Aquatic organism adhesion prevention material and method for manufacturing underwater structure using same

The antifouling material with diiodomethyl para-tolyl sulfone and styrene elastomer addresses the challenges of adhering to complex shapes and providing long-term stain resistance, effectively preventing aquatic organism adhesion and reducing environmental hazards, offering improved safety and durability.

WO2024232345A1PCT designated stage expired Publication Date: 2024-11-14GOYO PAPER WORKING CO LTD

Patent Information

Application Number
PCT/JP2024/016906
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2024-05-02
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Existing antifouling materials struggle to effectively adhere to complex-shaped underwater structures and provide long-lasting stain resistance while avoiding environmental hazards and the use of toxic copper-based agents.

Method used

An antifouling material comprising a thermoplastic resin elastomer with diiodomethyl para-tolyl sulfone as the antifouling agent, combined with a styrene elastomer, which forms a durable antifouling layer with excellent adhesion properties and a detachable adhesive layer for easy application on variously shaped surfaces, reducing aquatic organism adhesion and maintaining effectiveness for an extended period.

Benefits of technology

The material effectively prevents aquatic organism adhesion on complex-shaped surfaces for an extended period, ensuring safer working conditions and reduced environmental impact by minimizing the use of hazardous substances, with improved adhesion and durability compared to existing solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016906_14112024_PF_FP_ABST
    Figure JP2024016906_14112024_PF_FP_ABST
Patent Text Reader

Abstract

An aquatic organism adhesion prevention material according to the present invention comprises an antifouling layer containing an antifouling material and a thermoplastic resin elastomer. The antifouling material includes a methyl para-tolylsulfone halide, and the thermoplastic elastomer includes a styrene-based elastomer. This aquatic organism adhesion prevention material can be easily attached to and detached from the surfaces of structural materials having various shapes. In addition, workers are not exposed to a dangerous work environment at the time of attaching and detaching, and a safer working environment can be provided as compared to the case of performing re-coating.
Need to check novelty before this filing date? Find Prior Art

Description

Material for preventing adhesion of aquatic organisms and method for manufacturing underwater structures using the same

[0001] The present invention relates to an aquatic organism adhesion prevention material and a method for manufacturing an underwater structure using the same, and more specifically to an aquatic organism adhesion prevention material that can prevent or reduce the adhesion of aquatic organisms to underwater structures placed in seawater or freshwater areas, and a method for manufacturing an underwater structure using the same.

[0002] There is a known technology for applying special coatings to the bottom of ships to prevent the adhesion of marine organisms such as barnacles and seaweed, with the aim of increasing ship speed and fuel efficiency, preventing corrosion of the bottom, and preventing deterioration of the ship's appearance. The bottom paints used for this purpose physiologically kill marine organisms by dissolving minute amounts of antifouling agent from the coating surface into seawater, thereby preventing fouling of the ship's bottom. Cuprous oxide or a combination of cuprous oxide and an organotin compound is the most commonly used antifouling agent.

[0003] However, due to the recent growing concern about marine environmental pollution, there is a tendency to avoid the use of copper zincate as an antifouling agent, and various antifouling agents have been proposed.

[0004] On the other hand, when paint containing antifouling agents is used, ships require periodic maintenance. In response to this, there has been a recent demand for improvements in the working environment for workers, and a technology has been proposed in which, instead of repainting, an antifouling film made of a resin molded product such as a tape, film, or sheet containing an antifouling agent is attached to a structural substrate such as the bottom of a ship.

[0005] For example, Patent Document 1 discloses an antifouling adhesive tape in which a silicone resin layer containing an antifouling agent is laminated to a substrate layer and an adhesive layer is provided on the opposite side. The use of liquid paraffin, silicone oil, surfactant, liquid hydrocarbon, fluorinated oil, or antibacterial agent as the antifouling agent is proposed. Patent Document 2 also discloses an adhesive tape for preventing the adhesion of aquatic organisms, comprising an antifouling layer, a substrate layer, and an adhesive layer. It proposes the use of a silicone resin in combination with other resins, such as polyurethane resin, polyurethane acrylic resin, rubber-based resin, or vinyl chloride resin, in the substrate layer. Patent Document 3 discloses an aquatic organism adhesion prevention film for application to underwater structures. This film proposes a method for improving stretch-peel strength, and teaches that the antifouling layer contains a silicone resin.

[0006] Furthermore, Patent Document 4 describes an anti-algae agent containing a hydroxybenzoic acid ester, and proposes its use in combination with an elastomer such as a styrene-based thermoplastic elastomer to treat bodies for ships and pools. Patent Document 5 discloses that an anti-fungal resin composition can be obtained by adding an organic iodine compound such as diiodomethyl-paratolyl sulfone to a polystyrene-based resin or a polyolefin-based resin.

[0007] However, the surfaces of structural substrates to which these films can be applied are not necessarily flat, and are often composed of surfaces with various shapes. For this reason, the development of antifouling films with excellent adhesion is desired. Furthermore, it is difficult to say that any of the above technologies provide sufficient antifouling effects after application to structural substrates. In this respect, further technological improvements are also required.

[0008] JP 2015-007201 A JP 2013-147629 A International Publication No. 2019 / 139171 JP 2021-116280 A JP 2009-263288 A

[0009] The present invention aims to solve the above problems, and its object is to provide an aquatic organism adhesion prevention material that can be easily attached to the surface of structural substrates of various shapes and that can exhibit anti-fouling properties for a long period of time, and a method for manufacturing underwater structures using the same.

[0010] The present invention relates to an aquatic organism adhesion prevention material comprising an antifouling layer containing an antifouling material and a thermoplastic resin elastomer, wherein the antifouling material contains methyl-para-tolyl sulfone halide, and the thermoplastic elastomer contains a styrene-based elastomer.

[0011] In one embodiment, the methyl paratolyl sulfone halide is diiodomethyl paratolyl sulfone.

[0012] In one embodiment, the thermoplastic resin elastomer has a surface hardness of 40 to 75 in accordance with Type A of JIS K6253.

[0013] In one embodiment, the antifouling layer has a thickness of 200 μm to 600 μm.

[0014] In one embodiment, the aquatic organism adhesion prevention material of the present invention further comprises an adhesive layer disposed on one side of the antifouling layer.

[0015] The present invention also relates to a method for producing an underwater structure, which comprises the step of attaching the above-mentioned aquatic organism adhesion prevention material.

[0016] According to the present invention, the coating can be easily applied to and removed from the surface of structural substrates having various shapes. Furthermore, the worker is not exposed to a dangerous working environment during the application and removal, which provides a safer working environment compared to repainting.

[0017] Fig. 1 is a cross-sectional view in the thickness direction showing an example of an aquatic organism adhesion prevention material of the present invention. Fig. 2 is a cross-sectional view in the thickness direction showing another example of an aquatic organism adhesion prevention material of the present invention. Fig. 3 is a photograph showing the surface condition of the aquatic organism adhesion prevention films produced in Examples 1 to 6 after immersion in seawater for one month. Fig. 4 is a photograph showing the surface condition of the aquatic organism adhesion prevention films produced in Examples 7 to 10 after immersion in seawater for one month. Fig. 5 is a photograph showing the surface condition of the aquatic organism adhesion prevention films produced in Comparative Examples 1 to 5 after immersion in seawater for one month.

[0018] The present invention will be described below with reference to the drawings.

[0019] 1, an aquatic organism adhesion prevention material 100 of the present invention includes an antifouling layer 110. This antifouling layer 110 has, for example, the form of a flat film with a constant thickness, and includes an antifouling material 120 and a thermoplastic elastomer 130.

[0020] The antifouling material 120 is a material that has the ability to prevent aquatic organisms from attaching to various substrates in a given water body (e.g., seawater or freshwater), and is sometimes called an antifouling agent. The antifouling material 120 can also repel, kill, inhibit the growth of, or inhibit the enzymes of constituent cells of, aquatic organisms, or a combination thereof, and may act specifically against any aquatic organism or against all aquatic organisms. The antifouling agent may also be an anti-algae agent that functions against aquatic organisms (aquatic plants) such as algae present in a water body.

[0021] The aquatic organism adhesion prevention material 100 of the present invention contains a methyl-para-tolyl sulfone halide as the antifouling material 120. Specific examples of the halide include fluoride, chloride, bromide, and iodide, as well as combinations thereof. The methyl-para-tolyl sulfone halide is preferably diiodomethyl-para-tolyl sulfone, as it is commercially available and is expected to provide an appropriate antifouling effect.

[0022] The antifouling material 120 may contain an antifouling component other than the above-mentioned methyl-para-tolyl sulfone halide. Examples of other antifouling components include, but are not limited to, antibacterial agents well known in the art; pharmaceuticals such as meditomidine; enzyme activity inhibitors such as alkylphenols and alkylresorcinols; algae inhibitors such as 3-(3,4-dichlorodiphenyl)-1,1-dimethylurea; diatom adhesion inhibitors such as bis(2-pyridinethiol-1-oxide) metal salts; and physical adhesion inhibitors such as wax, petrolactam, vegetable oils, and fatty acids; and combinations thereof.

[0023] The antifouling material 120 is preferably in the form of particles, for example, and is dispersed substantially uniformly within the antifouling layer 110 .

[0024] The content of the antifouling material 120 in the antifouling layer 110 is not necessarily limited, but is preferably 2% by mass to 20% by mass, and more preferably 3% by mass to 10% by mass, based on the total mass of the antifouling layer 110. If the content of the antifouling material in the antifouling layer is less than 2% by mass, the amount of antifouling material contained in the antifouling layer will be too small, and the resulting anti-adhesion material may not exhibit a sufficient effect of preventing the adhesion of aquatic organisms. If the content of the antifouling material in the antifouling layer is more than 20% by mass, the amount of antifouling material contained in the antifouling layer will be too large, and the antifouling material will not be able to be properly retained in the thermoplastic elastomer described below. This will easily cause the antifouling material to detach in water, making it difficult to maintain the effect of preventing the adhesion of aquatic organisms for a relatively long period of time.

[0025] The thermoplastic elastomer 130 serves to maintain the layer structure of the antifouling layer 110, and when placed in the water area, it comes into direct contact with the water area and plays a role in preventing the attachment of aquatic organisms to the surface.

[0026] The aquatic organism adhesion prevention material 100 of the present invention contains a styrene-based elastomer as the thermoplastic elastomer 130. The styrene-based elastomer is useful in the present invention because it is transparent or translucent, easily colorable, and has excellent moldability such as injection molding and extrusion molding.

[0027] Examples of styrene-based elastomers include styrene-ethylene-propylene block copolymers (SEP), styrene-ethylene-propylene-styrene block copolymers (SEPS), styrene-ethylene-ethylene-propylene-styrene block copolymers (SEEPS), styrene-butadiene-styrene block copolymers (SBS), styrene-ethylene-butylene-styrene block copolymers (SEBS), and styrene-isoprene-styrene block copolymers (SIS), and combinations thereof.

[0028] The aquatic organism adhesion prevention material 100 of the present invention may also contain elastomers other than styrene-based elastomers as the thermoplastic elastomer 130. Examples of other elastomers include polyamide-based elastomers, polyurethane-based thermoplastic elastomers, polyester-based elastomers, olefin-based elastomers, vinyl chloride-based elastomers, fluorine-based thermoplastic elastomers, syndiotactic 1,2-polybutadiene, and combinations thereof.

[0029] The thermoplastic elastomer itself preferably has a predetermined surface hardness. For example, the thermoplastic elastomer preferably has a surface hardness of 40 to 75, more preferably 45 to 72, in accordance with JIS K6253 Type A. When the surface hardness of the thermoplastic elastomer is within this range, adhesion of aquatic organisms can be prevented or reduced for a longer period of time, even when immersed in water.

[0030] The content of the thermoplastic elastomer 130 in the anti-fouling layer 110 is not necessarily limited, but is preferably 80% to 98% by mass, and more preferably 90% to 97% by mass, based on the total mass of the anti-fouling layer 110. If the content of the thermoplastic elastomer in the anti-fouling layer is less than 80% by mass, the moldability of the resulting anti-adhesion material decreases, making it difficult to retain the anti-fouling material and causing powdering. If the content of the thermoplastic elastomer in the anti-fouling layer is more than 98% by mass, the relative content of the anti-fouling material in the resulting anti-adhesion material decreases, making it difficult to obtain sufficient anti-fouling properties.

[0031] In the present invention, the antifouling layer 110 may contain other resins and other additives to the extent that the efficacy, moldability, etc. based on the antifouling material 120 and the thermoplastic elastomer 130 are not impaired.

[0032] Examples of other resins that may be contained in the anti-fouling layer 110 include, but are not necessarily limited to, polyolefin-based resins and modified products thereof, and ethylene-based ionomers. Examples of polyolefin-based resins include ethylene homopolymers, copolymers of ethylene and an α-olefin other than ethylene containing more than 50% by weight of an ethylene component, propylene homopolymers, copolymers of propylene and an α-olefin other than propylene containing more than 50% by weight of a propylene component, butene homopolymers, and homopolymers or copolymers of conjugated dienes such as butadiene and isoprene.

[0033] Examples of other additives that may be included in the anti-fouling layer 110 include, but are not limited to, antioxidants (e.g., phenolic antioxidants, sulfur-based antioxidants, and / or phosphorus-based antioxidants); ultraviolet absorbers (e.g., benzophenone-based ultraviolet absorbers and / or benzotriazole-based ultraviolet absorbers); antistatic agents (e.g., anionic surfactants, cationic surfactants, nonionic surfactants, and / or amphoteric surfactants); clarifying agents (e.g., metal salts of carboxylic acids, sorbitols, and / or metal salts of phosphate esters); lubricants (e.g., hydrocarbon-based lubricants, fatty acid-based lubricants, higher alcohol-based lubricants, fatty acid amide-based lubricants, metal soap-based lubricants, and / or ester-based lubricants); flame retardants (e.g., organic flame retardants and / or inorganic flame retardants); and plasticizers (e.g., epoxidized vegetable oils, phthalates, and / or polyester-based plasticizers); and combinations thereof. The content of the other additives is not particularly limited and can be selected by those skilled in the art.

[0034] In the aquatic organism adhesion prevention material 100 of the present invention, the antifouling layer 100 is designed to have a predetermined thickness so as to ensure a large absolute amount of the antifouling material 120 contained therein and to be able to withstand erosion caused by fluid movement in the water body (e.g., waves, tidal currents) for a relatively long period of time. The thickness of the antifouling layer 100 is preferably 200 μm to 600 μm, and more preferably 400 μm to 600 μm. If the thickness of the antifouling layer is less than 200 μm, the absolute amount of the antifouling material that can be contained in the antifouling layer decreases, making it difficult to use the resulting adhesion prevention material in the water body for a relatively long period of time and requiring early replacement. If the thickness of the antifouling layer exceeds 600 μm, it becomes difficult for the antifouling material inside the antifouling layer to appear in the water body, and sufficient aquatic organism adhesion prevention effect may not be achieved.

[0035] FIG. 2 is a cross-sectional view in the thickness direction showing another example of the aquatic organism adhesion prevention material of the present invention.

[0036] The aquatic organism adhesion material 200 of the present invention shown in FIG. 2 has an adhesive layer 140 disposed on one surface of the antifouling layer 110 shown in FIG.

[0037] The adhesive layer 140 has a function of providing sufficient adhesion to the underwater structure underwater, and is made of, for example, a water-resistant adhesive. Examples of adhesives that make up the adhesive layer 140 include acrylic resin adhesives, epoxy resin adhesives, amino resin adhesives, vinyl resin adhesives, and curable acrylic resin adhesives, as well as combinations thereof.

[0038] The thickness of the adhesive layer 140 is not particularly limited, but is preferably 10 μm to 40 μm, and more preferably 20 μm to 30 μm. When the adhesive layer 140 has a thickness within this range, the peelability of the adhesive layer can be controlled.

[0039] 2 has been described as an example in which the adhesive layer 140 is disposed so as to contact one surface of the antifouling layer 110, but the present invention is not limited to this arrangement. A chemical barrier layer (not shown), such as an aluminum foil or polyolefin layer, may be provided between the antifouling layer 110 and the adhesive layer 140. The thickness of this chemical barrier layer is not particularly limited, and an appropriate thickness can be selected by one skilled in the art as long as it does not impair the effects of the present invention achieved by the antifouling layer 110 and the adhesive layer 140.

[0040] In the present invention, the antifouling layer is produced by melting and kneading the antifouling material and the thermoplastic elastomer, followed by extrusion molding or injection molding using a method known to those skilled in the art. The adhesive layer may be provided simultaneously with the formation of the antifouling layer, or may be provided separately after the antifouling layer has been formed.

[0041] The aquatic organism adhesion prevention material of the present invention is used by adhering it to the surface of a structural substrate used in various water bodies, such as seawater, freshwater, and brackish water. Examples of structural substrates include various metal materials such as steel plates, various plastic materials such as fiber-reinforced plastics, concrete, ceramic, glass, and wood. Various underwater structures can be manufactured by adhering the aquatic organism adhesion prevention material of the present invention to the structural substrate. Examples of such underwater structures include, but are not limited to, ship hulls, ship bottoms, screws, anchors, rudders, and oars; tetrapods; bridge piers; floats for marine power generators; various buoys; aquariums; fishing reefs; seawater intakes; fishing nets; fishing cages; aquaculture nets; swimming pools; seaweed nets; fishing tackle; housing (e.g., exterior walls, roofs, kitchens, bathrooms, verandas, storage sheds, etc.); and gardening tools such as flower pots, planters, and seedling pots.

[0042] Furthermore, aquatic organisms whose adhesion can be prevented by an underwater structure equipped with the aquatic product adhesion prevention material of the present invention include any organisms such as animals, plants, microorganisms, etc. Specific examples include shellfish such as barnacles, mussels, and oysters; algae such as diatoms, seaweed, and aquatic plants; biofilms such as water worms; hydroids; etc.

[0043] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0044] Example 1: Preparation and evaluation of aquatic organism adhesion prevention film (E1) 95% by mass of a styrene-based thermoplastic elastomer having a surface hardness of 70 (AR-710N manufactured by Aron Chemical Industry Co., Ltd.) and 5% by mass of diiodomethyl-paratolylsulfone (Pacific Beam Mold Marine II manufactured by MIC Co., Ltd.), an antifouling agent, were kneaded together, and the mixture was extruded through a T-die extruder at an extrusion resin temperature of 200°C to obtain a 400 μm-thick aquatic organism adhesion prevention film (E1).

[0045] Three 10 cm x 10 cm samples were cut out from the obtained aquatic organism adhesion prevention film (E1), holes (approximately 8 mm) for fixing were drilled in the four corners, and the samples were fixed onto a wire mesh with approximately 1.0 cm sections through the holes in the four corners. This wire mesh was then immersed in water approximately 4 m deep at Sakai Port in Sakai City, Osaka Prefecture for one month in the summer (June to July 2022).

[0046] After one month had passed, the wire netting was lifted and three panelists visually inspected the condition of the three samples, and the level of fouling was judged and classified according to the following criteria: 5 points: No aquatic organisms were found attached to the sample. 4 points: Almost no aquatic organisms were attached to the sample, or even if some were attached, they could be easily removed with a finger. 3 points: Aquatic organisms were attached to about 20% of the sample surface. 2 points: Aquatic organisms were attached to about 30% of the sample surface. 1 point: Aquatic organisms were attached to more than about 50% of the sample surface.

[0047] The results are shown in Table 1, and a photograph of the film state is shown in FIG.

[0048] (Example 2: Preparation and evaluation of aquatic organism adhesion prevention film (E2)) An aquatic organism adhesion prevention film (E2) was prepared in the same manner as in Example 1, except that 95% by mass of a styrene thermoplastic elastomer (AR-SC5 manufactured by Aron Kasei Co., Ltd.) having a surface hardness of 3 was used instead of the styrene thermoplastic elastomer having a surface hardness of 70. A sample was prepared from this film (E2) and immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in FIG.

[0049] (Example 3: Preparation and evaluation of aquatic organism adhesion prevention film (E3)) An aquatic organism adhesion prevention film (E3) was prepared in the same manner as in Example 1, except that 95 mass % of a styrene thermoplastic elastomer (AR-SC15 manufactured by Aron Kasei Co., Ltd.) having a surface hardness of 13 was used instead of the styrene thermoplastic elastomer having a surface hardness of 70. A sample was prepared from this film (E3) and immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in FIG.

[0050] (Example 4: Preparation and evaluation of aquatic organism adhesion prevention film (E4)) An aquatic organism adhesion prevention film (E4) was prepared in the same manner as in Example 1, except that 95 mass % of a styrene thermoplastic elastomer (AR-SC45 manufactured by Aron Kasei Co., Ltd.) having a surface hardness of 41 was used instead of the styrene thermoplastic elastomer having a surface hardness of 70. A sample was prepared from this film (E4) and immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in FIG.

[0051] (Example 5: Preparation and evaluation of aquatic organism adhesion prevention film (E5)) An aquatic organism adhesion prevention film (E5) was prepared in the same manner as in Example 1, except that 95 mass% of a styrene thermoplastic elastomer having a surface hardness of 60 (AR-FL60 manufactured by Aron Kasei Co., Ltd.) was used instead of the styrene thermoplastic elastomer having a surface hardness of 70, and a sample was prepared from this film (E5) and immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in FIG.

[0052] (Example 6: Preparation and evaluation of aquatic organism adhesion prevention film (E6)) An aquatic organism adhesion prevention film (E6) was prepared in the same manner as in Example 1, except that 95 mass % of a styrene thermoplastic elastomer (AR-SC75 manufactured by Aron Kasei Co., Ltd.) having a surface hardness of 73 was used instead of the styrene thermoplastic elastomer having a surface hardness of 70. A sample was prepared from this film (E6) and immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in FIG.

[0053] (Example 7: Preparation and evaluation of aquatic organism adhesion prevention film (E7)) An aquatic organism adhesion prevention film (E7) was prepared in the same manner as in Example 1, except that 97% by mass of a styrene thermoplastic elastomer (AR-FL60 manufactured by Aron Chemical Industry Co., Ltd.) having a surface hardness of 60 was used instead of the styrene thermoplastic elastomer having a surface hardness of 70, and the content of diiodomethyl paratolyl sulfone was changed to 3% by mass. A sample was prepared from this film (E7) and immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in FIG.

[0054] (Example 8: Preparation and evaluation of aquatic organism adhesion prevention film (E8)) An aquatic organism adhesion prevention film (E8) was prepared in the same manner as in Example 1, except that 93% by mass of a styrene thermoplastic elastomer (AR-FL60 manufactured by Aron Chemical Industry Co., Ltd.) having a surface hardness of 60 was used instead of the styrene thermoplastic elastomer having a surface hardness of 70, and the content of diiodomethyl paratolyl sulfone was changed to 7% by mass. A sample was prepared from this film (E8) and immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in FIG.

[0055] (Example 9: Preparation and evaluation of aquatic organism adhesion prevention film (E9)) An aquatic organism adhesion prevention film (E9) was prepared in the same manner as in Example 1, except that 90% by mass of a styrene thermoplastic elastomer (AR-FL60 manufactured by Aron Chemical Industry Co., Ltd.) having a surface hardness of 60 was used instead of the styrene thermoplastic elastomer having a surface hardness of 70, and the content of diiodomethyl paratolyl sulfone was changed to 10% by mass. A sample was prepared from this film (E9) and immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in FIG.

[0056] (Example 10: Preparation and evaluation of aquatic organism adhesion prevention film (E10)) An aquatic organism adhesion prevention film (E10) was prepared in the same manner as in Example 1, except that 86% by mass of a styrene thermoplastic elastomer (AR-FL60 manufactured by Aron Kasei Co., Ltd.) having a surface hardness of 60 was used instead of the styrene thermoplastic elastomer having a surface hardness of 70, and the content of diiodomethyl paratolyl sulfone was changed to 14% by mass. A sample was prepared from this film (E10) and immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in FIG.

[0057] Comparative Example 1: Preparation and Evaluation of Silicone Resin Film (C1) A silicone resin (Silicone W Electro 225-1 manufactured by Shin-Etsu Chemical Co., Ltd.) was applied to a flat support plate, and this was irradiated with ultraviolet light to prepare a silicone thin film. Further silicone resin was applied to this silicone thin film, and ultraviolet light was irradiated. By this application of silicone resin and ultraviolet light irradiation, a silicone resin film (C1) having a thickness of 400 μm was obtained.

[0058] A sample was prepared in the same manner as in Example 1, except that this silicone resin film (C1) was used instead of the aquatic organism adhesion prevention film (E4) prepared in Example 1, and immersion in seawater for one month was also carried out in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in Figure 5.

[0059] Comparative Example 2: Preparation and Evaluation of Low-Density Polyethylene Film (C2) A low-density polyethylene film (C2) was prepared in the same manner as in Example 1, except that 95% by mass of low-density polyethylene (Sumikathen L405 manufactured by Sumitomo Chemical Co., Ltd.) was used instead of the styrene-based thermoplastic elastomer having a surface hardness of 70. A sample was prepared from this film (C2) and immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in FIG.

[0060] Comparative Example 3: Preparation and Evaluation of Polylactic Acid Film (C3) A polylactic acid film (C3) was prepared in the same manner as in Example 1, except that 95% by mass of polylactic acid was used instead of the styrene-based thermoplastic elastomer having a surface hardness of 70. A sample was prepared from this film (C3) and immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in FIG.

[0061] Comparative Example 4: Evaluation of PET film (C4) A commercially available polyethylene terephthalate (PET) film (C4) having a thickness of 75 μm was used instead of the aquatic organism adhesion prevention film (E1) produced in Example 1. A sample was produced from this film (C4) in the same manner as in Example 1, and a commercially available red ship bottom paint was applied to only one side (back side). The rest of the sample was immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film taken from the other side (front side) of the film (C4) is shown in FIG.

[0062] Comparative Example 5: Preparation and Evaluation of EVA Resin Film (C5) An EVA resin film (C5) was prepared in the same manner as in Example 1, except that 95% by mass of EVA resin (ethylene-vinyl acetate copolymer resin) was used instead of the styrene-based thermoplastic elastomer having a surface hardness of 70, and 5% by mass of hexyl benzoate (Hexylparaben GK-II manufactured by Ueno Pharmaceutical Co., Ltd.) as an antibacterial agent was used instead of diiodomethyl-paratolyl sulfone. A sample was prepared from this film (C5) and immersed in seawater for one month in the same manner as in Example 1. The results obtained are shown in Table 1, and a photograph of the state of the film is shown in FIG. 5.

[0063]

[0064] As shown in Table 1 and Figures 3 to 5, the aquatic organism adhesion-preventing films (E1) to (E10) produced in Examples 1 to 10 all showed little or no adhesion of shellfish or biofilms compared to the films (C1) to (C6) produced in Comparative Examples 1 to 5, demonstrating that they effectively prevented the adhesion of aquatic organisms. Furthermore, as is evident from the comparison of the surface hardness and fouling level of the styrene-based thermoplastic elastomers used in Examples 1 to 6, the higher the surface hardness of the styrene-based thermoplastic elastomer used, the less aquatic organisms were observed to adhere to the resulting film samples. Furthermore, as is evident from the results of Examples 8 to 10 (Table 1 and Figure 4), the higher the content of the antifouling agent in the produced films, the less aquatic organisms were observed to adhere to the film surface, and the films did not erode or disintegrate within one month.

[0065] The present invention is useful in various technical fields, such as shipbuilding, fisheries, marine surveys, undersea earthquake prediction, tidal current observation, undersea volcano observation, marine city construction, undersea cable communications, architecture, and gardening.

[0066] 100, 200 Aquatic organism adhesion prevention material 110 Antifouling layer 120 Antifouling material 130 Thermoplastic elastomer 140 Adhesive layer

Claims

1. An aquatic organism adhesion prevention material comprising an antifouling layer containing an antifouling material and a thermoplastic resin elastomer, the antifouling material containing methyl-para-tolyl sulfone halide, and the thermoplastic elastomer containing a styrene-based elastomer.

2. The aquatic organism adhesion prevention material according to claim 1, wherein the methyl paratolylsulfone halide is diiodomethyl paratolylsulfone.

3. The aquatic organism adhesion prevention material according to claim 1, wherein the thermoplastic resin elastomer has a surface hardness of 40 to 75 in accordance with Type A of JIS K6253.

4. The aquatic organism adhesion prevention material according to claim 1, wherein the antifouling layer has a thickness of 200 μm to 600 μm.

5. The aquatic organism adhesion prevention material according to claim 1, further comprising an adhesive layer disposed on one side of the antifouling layer.

6. A method for manufacturing an underwater structure, comprising a step of attaching the aquatic organism adhesion prevention material according to any one of claims 1 to 5 to the surface of a structural substrate.

Citation Information

Patent Citations

  • Fungicidal resin composition

    JP2009263288A

  • Adhesive tape preventing adhesion by aquatic organisms

    JP2013147629A

  • Aquatic Anti-biofouling pressure-sensitive adhesive tape

    JP2015007201A

  • Algicidal agent

    JP2021116280A

  • Film for preventing adhesion of aquatic organisms

    WO2019139171A1

Cited By

  • Tape for preventing adhesion of aquatic organisms

    WO2026048793A1