10+S Vmicro mill:

[0037] Mill-infiltrated sample, sulfur quantity adjusted to the volume of the micropores io

[0038] • CA10+S Vmicro+meso Gas:

[0039] Gas-infiltrated sample, sulfur quantity adjusted to the volume of the micro- and mesopores combined

[0040] • CA10+S Vmicro+meso mill:

[0041] Mill-infiltrated sample, sulfur quantity adjusted to the volume of the micro- and mesopores combined

[0042] • CA10+S Vmicro Extruder:

[0043] Sample infiltrated with the extruder, sulfur quantity adjusted to the volume of the micropores

[0044] • CA10+S Vmicro+meso melt infiltration:

[0045] Melt-infiltrated sample, sulfur quantity adjusted to the volume of the micro- and mesopores combined

[0046] Figure 1 shows that the amount of sulfur differed slightly between the various infiltration methods. The crucial sulfur content, which was only released at higher temperatures above 300 °C, was at least as high for the sample processed in the extruder as for the other methods. Figure 2 shows an extruder in which the sulfur-carbon aerogel composite was processed.

Claims

Patent claims:

1. Process for producing sulfur-carbon composites by introducing and reacting sulfur and a carbon material at a temperature of at least 300 °C in an extruder.

2. Process according to claim 1, characterized in that both sulfur and the carbon material are introduced separately into the extruder.

3. Process according to claim 1, characterized in that in a first step a homogeneous mixture of sulfur and the carbon material is first prepared and in a second step the aforementioned mixture is introduced into the extruder.

4. Process according to one of claims 1 to 3, characterized in that a single-screw or twin-screw extruder is used.

5. Process according to one of claims 1 to 4, characterized in that a porous carbon material, in particular carbon aerogel, is used as the carbon material.

6. Method according to one of claims 1 to 5, characterized in that the introduced material in the extruder undergoes one or more temperature steps.

7. Process according to claim 1 or 2, characterized in that the throughput time in the extruder is set in the range of 0.1 to 10 minutes.

8. Process according to one of claims 1 to 7, characterized in that in the further course of the process, after the first temperature treatment steps, additional materials in solid or liquid form are added.

9. Method according to one of claims 1 to 8, characterized in that different nozzle geometries are used for further processing in the further course of the process.

Citation Information

Patent Citations

  • Aerogel useful for producing carbon aerogel by pyrolysis of the aerogel, comprises resorcinol-formaldehyde

    DE102012218548A1

  • High performance all solid lithium sulfur battery with fast lithium ion conduction

    EP2966708B1

  • Production of a master batch based on sulphur and carbonaceous nanofillers, the master batch produced, and uses thereof

    US20170313844A1

  • Nano carbon sulfur composite material with network structure and preparation method of nano carbon composite material

    CN102142554A

  • Method for manufacturing a cathode, lithium-sulfur battery

    DE102014210249A1