Electrode and battery
By optimizing the interface perimeter of conductive additives in battery electrodes, the discharge capacity retention rate is improved through enhanced electron and ion conduction, addressing the issue of uneven distribution and poor conduction paths in conventional designs.
Patent Information
- Application Number
- PCT/JP2024/006946
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2024-02-27
- Publication Date
- 2024-11-14
AI Technical Summary
Conventional battery electrodes experience a decrease in discharge capacity retention rate due to uneven distribution of conductive additives, leading to poor electron conduction paths.
The electrode design incorporates a conductive aid with a specific interface perimeter of 0.58 μm/μm² or higher, ensuring uniform dispersion and improved electron transfer between active materials, achieved through careful processing and composition of active materials, solid electrolytes, and conductive additives like graphites and carbon fibers.
This configuration enhances the discharge capacity retention rate of batteries by forming effective electron and ion conduction paths, reducing internal resistance and improving battery output.
Smart Images

Figure JP2024006946_14112024_PF_FP_ABST
Abstract
Description
Electrodes and batteries
[0001] The present disclosure relates to electrodes and batteries.
[0002] Patent Document 1 discloses a negative electrode including a current collector and an active material layer in contact with at least one surface of the current collector. The active material layer contains aggregates of parts of a plurality of active materials or parts of a plurality of conductive additives.
[0003] Japanese Patent Application Laid-Open No. 2021-044195
[0004] In the prior art, further improvement in the discharge capacity retention rate of batteries is desired.
[0005] The electrode of the present disclosure includes an active material, a solid electrolyte, and a conductive additive, wherein the length of an interface of the conductive additive per unit area of a cross section of the electrode is 0.58 μm / μm. 2 Greater than.
[0006] According to the present disclosure, the discharge capacity retention rate of a battery can be improved.
[0007] Fig. 1 is a cross-sectional view showing a schematic configuration of an electrode in embodiment 1. Fig. 2 is a cross-sectional view showing a schematic configuration of a battery in embodiment 2.
[0008] (Findings underlying the present disclosure) Conductive additives are added to electrode materials containing active materials and solid electrolytes to improve electronic conductivity. For example, when an electrode is fabricated by applying a slurry containing the electrode material to a current collector, the aggregated conductive additives may sink in the direction of gravity, resulting in an uneven distribution of the conductive additive within the electrode. When the conductive additive distribution becomes uneven, it becomes difficult to form a good electron conduction path. As a result, the discharge capacity retention rate of the battery decreases.
[0009] The present inventors have conducted extensive research to improve the discharge capacity retention rate of a battery, and as a result have come up with the electrode of the present disclosure.
[0010] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. The present disclosure is not limited to the following embodiments.
[0011] First Embodiment FIG. 1 is a cross-sectional view showing a schematic configuration of an electrode 100 according to a first embodiment.
[0012] The electrode 100 includes an active material 10 , a solid electrolyte 11 , and a conductive additive 12 .
[0013] Here, the interface of the conductive additive 12 formed by contact between the solid electrolyte 11 or the active material 10 and the conductive additive 12 is defined as an interface 12f. The observed area when observing the cross section of the electrode 100 is defined as A (unit: μm 2 ) is defined as the total length of the interfaces 12f observed within the observation area. The total length of the interfaces 12f observed within the observation area is defined as L (unit: μm). In this case, the value obtained by L / A is defined as the interface perimeter Z. The interface perimeter Z represents the length of the interfaces 12f of the conductive additive 12 per unit area of the cross section of the electrode 100. In the electrode 100 of the first embodiment, the interface perimeter Z is 0.58 μm / μm 2 Since the capacitance is larger, a good electron conduction path can be formed, and as a result, the discharge capacity retention rate of the battery can be improved.
[0014] Conductive additives often form aggregates inside the electrode. If the size of the aggregates is too large or if the amount of aggregates is too large, the distribution of the conductive additive inside the electrode may become uneven. When the distribution of the conductive additive becomes uneven, it becomes difficult to form a good electron conduction path. As a result, the discharge capacity retention rate of the battery decreases.
[0015] As a result of extensive research, the inventors have found that the length of the interface of the conductive additive per unit area of the cross section of the electrode, i.e., the interface perimeter Z, can reflect the dispersion state of the conductive additive. The larger the interface perimeter Z, the more uniformly the conductive additive is dispersed, making it easier for the active material present in the electrode to exchange electrons. In the electrode 100 of this embodiment, the interface perimeter Z is 0.58 μm / μm 2 Since the capacitance is larger, a good electron conduction path can be formed, and as a result, the discharge capacity retention rate of the battery can be improved.
[0016] The interface perimeter Z is calculated using the following method.
[0017] The electrode 100 is processed with a cross-section polisher to form a smooth cross section. At this time, the direction of cross-section processing may be in any direction of the electrode 100. For example, when the electrode 100 has a plate-like shape, a cross section parallel to the in-plane direction of the plate-like electrode 100 may be formed, a cross section parallel to the thickness direction of the plate-like electrode 100 may be formed, or a cross section non-parallel to both the in-plane direction and the thickness direction may be formed.
[0018] The formed cross section is observed with a scanning electron microscope (SEM) to obtain a cross-sectional image (magnification: 500 times). Since it is desirable to evaluate the average shape of the electrode 100, it is desirable to observe a region with the SEM that is sufficiently large relative to the median diameter of the particles of the active material 10 contained in the electrode 100. For example, when the median diameter of the particles of the active material 10 contained in the electrode 100 is D (unit: μm), the area A of the measurement region is A≧(20D) 2 It is desirable to satisfy the following.
[0019] Next, from the obtained cross-sectional image, the area A of the measurement region is determined to be A≧(20D). 2 A measurement area that satisfies the above condition is selected and analyzed using the image processing software Image J. Using the Analyze Particles function of Image J, the conductive additive 12 is determined as a particle in the cross-sectional image of the electrode 100. The length of the interface 12f between the conductive additive 12 and the solid electrolyte 11 or the active material 10 is calculated. This image analysis method calculates the total length L of the interface 12f of the conductive additive 12 particles.
[0020] There is a possibility that other substances such as binders and dispersants are present at the interface 12 f between the conductive additive 12 and the solid electrolyte 11 or the active material 10. However, if these substances are not clearly visible in the cross-sectional image, the particle of the conductive additive 12 of interest is used as the subject of calculation of the total length L of the interface 12 f.
[0021] Next, the total length L of the interfaces 12f is divided by the observation area A to calculate the length of the interfaces 12f of the conductive additive 12 per unit area of the cross section of the electrode 100, i.e., the interface perimeter Z.
[0022] In addition, in the cross-sectional image, when the conductive additives 12 are connected to each other to form a single aggregate, the perimeter of this aggregate means the length of the interface 12f between the conductive additive 12 and the solid electrolyte 11 or the active material 10.
[0023] If it is difficult to calculate the total length L of the interfaces 12f by image analysis due to factors such as voids or low contrast between the conductive additive 12 and the solid electrolyte 11 or active material 10, the cross-sectional image may be appropriately processed using image processing software to make it easier to determine particles. If image processing using the cross-sectional image is difficult, a separate image may be prepared by tracing the interfaces 12f in the cross-sectional image, and the interface perimeter Z may be calculated by image processing the separate image. In this specification, "particle determination" means determining whether particles are present.
[0024] In addition, in order to remove noise after image processing, particles of the conductive additive 12 determined to be particles and having a particle area of 5 pixels or less are not used in calculating the interface perimeter Z.
[0025] The interface perimeter Z of the electrode 100 is 0.60 μm / μm 2 With this configuration, the discharge capacity retention rate of the battery can be further improved.
[0026] The interface perimeter Z of the electrode 100 is 0.70 μm / μm 2 It may be 0.80 μm / μm or more, and further, 2 It may be more than that.
[0027] The interface perimeter Z of the electrode 100 is 5 μm / μm 2 The interface perimeter Z may be 5 μm / μm or less. 2 If the content is less than this, the conductive additive 12 is likely to form an ion conduction path carried by the solid electrolyte 11. As a result, the internal resistance of the electrode 100 can be reduced, thereby enabling the battery to operate at a higher output.
[0028] (Conductive Aid) Examples of the conductive aid 12 include graphites such as natural graphite and artificial graphite, carbon blacks such as acetylene black and ketjen black, conductive fibers such as carbon fiber, vapor-grown carbon fiber, carbon nanotubes, carbon nanofibers, and metal fibers, metal powders such as carbon fluoride and aluminum, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, and conductive polymer compounds such as polyaniline, polypyrrole, and polythiophene. The conductive aid 12 may contain any one of these materials or may contain two or more of these materials. The conductive aid 12 may be composed of any one of these materials or may be composed of two or more of these materials.
[0029] The conductive additive 12 may contain a carbon material. According to the above configuration, the electrode 100 can be produced at low cost.
[0030] The conductive additive 12 may contain at least one selected from the group consisting of a fibrous carbon material and a particulate carbon material. With the above configuration, the dispersibility of the conductive additive 12 in the electrode 100 is likely to be improved, which can further improve the discharge capacity retention rate of the battery.
[0031] The conductive additive 12 preferably contains a fibrous carbon material. According to the above configuration, the conductive additive 12 more easily forms an ion conduction path carried by the solid electrolyte 11. As a result, the internal resistance of the electrode 100 can be further reduced.
[0032] The fibrous carbon material may have an average fiber diameter of 50 μm or less. According to the above configuration, the conductive additive 12 is less likely to aggregate, and therefore the dispersibility of the conductive additive 12 in the electrode 100 can be further improved.
[0033] The lower limit of the average fiber diameter of the fibrous carbon material is not particularly limited, and may be, for example, 0.4 nm.
[0034] The fibrous carbon material may have an average length of 5 nm or more. According to the above configuration, the conductive additive 12 is less likely to aggregate, and therefore the dispersibility of the conductive additive 12 in the electrode 100 can be further improved.
[0035] The upper limit of the average length of the fibrous carbon material is not particularly limited, and may be, for example, 500 μm.
[0036] The average fiber diameter and average length of the fibrous carbon material are determined by the following method. First, the fibrous carbon material is separated from the electrode 100 using a solvent. Next, the fibrous carbon material (for example, five fibers) dispersed on a sample stage is observed using an SEM, and the fiber diameter and length are measured by image analysis or the like. The measured fiber diameters and lengths are averaged to determine the average fiber diameter and average length of the fibrous carbon material. When the size of the fibrous carbon material is small, the average fiber diameter and average length of the fibrous carbon material may be determined by observation using a transmission electron microscope (TEM) instead of an SEM.
[0037] The particulate carbon material may have a median diameter of 100 nm or less. According to the above configuration, the dispersibility of the conductive additive 12 in the electrode 100 is likely to be improved.
[0038] The lower limit of the median diameter of the carbon material particles is not particularly limited, and may be, for example, 3 nm.
[0039] The conductive additive 12 may be a mixture of a fibrous carbon material and a particulate carbon material. For example, the conductive additive 12 may be a mixture of vapor-grown carbon fiber and acetylene black particles. By using a mixture of a fibrous carbon material and a particulate carbon material, it is possible to ensure a good electron conduction path inside the electrode 100 while reducing costs.
[0040] The median diameter of the conductive additive 12 may be smaller than the median diameter of the active material 10. This allows the active material 10 and the conductive additive 12 to be well dispersed. As a result, the electronic conductivity inside the electrode 100 can be further improved.
[0041] (Solid Electrolyte) The solid electrolyte 11 may include at least one selected from the group consisting of a halide solid electrolyte, a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, and a complex hydride solid electrolyte.
[0042] The solid electrolyte 11 may contain at least one selected from the group consisting of a halide solid electrolyte and a sulfide solid electrolyte. With the above configuration, the output density of the battery can be improved.
[0043] The solid electrolyte 11 may include a halide solid electrolyte. The solid electrolyte 11 may be a halide solid electrolyte.
[0044] The halide solid electrolyte is represented, for example, by the following composition formula (1): In composition formula (1), α, β, and γ each independently have a value greater than 0. M includes at least one element selected from the group consisting of metal elements and metalloid elements other than Li. X includes at least one element selected from the group consisting of F, Cl, Br, and I.
[0045] Li α M β X γ ...Formula (1)
[0046] Metalloid elements include B, Si, Ge, As, Sb, and Te. Metal elements include all elements in Groups 1 to 12 of the periodic table except for hydrogen, and all elements in Groups 13 to 16 of the periodic table except for B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se. In other words, metal elements are a group of elements that can become cations when forming an inorganic compound with a halogen compound.
[0047] Examples of halide solid electrolytes that can be used include LiYX, LiMgX, LiFeX, Li(Al, Ga, In)X, Li(Al, Ga, In)X, and Li(Al, Ti)X (X: F, Cl, Br, I).
[0048] In the present disclosure, when an element in a formula is expressed as "(Al, Ga, In)," this notation indicates at least one element selected from the group of elements in the parentheses. That is, "(Al, Ga, In)" is synonymous with "at least one element selected from the group consisting of Al, Ga, and In." The same applies to other elements. Halide solid electrolytes exhibit excellent ionic conductivity.
[0049] The above configuration can improve the output density of the battery, as well as the thermal stability of the battery and suppress the generation of harmful gases such as hydrogen sulfide.
[0050] In the composition formula (1), M may contain Y (yttrium). That is, the halide solid electrolyte may contain Y as a metal element.
[0051] The halide solid electrolyte containing Y may be a compound represented by the following composition formula (2).
[0052] Li a M b Y c X6...Formula (2)
[0053] Composition formula (2) satisfies a + mb + 3c = 6 and c > 0. In composition formula (2), M includes at least one element selected from the group consisting of metal elements and metalloid elements other than Li and Y. m is the valence of M. X includes at least one element selected from the group consisting of F, Cl, Br, and I. M includes at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta, and Nb.
[0054] Specific examples of Y-containing halide solid electrolytes include Li3YF6, Li3YCl6, Li3YBr6, Li3YI6, Li3YBrCl5, Li3YBr3Cl3, Li3YBr5Cl, Li3YBr5I, Li3YBr3I3, Li3YBrI5, Li3YClI5, Li3YCl3I3, Li3YCl5I, Li3YBr2Cl2I2, Li3YBrCl4I, Li 2.7 Y 1.1 Cl6, Li 2.5 Y0.5 Zr 0.5 Cl6, Li 2.5 Y 0.3 Zr 0.7 Cl6, etc. can be used.
[0055] According to the above configuration, the output density of the battery can be further improved.
[0056] The halide solid electrolyte may be a fluoride solid electrolyte, which has high resistance to high potentials and is therefore expected to reduce the initial resistance of the battery, for example.
[0057] The fluoride solid electrolyte may have any composition as long as it contains F. The fluoride solid electrolyte may contain, for example, Li and F.
[0058] The fluoride solid electrolyte may be, for example, a compound represented by the following composition formula (3).
[0059] Li 6-nx M x F6...Formula (3)
[0060] In the composition formula (3), x satisfies 0<x<2. M is at least one selected from the group consisting of metalloid atoms and metal atoms excluding Li. n represents the oxidation number of M.
[0061] In the composition formula (3), M may be composed of a single atom or a plurality of types of atoms. When M is composed of a plurality of types of atoms, n represents a weighted average of the oxidation numbers of the respective atoms.
[0062] For example, when M contains Ti (oxidation state = +4) and Al (oxidation state = +3), the molar ratio of Ti to Al is "Ti / Al = 3 / 7", and x = 1, n is calculated as 3.3 by the formula "n = 0.3 × 4 + 0.7 × 3".
[0063] In composition formula (3), x may satisfy, for example, 0.1≦x≦1.9, 0.2≦x≦1.8, 0.3≦x≦1.7, 0.4≦x≦1.6, 0.5≦x≦1.5, 0.6≦x≦1.4, 0.7≦x≦1.3, 0.8≦x≦1.2, or 0.9≦x≦1.1. M may, for example, include an atom having an oxidation number of +4. M may, for example, include an atom having an oxidation number of +3. M may, for example, include an atom having an oxidation number of +4 and an atom having an oxidation number of +3.
[0064] In composition formula (3), M may include at least one element selected from the group consisting of Ca, Mg, Al, Y, Ti, and Zr. M may include at least one element selected from the group consisting of Al, Y, and Ti. M may include at least one element selected from the group consisting of Al and Ti.
[0065] The fluoride solid electrolyte may be, for example, a compound represented by the following composition formula (4).
[0066] Li 3-x Ti x Al 1-x F6...Formula (4)
[0067] In composition formula (4), x may satisfy, for example, 0≦x≦1, 0.1≦x≦0.9, 0.2≦x≦0.8, 0.3≦x≦0.7, or 0.4≦x≦0.6.
[0068] The solid electrolyte 11 may include a sulfide solid electrolyte. The solid electrolyte 11 may be a sulfide solid electrolyte.
[0069] A sulfide solid electrolyte can exhibit high ionic conductivity, and therefore, when the solid electrolyte 11 includes a sulfide solid electrolyte, the output density of the battery can be improved.
[0070] The sulfide solid electrolyte may have any composition as long as it contains sulfur (S). The sulfide solid electrolyte may contain, for example, Li, P, and S. The sulfide solid electrolyte may further contain, for example, O, Ge, Si, or the like.
[0071] The sulfide solid electrolyte may further contain, for example, a halogen.
[0072] The sulfide solid electrolyte may be, for example, a glass ceramic type or an argyrodite type. Examples of sulfide solid electrolytes include LiI-LiBr-Li3PS4, Li2S-SiS2, LiI-Li2S-SiS2, Li2S-B2S3, LiI-Li2S-P2S5, LiI-Li2O-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-GeS2, Li2S-GeS2-P2S5, Li2S-P2S5, Li4P2S6, and Li7P3S 11 and Li3PS4.
[0073] The sulfide solid electrolyte may be LiI-LiBr-Li3PS4. Hereinafter, "LiI-LiBr-Li3PS4" may be referred to as "LPS."
[0074] According to the above configuration, the output density of the battery can be further improved.
[0075] The solid electrolyte 11 may include an oxide solid electrolyte. The solid electrolyte 11 may be an oxide solid electrolyte.
[0076] Examples of oxide solid electrolytes include NASICON-type solid electrolytes, such as LiTi2(PO4)3 and its elemental substitution products, (LaLi)TiO3-based perovskite-type solid electrolytes, and Li 14 ZnGeO 16 , Li4SiO4, LiGeO4 and their element substitution products, LiSICON type solid electrolytes, Li7La3Zr2O 12 Garnet-type solid electrolytes, such as those typified by element substitution products thereof, LiN and its H-substituted products, LiPO and its N-substituted products, and glasses or glass ceramics containing a base material containing a Li-B-O compound such as LiBO or LiBO to which a material such as LiSO or LiCO is added can be used.
[0077] The solid electrolyte 11 may include a polymer solid electrolyte. The solid electrolyte 11 may be a polymer solid electrolyte.
[0078] As the polymer solid electrolyte, for example, a compound of a polymer compound and a lithium salt can be used. The polymer compound may have an ethylene oxide structure. By having an ethylene oxide structure, a large amount of lithium salt can be contained, thereby further increasing ionic conductivity. As the lithium salt, LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2CF2F5)2, LiN(SO2CF3)(SO2CF4F9), LiC(SO2CF3)3, etc. can be used. As the lithium salt, one type of lithium salt selected from these can be used alone. Alternatively, as the lithium salt, a mixture of two or more types of lithium salts selected from these can be used.
[0079] The solid electrolyte 11 may include a complex hydride solid electrolyte.The solid electrolyte 11 may be a complex hydride solid electrolyte.
[0080] Examples of the complex hydride solid electrolyte that can be used include LiBH4-LiI and LiBH4-P2S5.
[0081] The shape of the solid electrolyte 11 is not particularly limited. The shape of the solid electrolyte 11 may be, for example, needle-like, spherical, oval-spherical, etc. For example, the shape of the solid electrolyte 11 may be particulate.
[0082] For example, when the solid electrolyte 11 has a particulate shape (e.g., a spherical shape), the median diameter may be 0.01 μm or more and 100 μm or less. When the median diameter is 0.01 μm or more, the contact interface between particles of the solid electrolyte 11 does not increase too much, and an increase in ionic resistance inside the electrode 100 can be suppressed. This enables the battery to operate at high output. When the median diameter is 100 μm or less, the active material 10 and the solid electrolyte 11 are likely to form a well-dispersed state in the electrode 100. This makes it easier to increase the capacity of the battery.
[0083] The median diameter of the solid electrolyte 11 may be smaller than the median diameter of the active material 10. This allows the solid electrolyte 11 and the active material 10 to be better dispersed in the electrode 100.
[0084] (Active Material) The active material 10 includes a material that has the property of absorbing and releasing metal ions (for example, lithium ions).
[0085] The active material 10 may include, for example, a positive electrode active material. Examples of the positive electrode active material include a composite oxide containing a transition element, a transition metal fluoride, a polyanion material, a fluorinated polyanion material, a transition metal sulfide, a transition metal oxysulfide, and a transition metal oxynitride. In particular, when a lithium-containing transition metal oxide is used as the positive electrode active material, the manufacturing cost can be reduced and the average discharge voltage of the battery can be increased.
[0086] The active material 10 may include, for example, a negative electrode active material. Examples of the negative electrode active material that can be used include metal materials, carbon materials, oxides, nitrides, tin compounds, and silicon compounds. The metal material may be a single metal. Alternatively, the metal material may be an alloy. Examples of the metal material include lithium metal and lithium alloys. Examples of the carbon material include natural graphite, coke, partially graphitized carbon, carbon fiber, spherical carbon, artificial graphite, and amorphous carbon. From the viewpoint of capacity density, silicon (Si), tin (Sn), silicon compounds, and tin compounds can be preferably used.
[0087] The active material 10 may include a composite oxide containing a transition element. The active material 10 may be a composite oxide containing a transition element. The above configuration can increase the average discharge voltage of the battery. The composite oxide containing a transition element selected as the active material 10 may include Li and at least one element selected from the group consisting of Mn, Co, Ni, and Al. Examples of such materials include Li(NiCoAl)O2, Li(NiCoMn)O2, and LiCoO2.
[0088] The active material 10 may contain Li(NiCoAl)O2. The active material 10 may be Li(NiCoAl)O2. With the above configuration, the energy density of the battery can be further increased. Hereinafter, "Li(NiCoAl)O2" may be referred to as "NCA."
[0089] The active material 10 may contain Li(NiCoMn)O2. The active material 10 may be Li(NiCoMn)O2. According to the above configuration, the energy density of the battery can be further increased.
[0090] The active material 10 may contain a single active material or may contain a plurality of active materials having different compositions. With the above configuration, the charge capacity of the battery can be improved.
[0091] At least a portion of the active material 10 may be coated with a coating material. This configuration makes it easier to suppress an increase in interfacial resistance and to control ionic conductivity, allowing the configuration of the electrode 100 to be designed over a wider range. Examples of coating materials that can be used include halide solid electrolytes, sulfide solid electrolytes, oxide materials, oxide solid electrolytes, and carbonates.
[0092] The coating layer made of a coating material may include multiple coating layers. The coating layer may include, for example, a first coating layer that covers at least a portion of the surface of the active material 10, and a second coating layer that covers at least a portion of the surface of the active material 10 and the first coating layer. This enables a wide range of material designs, such as using a material that exhibits high potential stability in the region of the coating layer that contacts the active material, and using a solid electrolyte with high ionic conductivity in the region of the coating layer that does not contact the active material, and is expected to improve battery life and input / output characteristics.
[0093] The halide solid electrolyte and sulfide solid electrolyte used as the coating material can be the materials exemplified as the solid electrolyte 11. Examples of oxide materials that can be used include SiO2, Al2O3, TiO2, BO, Nb2O5, WO3, and ZrO2. Examples of oxide solid electrolytes that can be used include Li-Nb-O compounds such as LiNbO3, Li-B-O compounds such as LiBO2 and Li3BO3, Li-Al-O compounds such as LiAlO2, Li-Si-O compounds such as LiSiO4, Li2SO4, and Li4TiO. 12 Li-Ti-O compounds such as Li2ZrO3, Li-Zr-O compounds such as Li2MoO3, Li-V-O compounds such as LiVO5, and Li-W-O compounds such as Li2WO4 can be used. Examples of carbonates that can be used include lithium carbonate and lithium hydrogen carbonate.
[0094] The coating material may contain a halide solid electrolyte. Halide solid electrolytes have high ionic conductivity and high potential stability. Therefore, by using a halide solid electrolyte as the coating material, the charge / discharge efficiency of the battery can be further improved.
[0095] The coating material is Li 2.7 Ti 0.3 Al 0.7 It may contain F6. 2.7 Ti 0.3 Al 0.7 F6 has higher ionic conductivity and higher high potential stability. 2.7 Ti 0.3 Al 0.7 By using F6, the charge and discharge efficiency can be further improved. 2.7 Ti 0.3 Al 0.7 "F6" is sometimes referred to as "LTAF."
[0096] The coating material may contain a sulfide solid electrolyte. Sulfide solid electrolytes have high ionic conductivity. Therefore, by using a sulfide solid electrolyte as the coating material, the input / output characteristics of the battery can be further improved.
[0097] Active material 10 may be a composite active material including a halide solid electrolyte that covers at least a portion of the surface of active material 10 and a sulfide solid electrolyte that covers the surface of active material 10 and at least a portion of the halide solid electrolyte. Active material 10 may be, for example, a composite active material including LTAF that covers at least a portion of the surface of NCA as active material 10, and LiI-LiBr-Li3PS4 (LPS) that covers the surface of NCA and at least a portion of LTAF.
[0098] By using a composite active material having the above-described structure, the charge / discharge capacity, charge / discharge efficiency, and input / output characteristics of the battery can be further improved.
[0099] The median diameter of the active material 10 may be 0.01 μm or more and 100 μm or less. When the median diameter of the active material 10 is 0.1 μm or more, the active material 10 and the solid electrolyte 11 are likely to form a well-dispersed state in the electrode 100. As a result, the charging characteristics of the battery are improved. When the median diameter of the active material 10 is 100 μm or less, the diffusion rate of lithium within the active material 10 is sufficiently ensured. This enables the battery to operate at high power.
[0100] The median diameter of the active material 10 may be larger than the median diameter of the solid electrolyte 11. This allows the active material 10 and the solid electrolyte 11 to form a well-dispersed state.
[0101] As shown in FIG. 1, in the electrode 100, the active material 10, the solid electrolyte 11, and the conductive additive 12 may be in contact with each other.
[0102] The electrode 100 may include a plurality of particles of the active material 10 , a plurality of particles of the solid electrolyte 11 , and a plurality of particles of the conductive additive 12 .
[0103] In the electrode 100, the content of the active material 10 and the content of the solid electrolyte 11 may be the same as or different from each other.
[0104] [Method for Manufacturing Electrode] The method for manufacturing the electrode 100 includes applying an electrode slurry containing the active material 10, the solid electrolyte 11, the conductive additive 12, and a solvent to a support to form the electrode 100. The support may be a current collector. 2 According to this manufacturing method, it is possible to manufacture an electrode 100 that can improve the discharge capacity retention rate of a battery.
[0105] More specifically, the method for manufacturing the electrode 100 includes mixing the active material 10, the solid electrolyte 11, the conductive additive 12, and a solvent to prepare an electrode slurry (step S1), and applying the electrode slurry to a support to form the electrode 100 (step S2).
[0106] In step S1, a binder may be further added to the electrode slurry. In step S2, the electrode 100 may be formed by applying the electrode slurry to a support and then drying it on a heated hot plate.
[0107] The method for controlling the interfacial perimeter Z in the electrode 100 is not particularly limited. For example, the interfacial perimeter Z can be controlled in step S1. In step S1, the electrode slurry may be mixed by applying a shear force. For example, the electrode slurry may be mixed using an automatic mortar, a planetary centrifugal mixer, or a rotary mixer with a mixing blade. In addition, in step S1, the electrode slurry may be mixed by applying ultrasonic waves. For example, the electrode slurry may be mixed using an ultrasonic homogenizer. In addition, in step S1, the electrode slurry may be mixed by applying pressure fluctuations. For example, the electrode slurry may be mixed using a high-pressure homogenizer.
[0108] In the electrode slurry prepared in step S1, the active material 10, the solid electrolyte 11, and the conductive additive 12 are well dispersed. The processing time required to achieve a good dispersion state varies depending on the materials contained in the electrode slurry. Therefore, an electrode slurry capable of forming an electrode 100 that satisfies the desired interfacial perimeter Z may be prepared by repeatedly recovering a portion of the electrode slurry during the execution of step S1, fabricating an electrode 100, and measuring the interfacial perimeter Z.
[0109] Second Embodiment FIG. 2 is a cross-sectional view showing a schematic configuration of a battery 200 according to a second embodiment.
[0110] Battery 200 includes positive electrode 201, negative electrode 202, and electrolyte layer 203 located between positive electrode 201 and negative electrode 202. At least one selected from the group consisting of positive electrode 201 and negative electrode 202 includes electrode 100 in embodiment 1. With the above configuration, the discharge capacity retention rate of battery 200 can be improved.
[0111] In the battery 200, at least one selected from the group consisting of the positive electrode 201 and the negative electrode 202 includes the electrode 100 of embodiment 1, so that the interface perimeter Z of the electrode 100 is 0.58 μm / μm 2 Therefore, a good electron conduction path can be formed in at least one selected from the group consisting of the positive electrode 201 and the negative electrode 202. As a result, the discharge capacity retention rate of the battery 200 can be improved.
[0112] 2 illustrates a case where the positive electrode 201 includes the electrode 100 according to the first embodiment. In the example shown in FIG. 2, the interface perimeter Z of the positive electrode 201 is 0.58 μm / μm. 2 Greater than.
[0113] 2, the positive electrode 201 may include the electrode 100 of embodiment 1. With the above configuration, the discharge capacity retention rate of the battery 200 can be improved.
[0114] Although not shown, the negative electrode 202 may include the electrode 100 in embodiment 1. With the above configuration, the discharge capacity retention rate of the battery 200 can be improved.
[0115] Although not shown, both the positive electrode 201 and the negative electrode 202 may include the electrode 100 of embodiment 1. With the above configuration, the discharge capacity retention rate of the battery 200 can be further improved.
[0116] (Positive Electrode) The positive electrode 201 includes, for example, a positive electrode active material. The positive electrode active material includes a material that has the property of absorbing and releasing metal ions (for example, lithium ions). As the positive electrode active material, the material exemplified as the active material 10 in Embodiment 1 may be used.
[0117] The positive electrode 201 may contain a conductive additive for the purpose of increasing electronic conductivity. As the conductive additive, the material exemplified as the conductive additive 12 in the first embodiment may be used.
[0118] The positive electrode 201 may contain a solid electrolyte. According to the above configuration, the ionic conductivity inside the positive electrode 201 is improved, thereby enabling the battery 200 to operate at high output. As the solid electrolyte, the material exemplified as the solid electrolyte 11 in the first embodiment may be used.
[0119] The ratio "v1:100-v1" of the volume (v1) of the positive electrode active material contained in the positive electrode 201 to the volume (100-v1) of the solid electrolyte may satisfy 30≦v1≦95. When 30≦v1 is satisfied, the energy density of the battery 200 is sufficiently ensured. When v1≦95 is satisfied, the battery 200 can operate at high output.
[0120] The thickness of the positive electrode 201 may be 10 μm or more and 500 μm or less. When the thickness of the positive electrode 201 is 10 μm or more, the energy density of the battery 200 is sufficiently ensured. When the thickness of the positive electrode 201 is 500 μm or less, the battery 200 can operate at high output.
[0121] (Negative Electrode) The negative electrode 202 includes, for example, a negative electrode active material. The negative electrode active material includes a material that has the property of absorbing and releasing metal ions (for example, lithium ions). As the negative electrode active material, the material exemplified as the active material 10 in Embodiment 1 may be used.
[0122] The negative electrode 202 may contain a conductive additive for the purpose of increasing electronic conductivity. As the conductive additive, the materials exemplified as the conductive additive 12 in the first embodiment may be used.
[0123] The negative electrode 202 may contain a solid electrolyte. According to the above configuration, the ionic conductivity inside the negative electrode 202 is improved, thereby enabling the battery 200 to operate at high output. As the solid electrolyte, the material exemplified as the solid electrolyte 11 in the first embodiment may be used.
[0124] The ratio "v2:100-v2" of the volume (v2) of the negative electrode active material contained in the negative electrode 202 to the volume (100-v2) of the solid electrolyte may satisfy 30≦v2≦95. When 30≦v2 is satisfied, the energy density of the battery 200 is sufficiently ensured. When v2≦95 is satisfied, the battery 200 can operate at high output.
[0125] The thickness of the negative electrode 202 may be 10 μm or more and 500 μm or less. When the thickness of the negative electrode 202 is 10 μm or more, the energy density of the battery 200 is sufficiently ensured. When the thickness of the negative electrode 202 is 500 μm or less, the battery 200 can operate at high output.
[0126] (Electrolyte Layer) The electrolyte layer 203 is a layer containing an electrolyte. The electrolyte is, for example, a solid electrolyte. That is, the electrolyte layer 203 may be a solid electrolyte layer. As the solid electrolyte, the material exemplified as the solid electrolyte 11 in the first embodiment may be used.
[0127] The thickness of the electrolyte layer 203 may be 1 μm or more and 300 μm or less. When the thickness of the electrolyte layer 203 is 1 μm or more, the cathode 201 and the anode 202 are less likely to short-circuit. When the thickness of the electrolyte layer 203 is 300 μm or less, the battery 200 can operate at high power.
[0128] Electrolyte layer 203 may contain two or more types of solid electrolytes selected from the materials exemplified as solid electrolyte 11 in the first embodiment.
[0129] At least one of the positive electrode 201, the negative electrode 202, and the electrolyte layer 203 may contain a binder to improve adhesion between particles. The binder is used to improve the binding properties of the electrode material. Examples of binders include polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polymethyl ester of acrylic acid, polyethyl ester of acrylic acid, polyhexyl ester of acrylic acid, polymethacrylic acid, polymethyl ester of methacrylic acid, polyethyl ester of methacrylic acid, polyhexyl ester of methacrylic acid, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, hexafluoropolypropylene, styrene-butadiene rubber, and carboxymethyl cellulose. Furthermore, a styrene-based elastomer may be used as the binder.
[0130] Examples of styrene-based elastomers include styrene-ethylene / butylene-styrene block copolymer (SEBS), styrene-ethylene / propylene-styrene block copolymer (SEPS), styrene-ethylene / ethylene / propylene-styrene block copolymer (SEEPS), styrene-butadiene rubber (SBR), styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), and hydrogenated styrene-butadiene rubber (HSBR).
[0131] Furthermore, as the binder, a copolymer of two or more materials selected from tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene can be used.
[0132] Two or more binders selected from the above binders may be mixed and used as the binder.
[0133] The battery 200 in the second embodiment can be configured as a battery of various shapes, such as a coin type, a cylindrical type, a square type, a sheet type, a button type, a flat type, or a laminated type.
[0134] (Other Embodiments) (Additional Notes) The above description of the embodiments discloses the following techniques.
[0135] (Technology 1) An electrode comprising: an active material; a solid electrolyte; and a conductive additive, wherein the length of the interface of the conductive additive per unit area of a cross section of the electrode is 0.58 μm / μm 2 Larger electrodes.
[0136] The electrode of Technology 1 can improve the discharge capacity retention rate of the battery.
[0137] (Technology 2) The electrode according to Technology 1, wherein the conductive additive contains a carbon material. With this configuration, the electrode can be produced at low cost.
[0138] (Technology 3) The electrode according to Technology 1 or 2, wherein the solid electrolyte includes at least one selected from the group consisting of a halide solid electrolyte and a sulfide solid electrolyte. With this configuration, the output density of the battery can be improved.
[0139] (Technology 4) The electrode according to any one of Technologies 1 to 3, wherein the active material includes a composite oxide containing a transition element. With this configuration, the average discharge voltage of the battery can be improved.
[0140] (Technology 5) A battery comprising: a positive electrode; a negative electrode; and an electrolyte layer located between the positive electrode and the negative electrode, wherein at least one selected from the group consisting of the positive electrode and the negative electrode includes the electrode according to any one of Technologies 1 to 4.
[0141] In the battery of Technique 5, the discharge capacity retention rate can be improved.
[0142] The present disclosure will now be described in detail with reference to the following examples and reference examples.
[0143] [Positive Electrode] Positive electrodes of Examples 1 to 5 and Reference Example 1 were prepared by the following method.
[0144] Example 1 (Composite active material) A fluoride solid electrolyte was synthesized by mixing LiF, TiF4, and AlF3 by mechanochemical milling. 2.7 Ti 0.3 Al 0.7 F6(LTAF).
[0145] In an argon glove box with a dew point of -60°C or less, Li2S and PS2S5 were weighed out to a molar ratio of Li2S:PS5 = 75:25. These were crushed and mixed in a mortar to obtain a mixture. The mixture was then milled for 10 hours at 510 rpm using a planetary ball mill (Fritsch, Model P-7). This yielded a glassy solid electrolyte. The glassy solid electrolyte was then heat-treated in an inert atmosphere at 270°C for 2 hours. This yielded a glass-ceramic sulfide solid electrolyte, Li2S-PS2S5 (LPS).
[0146] Li(NiCoAl)O2 (NCA) with a median diameter of 5 μm was prepared as the positive electrode active material. NCA and LTAF were mixed in a weight ratio of 97.4:2.6 to obtain a mixture. The mixture was then subjected to a compounding process using a particle compounding device to produce a coated active material in which the surface of NCA was coated with LTAF. Hereinafter, the coated active material in which the surface of NCA was coated with LTAF may be referred to as "LTAF / NCA." A Nobilta NOB-MINI manufactured by Hosokawa Micron Corporation was used as the particle compounding device. The operating conditions of the device were as follows: Power: 12 W per 1 g of material, Rotational speed: 6000 rpm, Processing time: 30 minutes
[0147] Using a dispersing device, LPS was dispersed in tetralin (THN) as an organic solvent to prepare an LPS dispersion with a solids content of 30%. An ultrasonic homogenizer was used as the dispersing device. Next, 9,000 parts by mass of LTAF / NCA and 275.1 parts by mass of the LPS dispersion were fed into a mixing device. A planetary mixer was used as the mixing device. A composite active material in which LPS was coated on the surface of LTAF / NCA was prepared by alternating mixing and solvent addition in the following order. Hereinafter, this composite active material in which LPS was coated on the surface of LTAF / NCA may be referred to as "LPS / LTAF / NCA." All of the above operations were performed in an environment controlled to a dew point temperature of -70°C or below. The operating conditions of the mixing device were as follows: (1) Mixing Rotation speed: 70 rpm, Time: 15 minutes (2) Addition of solvent THN (34 parts by mass) (3) Mixing Rotation speed: 100 rpm, Time: 15 minutes (4) Addition of solvent THN (30 parts by mass) (5) Mixing Rotation speed: 100 rpm, Time: 15 minutes (6) Addition of solvent THN (23 parts by mass) (7) Mixing Rotation speed: 100 rpm, Time: 3 hours
[0148] (Binder Solution) Binder A was dissolved in tetralin in an argon glove box with a dew point of -60°C or less to prepare binder solution A with a solids content of 5%. Styrene-butadiene rubber (SBR) was used as binder A. The viscosity of the prepared binder solution A was measured using a viscosity measuring device. The viscosity measuring device used was a HAAKE MARS40 manufactured by Thermo Scientific. The viscosity of binder solution A was 388 mPa·s at a measurement temperature of 25°C and a shear rate of 40 / s.
[0149] (Positive electrode slurry) LPS / LTAF / NCA was prepared as the positive electrode active material. LPS was prepared as the solid electrolyte. Acetylene black (Li-435, manufactured by Denka Co., Ltd., average particle size: 23 nm) and vapor-grown carbon fiber (VGCF-H, manufactured by Resonac Corporation, average fiber diameter: 150 nm, average length: 6 μm) were prepared as the conductive additive. Hereinafter, the acetylene black may be referred to as "AB," and the vapor-grown carbon fiber may be referred to as "VGCF" (registered trademark).
[0150] First, a positive electrode active material, a solid electrolyte, a dispersant, binder solution A, and tetralin were mixed in an argon glove box with a dew point of -60°C or less to obtain a first mixed solution. The first mixed solution was dispersed for 30 minutes using an ultrasonic homogenizer to obtain a first dispersion. Next, a conductive additive was added to the first dispersion and mixed to obtain a second mixed solution. The second mixed solution was dispersed for 50 minutes using an ultrasonic homogenizer to obtain a positive electrode slurry. Hereinafter, the dispersion time of the second mixed solution using the ultrasonic homogenizer is referred to as the "second dispersion time."
[0151] The solid content of the positive electrode slurry was 72.0% by mass, with the mass ratio of LPS / LTAF / NCA:LPS:dispersant:binder A:VGCF:AB being 80.7:16.5:0.0740:0.310:2.24:0.221.
[0152] In an argon glove box with a dew point of −60° C. or less, the positive electrode slurry was applied to one surface of an aluminum foil serving as a positive electrode current collector, and the applied positive electrode slurry was dried for 10 minutes on a hot plate heated to 120° C. In this way, the positive electrode of Example 1 was obtained.
[0153] Example 2 A positive electrode of Example 2 was obtained in the same manner as in Example 1, except that the second dispersion time was changed to 30 minutes.
[0154] Example 3 A positive electrode of Example 3 was obtained in the same manner as in Example 1, except that the second dispersion time was changed to 20 minutes.
[0155] Example 4 (Binder Solution) Binder B was dissolved in tetralin in an argon glove box with a dew point of -60°C or less to prepare binder solution B with a solids ratio of 5%. Styrene-butadiene rubber (SBR), which has a different composition from binder A, was used as binder B. The viscosity of the prepared binder solution B was measured using a viscosity measuring device (HAAKE MARS40, manufactured by Thermo Scientific). The viscosity of binder solution B was 187 mPa·s at a measurement temperature of 25°C and a shear rate of 40 / s.
[0156] A positive electrode of Example 4 was obtained in the same manner as in Example 1, except that binder B was used instead of binder A and the second dispersion time was changed to 90 minutes.
[0157] Example 5 A positive electrode of Example 5 was obtained in the same manner as in Example 4, except that the second dispersion time was changed to 30 minutes.
[0158] Reference Example 1 A positive electrode of Reference Example 1 was obtained in the same manner as in Example 4, except that the second dispersion time was changed to 20 minutes.
[0159] [Measurement of Interfacial Perimeter] The interfacial perimeter Z of each of the positive electrodes of Examples 1 to 5 and Reference Example 1 was measured by the following method.
[0160] First, positive electrodes formed on one side of aluminum foil were stacked in a mold so that the positive electrodes faced each other to obtain a laminate. The laminate was then pressed using a flat heat press heated to 120°C. This resulted in an electrode pellet in which aluminum foil, positive electrode, and aluminum foil were stacked in this order.
[0161] Next, the electrode pellet was processed with a cross-section polisher (SM-09010, manufactured by JEOL) to form a smooth cross section. At this time, the cross section processing was carried out so that a cross section parallel to the thickness direction of the electrode pellet was formed.
[0162] The cross section of the electrode pellet was observed using an SEM (SU-70, manufactured by Hitachi High-Technologies Corporation) to obtain a cross-sectional image (magnification: 500 times). The area A of the measurement region of the cross-sectional image was 4.5 × 10 4 μm 2 Since the median diameter D of the active material NCA was 5 μm, the area A of the measurement region was A≧(20D) 2 It met the following criteria.
[0163] Next, the cross-sectional image was analyzed using image processing software Image J. First, a white background was specified for the SEM observation area to obtain a binarized image. Next, using the Analyze Particles function, conductive additive particles were determined from the binarized image, and the total interface length L of conductive additive particles determined to be particles was calculated. Note that, to remove noise after image processing, particles determined to be particles with a particle area of 5 pixels or less were not used in calculating the interface perimeter. Finally, the total L was divided by the observation area A to calculate the interface length of the conductive additive per unit area of the electrode cross section, i.e., the interface perimeter Z. The interface perimeter Z for the positive electrodes of Examples 1 to 5 and Reference Example 1 obtained by the above method is shown in Table 1.
[0164] [Negative Electrode] Negative electrodes of Examples 1 to 5 and Reference Example 1 were prepared by the following method.
[0165] As the negative electrode active material, Li4Ti5O 12 The following is a description of "Li4Ti5O 12 " is sometimes referred to as "LTO." LPS was prepared as the solid electrolyte. VGCF was prepared as the conductive additive. The same binder solution B as in Example 4 was prepared as the binder solution.
[0166] First, the negative electrode active material, solid electrolyte, dispersant, and binder solution A were mixed in an argon glove box with a dew point of −60°C or less to obtain a first mixed solution. The first mixed solution was dispersed for 30 minutes using an ultrasonic homogenizer to obtain a first dispersion. Next, a conductive additive was added to the first dispersion and mixed to obtain a second mixed solution. The second mixed solution was dispersed for 50 minutes using an ultrasonic homogenizer to obtain a negative electrode slurry.
[0167] The solid content of the negative electrode slurry was LTO / dispersant / LPS / VGCF / binder A = 100 / 1.88 / 33.6 / 1.1 / 0.86 (mass ratio). The solid content of the slurry was 56.0%.
[0168] In an argon glove box with a dew point of −60° C. or less, the negative electrode slurry was applied to one surface of an aluminum foil serving as a negative electrode current collector, and the resulting material was dried for 10 minutes on a hot plate heated to 120° C. In this manner, a negative electrode was obtained.
[0169] In the negative electrodes of Examples 1 to 5 and Reference Example 1, the basis weight of the negative electrode fabricated on one side of the aluminum foil was adjusted as follows. The charge capacity per unit area of the negative electrode fabricated on one side of the aluminum foil was adjusted to be 1.1 relative to the charge capacity per unit area of the positive electrode fabricated on one side of the aluminum foil. At this time, a value of 210 mAh / g (theoretical capacity) was used as the charge capacity per unit mass of the positive electrode active material. Furthermore, a value of 175 mAh / g (theoretical capacity) was used as the charge capacity per unit mass of the negative electrode active material.
[0170] [Electrolyte Layer] The electrolyte layers of Examples 1 to 5 and Reference Example 1 were prepared by the following method.
[0171] LPS was prepared as the solid electrolyte, and the same binder solution B as in Example 4 was prepared as the binder solution.
[0172] First, a solid electrolyte, a dispersant, and binder solution A were mixed in an argon glove box with a dew point of −60° C. or less to obtain a mixed solution. The mixed solution was dispersed in tetralin using an ultrasonic homogenizer to obtain a solid electrolyte slurry.
[0173] In an argon glove box with a dew point of −60° C. or less, the solid electrolyte slurry was applied to one side of an aluminum foil and dried for 10 minutes on a hot plate heated to 120° C. In this way, an electrolyte layer was obtained.
[0174] [Negative Counter Electrode] Negative counter electrodes of Examples 1 to 5 and Reference Example 1 were prepared by the following method.
[0175] The electrolyte layer was laminated on the negative electrode so that the electrolyte layer formed on one side of the metal foil and the negative electrode formed on one side of the aluminum foil faced each other, to obtain a laminate. The laminate was pressed using a flat heat press heated to 120 ° C. After the heat press, the metal foil was removed from the electrolyte layer. In this way, a negative electrode counter electrode was obtained in which the electrolyte layer, the negative electrode, and the aluminum foil were laminated in this order.
[0176] [Battery] The batteries of Examples 1 to 5 and Reference Example 1 were fabricated by the following method.
[0177] First, a positive electrode was laminated on a negative electrode counter electrode in a mold so that the positive electrode formed on one side of the aluminum foil and the electrolyte layer of the negative electrode counter electrode faced each other, thereby obtaining a laminate. The laminate was then pressed using a flat plate hot press heated to 120°C. In this way, a power generating element was obtained in which aluminum foil, a positive electrode, an electrolyte layer, a negative electrode, and aluminum foil were laminated in this order.
[0178] Next, a current collecting lead was attached to each piece of aluminum foil using carbon tape, and finally, an aluminum laminate film was used to isolate the power generating element from the outside atmosphere, thereby completing the battery.
[0179] The current collecting leads attached to the aluminum foil extended from the space in which the power generating element was sealed by the aluminum laminate film to the unsealed outside. During charge / discharge measurements, the power generating element and the measuring device were attached so as to be electrically connected via the current collecting leads. Furthermore, the current collecting leads were not in electrical contact with the aluminum vapor deposition film included in the aluminum laminate film.
[0180] [Charge / Discharge Test] Using the batteries of Examples 1 to 5 and Reference Example 1, a charge / discharge test was carried out under the following conditions.
[0181] The battery was placed in a constant temperature bath at 25°C.
[0182] The battery was charged at a constant current of 0.68 mA, which corresponds to a 0.333 C rate (3-hour rate) relative to the theoretical capacity of the battery, and charging was terminated when the voltage reached 2.7 V.
[0183] Next, constant voltage charging was performed at a voltage of 2.7 V, and charging was terminated when the current value fell below 20 μA, which corresponds to a 0.01 C rate.
[0184] After a 10-minute rest, the battery was discharged at a constant current of 0.68 mA, which was a 0.333 C rate (3-hour rate) relative to the theoretical capacity of the battery, and the discharge was terminated when the voltage reached 1.5 V.
[0185] Next, constant voltage discharge was performed at a voltage of 1.5 V, and the discharge was terminated when the current value fell below 20 μA, which corresponds to a 0.01 C rate.
[0186] A total of two charge / discharge tests were carried out using the same method as described above, and the discharge capacity C when the battery was discharged at a constant current of 0.333 C during the second charge / discharge test was 0.333 was measured.
[0187] Next, the battery was charged at a constant current of 0.68 mA, which corresponds to a 0.333 C rate (3-hour rate) relative to the theoretical capacity of the battery, and charging was terminated when the voltage reached 2.7 V.
[0188] Next, constant voltage charging was performed at a voltage of 2.7 V, and charging was terminated when the current value fell below 20 μA, which corresponds to a 0.01 C rate.
[0189] After a 10-minute rest, the battery was discharged at a constant current of 40 mA, which corresponds to a 20 C rate relative to the theoretical capacity of the battery, and the discharge was terminated when the voltage reached 1.5 V.
[0190] Next, constant voltage discharge was performed at a voltage of 1.5 V, and the discharge was terminated when the current value fell below 20 μA, which corresponds to a 0.01 C rate.
[0191] Discharge capacity C when discharged at a constant current of 20C 20 was measured.
[0192] Discharge capacity C 20 Discharge capacity C 0.333 The value divided by (C 20 / C 0.333 The ratio calculated by multiplying the discharge capacity by 100 was taken as the discharge capacity retention rate (%). The results are shown in Table 1.
[0193]
[0194] <<Discussion>> As shown in Table 1, the interface perimeter Z in the positive electrodes of Examples 1 to 5 was 0.58 μm / μm. 2 On the other hand, the interface perimeter Z in the positive electrode of Reference Example 1 was 0.58 μm / μm 2 As can be seen from the comparison between Examples 4 and 5 and Reference Example 1, in the positive electrode of Reference Example 1, the second dispersion time was shorter than in Examples 4 and 5, which made it easier for aggregates of the conductive additive to form, and it is presumed that this reduced dispersibility of the conductive additive resulted in a decrease in the interfacial perimeter Z. Furthermore, although the second dispersion time in both Example 3 and Reference Example 1 was 20 minutes, the interfacial perimeter Z in the positive electrode of Reference Example 1 was smaller than the interfacial perimeter Z in the positive electrode of Example 3. This is presumed to be because the viscosity of binder solution B was smaller than that of binder solution A, being half or less, which made it easier for aggregates of the conductive additive to form, and this reduced dispersibility of the conductive additive resulted in a decrease in the interfacial perimeter Z. By using the positive electrodes of Examples 1 to 5, the discharge capacity retention rate of the battery was improved.
[0195] In the above examples, the electrode of the present disclosure was used as a positive electrode, but similar effects are expected when the electrode of the present disclosure is used as a negative electrode.
[0196] As described above, according to the present disclosure, an electrode suitable for improving the discharge capacity retention rate of a battery can be provided.
[0197] The electrodes of the present disclosure are used, for example, in batteries (e.g., all-solid-state lithium-ion secondary batteries).
[0198] REFERENCE SIGNS LIST 100 Electrode 10 Active material 11 Solid electrolyte 12 Conductive additive 12f Interface 200 Battery 201 Positive electrode 202 Negative electrode 203 Electrolyte layer
Claims
1. An electrode comprising an active material, a solid electrolyte, and a conductive additive, wherein the length of the interface of the conductive additive per unit area of the cross section of the electrode is 0.58 μm / μm. 2 The larger the electrode.
2. The electrode according to claim 1, wherein the conductive additive comprises a carbon material.
3. The electrode according to claim 1, wherein the solid electrolyte comprises at least one selected from the group consisting of a halide solid electrolyte and a sulfide solid electrolyte.
4. The electrode according to claim 1, wherein the active material comprises a complex oxide containing a transition element.
5. A battery comprising: a positive electrode; a negative electrode; and an electrolyte layer located between the positive electrode and the negative electrode, wherein at least one selected from the group consisting of the positive electrode and the negative electrode includes the electrode according to any one of claims 1 to 4.
Citation Information
Patent Citations
Negative electrode for lithium ion secondary battery and lithium ion secondary battery
JP2021044195A
Electrode material and battery
WO2021176759A1
Solid-state battery
WO2021187443A1
Electrode for all-solid-state battery and all-solid-state battery
WO2023189818A1