Latent heat storage particles and method for producing same

The development of latent heat storage particles with a polyurethane polyurea resin shell and a specific latent heat storage material core addresses leakage and manufacturing complexity issues, providing durable and efficient temperature control without aldehyde generation.

WO2024232375A1PCT designated stage expired Publication Date: 2024-11-14NEGAMI CHEM IND
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017051
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2024-05-08
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Existing latent heat storage particles face issues with material leakage due to expansion and contraction, especially with high phase transition temperatures, and require complex manufacturing processes, while also generating aldehydes that contribute to sick building syndrome.

Method used

Development of latent heat storage particles with a polyurethane polyurea resin shell and a latent heat storage material core, having a melting point of 30°C to 60°C, and a water/octanol partition coefficient of 8 to 10, which are produced using a simplified method involving a polyisocyanate, polyol, and polyamine reaction, resulting in particles with minimal weight loss and enhanced durability.

Benefits of technology

The solution prevents material leakage during long-term storage and use, allows for the creation of particles with high melting points, and simplifies the manufacturing process, ensuring effective temperature control and mechanical strength without generating harmful aldehydes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017051_14112024_PF_FP_ABST
    Figure JP2024017051_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: latent heat storage particles from which a latent heat storage substance does not leak even after long-term storage and / or long-term use; latent heat storage particles where formation of the particles is possible even when using a latent heat storage substance having a melting point of 30°C or higher as measured by JIS-K7121; and / or latent heat storage particles that can be produced using a relatively small number of steps. The present invention provides latent heat storage particles having a shell part that has a polyurethane polyurea resin, and a core part that has the latent heat storage substance. The heating loss, which is the weight loss after heating at 110°C for 6 hours, is 2 wt% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Latent heat storage particles and their manufacturing method

[0001] The present invention relates to latent heat storage particles, a method for producing the same, and a material containing the latent heat storage particles.

[0002] Core-shell type latent heat storage particles are known, in which latent heat storage materials that utilize the latent heat (heat of transition) associated with changes in the physical state of a substance (phase transition; solidification and melting) are encapsulated in resin. These particles are used for temperature control in structural materials such as buildings and structures, and for air conditioning in buildings, houses, underground shopping malls, etc.

[0003] For example, Patent Documents 1 and 2 disclose latent heat storage particles having a shell made of one of polyurethane polyurea, polyurethane, and polyurea, and Patent Document 3 discloses heat storage particles using a vinyl monomer for the shell and n-paraffin for the core.

[0004] Furthermore, Patent Document 4 discloses heat storage particles that use a melamine resin for the shell and n-paraffin for the core. However, when a melamine resin is used for the shell, there is a problem in that aldehyde, which is a causative substance of sick house syndrome, is generated.

[0005] In core-shell latent heat storage particles in which a latent heat storage material is encapsulated in a resin, heat is released and released as the latent heat storage material contained in the core solidifies and melts. However, this solidification and melting is accompanied by contraction and expansion of the core, which leads to a load on the shell. Therefore, if the core contracts and expands over a long period of time, the shell may be unable to withstand the load and may be destroyed, resulting in leakage of the latent heat storage material. In particular, latent heat storage materials with high phase transition (solidification and melting) temperatures generally experience large volume changes due to contraction and expansion associated with solidification and melting, which makes the shell more prone to destruction, exacerbating the problem of leakage of the latent heat storage material.

[0006] On the other hand, with the recent increase in CPU performance, there is a growing need to prevent overheating in electronic devices and to prevent low-temperature burns in devices that come into contact with the human body. There is therefore hope for the commercialization of latent heat storage particles that can be embedded in devices and have a melting point of 30°C or higher as measured in accordance with JIS-K7121.

[0007] For example, Patent Document 5 discloses latent heat storage particles that do not generate aldehyde, solve the problem of leakage of the latent heat storage material, and have excellent durability. However, when a latent heat storage material with a phase transition temperature exceeding 30°C is used, there is a problem that it cannot be granulated into latent heat storage particles. Furthermore, for example, Patent Document 6 discloses heat storage microcapsules consisting of a polyurethane film or a polyurea film and a specific fatty acid ester. However, there is a problem that when the material is repeatedly expanded and contracted by melting and solidifying during long-term use, the fatty acid ester leaks due to deterioration of the film material.

[0008] Furthermore, for example, Patent Document 7 discloses a method for producing latent heat storage particles by producing porous hollow particles, impregnating them with a latent heat storage material through the pores, and then coating them with polyamide to close the pores, and the latent heat storage particles obtained thereby. However, this production method requires multiple steps and complicated production processes, and is therefore not suitable for practical use.

[0009] Japanese Patent Publication No. 2009-91473, Japanese Patent Publication No. 2009-148676, Japanese Patent No. 5651272, Japanese Patent No. 4808476, Japanese Patent Publication No. 2017-137437, Japanese Patent No. 6899307, Japanese Patent Publication No. 2016-34622.

[0010] However, latent heat storage particles that solve the above problems have not yet been developed or commercialized. Therefore, an object of the present invention is to solve the above problems. That is, an object of the present invention is to provide latent heat storage particles that do not leak the latent heat storage material even after long-term storage and / or long-term use. Furthermore, in addition to or in addition to the above objects, an object of the present invention is to provide latent heat storage particles that can be granulated even when using a latent heat storage material that has a melting point of 30°C or higher as measured according to JIS-K7121.

[0011] Furthermore, an object of the present invention is to provide latent heat storage particles that can be produced in a relatively simple process and a method for producing the same, in addition to or in addition to the above-mentioned object. Also, an object of the present invention is to provide a material having the latent heat storage particles.

[0012] The present inventors have discovered the following inventions in order to solve the above problems: <1> Latent heat storage particles having a shell portion containing a polyurethane polyurea resin and a core portion containing a latent heat storage material, wherein the loss on heating, which is the weight loss after heating at 110°C for 6 hours, is 2% by weight or less.

[0013] <2> In the above item <1>, the latent heat storage particles preferably have a melting point, as measured in accordance with JIS-K7121, of 30° C. or more and 60° C. or less, preferably 35 to 55° C., and more preferably 35 to 50° C. <3> In the above item <1> or <2>, the latent heat storage material preferably has a water / octanol partition coefficient Log P of 8 to 10, and is preferably at least one selected from fatty acid esters (A) having a water / octanol partition coefficient Log P of 8.0 to 10.0, and n-paraffins (B) having a water / octanol partition coefficient Log P of 9.2 to 10.0.

[0014] <4> In any of the above items <1> to <3>, the polyurethane polyurea resin may have a structure derived from an alicyclic diisocyanate. <5> In any of the above items <1> to <4>, the latent heat storage particles may have a volume average particle diameter of 1 to 500 μm, preferably 5 to 300 μm, more preferably 10 to 250 μm, and most preferably 20 to 200 μm.

[0015] <6> In any of the above items <1> to <5>, the shell portion may consist essentially of a polyurethane polyurea resin. In this specification, "consisting essentially of a polyurethane polyurea resin" means that, out of 100 parts by weight of the material constituting the shell portion, the "polyurethane polyurea resin" accounts for 95 parts by weight or more, preferably 97 parts by weight or more, more preferably 99 parts by weight or more, and most preferably 100 parts by weight. <7> In any of the above items <1> to <6>, the shell portion may consist solely of a polyurethane polyurea resin.

[0016] <8> In any of the above items <1> to <7>, the core portion may consist essentially of a latent heat storage material. In this specification, "consisting essentially of a latent heat storage material" means that the amount and type of the latent heat storage material and the amount and type of materials other than the latent heat storage material are not important, as long as the melting point of the latent heat storage particles, as measured according to JIS-K7121, is 30°C or higher and 60°C or lower. Note that "consisting essentially of a latent heat storage material" means that, out of 100 parts by weight of the material constituting the core portion, the "latent heat storage material" accounts for 95 parts by weight or more, preferably 97 parts by weight or more, more preferably 99 parts by weight or more, and most preferably 100 parts by weight. <9> In any of the above items <1> to <8>, the core portion may consist solely of a latent heat storage material.

[0017] <10> In any of the above items <1> to <9>, the latent heat storage particles preferably consist essentially of a shell portion and a core portion. Here, in the present specification, "consisting essentially of a shell portion and a core portion" means that the particles may contain portions other than the "shell portion" and the "core portion," but that, per 100 parts by weight of the latent heat storage particles, the portions other than the "shell portion" and the "core portion" are 5 parts by weight or less, preferably 3 parts by weight or less, more preferably 1 part by weight or less, and most preferably 0 part by weight. <11> In any of the above items <1> to <10>, the latent heat storage particles preferably consist only of the shell portion and the core portion.

[0018] <12> A material having the latent heat storage particles according to any one of the above items <1> to <11>. Examples of the material include, but are not limited to, a resin sheet, a rubber sheet, synthetic paper, a medium (water, a heat medium), a thermoplastic resin, a thermosetting resin, and rubber. <13> A manufacturing method for the latent heat storage particles according to any one of the above items <1> to <12>.

[0019] <14> A method for producing latent heat storage particles, comprising: a step of dispersing a raw material composition containing a polyisocyanate and a latent heat storage material in a dispersion medium containing water to obtain a suspension; and a step of adding a polyol and a polyamine to the suspension and reacting the polyisocyanate, the polyamine, and the polyol; thereby obtaining latent heat storage particles having a shell portion containing a polyurethane polyurea resin and a core portion containing the latent heat storage material, and having a loss on heating, which is the weight loss after heating at 110°C for 6 hours, of 2% by weight or less.

[0020] The present inventors have also discovered the following invention. <A1> Latent heat storage particles having a shell portion containing a polyurethane polyurea resin and a core portion containing a latent heat storage material, wherein the polyurethane polyurea resin has a structure derived from an alicyclic diisocyanate, and the latent heat storage material has a water / octanol partition coefficient Log P of 8 or more and 10 or less and a melting point measured according to JIS-K7121 of 30°C or more and 60°C or less. The melting point of the latent heat storage particles measured according to JIS-K7121 is preferably 35 to 55°C, more preferably 35 to 50°C.

[0021] <A2> In the above <A1>, it is preferable that the latent heat storage material having a water / octanol partition coefficient Log P of 8 or more and 10 or less is at least one selected from the group consisting of methyl stearate, myristyl myristate, cetyl myristate, and n-docosane. <A3> In the above <A1> or <A2>, it is preferable that the alicyclic diisocyanate is at least one selected from the group consisting of 1,3-bis(isocyanatemethyl)cyclohexane (hydrogenated XDI), 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), isophorone diisocyanate, and norbornane diisocyanate.

[0022] <A4> In any of the above items <A1> to <A3>, the latent heat storage particles have a volume average particle diameter of 1 to 500 μm, preferably 5 to 300 μm, more preferably 10 to 250 μm, and most preferably 20 to 200 μm. <A5> A material containing the latent heat storage particles according to any one of the above items <A1> to <A4>.

[0023] <A6> A method for producing latent heat storage particles, comprising the steps of: dispersing a raw material composition containing a polyisocyanate and a latent heat storage material in a dispersion medium containing water to obtain a suspension; and adding a polyol and a polyamine to the suspension and reacting the polyisocyanate, the polyamine, and the polyol; thereby obtaining latent heat storage particles having a shell portion containing a polyurethane polyurea resin and a core portion containing the latent heat storage material, wherein the polyurethane polyurea resin has a structure derived from an alicyclic diisocyanate, and the latent heat storage material has a water / octanol partition coefficient LogP of 8 or more and 10 or less and a melting point measured in accordance with JIS-K7121 of 30°C or more and 60°C or less.

[0024] The present invention can solve the above problems. The present invention can provide latent heat storage particles that do not leak the latent heat storage material even after long-term storage and / or long-term use. Furthermore, in addition to or in addition to the above effects, the present invention can provide latent heat storage particles that can be granulated even when using a latent heat storage material whose melting point, as measured according to JIS-K7121, is 30°C or higher.

[0025] Furthermore, in addition to or in addition to the above-mentioned effects, the present invention can provide latent heat storage particles that can be produced in a relatively simple process and a method for producing the same.Furthermore, in addition to or in addition to the above-mentioned effects, the present invention can provide a material having the latent heat storage particles.

[0026] 1 is a cross-sectional view showing an example of a latent heat storage particle of the present invention. FIG. 2 is a cross-sectional view showing an example of a material having latent heat storage particles of the present invention.

[0027] The invention described in this application (hereinafter sometimes abbreviated as "the present invention") will be described below. The present application provides latent heat storage particles having a shell portion containing a polyurethane polyurea resin and a core portion containing a latent heat storage material, wherein the heat loss of the latent heat storage particles is 2% by weight or less, preferably 1.5% by weight or less, more preferably 1.0% by weight or less, and most preferably 0.5% by weight or less. The present application also provides a method for producing the latent heat storage particles. Furthermore, the present application provides a material containing the latent heat storage particles.

[0028] <Latent Heat Storage Particles> The latent heat storage particles of the present invention have a shell portion containing a polyurethane polyurea resin and a core portion containing a latent heat storage material. Figure 1 shows a cross-sectional view of an example of a latent heat storage particle of the present invention. The latent heat storage particle 10 has a core portion 12 containing a latent heat storage material and a shell portion 14 containing a polyurethane polyurea resin that coats the core portion 12.

[0029] The latent heat storage particles of the present invention preferably have a weight loss on heating of 2% by weight or less, preferably 1.5% by weight or less, more preferably 1.0% by weight or less, and most preferably 0.5% by weight or less. The weight loss on heating can be determined by measuring the weight of the latent heat storage particles before heating, heating the latent heat storage particles at 110°C for 6 hours, and then measuring the weight of the latent heat storage particles again, and then calculating the weight loss, which is the difference between the weight loss and the weight loss. By having the weight loss on heating in the above range, it is possible to provide latent heat storage particles having desired properties, such as latent heat storage particles that do not leak the latent heat storage material even after long-term storage and / or long-term use. Furthermore, by having the weight loss on heating in the above range, it is possible to provide latent heat storage particles having desired properties, such as latent heat storage particles that can be granulated even when using a latent heat storage material with a phase transition temperature exceeding 30°C.

[0030] The latent heat storage particles of the present invention have a melting point measured according to JIS-K7121 of 30°C or higher and 60°C or lower, preferably 35 to 55°C, and more preferably 35 to 50°C.

[0031] The latent heat storage particle of the present invention may have an outermost layer outside the shell, in addition to the shell and core. The outermost layer is preferably a layer that imparts functions such as heat resistance, solvent resistance, and water resistance to the latent heat storage particle, and examples of materials for the outermost layer include, but are not limited to, thermoplastic resins, cured products of curable resins, and inorganic compounds.

[0032] The latent heat storage particles of the present invention preferably consist essentially of a shell portion and a core portion, and more preferably consist only of a shell portion and a core portion. Note that "consisting essentially of a shell portion and a core portion" means that, although the particles may contain portions other than the "shell portion" and the "core portion," the portions other than the "shell portion" and the "core portion" are 5 parts by weight or less, preferably 3 parts by weight or less, more preferably 1 part by weight or less, and most preferably 0 part by weight per 100 parts by weight of the latent heat storage particles.

[0033] The latent heat storage particles of the present invention preferably have a volume-average particle diameter of 1 to 500 μm, preferably 5 to 300 μm, more preferably 10 to 250 μm, and most preferably 20 to 200 μm. The term "volume-average particle diameter" refers to the volume-based median diameter measured using a laser diffraction particle size analyzer. When the volume-average particle diameter of the latent heat storage particles is equal to or greater than the lower limit of the aforementioned range, the latent heat storage capacity of the latent heat storage particles is sufficiently large. Furthermore, the latent heat storage material in the core portion is less likely to leach out even when repeatedly heated and cooled. Furthermore, the mechanical strength of the shell portion is increased, making the shell less likely to be damaged by compression or the like. When the volume-average particle diameter of the latent heat storage particles is equal to or less than the upper limit of the aforementioned range, the latent heat storage particles are less noticeable when used in a material containing the latent heat storage particles and other materials (building materials, media, etc.), such as a heat storage material, resulting in a good appearance of the material, such as a heat storage material. The volume average particle size of the latent heat storage particles can be decreased by increasing the content of dispersant in the dispersion medium in the method for producing latent heat storage particles described below, and can be increased by decreasing the content of dispersant.

[0034] The shape of the latent heat storage particles may include, but is not limited to, a perfect sphere, a partially distorted sphere, a potbellied shape, a cylindrical shape, a cone shape, a rectangular parallelepiped shape, etc. The amount of the latent heat storage material in the latent heat storage particles is 30 to 99.9 parts by weight, preferably 50 to 99 parts by weight, more preferably 60 to 99 parts by weight, and most preferably 70 to 90 parts by weight, per 100 parts by weight of the latent heat storage particles, in terms of the mechanical strength of the shell portion and the latent heat storage amount of the core portion.

[0035] <Shell Portion> The shell portion of the latent heat storage particles of the present invention comprises a polyurethane polyurea resin. Here, "polyurethane polyurea" refers to a polymer compound having a urethane bond (-NHC(O)O-) and a urea bond (-NHC(O)NH-). Preferably, there are multiple urethane bonds and multiple urea bonds. The shell portion of the latent heat storage particles of the present invention may comprise a material other than a polyurethane polyurea resin, as long as the above-mentioned problems, such as leakage of the latent heat storage material, do not occur. Examples of materials other than a polyurethane polyurea resin include, but are not limited to, resins other than polyurethane polyurea, rubber, fillers, function-imparting agents, and unavoidable impurities. The polyurethane polyurea resin should account for at least 50 parts by weight, preferably at least 70 parts by weight, more preferably at least 90 parts by weight, and most preferably 100 parts by weight, of 100 parts by weight of the material constituting the shell portion. The content of other components is preferably 50 parts by weight or less, more preferably 30 parts by weight or less, more preferably 10 parts by weight or less, and most preferably 0 part by weight, per 100 parts by weight of polyurethane polyurea.

[0036] The shell of the latent heat storage particles of the present invention preferably consists essentially of a polyurethane-polyurea resin, and more preferably consists solely of a polyurethane-polyurea resin. Here, "consisting essentially of a polyurethane-polyurea resin" means that out of 100 parts by weight of the material constituting the shell, the "polyurethane-polyurea resin" accounts for 95 parts by weight or more, preferably 97 parts by weight or more, more preferably 99 parts by weight or more, and most preferably 100 parts by weight.

[0037] The thickness of the shell portion of the latent heat storage particles of the present invention depends on the particle size of the obtained latent heat storage particles, the material of the shell portion used, particularly the polyurethane polyurethane resin used, etc., but from the viewpoint of mechanical strength and / or prevention of volatilization of the latent heat storage material, it is preferably 0.03 to 40 μm, preferably 0.1 to 25 μm, more preferably 0.2 to 20 μm, and most preferably 0.5 to 15 μm.

[0038] In order to further increase the mechanical strength of the shell portion, it is preferable that the polyurethane polyurea resin has both a urethane bond derived from the reaction of a polyisocyanate and a polyol and a urea bond derived from the reaction of a polyisocyanate and a polyamine. That is, the polyurethane polyurea resin is derived from a polyisocyanate, a polyol, and a polyamine, and it is preferable to use such a resin in the method for producing latent heat storage particles of the present invention described below. Note that there is no limitation on the origin of these materials, and they may be derived from, for example, fossil fuels or biomass.

[0039] <<Polyisocyanate>> Examples of polyisocyanates include bifunctional isocyanates having two isocyanate groups and polyfunctional isocyanates having three or more isocyanate groups.

[0040] Bifunctional isocyanates include tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate, lysine diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), methylcyclohexane-2,4 (or 2,6)-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane (hydrogenated XDI), isophorone diisocyanate, trimethylhexamethylene diisocyanate, dimer acid diisocyanate, and dianisidine diisocyanate. Phenyl diisocyanate, halogenated phenyl diisocyanate, methylene diisocyanate, ethylene diisocyanate, butylene diisocyanate, propylene diisocyanate, octadecylene diisocyanate, 1,5-naphthalene diisocyanate, polymethylene polyphenylene diisocyanate, naphthalene diisocyanate, tolylene diisocyanate polymer, diphenylmethane diisocyanate polymer, hexamethylene diisocyanate polymer, 3-phenyl-2-ethylene diisocyanate , cumene-2,4-diisocyanate, 4-methoxy-1,3-phenylene diisocyanate, 4-ethoxy-1,3-phenylene diisocyanate, 2,4'-diisocyanate diphenyl ether, 5,6-dimethyl-1,3-phenylene diisocyanate, 4,4'-diisocyanate diphenyl ether, benzidine diisocyanate, 9,10-anthracene diisocyanate, 4,4'-diisocyanate benzyl, 3,3'-dimethyl-4,4'-diisocyanate diphenylmethane, 2,6-dimethyl Examples of the isocyanate include, but are not limited to, 4,4'-methyl-4,4'-diisocyanatodiphenyl, 3,3'-dimethoxy-4,4'-diisocyanatodiphenyl, 1,4-anthracene diisocyanate, phenylene diisocyanate, 1,4-tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,10-decamethylene diisocyanate, 1,3-cyclohexylene diisocyanate, 4,4'-methylene-bis(cyclohexyl isocyanate), and norbornane diisocyanate.

[0041] Examples of polyfunctional isocyanates include triphenylmethane-4,4',4"-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, 2,4,4'-triisocyanatodiphenyl ether, 4,4'-dimethyldiphenylmethane-2,2',5,5'-tetraisocyanate, and trimers of bifunctional isocyanates (biuret, isocyanurate, adduct).

[0042] In the present invention, the polyisocyanate is preferably an alicyclic diisocyanate. If the polyisocyanate is alicyclic, the formation of the shell and core portions during polymerization proceeds uniformly due to its compatibility with the latent heat storage material, and latent heat storage particles that are dense, have sufficient strength, and are excellent in durability can be obtained. Examples of alicyclic diisocyanates include, but are not limited to, 1,3-bis(isocyanatomethyl)cyclohexane (hydrogenated XDI), 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), isophorone diisocyanate, and norbornane diisocyanate. One type of polyisocyanate may be used alone, or two or more types may be used in combination.

[0043] <<Polyol>> A polyol refers to a compound containing two or more hydroxyl groups (OH groups). Examples of polyols include polyester polyols, polyether polyols, polycarbonate polyols, polybutadiene polyols, hydrogenated polybutadiene polyols, acrylic polyols, polycaprolactone polyols, and aliphatic polyhydric alcohols having 1 to 20 carbon atoms, but are not limited to these.

[0044] Furthermore, as the polyol, an aliphatic polyhydric alcohol having 1 to 20 carbon atoms is preferred because it makes it easier to obtain latent heat storage particles with high mechanical strength and prevents the latent heat storage material from seeping out. Examples of aliphatic polyhydric alcohols having 1 to 20 carbon atoms include, but are not limited to, ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, 3-methyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-methyl-1,3-propanediol, trimethylolpropane, trimethylolethane, glycerin, pentaerythritol, and sorbitol. One type of polyol may be used alone, or two or more types may be used in combination.

[0045] <<Polyamine>> Polyamine is a compound that contains an amino group (NH 2 Examples of polyamines include aliphatic polyamines such as ethylenediamine, tetramethylenediamine, octamethylenediamine, decamethylenediamine, piperazine, diethylenetriamine, triethylenetetraamine, dihexamethylenetriamine, and 1,4-diaminocyclohexane, and aromatic polyamines such as paraphenylenediamine, metaphenylenediamine, paraxylylenediamine, metaxylylenediamine, 4,4'-diaminobiphenyl, and 4,4'-diaminodiphenylmethane, but are not limited to these.

[0046] The preferred proportions of the polyisocyanate-derived structural units, polyol-derived structural units, and polyamine-derived structural units in the polyurethane polyurea are the same as the preferred proportions of the polyisocyanate, polyol, and polyamine in the method for producing latent heat storage particles described below.

[0047] <Core> The core contains a latent heat storage material. The core may contain other components as needed, as long as the effects of the present invention are not impaired. Examples of other components include, but are not limited to, resins, rubbers, fillers, function-imparting agents, and inevitable impurities. Examples of fillers include, but are not limited to, metals, metal compounds, carbon materials (carbon black, carbon nanotubes, expanded graphite, carbon fibers), glass, and minerals.

[0048] Examples of the function-imparting agent include, but are not limited to, antioxidants, antistatic agents, weathering agents, ultraviolet absorbers, antiblocking agents, crystal nucleating agents, flame retardants, vulcanizing agents, vulcanization aids, antibacterial and antifungal agents, dispersants, coloration inhibitors, foaming agents, rust inhibitors, heavy metal deactivators, melting point adjusters (freezing point depressants), hydrolysis inhibitors, etc. The amount of other components is preferably 3 parts by weight or less, preferably 2 parts by weight or less, more preferably 1 part by weight or less, and most preferably 0 part by weight, relative to 100 parts by weight of the latent heat storage material.

[0049] The core portion preferably consists essentially of a latent heat storage material, and preferably consists solely of a latent heat storage material. Here, in this specification, "consisting essentially of a latent heat storage material" means that the melting point of the latent heat storage particles, as measured according to JIS-K7121, is 30°C or higher and 60°C or lower, and the amount and type of the latent heat storage material, as well as the amount and type of materials other than the latent heat storage material, are not important. Note that "consisting essentially of a latent heat storage material" means that, out of 100 parts by weight of the material constituting the core portion, the "latent heat storage material" is 95 parts by weight or more, preferably 97 parts by weight or more, more preferably 99 parts by weight or more, and most preferably 100 parts by weight.

[0050] The latent heat storage material preferably has a water / octanol partition coefficient Log P of 8 or more and 10 or less, and is preferably at least one selected from fatty acid esters (A) having a water / octanol partition coefficient Log P of 8.0 or more and 10.0 or less, and / or n-paraffins (B) having a water / octanol partition coefficient Log P of 9.2 or more and 10.0 or less. When the Log P values ​​of the fatty acid esters (A) and n-paraffins (B) are within the specified range, the following three advantages are obtained. (1) Due to their compatibility, the formation of the shell and core portions during polymerization proceeds uniformly, resulting in dense latent heat storage particles that are sufficiently strong and highly durable. (2) Because the melting point of the latent heat storage material, as measured according to JIS-K7121, is higher than 30°C, it remains in a solid state at room temperature and is less likely to volatilize even after becoming latent heat storage particles, resulting in excellent long-term storage properties. (3) Since the melting point of the latent heat storage material measured according to JIS-K7121 is lower than 60°C, it is in a liquid state at the polymerization temperature of 65°C, and therefore it is possible to polymerize latent heat storage particles having a good core-shell structure.

[0051] The water / octanol partition coefficient (Log P value) can be measured by the flask shaking method described in JIS Z-7260-107 (2000). The water / octanol partition coefficient (Log P value) can also be estimated by computational chemistry or empirical methods instead of actual measurement.

[0052] As a method for calculating LogP, Crippen's fragmentation method (J. Chem. Inf. Comput. Sci., 27, p. 21 (1987)), Viswanadhan's fragmentation method (J. Chem. Inf. Comput. Sci., 29, p. 163 (1989)), Broto's fragmentation method (Eur. J. Med. Chem. Chim. Theor., 19, p. 71 (1984)), CLogP method (reference: Leo, A., Jow, PYC, Silipo, C., Hansch, C., J. Med. Chem., 18, 865 (1975)), etc. are preferably used, with Crippen's fragmentation method and CLogP method being more preferred. When the CLogP method is used, calculations can be performed using free software available on the Molinspiration Cheminformatics website.

[0053] As described above, a latent heat storage material is used for the core of the latent heat storage particles of the present invention, from the viewpoints of a large heat storage capacity, precise temperature control, and ease of particle production. The latent heat storage material is preferably selected depending on the application of the latent heat storage particles. The latent heat storage material is a fatty acid ester (A) having a water / octanol partition coefficient Log P of 8.0 or more and 10.0 or less, and an n-paraffin (B) having a water / octanol partition coefficient Log P of 9.2 or more and 10.0 or less. The fatty acid ester (A) and the n-paraffin (B) may be used alone or in combination.

[0054] Examples of fatty acid esters (A) having a water / octanol partition coefficient Log P of 8.0 or more and 10.0 or less (a melting point of 30°C or more and 60°C or less as measured according to JIS-K7121) include methyl stearate, methyl arachidate, methyl behenate, methyl lignocerate, myristyl myristate, cetyl myristate, and cetyl palmitate. Methyl stearate, myristyl myristate, cetyl myristate, and cetyl palmitate are preferred as fatty acid esters (A), with methyl stearate, myristyl myristate, and cetyl myristate being more preferred. Methyl stearate, myristyl myristate, and cetyl myristate are particularly preferred because they are inexpensive, highly pure industrial products available, have good compatibility with alicyclic isocyanates, and allow for uniform formation of the shell portion (wall film) of the core-shell structure during polymerization, resulting in latent heat storage particles with sufficient strength. The fatty acid ester (A) may be used alone or in combination of two or more.

[0055] Examples of n-paraffins (B) having a water / octanol partition coefficient LogP of 9.2 or more and 10.0 or less (a melting point measured according to JIS-K7121 of 30°C or more and 60°C or less) include eicosane, docosane, tetracosane, and hexacosane. Eicosane and docosane are preferred as n-paraffins (B). Eicosane and docosane are particularly preferred because they are available as inexpensive, high-purity industrial products. The n-paraffins (B) may be used alone or in combination of two or more.

[0056] In the present invention, the entire amount of the core is preferably fatty acid ester (A) and / or n-paraffin (B), but latent heat storage materials other than these may be used in combination. When a latent heat storage material other than fatty acid ester (A) and n-paraffin (B) is used in combination, the total weight ratio of fatty acid ester (A) and / or n-paraffin (B) is preferably 80% by weight or more, more preferably 90% by weight or more, and even more preferably 95% by weight.

[0057] Examples of latent heat storage materials other than the fatty acid ester (A) and n-paraffin (B) include "fatty acid esters other than the fatty acid ester (A)," "n-paraffins other than n-paraffin (B)," "petroleum waxes (paraffin wax, microcrystalline wax)," "fatty acids," "aliphatic ethers," "aliphatic ketones," and "aliphatic alcohols."

[0058] The following fatty acid esters can be used as fatty acid esters other than the fatty acid ester (A). For example, examples of fatty acid esters having a water / octanol partition coefficient Log P of less than 8.0 (a melting point measured according to JIS-K7121 of less than 30°C) include, but are not limited to, methyl palmitate, methyl myristate, methyl laurate, and lauryl laurate. For example, examples of fatty acid esters having a water / octanol partition coefficient Log P of more than 10.0 (a melting point measured according to JIS-K7121 of more than 30°C) include, but are not limited to, stearyl stearate.

[0059] The following n-paraffins can be used as n-paraffins other than n-paraffin (B). For example, n-paraffins having a water / octanol partition coefficient Log P of less than 9.2 (melting point of less than 30°C as measured according to JIS-K7121) include, but are not limited to, nonadecane, octadecane, heptadecane, hexadecane, pentadecane, and tetradecane. Furthermore, for example, n-paraffins having a water / octanol partition coefficient Log P of more than 10.0 (melting point of more than 60°C as measured according to JIS-K7121) include, but are not limited to, octacosane, nonacosane, and triacontane.

[0060] Petroleum waxes having a carbon number of 20 or more are preferred. Examples of petroleum waxes include, but are not limited to, paraffin wax and microcrystalline wax. Paraffin wax is a saturated hydrocarbon that is solid at room temperature and is produced by separating and refining the distillate from reduced-pressure distillation of petroleum or natural gas as a raw material.

[0061] Paraffin waxes having a carbon number of 20 to 40 are preferred. Commercially available paraffin waxes include, but are not limited to, HNP-9, HNP-51, FNP-0090, and FT115 manufactured by Nippon Seiro Co., Ltd. Microcrystalline waxes are saturated hydrocarbons that are solid at room temperature and are produced by separating and refining vacuum distillation residue oil or heavy distillate oil using petroleum as a raw material. Microcrystalline waxes having a carbon number of 30 to 60 are preferred.

[0062] Fatty acids having 8 to 30 carbon atoms are preferred. The fatty acids may be straight-chain saturated fatty acids, straight-chain unsaturated fatty acids, branched saturated fatty acids, or branched unsaturated fatty acids, with straight-chain saturated fatty acids being preferred due to their large latent heat capacity. Examples of straight-chain saturated fatty acids include, but are not limited to, octanoic acid, nonanoic acid, decanoic acid (capric acid), dodecanoic acid (lauric acid), tetradecanoic acid (myristic acid), hexadecanoic acid (palmitic acid), octadecanoic acid (stearic acid), eicosanoic acid, docosanoic acid, tetracosanoic acid, hexacosanoic acid, octacosanoic acid, and triacontanoic acid. Examples of fatty acid metal salts include, but are not limited to, lithium 12-hydroxystearate and aluminum 2-ethylhexanoate.

[0063] The aliphatic ether is preferably a fatty acid ether having 14 to 60 carbon atoms. Examples of aliphatic ethers include heptyl ether, octyl ether, tetradecyl ether, and hexadecyl ether. Ethers having one oxygen atom and a symmetrical structure are preferred. Examples of aliphatic ketones include, but are not limited to, 2-octanone, 3-octanone, 2-nonanone, 3-nonanone, and cycloheptanone. Examples of aliphatic alcohols include, but are not limited to, 2-dodecanol, 1-tetradecanol, 7-tetradecanol, 1-octadecanol, 1-eicosanol, and 1,10-decanediol. The origin of the latent heat storage material is not limited, and it may be derived from, for example, a fossil fuel or biomass, including fatty acid esters (A) and n-paraffins (B).

[0064] <Method for producing latent heat storage particles> The present application also provides a method for producing the above-mentioned latent heat storage particles. The method includes, for example, a step of dispersing a raw material composition containing a polyisocyanate and a latent heat storage material in a dispersion medium containing water to obtain a suspension; and a step of adding a polyol and a polyamine to the suspension and reacting the polyisocyanate, the polyamine, and the polyol.

[0065] As a result, as described above, latent heat storage particles can be obtained which have a shell portion containing a polyurethane polyurea resin and a core portion containing the latent heat storage material, and which have a heat loss of 2% by weight or less after heating for 6 hours at 110° C. Note that the terms "polyisocyanate," "polyol," "latent heat storage material," "polyamine," "polyurethane polyurea resin," "shell portion," "core portion," and "latent heat storage particles" have the same definitions as those described above.

[0066] The process of dispersing a raw material composition containing a polyisocyanate and a latent heat storage material in a dispersion medium containing water to obtain a suspension depends on the polyisocyanate, latent heat storage material, dispersion medium, etc., and the conditions may be, but are not limited to, conventionally known conditions depending on the polyisocyanate, etc., used. It is preferable to stir the dispersoid and dispersion medium during dispersion. Note that in this process, components other than the latent heat storage material contained in the core portion may be added.

[0067] The dispersion medium includes water. The dispersion medium may contain a dispersant other than water. Examples of dispersants include, but are not limited to, cellulose-based water-soluble resins (methyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, etc.), polyvinyl alcohol, polyacrylates, polyethylene glycol, polyvinylpyrrolidone, polyacrylamide, tertiary phosphates, and colloidal silica. One dispersant may be used alone, or two or more may be used in combination. The content of the dispersant is 0.001 to 5 parts by weight, preferably 0.1 to 4.9 parts by weight, more preferably 0.5 to 4.8 parts by weight, and most preferably 1.0 to 4.7 parts by weight, per 100 parts by weight of water.

[0068] The dispersion medium may contain a surfactant. Examples of the surfactant include, but are not limited to, anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants. One type of surfactant may be used alone, or two or more types may be used in combination.

[0069] The raw material composition preferably contains a urethanization catalyst, examples of which include, but are not limited to, metal catalysts such as dibutyltin laurate and amine catalysts such as triethylamine.

[0070] Next, the production method of the present invention carries out a step of adding a polyol and a polyamine to the suspension and reacting the polyisocyanate, the polyamine, and the polyol. This step depends on the suspension used, specifically the polyisocyanate, the latent heat storage material, the dispersion medium, etc., as well as the polyol and the polyamine, etc. During and after the addition of the polyol and the polyamine, it is preferable to stir the suspension.

[0071] The amounts of polyisocyanate, polyol, and polyamine depend on the polyisocyanate, polyol, latent heat storage material, dispersion medium, and polyamine used. For example, the amount of polyisocyanate is 5 to 99.5 parts by weight, preferably 45 to 98.0 parts by weight, more preferably 55 to 96.5 parts by weight, and most preferably 65 to 95.0 parts by weight, per 100 parts by weight of the polyisocyanate, polyol, and polyamine combined. For example, the amount of polyol is 1 to 80 parts by weight, preferably 2 to 50 parts by weight, more preferably 3 to 30 parts by weight, and most preferably 5 to 20 parts by weight, per 100 parts by weight of the polyisocyanate, polyol, and polyamine combined. Furthermore, for example, the amount of polyamine is preferably 0.5 to 15 parts by weight, more preferably 1.5 to 14 parts by weight, more preferably 2.0 to 12 parts by weight, and most preferably 3.0 to 10 parts by weight, per 100 parts by weight of the total of polyisocyanate, polyol, and polyamine.

[0072] It is preferable to heat the suspension during the reaction step. The heating conditions depend on the suspension used, specifically the polyisocyanate, latent heat storage material, and dispersion medium used, as well as the polyol and polyamine used, but examples of the heating conditions include, but are not limited to, a temperature of 50 to 70°C for 1 to 6 hours, followed by a temperature of 90 to 100°C for 1 to 3 hours. It is preferable to stir the suspension during heating.

[0073] After the reaction step, the mixture is cooled to room temperature, and the latent heat storage particles are recovered by a conventionally known solid-liquid separation method. The recovered latent heat storage particles are preferably washed and dried.

[0074] <Material Comprising Latent Heat Storage Particles of the Present Invention> The present application provides a material comprising latent heat storage particles. The latent heat storage particles of the present invention may be used as is or mixed with other materials to form a material comprising latent heat storage particles. Examples of materials include, but are not limited to, paper, a medium (water, a heat medium), a thermoplastic resin, a thermosetting resin, rubber, an elastomer, and a thermoplastic elastomer. For example, the latent heat storage particles of the present invention may be disposed on at least one side of a support made of a sheet-like material such as synthetic paper, a plastic film, a rubber sheet, a metal sheet, or glass. This latent heat storage particle layer may further contain, as necessary, a binder resin (e.g., a UV-curable resin such as urethane acrylate or acrylic acrylate, or a water-soluble resin such as polyvinyl alcohol or polyacrylamide), a thickener, a leveling agent, a binder resin curing agent (organic peroxide, photoradical generator), or the like. These may be used in combination. In particular, the latent heat storage particles of the present invention are preferably mixed with a resin to form a resin sheet or rubber sheet comprising latent heat storage particles. The content of the latent heat storage particles in the material having latent heat storage particles is not particularly limited. Figure 2 shows a cross-sectional view of an example of a material having latent heat storage particles of the present invention. For example, by mixing the latent heat storage particles 10 of the present invention with a resin 22 such as a thermoplastic resin or a thermosetting resin, applying the resulting material 20 to a substrate 24, and then drying it, it is possible to provide a heat storage sheet or the like, which is a material having the latent heat storage particles of the present invention on its surface.

[0075] The latent heat storage particles and materials containing latent heat storage particles of the present invention can be used in a variety of applications. Examples include, but are not limited to, electronic devices (e.g., mobile phones (especially smartphones), wearables, personal digital assistants, personal computers (especially portable personal computers), game consoles, and remote controls); battery cases for electrically powered mobility (cars, motorcycles, and drones); building materials suitable for temperature control during sudden daytime temperature increases or indoor heating and cooling (e.g., flooring, roofing, and wall materials); clothing suitable for temperature control in response to changes in ambient temperature or changes in body temperature during exercise or rest (e.g., underwear, jackets, winter clothing, and gloves); bedding; and exhaust heat utilization systems that store unnecessary exhaust heat and use it as thermal energy. Examples of applications include, but are not limited to, the following, as long as the latent heat storage particles can be used to store and release heat. Heat pumps; air conditioning applications in buildings, houses, underground shopping malls, etc.; vehicle air conditioning and canister applications; applications to prevent temperature increases in electronic components and electrical and electronic equipment such as IC chips; constant temperature applications for clothing; cold storage applications for transporting fresh food or organs; constant temperature applications for structural materials in buildings (houses, buildings, etc.) and structures (roads, bridges, etc.); anti-fogging applications for mirror surfaces such as convex mirrors; anti-freezing applications for road surfaces; cooling and constant temperature applications for home appliances such as refrigerators; ice packs and hand warmers as everyday items, etc.

[0076] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples. (Example 1) 800 g of water was charged into a 2 L separable flask equipped with a stirrer, and 10 g of hydroxypropyl methylcellulose was dissolved in the water to prepare a dispersion medium. 210 g of cetyl myristate (Log P: 9.93, melting point 47°C, latent heat 230 J / g) and 80 g of hydrogenated XDI isocyanurate were mixed to prepare a raw material composition. Note that Log P was calculated using free software based on the CLogP method available on the Molinspiration Cheminformatics website. The dispersion medium was heated to 50°C, and the raw material composition was added to the dispersion medium while stirring at 300 rpm to prepare a polymerization suspension. While stirring the polymerization suspension, 5 g of ethylene glycol and 5 g of ethylenediamine were added to the solution and stirred for 1 hour. The polymerization suspension was then heated to 60° C. and stirred for 2 hours, and further heated to 95° C. and stirred for 1 hour. The dispersion was cooled to room temperature, and the particles in the dispersion were recovered by solid-liquid separation.

[0077] The resulting particles were thoroughly washed with water and then dried at 60°C for 20 hours to obtain heat storage particles with a volume average particle diameter of 151 μm. The volume average particle diameter was measured using a laser diffraction particle size distribution analyzer (HORIBA, Ltd., LA-950V2), and the volume-based median diameter was used as the volume average particle diameter. The particles described above were measured using a differential scanning calorimeter (DSC, Rigaku Corporation, DSCvesta) in accordance with JIS K-7121. The melting point and latent heat were confirmed from the obtained DSC chart, and were found to be 47°C and 170 J / g, respectively. Furthermore, in order to confirm the durability of the resulting particles over long-term use, the particles were subjected to 100 melt-solid cycles in which they were heated from 25°C to 65°C over 30 minutes and then cooled to 25°C over 30 minutes. Thereafter, a thermal shock test was performed to confirm the elution of the material contained in the core into the oil blotting paper. No elution of the material into the oil blotting paper was confirmed.

[0078] Furthermore, in order to confirm long-term storage stability, an accelerated test was carried out in which the loss on heating was measured at 110°C for 6 hours, and the result was 0.1%. The loss on heating was calculated from the change in weight before and after heat treatment using the following formula (1). The loss on heating was evaluated three times, and the average value was used. [Loss on heating (%)] = 100 x {[Weight of latent heat storage particles before heat treatment (g)] - [Weight of latent heat storage particles after treatment (g)]} / [Weight of latent heat storage particles before heat treatment (g)] Formula (1)

[0079] (Examples 2 to 11, Comparative Examples 1 to 8) Latent heat storage particles were obtained in the same manner as in Example 1, except that the types or amounts of the solvent, polyisocyanate, latent heat storage material, and dispersion medium were changed as shown in Table 1. When a "solvent" was used, it was mixed with the latent heat storage material and polyisocyanate to prepare a raw material composition. The "solvent" was then volatilized from the particles in a process of heating to 95°C and stirring for 1 hour. The latent heat storage materials used in the examples and comparative examples are described below. The melting point and latent heat quantity of the latent heat storage material were measured using the same methods as those for measuring the particles described above. Cetyl myristate (Log P: 9.93, melting point 47°C, latent heat 230 J / g) Methyl stearate (Log P: 8.32, melting point 38°C, latent heat 220 J / g) n-docosane (Log P: 9.56, melting point 42°C, latent heat 250 J / g) Stearyl stearate (Log P: 10.29, melting point 62°C, latent heat 230 J / g) Methyl hexadecanoate (Log P: 7.37, melting point 27°C, latent heat 220 J / g) Methyl tetradecanoate (Log P: 6.36, melting point 18°C, latent heat 210 J / g) n-heptadecane (Log P: 8.79, melting point 9.19°C, latent heat 230 J / g) n-Octacosane (Log P 10.1, melting point 64°C, latent heat 165 J / g).

[0080] The obtained particles were subjected to volume average particle size measurement, melting point measurement, thermal shock test, and heat loss measurement in the same manner as in Example 1. The results are shown in Table 2. In the "thermal shock test" in Table 2, "○" indicates that no elution of the latent heat storage material was confirmed after the thermal shock test, and "×" indicates that elution of the latent heat storage material was confirmed after the thermal shock test. It can be seen from Tables 1 and 2 that Examples 1 to 11 have the desired properties, i.e., the desired heat loss value, the desired melting point, the desired thermal shock test resistance, and the desired volume average particle size.

[0081] On the other hand, in Comparative Example 1, an isocyanurate of HDI was used as the polyisocyanate, but it was found that it could not be granulated by the above method. Also, in Comparative Example 2, stearyl stearate was used as the latent heat storage material, but it was found that it could not be granulated by the above method. Furthermore, in Comparative Example 5, n-octacosane was used as the latent heat storage material, but it was found that it could not be granulated by the above method.

[0082] In Comparative Example 3, methyl tetradecanoate was used as the latent heat storage material to produce granules, but the loss on heating (2.2%) was not the desired value, and the melting point (18°C) was also not the desired value. In Comparative Example 4, n-heptadecane was used as the latent heat storage material to produce granules, but the loss on heating (2.5%) was not the desired value, the melting points (9°C and 19°C) were not the desired values, and the granules did not have thermal shock test resistance. In Comparative Examples 6 to 8, the granules were produced without using a polyol (Comparative Example 6), a polyamine (Comparative Example 7), or neither a polyol nor a polyamine (Comparative Example 8), but none of them had thermal shock test resistance.

[0083]

[0084]

Claims

1. A latent heat storage particle having a shell portion having a polyurethane polyurea resin and a core portion having a latent heat storage material, wherein the polyurethane polyurea resin has a structure derived from an alicyclic diisocyanate, and the latent heat storage material has a water / octanol partition coefficient Log P of 8 or more and 10 or less, and a melting point measured according to JIS-K7121 of 30°C or more and 60°C or less.

2. The latent heat storage particles according to claim 1, wherein the latent heat storage material having a water / octanol partition coefficient Log P of 8 or more and 10 or less is at least one selected from the group consisting of methyl stearate, myristyl myristate, cetyl myristate, and n-docosane.

3. The latent heat storage particles according to claim 1, wherein the alicyclic diisocyanate is at least one selected from the group consisting of 1,3-bis(isocyanatemethyl)cyclohexane (hydrogenated XDI), 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), isophorone diisocyanate, and norbornane diisocyanate.

4. The latent heat storage particles according to claim 1, wherein the latent heat storage particles have a volume average particle size of 1 to 500 μm.

5. A material comprising the latent heat storage particles according to any one of claims 1 to 4.

6. A method for producing latent heat storage particles, comprising the steps of: dispersing a raw material composition containing a polyisocyanate and a latent heat storage material in a dispersion medium containing water to obtain a suspension; and adding a polyol and a polyamine to the suspension and reacting the polyisocyanate, the polyamine and the polyol; thereby obtaining latent heat storage particles having a shell portion containing a polyurethane polyurea resin and a core portion containing the latent heat storage material, wherein the polyurethane polyurea resin has a structure derived from an alicyclic diisocyanate, and the latent heat storage material has a water / octanol distribution coefficient LogP of 8 or more and 10 or less and a melting point measured according to JIS-K7121 of 30°C or more and 60°C or less.

Citation Information

Patent Citations

  • Wall material for building

    JP2019112929A

  • Heat storage particles, method for producing same, and heat storage material

    WO2017135025A1

  • Thermal storage sheet, thermal storage member, and electronic device

    WO2020110662A1

  • Microcapsule, heat storage composition, heat storage sheet, and method for producing microcapsule