Adhesive tape, chemical solution tank, and method for producing chemical solution tank
The adhesive tape, featuring a fluororesin resin film and (meth)acrylic copolymer-based adhesive layers, effectively bonds fluororesins with improved retention and reduced contamination, addressing the challenges of existing bonding methods and environmental concerns.
Patent Information
- Application Number
- PCT/JP2024/017302
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-10-13
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-14
AI Technical Summary
Conventional adhesive tapes struggle to bond fluororesins effectively due to lack of adhesive properties, leading to complex processes and environmental pollution issues with existing treatment methods.
A pressure-sensitive adhesive tape with a base material containing a fluororesin resin film and adhesive layers composed of a (meth)acrylic copolymer and styrene elastomer, incorporating a tackifying resin for enhanced adhesion and reduced contamination.
The adhesive tape provides excellent retention performance, low contamination, and easy bonding of fluororesins, improving adhesion while minimizing environmental impact.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Adhesive tape, chemical tank, and method for manufacturing chemical tank
[0001] The present invention relates to an adhesive tape. The present invention also relates to a chemical liquid tank having the adhesive tape attached thereto. Furthermore, the present invention also relates to a method for manufacturing a chemical liquid tank using the adhesive tape.
[0002] Conventionally, adhesive tapes have been widely used to fix components in electronic devices. Specifically, adhesive tapes are used, for example, to adhere a cover panel for protecting the surface of a portable electronic device to a touch panel module or a display panel module, or to adhere a touch panel module to a display panel module. Adhesive tapes used to fix such electronic device components are required to have not only high adhesiveness but also functions such as heat resistance, thermal conductivity, and impact resistance depending on the environment of the location where they are used (e.g., Patent Documents 1 to 3).
[0003] JP 2015-052050 A JP 2015-021067 A JP 2015-120876 A
[0004] In recent years, demand for fluororesins has been increasing in various fields due to their excellent heat resistance, chemical resistance, low dielectric properties, and water repellency. For example, tetrafluoroethylene copolymer (PTFE) is used in a wide range of fields, such as wire coating materials and building materials, due to its high mechanical strength and excellent processability.
[0005] Fluoropolymers are commonly used to bond dissimilar materials, but they do not readily exhibit the adhesive properties of adhesive tapes, making bonding difficult with standard adhesive tapes. Therefore, bonding between fluoropolymers and dissimilar materials typically involves applying a liquid adhesive to a fluoropolymer surface that has been treated for improved adhesion, attaching the material via a silicone adhesive tape, or treating the fluoropolymer surface with an alkaline hydrophilic agent to improve the adhesive strength of the adhesive. However, each of these methods presents challenges, including the complicated process involved with using liquid adhesives, contamination of the bonded components due to the volatilization and penetration of low-molecular-weight components in silicone adhesives, and environmental pollution caused by wastewater generated during the alkaline hydrophilic treatment.
[0006] The present invention provides an adhesive tape that has excellent holding performance, is less likely to contaminate an adherend, and can easily bond fluororesins. Another object of the present invention is to provide a chemical tank to which the adhesive tape is attached. Furthermore, the present invention provides a method for manufacturing a chemical tank using the adhesive tape.
[0007] Disclosure 1 is a pressure-sensitive adhesive tape having a substrate and a first pressure-sensitive adhesive layer adjacent to one surface of the substrate, the substrate comprising a resin film containing a fluororesin, the first pressure-sensitive adhesive layer comprising a base polymer (P1) and a tackifier resin, the base polymer (P1) comprising at least one selected from the group consisting of (meth)acrylic copolymers and styrene-based elastomers. Disclosure 2 is a pressure-sensitive adhesive tape of Disclosure 1, having, in this order, the substrate, the first pressure-sensitive adhesive layer, an intermediate layer, and a second pressure-sensitive adhesive layer, the second pressure-sensitive adhesive layer comprising a base polymer (P2), the base polymer (P2) comprising at least one selected from the group consisting of (meth)acrylic copolymers and styrene-based elastomers.
[0014] Disclosure 3 is the pressure-sensitive adhesive tape of Disclosure 2, wherein the second pressure-sensitive adhesive layer has a probe tack value of 20 N / 5 mmφ or less, measured under conditions of 23°C, a pressure of 98 gf, a pressure-applying rate of 100 mm / sec, a pressure-applying time of 10 seconds, and a peel-off rate of 5 mm / sec. Disclosure 4 is the pressure-sensitive adhesive tape of Disclosure 1, comprising the substrate, the first pressure-sensitive adhesive layer, and a hot-melt pressure-sensitive adhesive layer, in this order. Disclosure 5 is the pressure-sensitive adhesive tape of Disclosure 1, 2, 3, or 4, wherein the (meth)acrylic copolymer in the base polymer (P1) has a structural unit derived from an alkyl (meth)acrylate having an alkyl group having from 4 to 12 carbon atoms at its ester terminal, and at least one structural unit selected from the group consisting of a structural unit derived from a carboxy group-containing (meth)acrylate and a structural unit derived from a hydroxy group-containing (meth)acrylate. Disclosure 6 is the pressure-sensitive adhesive tape of Disclosure 5, wherein the alkyl(meth)acrylate having an alkyl group having from 4 to 12 carbon atoms at its ester terminal comprises an alkyl(meth)acrylate having an alkyl group having from 6 to 8 carbon atoms at its ester terminal. Disclosure 7 is the pressure-sensitive adhesive tape of Disclosure 5 or 6, wherein the alkyl(meth)acrylate having an alkyl group having from 4 to 12 carbon atoms at its ester terminal comprises n-heptyl(meth)acrylate.
[0014] The present disclosure 8 is the pressure-sensitive adhesive tape of disclosure 6 or 7, wherein the (meth)acrylic copolymer contains 50% by mass or more and 99.5% by mass or less of the structural unit derived from alkyl (meth)acrylate having an alkyl group having from 6 to 8 carbon atoms at the ester terminal.
[0015] The present disclosure 9 is the pressure-sensitive adhesive tape of disclosure 1, 2, 3, 4, 5, 6, 7, or 8, wherein the tackifier resin comprises a tackifier resin (T1) having at least one structural unit (A) selected from the group consisting of structural units (A-1), (A-1'), (A-2), (A-2'), (A-3), (A-3'), (A-4), and (A-4') represented by the following formula.
[0016] The present disclosure 10 is the pressure-sensitive adhesive tape of disclosure 9, wherein the tackifier resin (T1) further contains a structural unit (B) derived from at least one monomer (b) selected from the group consisting of terpene monomers and vinyl monomers.
[0023] Disclosure 11 is the pressure-sensitive adhesive tape of Disclosure 9 or 10, wherein the content of the tackifier resin (T1) is 5 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the base polymer (P1). Disclosure 12 is the pressure-sensitive adhesive tape of Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, or 11, wherein the tackifier resin comprises at least one tackifier resin (T2) selected from the group consisting of rosin ester-based resins, terpene-based resins, terpene phenolic resins, and petroleum-based resins. Disclosure 13 is the pressure-sensitive adhesive tape of Disclosure 12, wherein the tackifier resin (T2) comprises a rosin ester-based resin. Disclosure 14 is the pressure-sensitive adhesive tape of Disclosure 12 or 13, wherein the softening temperature of the tackifier resin (T2) is 50°C or more and 200°C or less.
[0023] The present disclosure 15 is the pressure-sensitive adhesive tape of disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, or 14, wherein the first pressure-sensitive adhesive layer does not contain an organosilicon compound or the content of the organosilicon compound in the first pressure-sensitive adhesive layer is 3.0 mass% or less.
[0024] The present disclosure 16 is the pressure-sensitive adhesive tape of disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15, wherein the first pressure-sensitive adhesive layer has a 180° peel strength from the substrate at 23°C of 2.5 N / 25 mm or more.Disclosure 17 is the pressure-sensitive adhesive tape of Disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, or 16, wherein the first pressure-sensitive adhesive layer has a loss tangent (tan δ) measured at a frequency of 10 Hz in dynamic viscoelasticity measurement that peaks in a temperature range of −30° C. or higher and 15° C. or lower. Disclosure 18 is the pressure-sensitive adhesive tape of Disclosure 18, wherein the first pressure-sensitive adhesive layer has a shear storage modulus of 1.0×10 at 25° C. measured at a frequency of 10 Hz in dynamic viscoelasticity measurement. 4 Pa or more 5.0×10 5The pressure-sensitive adhesive tape of Disclosure 17, wherein the loss tangent (tan δ) measured in dynamic viscoelasticity measurement at a frequency of 10 Hz has a peak in a temperature range of -30°C or more and 15°C or less. Disclosure 19 is the pressure-sensitive adhesive tape of Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, or 18, wherein the first pressure-sensitive adhesive layer has a gel fraction of 15% by mass or more and 70% by mass or less. Disclosure 20 is the pressure-sensitive adhesive tape of Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, or 19, wherein the first pressure-sensitive adhesive layer has a thickness of 20 μm or more and 500 μm or less.
[0023] Disclosure 21 is the pressure-sensitive adhesive tape of Disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20, wherein the resin film containing a fluororesin includes at least one selected from the group consisting of a fluororesin-impregnated glass cloth and a laminate film in which a fluororesin layer and a glass cloth layer are laminated together. Disclosure 22 is the pressure-sensitive adhesive tape of Disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, or 21, wherein the substrate has a thickness of 50 μm or more and 5000 μm or less. Disclosure 23 is the pressure-sensitive adhesive tape of Disclosures 2 or 3, wherein the second pressure-sensitive adhesive layer has a 180° peel strength from SUS at 23°C of 8.0 N / 25 mm or less.
[0023] Disclosure 24 is the pressure-sensitive adhesive tape of Disclosures 2, 3, or 23, wherein the second pressure-sensitive adhesive layer has a thickness of 20 μm or more and 500 μm or less. Disclosure 25 is the pressure-sensitive adhesive tape of Disclosures 2, 3, 23, or 24, wherein the intermediate layer comprises at least one selected from the group consisting of polyester resin, polyimide resin, polyolefin resin, polyurethane resin, glass fiber, carbon fiber, and metal. Disclosure 26 is the pressure-sensitive adhesive tape of Disclosures 2, 3, 23, 24, or 25, wherein the intermediate layer has a foam structure. Disclosure 27 is the pressure-sensitive adhesive tape of Disclosure 4, wherein the hot-melt pressure-sensitive adhesive layer has a 180° peel strength from SUS at 23°C of 5.0 N / 25 mm or more when pressure-bonded to SUS in a 150°C environment at 0.1 MPa for 10 minutes.Disclosure 28 is the pressure-sensitive adhesive tape of Disclosure 4 or 27, wherein the hot melt pressure-sensitive adhesive layer contains a base polymer (P3), and the base polymer (P3) comprises at least one selected from the group consisting of a (meth)acrylic copolymer, a styrene-based elastomer, an ethylene-vinyl acetate copolymer, a chloroprene rubber, a nitrile rubber, a polyurethane resin, a polyamide resin, a polyolefin resin, a polyester resin, and an epoxy resin. Disclosure 29 is the pressure-sensitive adhesive tape of Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, or 28, which is used to protect an adherend. Disclosure 30 is the pressure-sensitive adhesive tape of Disclosure 29, which is used to protect an adherend from a chemical solution. The present disclosure 31 is the adhesive tape of the present disclosure 30 used for lining the can body of a chemical tank for semiconductors or a chemical tank for the chemical industry. The present disclosure 32 is a chemical tank in which the adhesive tape of the present disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, or 31 is attached to the inner surface of the can body. Disclosure 33 is a method for manufacturing a chemical tank for semiconductors or a chemical tank for the chemical industry, the method including a step of attaching the adhesive tape of Disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, or 31 to the inner surface of a can body of the chemical tank.
[0008]
[0009]
[0010]
[0011]
[0012] In the formula, R 1 ~R 7each represents a hydrogen atom, an aliphatic hydrocarbon group, an aromatic hydrocarbon group, a polar functional group, an aliphatic hydrocarbon group having a polar functional group, or an aromatic hydrocarbon group having a polar functional group. n and l each represent an integer of 2 or more and 4 or less, and n' and l' each represent an integer of 2 or more and 5 or less. m and k each represent an integer of 1 or more and 4 or less, and m' and k' each represent an integer of 1 or more and 5 or less. * represents a linking moiety. The present invention will be described in detail below.
[0013] The present inventors investigated a pressure-sensitive adhesive tape having a substrate and a pressure-sensitive adhesive layer adjacent to the substrate by incorporating a resin film containing a fluororesin into the substrate, by using a (meth)acrylic copolymer or a styrene-based elastomer as the base polymer of the pressure-sensitive adhesive layer, and by incorporating a tackifier resin into the pressure-sensitive adhesive layer. As a result, they found that a pressure-sensitive adhesive tape having excellent holding performance, low contamination of the adherend, and easy bonding of the fluororesin can be obtained, leading to the completion of the present invention. In this specification, "(meth)acrylic" means acrylic or methacrylic. In this specification, "base polymer" means a polymer that accounts for 50% by mass or more of the polymer contained in the pressure-sensitive adhesive layer and has a weight-average molecular weight of 50,000 or more.
[0014] The pressure-sensitive adhesive tape of the present invention has a substrate. The substrate includes a resin film containing a fluororesin. By including a resin film containing a fluororesin in the substrate, the pressure-sensitive adhesive tape of the present invention can easily bond the fluororesin to a different material. Examples of fluororesins contained in the fluororesin-containing resin film include polytetrafluoroethylene (PTFE), perfluoroalkoxyalkane (PFA), perfluoroethylenepropene copolymer (FEP), ethylenetetrafluoroethylene copolymer (ETFE), polyvinylidene fluoride (PVDF), polyvinyl fluoride (PVF), polychlorotrifluoroethylene (PCTFE), and ethylenechlorotrifluoroethylene copolymer (ECTFE). Among these, PTFE is preferred due to its excellent heat resistance and chemical resistance.
[0015] The fluororesin-containing resin film is not particularly limited as long as it is a film, and may include at least one selected from the group consisting of a fluororesin-impregnated glass cloth film and a laminate film formed by laminating a fluororesin layer and a glass cloth layer. When the fluororesin-containing resin film includes at least one selected from the group consisting of a fluororesin-impregnated glass cloth film and a laminate film formed by laminating a fluororesin layer and a glass cloth layer, the interface between the substrate and the first pressure-sensitive adhesive layer is increased, resulting in more reliable bonding between the substrate and the first pressure-sensitive adhesive layer. Examples of the fluororesin-impregnated glass cloth film include a PTFE-impregnated glass cloth sheet (manufactured by Chukoh Chemical Industry Co., Ltd.). Examples of the laminate film formed by laminating a fluororesin layer and a glass cloth layer include a glass back sheet (manufactured by Yodogawa Hu-Tech Co., Ltd.).
[0016] The preferred lower limit of the thickness of the substrate is 20 μm, and the preferred upper limit is 5000 μm. When the thickness of the substrate is 20 μm or more, a sufficient thickness of fluororesin can be bonded to the adherend, making the resulting adhesive tape more suitable for protecting the adherend, etc. When the thickness of the substrate is 5000 μm or less, the adhesive tape can be easily rolled, further improving the manufacturing efficiency of the adhesive tape. A more preferred lower limit of the thickness of the substrate is 40 μm, and a more preferred upper limit is 3000 μm. In this specification, the thickness can be measured using a dial thickness meter (such as the "ABS Digimatic Indicator" manufactured by Mitutoyo Corporation).
[0017] The pressure-sensitive adhesive tape of the present invention has a first pressure-sensitive adhesive layer adjacent to one surface of the substrate. The first pressure-sensitive adhesive layer contains a base polymer (P1). The base polymer (P1) contains one selected from the group consisting of (meth)acrylic copolymers and styrene-based elastomers. When the first pressure-sensitive adhesive layer contains one selected from the group consisting of (meth)acrylic copolymers and styrene-based elastomers, the resulting pressure-sensitive adhesive tape can be less susceptible to contamination of an adherend. In particular, from the viewpoint of further improving the holding performance of the resulting pressure-sensitive adhesive tape by forming a crosslinked structure, it is preferable that the base polymer (P1) contains a (meth)acrylic copolymer.
[0018] The (meth)acrylic copolymer preferably has a structural unit derived from an alkyl (meth)acrylate. The alkyl (meth)acrylate preferably includes an alkyl (meth)acrylate having an alkyl group having from 4 to 12 carbon atoms at the ester terminal. That is, the (meth)acrylic copolymer preferably has a structural unit derived from an alkyl (meth)acrylate having an alkyl group having from 4 to 12 carbon atoms at the ester terminal. By including a structural unit derived from an alkyl (meth)acrylate having an alkyl group having from 4 to 12 carbon atoms at the ester terminal, the glass transition temperature (Tg) of the (meth)acrylic copolymer is further reduced. As a result, the shear storage modulus at 25°C measured at a frequency of 10 Hz in the dynamic viscoelasticity measurement of the first pressure-sensitive adhesive layer described below (hereinafter, sometimes simply referred to as the "shear storage modulus at 25°C of the first pressure-sensitive adhesive layer") is appropriately reduced, and the flexibility of the first pressure-sensitive adhesive layer is further improved, thereby improving the adhesive strength of the first pressure-sensitive adhesive layer to fluororesins and the adhesion to the substrate. In this specification, "(meth)acrylate" means acrylate or methacrylate. In addition, in this specification, "alkyl(meth)acrylate having an alkyl group at the ester terminal" means a (meth)acrylate in which an alkyl group is bonded to the oxygen atom of the ester bond.
[0019] Examples of the alkyl(meth)acrylate having an alkyl group having from 4 to 12 carbon atoms at the ester terminal include n-butyl(meth)acrylate, tert-butyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, n-hexyl(meth)acrylate, n-heptyl(meth)acrylate, n-octyl(meth)acrylate, isooctyl(meth)acrylate, n-nonyl(meth)acrylate, isononyl(meth)acrylate, 1-methylheptyl(meth)acrylate, lauryl(meth)acrylate, etc. Among these, the alkyl(meth)acrylate having an alkyl group having from 4 to 12 carbon atoms at the ester terminal preferably includes an alkyl(meth)acrylate having an alkyl group having from 6 to 8 carbon atoms at the ester terminal, and more preferably includes n-heptyl(meth)acrylate, because this further improves the adhesive strength of the pressure-sensitive adhesive tape (particularly the adhesive strength to fluororesins). These alkyl (meth)acrylates having an alkyl group with 4 to 12 carbon atoms at the ester terminal may be used alone or in combination of two or more. Generally, alkyl (meth)acrylates having an alkyl group with an odd number of carbon atoms at the ester terminal tend to be less prone to molecular packing, resulting in a lower glass transition temperature (Tg) of the alkyl (meth)acrylate. Therefore, by including a structural unit derived from n-heptyl (meth)acrylate in the (meth)acrylic copolymer, it is possible to further suppress packing between the alkyl groups at the ester terminal in the (meth)acrylic copolymer, thereby further lowering the glass transition temperature (Tg) of the (meth)acrylic copolymer. As a result, the shear storage modulus at 25°C of the first pressure-sensitive adhesive layer (described below) is appropriately reduced, and the flexibility of the first pressure-sensitive adhesive layer is further improved, resulting in improved adhesion of the first pressure-sensitive adhesive layer to fluororesins and improved adhesion to the substrate.
[0020] The content of the structural units derived from alkyl(meth)acrylate having an alkyl group with 4 to 12 carbon atoms at the ester terminal in the (meth)acrylic copolymer is preferably 50% by mass or more. When the content of the structural units derived from alkyl(meth)acrylate having an alkyl group with 4 to 12 carbon atoms at the ester terminal is 50% by mass or more, the glass transition temperature (Tg) of the (meth)acrylic copolymer is further reduced, resulting in an appropriate reduction in the shear storage modulus at 25°C of the pressure-sensitive adhesive layer described below, and further improved flexibility of the first pressure-sensitive adhesive layer, thereby further improving adhesion to the substrate. A more preferred lower limit of the content of the structural units derived from alkyl(meth)acrylate having an alkyl group with 4 to 12 carbon atoms at the ester terminal is 90% by mass, and an even more preferred lower limit is 95% by mass. Furthermore, the upper limit of the constituent units derived from alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms at the ester end may be 99.99% by mass, but from the viewpoint of the cohesive strength of the bulk of the first adhesive layer, a preferred upper limit is 99% by mass.
[0021] The content of the structural units derived from alkyl(meth)acrylate having an alkyl group with 6 to 8 carbon atoms at the ester terminal in the (meth)acrylic copolymer is preferably 50% by mass or more. When the content of the structural units derived from alkyl(meth)acrylate having an alkyl group with 6 to 8 carbon atoms at the ester terminal is 50% by mass or more, the glass transition temperature (Tg) of the (meth)acrylic copolymer is further reduced, resulting in an appropriate reduction in the shear storage modulus at 25°C of the pressure-sensitive adhesive layer described below, and further improved flexibility of the first pressure-sensitive adhesive layer, thereby further improving adhesion to the substrate. A more preferred lower limit of the content of the structural units derived from alkyl(meth)acrylate having an alkyl group with 6 to 8 carbon atoms at the ester terminal is 85% by mass, and an even more preferred lower limit is 90% by mass. Furthermore, from the viewpoint of the bulk cohesive strength of the first adhesive layer, the preferred upper limit of the structural units derived from alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms at the ester terminal is 99.5 mass %, and the more preferred upper limit is 99 mass %.
[0022] The alkyl (meth)acrylate may contain alkyl (meth)acrylates other than the alkyl (meth)acrylates having an alkyl group having from 4 to 12 carbon atoms at the ester terminal. Examples of the other alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, myristyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, esters of 5,7,7-trimethyl-2-(1,3,3-trimethylbutyl)octanol-1 and (meth)acrylic acid, esters of alcohols having a total of 18 carbon atoms and one or two methyl groups in the linear main chain and (meth)acrylic acid, behenyl (meth)acrylate, and arachidyl (meth)acrylate. These other alkyl (meth)acrylates may be used alone or in combination of two or more.
[0023] The (meth)acrylic copolymer preferably further comprises a structural unit derived from a polar functional group-containing monomer. By including a structural unit derived from a polar functional group-containing monomer in the (meth)acrylic copolymer, the bulk cohesive strength of the first pressure-sensitive adhesive layer is increased, and the adhesive strength and holding performance of the resulting pressure-sensitive adhesive tape are further improved.
[0024] The polar functional group is reactive for crosslinking reactions and the like, and is preferably at least one selected from the group consisting of a carboxy group, a hydroxyl group, an amino group, and an epoxy group. Among these, a carboxy group and a hydroxyl group are more preferred because they contribute to improving the adhesive strength and retention performance of the resulting pressure-sensitive adhesive tape. That is, the (meth)acrylic copolymer preferably has at least one structural unit selected from the group consisting of a structural unit derived from a carboxy group-containing (meth)acrylate and a structural unit derived from a hydroxyl group-containing (meth)acrylate. Examples of the carboxy group-containing monomer include (meth)acrylic acid. Examples of the hydroxy group-containing monomer include 4-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2-hydroxyethyl (meth)acrylate. Examples of the epoxy group-containing monomer include glycidyl (meth)acrylate. These polar functional group-containing monomers may be used alone, or two or more may be used in combination.
[0025] The content of the structural units derived from the carboxyl group-containing monomer in the (meth)acrylic copolymer is preferably 0.01% by mass at the lower limit and 7.0% by mass at the upper limit. By ensuring that the content of the structural units derived from the carboxyl group-containing monomer is within this range, the cohesive strength of the bulk of the first pressure-sensitive adhesive layer can be appropriately adjusted, resulting in an adhesive tape having superior adhesive strength and holding performance. The content of the structural units derived from the carboxyl group-containing monomer is more preferably 0.05% by mass at the lower limit and 5.0% by mass at the upper limit.
[0026] The content of the structural units derived from the hydroxyl group-containing monomer in the (meth)acrylic copolymer is preferably 0.01% by mass at the lower limit and 3.0% by mass at the upper limit. By ensuring that the content of the structural units derived from the hydroxyl group-containing monomer is within this range, the cohesive strength of the bulk of the first pressure-sensitive adhesive layer can be appropriately adjusted, resulting in an adhesive tape having superior adhesive strength and holding performance. The content of the structural units derived from the hydroxyl group-containing monomer is more preferably 0.05% by mass at the lower limit and 2.0% by mass at the upper limit.
[0027] The total content of the structural units derived from the polar functional group-containing monomer in the (meth)acrylic copolymer is preferably 0.01% by mass at the lower limit and 10.0% by mass at the upper limit. By ensuring that the total content of the structural units derived from the polar functional group-containing monomer falls within this range, the bulk cohesive strength of the first pressure-sensitive adhesive layer can be appropriately adjusted, resulting in a pressure-sensitive adhesive tape with superior adhesive strength and holding performance. The total content of the structural units derived from the polar functional group-containing monomer is more preferably 0.1% by mass at the lower limit and 7.0% by mass at the upper limit.
[0028] The (meth)acrylic copolymer may optionally contain structural units derived from other copolymerizable polymerizable monomers other than the structural units derived from the alkyl (meth)acrylates and the structural units derived from the polar functional group-containing monomers described above. Examples of such other monomers include benzyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, and polypropylene glycol mono(meth)acrylate. Furthermore, examples of such other monomers include various monomers commonly used in acrylic polymers, such as vinyl carboxylates such as vinyl acetate and styrene. These other monomers may be used alone or in combination of two or more.
[0029] The weight-average molecular weight (Mw) of the (meth)acrylic copolymer preferably has a lower limit of 200,000 and an upper limit of 2,000,000. When the weight-average molecular weight (Mw) of the (meth)acrylic copolymer is 200,000 or more, the bulk cohesive strength of the first pressure-sensitive adhesive layer is improved, and the adhesive strength and holding performance of the resulting pressure-sensitive adhesive tape are further improved. When the weight-average molecular weight (Mw) of the (meth)acrylic copolymer is 2,000,000 or less, the adhesion of the first pressure-sensitive adhesive layer to the substrate is further improved. The weight-average molecular weight (Mw) of the (meth)acrylic copolymer more preferably has a lower limit of 300,000, a more preferred upper limit of 1,600,000, an even more preferred lower limit of 500,000, and an even more preferred upper limit of 1,200,000.
[0030] The ratio of the weight-average molecular weight (Mw) to the number-average molecular weight (Mn) of the (meth)acrylic copolymer (molecular weight distribution, Mw / Mn) preferably has a lower limit of 1.05 and an upper limit of 10.0. When the (meth)acrylic copolymer has a molecular weight distribution (Mw / Mn) of 1.05 or more, the flexibility of the first pressure-sensitive adhesive layer is further improved, and the adhesive strength of the resulting pressure-sensitive adhesive tape to fluororesin is further improved. When the (meth)acrylic copolymer has a molecular weight distribution (Mw / Mn) of 10.0 or less, the proportion of low-molecular-weight components is reduced, the cohesive strength of the bulk of the first pressure-sensitive adhesive layer is improved, and the adhesive strength and holding performance of the resulting pressure-sensitive adhesive tape are further improved. The upper limit of the molecular weight distribution (Mw / Mn) of the (meth)acrylic copolymer is more preferably 8.0, even more preferably 6.0, and even more preferably 4.0.
[0031] In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) refer to the weight average molecular weight in terms of standard polystyrene measured by gel permeation chromatography (GPC). Specifically, the (meth)acrylic copolymer is diluted 50 times with tetrahydrofuran (THF), and the diluted solution is filtered through a filter (material: polytetrafluoroethylene, pore diameter: 0.2 μm). The obtained filtrate is supplied to a gel permeation chromatograph (Waters, "2690 Separations Module", etc.), and GPC measurement is performed under conditions of a sample flow rate of 1 mL / min and a column temperature of 40 ° C., and the polystyrene-equivalent molecular weight of the (meth)acrylic copolymer is measured to determine the weight average molecular weight (Mw) and number average molecular weight (Mn). As the column, for example, a GPC KF-802.5L (Showa Denko KK) or the like is used, and as the detector, for example, a differential refractometer or the like can be used. Furthermore, the molecular weight distribution (Mw / Mn) can be measured using the weight average molecular weight (Mw) and number average molecular weight (Mn) thus obtained.
[0032] The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the (meth)acrylic copolymer can be adjusted to fall within the above ranges by, for example, adjusting the composition, polymerization method, polymerization conditions, etc. of the (meth)acrylic copolymer.
[0033] The glass transition temperature (Tg) of the (meth)acrylic copolymer preferably has a lower limit of −70°C and an upper limit of −30°C. When the glass transition temperature of the (meth)acrylic copolymer is within the above range, it becomes easier to adjust the shear storage modulus at 25°C of the first pressure-sensitive adhesive layer (described below) to an appropriate range, thereby resulting in an adhesive tape having superior adhesive strength and retention performance to fluororesins. The glass transition temperature (Tg) of the (meth)acrylic copolymer is more preferably −60°C in lower limit and more preferably −40°C in upper limit. In this specification, the glass transition temperature can be the value obtained in one run when measured using a differential scanning calorimeter (e.g., SII Exstar 6000 / DSC 6220 manufactured by Hitachi High-Tech Science Corporation) under conditions of a nitrogen atmosphere and a heating rate of 10°C / min.
[0034] The polymerization method for synthesizing the (meth)acrylic copolymer may be a conventionally known method in which monomers from which the above-mentioned structural units are derived are subjected to a radical reaction in the presence of a polymerization initiator, and examples thereof include solution polymerization (boiling point polymerization or constant temperature polymerization), emulsion polymerization, suspension polymerization, bulk polymerization, etc. Among these, solution polymerization is preferred because of its ease of synthesis.
[0035] When solution polymerization is used as the polymerization method, examples of the reaction solvent include ethyl acetate, toluene, methyl ethyl ketone, methyl sulfoxide, ethanol, acetone, diethyl ether, etc. These reaction solvents may be used alone or in combination of two or more.
[0036] Examples of the polymerization initiator include organic peroxides and azo compounds. Examples of the organic peroxides include 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane, t-hexylperoxypivalate, t-butylperoxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyisobutyrate, t-butylperoxy-3,5,5-trimethylhexanoate, and t-butylperoxylaurate. Examples of the azo compounds include azobisisobutyronitrile and azobiscyclohexanecarbonitrile. These polymerization initiators may be used alone or in combination of two or more.
[0037] The styrene-based elastomer may be a block copolymer having a block derived from the styrene-based monomer and a block derived from the conjugated diene-based monomer, having rubber elasticity at room temperature, and having a hard segment portion and a soft segment portion, where the block derived from the styrene-based monomer is the hard segment portion and the block derived from the conjugated diene-based monomer is the soft segment portion.
[0038] Examples of the styrene-based monomer include styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-t-butylstyrene, 5-t-butyl-2-methylstyrene, vinylethylbenzene, divinylbenzene, trivinylbenzene, divinylnaphthalene, t-butoxystyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, N,N-dimethylaminoethylstyrene, N,N-dimethylaminomethylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2-t-butylstyrene, 3-t-butylstyrene, 4-t-butylstyrene, vinylxylene, vinylnaphthalene, vinylpyridine, diphenylethylene, and tertiary amino group-containing diphenylethylene. Among these, styrene is preferred because of its industrial availability. Examples of the tertiary amino group-containing diphenylethylene include 1-(4-N,N-dimethylaminophenyl)-1-phenylethylene. These styrene-based monomers may be used alone or in combination of two or more.
[0039] Examples of the conjugated diene monomer include isoprene, 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 1,3-heptadiene, 2-phenyl-1,3-butadiene, 3-methyl-1,3-pentadiene, and 2-chloro-1,3-butadiene. Among these, 1,3-butadiene and isoprene are preferred because of their high polymerization reactivity and industrial ease of availability. These conjugated diene monomers may be used alone or in combination of two or more.
[0040] Specific examples of the styrene-based elastomer include styrene-isoprene-styrene (SIS) block copolymers, styrene-butadiene-styrene (SBS) block copolymers, and styrene-chloroprene-styrene block copolymers. Among these, SIS block copolymers and SBS block copolymers are preferred, with SIS block copolymers being more preferred, because the resulting pressure-sensitive adhesive tape is likely to exhibit high adhesive strength and is unlikely to peel from the adherend even when immersed in an alkaline chemical solution. These styrene-based elastomers may be used alone, or two or more types may be used in combination.
[0041] The styrene-based elastomer may contain, in addition to a triblock copolymer of the block derived from the styrene-based monomer and the block derived from the conjugated diene-based monomer, a diblock copolymer of the block derived from the styrene-based monomer and the block derived from the conjugated diene-based monomer. The preferred lower limit of the content of the diblock copolymer in the styrene-based elastomer (hereinafter sometimes referred to as the "diblock ratio") is 50% by mass. A diblock ratio of 50% by mass or more enhances the adhesion of the first pressure-sensitive adhesive layer to an adherend, further improving the adhesive strength of the resulting pressure-sensitive adhesive tape. Furthermore, the shear storage modulus at 25°C of the first pressure-sensitive adhesive layer (described below) is appropriately reduced, further improving the flexibility of the first pressure-sensitive adhesive layer, thereby improving the adhesive strength of the first pressure-sensitive adhesive layer to the fluororesin and the adhesion to the substrate. A more preferred lower limit of the diblock ratio is 70% by mass. From the viewpoint of further improving the cohesive strength of the first pressure-sensitive adhesive layer, a preferred upper limit of the diblock ratio is 90% by mass. The diblock ratio can be calculated from the peak area ratio of each copolymer measured by gel permeation chromatography (GPC).
[0042] The content of the block derived from the styrene-based monomer in the styrene-based elastomer (hereinafter sometimes referred to as "styrene content") is preferably 20% by mass at its upper limit. When the styrene content is 20% by mass or less, the first pressure-sensitive adhesive layer does not become too hard, and the adhesion to the adherend is increased, further improving the adhesive strength of the resulting pressure-sensitive adhesive tape. A more preferred upper limit of the styrene content is 16% by weight. Furthermore, from the viewpoint of further improving the cohesive strength of the first pressure-sensitive adhesive layer, a preferred lower limit of the styrene content is 8% by mass. The styrene content is 1 It can be calculated from the peak area ratio of each block measured by H-NMR.
[0043] The weight-average molecular weight of the styrene-based elastomer preferably has a lower limit of 50,000 and an upper limit of 600,000. When the weight-average molecular weight of the styrene-based elastomer is 50,000 or more, the bulk strength of the first pressure-sensitive adhesive layer increases, and the adhesive strength of the resulting pressure-sensitive adhesive tape is further improved. When the weight-average molecular weight of the styrene-based elastomer is 600,000 or less, the compatibility of the styrene-based elastomer with other components is further improved. A more preferred lower limit of the weight-average molecular weight of the styrene-based elastomer is 100,000, and a more preferred upper limit is 500,000.
[0044] The preferred lower limit of the content of the base polymer (P1) in the first pressure-sensitive adhesive layer is 30% by mass, and the preferred upper limit is 99.5% by mass. By having the content of the base polymer (P1) within the above range, the adhesive strength of the first pressure-sensitive adhesive layer to fluororesins is further improved. The more preferred lower limit of the content of the base polymer (P1) is 40% by mass, and the more preferred upper limit is 99% by mass, and the even more preferred lower limit is 50% by mass, and the even more preferred upper limit is 95% by mass.
[0045] The pressure-sensitive adhesive layer contains a tackifier resin. The tackifier resin preferably contains a tackifier resin (T1) having at least one structural unit (A) selected from the group consisting of the structural unit (A-1), the structural unit (A-1'), the structural unit (A-2), the structural unit (A-2'), the structural unit (A-3), the structural unit (A-3'), the structural unit (A-4), and the structural unit (A-4') represented by the above formula. By containing the tackifier resin (T1) in the first pressure-sensitive adhesive layer, the first pressure-sensitive adhesive layer can exhibit higher adhesive strength, particularly high adhesive strength to adherends with low polarity (e.g., fluororesins, etc.), and further improve adhesion to the substrate. In particular, the structural unit (A) is preferably at least one selected from the group consisting of the structural unit (A-1), the structural unit (A-1'), the structural unit (A-2), the structural unit (A-2'), the structural unit (A-3), and the structural unit (A-3'), because this can greatly improve the interaction with the adherend and further increase the adhesive strength to the adherend, and more preferably at least one selected from the group consisting of the structural unit (A-1) and the structural unit (A-1'). When the structural unit (A) is at least one selected from the group consisting of the structural unit (A-1) and the structural unit (A-1'), the interaction with the adherend can be further greatly improved. Furthermore, since it is easy to use monomers containing biological materials, as described below, as monomers constituting the structural unit (A-1) and the structural unit (A-1'), this is preferable from the perspective of conserving petroleum resources. Furthermore, when the base polymer (P1) is a (meth)acrylic copolymer, the tackifier resin (T1) has an appropriate polarity, which results in better compatibility with the (meth)acrylic copolymer.
[0046] The tackifier resin (T1) may have the structural unit (A) in a side chain, or in the main chain skeleton or at an end of the main chain skeleton. In particular, the tackifier resin (T1) preferably has the structural unit (A) in the main chain skeleton or at an end of the main chain skeleton, since this allows the tackifier resin to have suitable physical properties required as a tackifier resin.
[0047] In the structural unit (A), R 1 ~R 7 respectively represent a hydrogen atom, an aliphatic hydrocarbon group, an aromatic hydrocarbon group, a polar functional group, an aliphatic hydrocarbon group having a polar functional group, or an aromatic hydrocarbon group having a polar functional group. Examples of the aliphatic hydrocarbon group include linear, branched, or cyclic alkyl groups having 1 to 20 carbon atoms. Examples of the aromatic hydrocarbon group include substituted or unsubstituted aryl groups having 1 to 20 carbon atoms. The polar functional group is not particularly limited, and R 1 As the polar functional group other than the hydroxyl group, R 2 is a polar functional group other than a carboxy group, 3 As OR 4 A polar functional group other than the group represented by R 5 As for NR 6 R 7 Polar functional groups other than those represented by the formula (I) can be used. Specific examples of the polar functional group include an amino group, a carboxy group, a carbonyl group, an alkoxy group, a hydroxyl group, a nitrile group, and a nitro group. Examples of the aliphatic hydrocarbon group having the polar functional group include a group in which one or more hydrogen atoms in the aliphatic hydrocarbon group have been substituted with a polar functional group such as those described above. Examples of the aromatic hydrocarbon group having the polar functional group include a group in which one or more hydrogen atoms in the aromatic hydrocarbon group have been substituted with a polar functional group such as those described above.
[0048] In the tackifier resin (T1), multiple R 1 may be the same or different. 1 Similarly, the multiple R 1 may be the same or different. 1 may be the same or different.
[0049] Similarly, multiple R 2 may be the same or different. 2 Similarly, the multiple R 2 may be the same or different. 2 may be the same or different.
[0050] Similarly, multiple R 3 may be the same or different. 3 Similarly, the multiple R 3 may be the same or different. 3 may be the same or different.
[0051] Similarly, multiple R 4 may be the same or different. 4 Similarly, the multiple R 4 may be the same or different. 4 may be the same or different.
[0052] Similarly, multiple R 5 may be the same or different. In addition, multiple R 5Similarly, the multiple R 5 may be the same or different. 5 may be the same or different.
[0053] Similarly, multiple R 6 and R 7 may be the same or different. In addition, multiple R 6 and R 7 Similarly, the multiple R 6 and R 7 may be the same or different. 6 and R 7 may be the same or different.
[0054] In the structural unit (A), n and l are each an integer of 2 or more and 4 or less, and n' and l' are each an integer of 2 or more and 5 or less, and are not particularly limited thereto. However, from the viewpoint of ease of obtaining raw materials, it is preferable that n, l, n', and l' are 2 or 3, and it is more preferable that n, l, n', and l' are 3, as this can further increase the adhesive strength of the first pressure-sensitive adhesive layer.
[0055] In the structural unit (A), m and k are each an integer of 1 or more and 4 or less, and m' and k' are each an integer of 1 or more and 5 or less, and are not particularly limited thereto. However, from the viewpoint of ease of obtaining raw materials, it is preferable that m, k, m', and k' are 1, 2, or 3, and it is more preferable that m, k, m', and k' are 1, as this can further increase the adhesive strength of the first pressure-sensitive adhesive layer.
[0056] More specific examples of the structural unit (A-1) and the structural unit (A-1') include a structural unit derived from dihydroxybenzene or a derivative thereof (when n and n' are 2), and a structural unit derived from trihydroxybenzene or a derivative thereof (when n and n' are 3). These structural units may be used alone, or two or more types may be used in combination. Examples of the dihydroxybenzene or a derivative thereof include resorcinol, pyrocatechol, hydroquinone, dihydroxytoluene, dihydroxyxylene, dihydroxyphenylethylamine hydrochloride, dihydroxybenzoic acid, dihydroxyphenylacetic acid, dihydroxyhydrocinnamic acid, dihydroxyphenylpropionic acid, dihydroxyphenylalanine, dihydroxybenzaldehyde, dihydroxyacetophenone, diacetyldihydroxybenzene, dihydroxyphenyl-2-butanone, dihydroxyphenylmethyl acetate, benzyl dihydroxyphenyl ketone, dihydroxybenzamide, dihydroxymethoxybenzene, dihydroxybenzyl alcohol, dihydroxyphenylethanol, dihydroxyphenyl glycol, dihydroxyphenylacetonitrile, and dihydroxynitrobenzene. Among these, pyrocatechol is preferred because it has little steric hindrance and easily interacts with the adherend. These dihydroxybenzenes or derivatives thereof may be used alone, or two or more may be used in combination. Examples of the trihydroxybenzenes or derivatives thereof include pyrogallol, 1,2,4-trihydroxybenzene, phloroglucinol, trihydroxytoluene, trihydroxydiphenylmethane, 6-hydroxy-L-dopa, gallic acid, methyl gallate, butyl gallate, isobutyl gallate, isoamyl gallate, hexadecyl gallate, stearyl gallate, trihydroxyacetophenone, trihydroxyphenylethanone, trihydroxyphenylbutanone, trihydroxybenzaldehyde, trihydroxybenzamide, and trihydroxynitrobenzene. Among these, pyrogallol is preferred because it has little steric hindrance and easily interacts with the adherend. These trihydroxybenzenes or derivatives thereof may be used alone, or two or more may be used in combination.
[0057] More specific examples of the structural unit (A-2) and the structural unit (A-2') include structural units derived from benzoic acid, salicylic acid, dihydroxybenzoic acid, gallic acid, 2-methylbenzoic acid, 3-methylbenzoic acid, 4-methylbenzoic acid, 2-ethylbenzoic acid, 3-ethylbenzoic acid, 4-ethylbenzoic acid, 4-tert-butylbenzoic acid, 2-vinylbenzoic acid, 3-vinylbenzoic acid, 4-vinylbenzoic acid, 4,4'-stilbene dicarboxylic acid, and derivatives thereof. Of these, 4-vinylbenzoic acid is preferred because it has little steric hindrance and easily interacts with the adherend. These structural units may be used alone, or two or more types may be used in combination.
[0058] More specific examples of the structural unit (A-3) and the structural unit (A-3') include a structural unit derived from a dialkoxybenzene or a derivative thereof (when l and l' are 2), and a structural unit derived from a trialkoxybenzene or a derivative thereof (when l and l' are 3). Examples of the dialkoxybenzene or a derivative thereof include 1,2-dimethoxybenzene, 1,3-dimethoxybenzene, and 1,4-dimethoxybenzene. Examples of the trialkoxybenzene or a derivative thereof include 1,2,3-trimethoxybenzene, 1,2,4-trimethoxybenzene, and 1,3,5-trimethoxybenzene. Of these, 1,2,3-trimethoxybenzene is preferred because it has little steric hindrance and easily interacts with the adherend. These trialkoxybenzenes or derivatives thereof may be used alone, or two or more types may be used in combination.
[0059] More specific examples of the structural unit (A-4) and the structural unit (A-4') include structural units derived from aminobenzene or derivatives thereof (when k and k' are 1). Examples of the aminobenzene or derivatives thereof include aniline, methylaniline, ethylaniline, dimethylaniline, and diethylaniline. These aminobenzenes or derivatives thereof may be used alone, or two or more types may be used in combination.
[0060] The structural unit (A) may consist solely of petroleum-derived materials, but preferably contains a biologically-derived material. The depletion of petroleum resources and carbon dioxide emissions from the combustion of petroleum-derived products are becoming problems. Therefore, attempts have been made to conserve petroleum resources by using biologically-derived materials instead of petroleum-derived materials. It is preferable for the structural unit (A) to contain a biologically-derived material from the perspective of conserving petroleum resources. Furthermore, if the structural unit (A) contains a biologically-derived material, since biologically-derived materials are originally produced by absorbing carbon dioxide from the atmosphere, it is thought that burning it will not increase the total amount of carbon dioxide in the atmosphere, which is also preferable from the perspective of reducing carbon dioxide emissions. Examples of monomers that constitute the structural unit (A) containing a biological material include resorcinol, dihydroxyphenylethylamine hydrochloride, dihydroxyhydrocinnamic acid, dihydroxyphenylalanine, dihydroxybenzaldehyde, dihydroxybenzyl alcohol, pyrogallol, 1,2,4-trihydroxybenzene, phloroglucinol, 6-hydroxy-L-dopa, gallic acid, methyl gallate, butyl gallate, isobutyl gallate, isoamyl gallate, hexadecyl gallate, stearyl gallate, trihydroxyacetophenone, trihydroxybenzaldehyde, trihydroxybenzamide, and trihydroxynitrobenzene.
[0061] The content (by mole) of the structural unit (A) in the tackifier resin (T1) is not particularly limited, but a preferred lower limit is 1 mol% and a preferred upper limit is 60 mol%. When the content of the structural unit (A) is 1 mol% or more, the adhesive strength of the first pressure-sensitive adhesive layer can be further increased by incorporating the tackifier resin (T1) into the first pressure-sensitive adhesive layer. When the content of the structural unit (A) is 60 mol% or less, the tackifier resin (T1) can have suitable physical properties required as a tackifier resin. A more preferred lower limit of the content of the structural unit (A) is 5 mol%, a more preferred upper limit is 50 mol%, an even more preferred lower limit is 10 mol%, and an even more preferred upper limit is 30 mol%. The content (by mass) of the structural unit (A) in the tackifier resin (T1) is not particularly limited, but a preferred lower limit is 0.9 mass% and a preferred upper limit is 60 mass%. When the content of the structural unit (A) is 0.9% by mass or more, by incorporating the tackifier resin (T1) into the first pressure-sensitive adhesive layer, the adhesive strength of the first pressure-sensitive adhesive layer can be further increased. When the content of the structural unit (A) is 60% by mass or less, the tackifier resin (T1) can have suitable physical properties required as a tackifier resin. The lower limit of the content of the structural unit (A) is more preferably 5% by mass, the upper limit is more preferably 50% by mass, the even more preferably 10% by mass, and the even more preferably 30% by mass.
[0062] The tackifier resin (T1) preferably further contains a structural unit (B) derived from at least one monomer (b) selected from the group consisting of a terpene monomer and a vinyl monomer. By including the structural unit (B), the tackifier resin (T1) can have the suitable physical properties required for a tackifier resin. Among these, a structural unit derived from a terpene monomer or a structural unit derived from a vinyl monomer is preferred because it can further enhance the adhesive strength of the first pressure-sensitive adhesive layer. It is also preferred to use a structural unit derived from a terpene monomer in combination with a structural unit derived from a vinyl monomer. Furthermore, from the viewpoint of improving the compatibility between the tackifier resin (T1) and the base polymer, a structural unit derived from a terpene monomer is preferred. Because a structural unit derived from a terpene monomer has an aliphatic hydrocarbon group having an unsaturated double bond, the inclusion of a structural unit derived from a terpene monomer in the tackifier resin (T1) improves the compatibility between the tackifier resin (T1) and the base polymer, thereby preventing a decrease in the adhesive strength of the first pressure-sensitive adhesive layer due to poor compatibility.
[0063] Examples of the terpene monomer include α-pinene, β-pinene, limonene, dipentene, δ-3-carene, dimethyloctatriene, alloocimene, myrcene, ocimene, linalool, and cosmene. Among these, α-pinene, β-pinene, or limonene is preferred because it can further enhance the adhesive strength of the first pressure-sensitive adhesive layer. The vinyl monomer is not particularly limited, but from the viewpoint of improving the compatibility between the tackifier resin (T1) and the base polymer, a vinyl monomer that does not have a structure containing two or more aromatic rings in one molecule (e.g., a naphthalene structure, an anthracene structure, a biphenyl structure, an anthraquinone structure, a benzophenone structure, etc.) is preferred. Examples of the vinyl monomer not having a structure containing two or more aromatic rings per molecule include ethylene, propylene, butylene, hexene, vinyl acetate, vinyl chloride, styrene, α-methylstyrene, coumarone, indene, vinyltoluene, divinylbenzene, divinyltoluene, and 2-phenyl-2-butene. Among these, styrene is preferred because it can further enhance the adhesive strength of the first pressure-sensitive adhesive layer. These monomers (b) may be used alone or in combination of two or more.
[0064] The structural unit (B) may consist solely of petroleum-derived materials, but preferably contains a biologically-derived material. The depletion of petroleum resources and carbon dioxide emissions from the combustion of petroleum-derived products are becoming increasingly problematic. Therefore, attempts have been made to conserve petroleum resources by using biologically-derived materials instead of petroleum-derived materials. It is preferable for the structural unit (B) to contain a biologically-derived material from the perspective of conserving petroleum resources. Furthermore, since the biologically-derived material is originally produced by absorbing carbon dioxide from the atmosphere, its combustion is thought to not increase the total amount of carbon dioxide in the atmosphere, which is also preferable from the perspective of reducing carbon dioxide emissions. Examples of the monomer (b) constituting the structural unit (B) containing a biologically-derived material include terpene monomers, ethylene, propylene, and hexene.
[0065] The content of the structural unit (B) in the tackifier resin (T1) is preferably 40 mol% or more at the lower limit and 99 mol% or more at the upper limit. When the content of the structural unit (B) is 40 mol% or more, the tackifier resin (T1) can have the suitable physical properties required for a tackifier resin. When the content of the structural unit (B) is 99 mol% or less, the content of the structural unit (A) can be sufficiently ensured, thereby further increasing the adhesive strength of the first pressure-sensitive adhesive layer, and particularly, further increasing the adhesive strength even to adherends with low polarity. The more preferred lower limit of the content of the structural unit (B) is 50 mol% and the more preferred upper limit is 90 mol%.
[0066] The tackifier resin (T1) is not particularly limited as long as it is a compound having the structural unit (A), but is preferably a copolymer having a structure represented by the following formula: When the structural unit (A) is contained in the main chain skeleton or at the end of the main chain skeleton, it is preferably a copolymer having a structure represented by the following formula: A copolymer having such a structure is a copolymer obtained by a method using cationic polymerization as described below, and can further increase the adhesive strength of the first pressure-sensitive adhesive layer, and can particularly further increase the adhesive strength even to adherends with low polarity.
[0067]
[0068] In the formula, A represents the structural unit (A), B represents the structural unit (B), and s and t each represent an integer of 1 or greater. * represents a linking moiety.
[0069] The tackifier resin (T1) is not particularly limited as long as it is a compound having the structural unit (A), but is preferably a copolymer having the structural unit (A) and the structural unit (B), and may further contain other structural units. When it is a copolymer, the structural units (A) and (B) may be copolymerized randomly, or may be copolymerized with regularity or periodicity, for example, in which each of them forms a block segment and then the block segments are bonded to each other.
[0070] The tackifier resin (T1) preferably has an aliphatic hydrocarbon group having an unsaturated double bond. The tackifier resin (T1) may have the aliphatic hydrocarbon group having an unsaturated double bond in the structural unit (A) or the structural unit (B), or in another structural unit. From the viewpoint of ease of synthesis and improving the compatibility of the tackifier resin (T1) with the base polymer, particularly the compatibility of the tackifier resin (T1) with the styrene-based elastomer, it is preferable for the aliphatic hydrocarbon group having an unsaturated double bond to be contained in the structural unit (B) or another structural unit. The structural unit (B) or other structural unit having the aliphatic hydrocarbon group having an unsaturated double bond is not particularly limited, but a structural unit (B) derived from at least one monomer (b) selected from the group consisting of terpene-based monomers and vinyl-based monomers is preferred. That is, the tackifier resin (T1) preferably has the aliphatic hydrocarbon group having an unsaturated double bond in a structural unit (B) derived from at least one monomer (b) selected from the group consisting of a terpene monomer and a vinyl monomer, and more preferably in a structural unit derived from a terpene monomer, since this can further enhance the adhesive strength of the first pressure-sensitive adhesive layer.
[0071] Furthermore, examples of the other structural units include structural units derived from other phenolic monomers not included in the structural unit (A), structural units derived from maleic anhydride, etc. Examples of the other phenolic monomers include phenol, cresol, xylenol, propylphenol, norylphenol, methoxyphenol, bromophenol, bisphenol A, bisphenol F, bisphenol S, dihydroxynaphthalene, etc. These other phenolic monomers may be used alone, or two or more types may be used in combination.
[0072] The molecular weight of the tackifier resin (T1) is not particularly limited, but the preferred lower limit of the weight average molecular weight (Mw) is 400, and the preferred upper limit is 10,000. If the weight average molecular weight (Mw) of the tackifier resin (T1) is within the above range, the tackifier resin (T1) can have suitable physical properties required as a tackifier resin. The more preferred lower limit of the weight average molecular weight (Mw) of the tackifier resin (T1) is 500, the more preferred upper limit is 5,000, the even more preferred lower limit is 550, and the even more preferred upper limit is 3,000. The weight average molecular weight (Mw) can be adjusted to fall within the above range by, for example, adjusting the composition, polymerization method, polymerization conditions, etc. of the tackifier resin (T1).
[0073] The Young's modulus of the tackifier resin (T1) at 25°C preferably has a lower limit of 10 MPa. When the Young's modulus of the tackifier resin (T1) at 25°C is 10 MPa or more, the tackifier resin (T1) has appropriate hardness and can have suitable physical properties required as a tackifier resin. The lower limit of the Young's modulus of the tackifier resin (T1) at 25°C is more preferably 50 MPa, and even more preferably 70 MPa. Furthermore, from the viewpoint of preventing the first pressure-sensitive adhesive layer from becoming too hard and reducing its adhesive strength, the upper limit of the Young's modulus of the tackifier resin (T1) at 25°C is preferably 10,000 MPa, and even more preferably 5,000 MPa. The Young's modulus of the tackifier resin (T1) at 25°C can be measured by a tensile test using a tensile tester (e.g., "Tensilon" manufactured by ORIENTEC Co., Ltd.) under conditions of a pulling speed of 200 mm / min, a gripper distance of 15 mm, and 25°C. The measurement sample in this case can be obtained, for example, by filling the tackifier resin (T1) into a mold having a size of 10 × 50 mm, melting it at a temperature 100°C higher than the glass transition temperature, and preparing a test piece having a thickness of 1 mm.
[0074] The Young's modulus at 25°C of the tackifier resin (T1) can be adjusted to fall within the above range by, for example, adjusting the molecular weight or weight average molecular weight of the tackifier resin (T1), or the composition and content of the structural unit (A) and the structural unit (B) in the tackifier resin (T1).
[0075] The glass transition temperature of the tackifier resin (T1) preferably has a lower limit of 0°C and an upper limit of 200°C. If the glass transition temperature of the tackifier resin (T1) is within the above range, the Young's modulus at 25°C of the tackifier resin (T1) can be easily adjusted to be within the above range, and the tackifier resin (T1) can have suitable physical properties required as a tackifier resin. The lower limit of the glass transition temperature of the tackifier resin (T1) is more preferably 10°C and the upper limit is more preferably 150°C.
[0076] The iodine value of the tackifier resin (T1) is preferably 2 g / 100 g at its lower limit and 180 g / 100 g at its upper limit. When the iodine value of the tackifier resin (T1) is 2 g / 100 g or more, it is possible to prevent a decrease in the adhesive strength of the first pressure-sensitive adhesive layer due to a deterioration in the compatibility between the tackifier resin (T1) and the base polymer. When the iodine value of the tackifier resin (T1) is 180 g / 100 g or less, it is possible to further increase the adhesive strength of the first pressure-sensitive adhesive layer, particularly to an adherend with low polarity. The iodine value of the tackifier resin (T1) is more preferably 70 g / 100 g at its lower limit and 170 g / 100 g at its upper limit. The iodine value is an index indicating the amount of unsaturated double bonds (C═C bond amount) and is measured in accordance with the method described in "JIS K 0070:1992."
[0077] The preferred lower limit of the content of biologically-derived carbon (carbon atoms) in the total carbon (carbon atoms) in the tackifier resin (T1) is 10%. A biologically-derived carbon content of 10% or more is an indicator of a "bio-based product." A biologically-derived carbon content of 10% or more in the tackifier resin (T1) is preferred from the perspective of saving petroleum resources and reducing carbon dioxide emissions. A more preferred lower limit of the biologically-derived carbon content in the tackifier resin (T1) is 30%, an even more preferred lower limit is 60%, an even more preferred lower limit is 70%, and an especially preferred lower limit is 90%. The upper limit of the biologically-derived carbon content in the tackifier resin (T1) is not particularly limited and may be 100%. Note that biologically-derived carbon contains a certain percentage of the radioactive isotope (C-14), whereas petroleum-derived carbon contains almost no C-14. Therefore, the biologically-derived carbon content in the tackifier resin (T1) can be calculated by measuring the concentration of C-14 contained in the compound. Specifically, it can be measured in accordance with ASTM D6866-22, a standard used in many bioplastic industries.
[0078] The tackifier resin (T1) also includes hydrogenated products of the compounds described above. The hydrogenated products are compounds in which the carbon-carbon double bonds present in the tackifier resin (T1) are at least partially saturated by hydrogenation. That is, the first PSA layer may contain a hydrogenated product in which some of the carbon-carbon double bonds in the tackifier resin (T1) are hydrogenated, or a hydrogenated product in which all of the carbon-carbon double bonds in the tackifier resin (T1) are hydrogenated. Even such hydrogenated products are suitable for use as the tackifier resin to be incorporated into the first PSA layer, and can increase the adhesive strength of the first PSA layer, particularly to adherends with low polarity.
[0079] Although there are no particular limitations on the method for producing the tackifier resin (T1), when the structural unit (A) is contained in the main chain skeleton or at the end of the main chain skeleton, the following method is preferred, for example: That is, a method of copolymerizing a monomer (a) constituting the structural unit (A) with at least one monomer (b) selected from the group consisting of terpene monomers and vinyl monomers constituting the structural unit (B) (hereinafter, also referred to as production method [I]).
[0080] The monomer (a) is preferably at least one selected from the group consisting of monomer (a-1), monomer (a-2), monomer (a-3), and monomer (a-4) represented by the following formulas:
[0081]
[0082]
[0083]
[0084]
[0085] In formulas (a-1) to (a-4), R 1 ~R 7 respectively represent a hydrogen atom, an aliphatic hydrocarbon group, an aromatic hydrocarbon group, a polar functional group, an aliphatic hydrocarbon group having a polar functional group, or an aromatic hydrocarbon group having a polar functional group. n'' represents an integer of 2 or more and 5 or less, preferably 2 or 3, and more preferably 3. m'' represents an integer of 1 or more and 5 or less. l'' represents an integer of 2 or more and 5 or less. k'' represents an integer of 1 or more and 5 or less.
[0086] In the method [I] for producing the tackifier resin (T1), it is preferable to copolymerize the monomer (a) and the monomer (b) by cationic polymerization. By using cationic polymerization, the monomer (a) and the monomer (b) can be copolymerized without first protecting the functional groups of the monomer (a), such as the phenolic hydroxyl group, carboxy group, alkoxy group, and amino group, by chemical modification, and subsequent deprotection is also unnecessary. Therefore, the monomer (a) and the monomer (b) can be copolymerized by a simpler one-step reaction process, which also leads to a reduction in impurities and an improvement in yield.
[0087] As a method for copolymerizing the monomer (a) and the monomer (b) by cationic polymerization, a method in which the monomer (a) and the monomer (b) are reacted in the presence of a Lewis acid is preferred. According to such a method, it is believed that a cation of the monomer (b) is generated, and the cationic polymerization of the monomers (b) proceeds, while the Friedel-Crafts alkylation reaction between the monomers (a) and (b) proceeds. By repeating such a reaction, a copolymer having a structural unit (A) derived from the monomer (a) and a structural unit (B) derived from the monomer (b) can be obtained. The Lewis acid is not particularly limited, and a conventionally known Lewis acid can be used, for example, aluminum chloride (AlCl 3 ), diethylaluminum chloride (Et 2 AlCl 2 ), tin(IV) chloride (SnCl 4 ), titanium(IV) chloride (TiCl 4 ), boron trichloride (BCl 3 ), boron trifluoride ether complex (BF 3 Among them, aluminum chloride (AlCl ) is preferred because it can produce a copolymer in a higher yield. 3 ) is preferred.
[0088] More specifically, for example, pyrogallol is used as the monomer (a) and α-pinene is used as the monomer (b), and these are reacted with aluminum chloride (AlCl), which is a Lewis acid, to form a copolymer. 3When the reaction is carried out in the presence of a monomer (b), the reaction shown in the following scheme is believed to proceed. That is, a cation of α-pinene, the monomer (b), is generated, and cationic polymerization of α-pinenes proceeds (upper part of the scheme below), while a Friedel-Crafts alkylation reaction between pyrogallol, the monomer (a), and α-pinene, the monomer (b), proceeds (middle part of the scheme below). By repeating this reaction, a copolymer having structural units derived from pyrogallol and structural units derived from α-pinene can be obtained (lower part of the scheme below). Note that such a copolymer has structural units derived from pyrogallol in the main chain skeleton or at the terminal of the main chain skeleton.
[0089]
[0090] In the formula, s and t each represent an integer of 1 or more, and * represents a linking moiety.
[0091] When the structural unit (A) is contained in a side chain, the following method is preferred as a method for producing the tackifier resin (T1): That is, a method of copolymerizing a monomer (a') obtained by further introducing an unsaturated double bond into the monomer (a) constituting the structural unit (A) with at least one monomer (b) selected from the group consisting of terpene monomers and vinyl monomers constituting the structural unit (B) (hereinafter, also referred to as production method [II]).
[0092] Examples of the monomer (a') include 2-vinylbenzoic acid, 3-vinylbenzoic acid, 4-vinylbenzoic acid, and 4,4'-stilbene dicarboxylic acid. Among these, 4-vinylbenzoic acid is preferred because it has little steric hindrance and easily interacts with the adherend. These monomers (a') may be used alone or in combination of two or more.
[0093] In the method [II] for producing the tackifier resin (T1), it is preferable to copolymerize the monomer (a') and the monomer (b) by cationic polymerization, as in the method [I] for producing the tackifier resin (T1). A preferred method for copolymerizing the monomer (a') and the monomer (b) by cationic polymerization is to react the monomer (a') and the monomer (b) in the presence of a Lewis acid as described above. According to this method, cationic polymerization of the unsaturated double bond in the monomer (a') and the unsaturated double bond in the monomer (b) proceeds, thereby producing a copolymer having the structural unit (A) derived from the monomer (a') and the structural unit (B) derived from the monomer (b).
[0094] The tackifier resin (T1) can enhance the adhesive strength of the first pressure-sensitive adhesive layer even in a smaller amount than conventional tackifier resins. The content of the tackifier resin (T1) relative to 100 parts by mass of the base polymer (P1) preferably has a lower limit of 5 parts by mass and an upper limit of 50 parts by mass. When the content of the tackifier resin (T1) is 5 parts by mass or more, the adhesive strength of the first pressure-sensitive adhesive layer can be further enhanced, particularly with respect to adherends with low polarity (e.g., fluororesins, etc.). When the content of the tackifier resin (T1) is 50 parts by mass or less, the first pressure-sensitive adhesive layer can be prevented from becoming too hard and losing its adhesive strength. A more preferred lower limit of the content of the tackifier resin (T1) is 10 parts by mass, and a more preferred upper limit is 35 parts by mass.
[0095] The tackifier resin preferably contains at least one tackifier resin (T2) selected from the group consisting of rosin ester resins, terpene resins, terpene phenol resins, and petroleum-based resins. When the tackifier resin contains the tackifier resin (T2), the adhesive strength of the resulting pressure-sensitive adhesive tape can be further enhanced.
[0096] The rosin ester resin is a resin obtained by esterifying, with an alcohol, a rosin resin primarily composed of abietic acid, a disproportionated rosin resin, a hydrogenated rosin resin, a dimer (polymerized rosin resin) of a resin acid such as abietic acid, or the like. The hydroxyl value is adjusted to the above-mentioned range by retaining some of the hydroxyl groups of the alcohol used in the esterification without being used in the esterification and remaining in the resin. Examples of the alcohol include polyhydric alcohols such as ethylene glycol, glycerin, and pentaerythritol. Examples of the rosin ester resin include Pine Crystal KE-359, Ester Gum AA-V, and Ester Gum H (all manufactured by Arakawa Chemical Industries, Ltd.).
[0097] The terpene resin is a resin having a structural unit derived from a monoterpene compound and not having a structural unit derived from an aromatic compound. Examples of the terpene resin include YS Resin PX1250 (manufactured by Yasuhara Chemical Co., Ltd.).
[0098] The terpene phenolic resin is a resin having structural units derived from a monoterpene compound and structural units derived from a phenolic compound. In this specification, the term "phenolic compound" in the terpene phenolic resin refers to a compound that contains an aromatic ring structure having only one phenolic hydroxyl group and does not contain an aromatic ring structure having two or more phenolic hydroxyl groups. The structural units derived from the phenolic compound in the terpene phenolic resin do not include the structural units (A-1) and (A-1'). Examples of the terpene phenolic resin include YS Polystar G150 (manufactured by Yasuhara Chemical Co., Ltd.).
[0099] Examples of the petroleum-based resin include Alcon P-140 (manufactured by Arakawa Chemical Industries, Ltd.).
[0100] The softening temperature of the tackifier resin (T2) preferably has a lower limit of 50°C and an upper limit of 200°C. When the softening temperature of the tackifier resin (T2) is 50°C or higher, it is possible to prevent the first pressure-sensitive adhesive layer from becoming too soft and losing its adhesive strength. When the softening temperature of the tackifier resin (T2) is 200°C or lower, it is possible to improve the wettability of the interface of the first pressure-sensitive adhesive layer and prevent interfacial peeling. Furthermore, the glass transition temperature (Tg) of the (meth)acrylic copolymer is further reduced. As a result, the shear storage modulus at 25°C of the first pressure-sensitive adhesive layer (described below) is appropriately reduced, and the flexibility of the first pressure-sensitive adhesive layer is further improved. This improves the adhesive strength of the first pressure-sensitive adhesive layer to the fluororesin and the adhesion to the substrate. The softening temperature of the tackifier resin (T2) is more preferably 60°C, more preferably 150°C, even more preferably 70°C, and even more preferably 90°C. The softening temperature is measured in accordance with JIS K2207 (ring and ball method).
[0101] The tackifier resin (T2) preferably has a lower limit of 0 mgKOH / g and an upper limit of 200 mgKOH / g for the hydroxyl value. When the tackifier resin (T2) has a hydroxyl value within the above range, the wettability of the interface of the first pressure-sensitive adhesive layer is improved, and interfacial peeling can be suppressed. The hydroxyl value of the tackifier resin (T2) is more preferably 30 mgKOH / g for the lower limit and 130 mgKOH / g for the upper limit. The hydroxyl value can be measured according to JIS K1557 (phthalic anhydride method).
[0102] The content of the tackifier resin (T2) relative to 100 parts by mass of the base polymer (P1) is preferably 10 parts by mass or more at a lower limit and 200 parts by mass or more at a higher limit. When the content of the tackifier resin (T2) is 10 parts by mass or more, the adhesive strength of the first pressure-sensitive adhesive layer can be further increased. When the content of the tackifier resin (T2) is 200 parts by mass or less, the first pressure-sensitive adhesive layer can be prevented from becoming too hard and losing its adhesive strength. The lower limit of the content of the tackifier resin (T2) is more preferably 15 parts by mass, and more preferably 160 parts by mass or more at a higher limit, and even more preferably 50 parts by mass or more at a higher limit, and even more preferably 140 parts by mass or more at a higher limit.
[0103] From the viewpoint of further reducing contamination of the substrate of the pressure-sensitive adhesive tape, the first pressure-sensitive adhesive layer preferably does not contain an organosilicon compound, or the content of the organosilicon compound in the first pressure-sensitive adhesive layer is preferably 3.0 mass% or less. When the first pressure-sensitive adhesive layer contains the organosilicon compound, the upper limit of the content is more preferably 1.0 mass%. It is particularly preferred that the first pressure-sensitive adhesive layer does not contain the organosilicon compound.
[0104] In this specification, the organosilicon compound is not particularly limited as long as it is an organic compound containing a silicon atom, and examples thereof include commercially available silicone adhesives, silane coupling agents, silicone oils, etc.
[0105] When the base polymer (P1) contains a (meth)acrylic copolymer, the first pressure-sensitive adhesive layer preferably further contains a curing agent. By containing a curing agent in the first pressure-sensitive adhesive, the (meth)acrylic copolymer can form a structure crosslinked by chemical crosslinking, thereby further improving the bulk cohesive strength of the first pressure-sensitive adhesive layer and increasing the gel fraction of the first pressure-sensitive adhesive layer, as described below, thereby further improving the adhesive strength and holding performance of the resulting pressure-sensitive adhesive tape.
[0106] Examples of the curing agent include an isocyanate-based curing agent, an aziridine-based curing agent, an epoxy-based curing agent, a metal chelate-based curing agent, etc. Among these, it is preferable that the first pressure-sensitive adhesive layer contains an isocyanate-based curing agent, from the viewpoint of enabling appropriate chemical crosslinking of the (meth)acrylic copolymer and further improving the adhesive strength and holding performance of the resulting pressure-sensitive adhesive tape.
[0107] Examples of the isocyanate curing agent include Coronate L-45 (manufactured by Tosoh Corporation), Takenate 500 (manufactured by Mitsui Chemicals, Inc.), and Desmodur L-75 (manufactured by Covestro).
[0108] The content of the curing agent relative to 100 parts by mass of the (meth)acrylic copolymer is preferably 0.01 parts by mass at the lower limit and 10 parts by mass at the upper limit. By ensuring that the content of the curing agent is within the above range, appropriate chemical crosslinking of the (meth)acrylic copolymer is possible, thereby further improving the adhesive strength and holding performance of the resulting pressure-sensitive adhesive tape. The lower limit of the content of the curing agent is more preferably 0.1 parts by mass, more preferably 5.0 parts by mass at the upper limit, even more preferably 0.5 parts by mass at the lower limit, and even more preferably 2.0 parts by mass at the upper limit.
[0109] The first pressure-sensitive adhesive layer may further contain a colorant for the purpose of imparting light-blocking properties. Examples of the colorant include carbon black, aniline black, titanium oxide, etc. Among these, carbon black is preferred because it is relatively inexpensive and chemically stable.
[0110] The first pressure-sensitive adhesive layer may contain conventionally known fine particles and additives, such as inorganic fine particles, conductive fine particles, antioxidants, foaming agents, organic fillers, and inorganic fillers, as needed.
[0111] The first pressure-sensitive adhesive layer has a 180° peel strength from the substrate at 23°C of preferably 2.5 N / 25 mm or more. When the 180° peel strength from the substrate at 23°C of the first pressure-sensitive adhesive layer is 2.5 N / 25 mm or more, the adhesion of the first pressure-sensitive adhesive layer to the substrate is further improved. The lower limit of the 180° peel strength from the substrate at 23°C of the first pressure-sensitive adhesive layer is more preferably 3.0 N / 25 mm, and even more preferably 3.5 N / 25 mm. There is no particular upper limit of the 180° peel strength from the substrate at 23°C of the first pressure-sensitive adhesive layer, but a substantial upper limit is about 100 N / 25 mm. The 180° peel strength from the substrate at 23°C of the first pressure-sensitive adhesive layer can be measured by the following method. That is, the adhesive tape is cut into a size of 25 mm wide x 100 mm long, and then pressed onto a 23 μm thick PET film using a 2 kg rubber roller, with a reciprocating motion at a speed of 300 mm / min. The tape is then left to stand for 20 minutes in an environment of 23°C and 50% RH to age, thereby preparing a test sample. The obtained test sample is subjected to a 180° peel test in accordance with JIS Z0237 using a tensile tester (such as ORIENTEC's "Tensilon") at 23°C, 50% RH, and a peel speed of 300 mm / min, to peel the first adhesive layer from the substrate, thereby measuring the 180° peel strength of the first adhesive layer against the substrate at 23°C.
[0112] The first pressure-sensitive adhesive layer preferably has a loss tangent (tan δ) measured at a frequency of 10 Hz in dynamic viscoelasticity measurement (hereinafter sometimes referred to as "the loss tangent of the first pressure-sensitive adhesive layer measured at a frequency of 10 Hz") that has a peak in the temperature range of -30°C or higher and 15°C or lower. When the loss tangent (tan δ) of the first pressure-sensitive adhesive layer measured at a frequency of 10 Hz has a peak in the temperature range of -30°C or higher, the adhesion of the first pressure-sensitive adhesive layer to the substrate is further improved. Furthermore, when the loss tangent (tan δ) of the first pressure-sensitive adhesive layer measured at a frequency of 10 Hz has a peak in the temperature range of 15°C or lower, the zipping phenomenon that occurs when peeling off a film that protects the pressure-sensitive adhesive layer of the pressure-sensitive adhesive tape can be suppressed, and the resulting pressure-sensitive adhesive tape can be used without losing its adhesive strength. The peak temperature at which the loss tangent of the first pressure-sensitive adhesive layer measured at a frequency of 10 Hz reaches its peak (hereinafter, may be simply referred to as the "peak temperature of the loss tangent") is more preferably -25°C in lower limit, more preferably 13°C in upper limit, even more preferably -20°C in lower limit, and even more preferably 11°C in upper limit.
[0113] The first pressure-sensitive adhesive layer has a shear storage modulus at 25°C measured at a frequency of 10 Hz in dynamic viscoelasticity measurement of 1.0 × 10 4 Pa, and the preferred upper limit is 5.0 × 10 5 Pa. When the shear storage modulus at 25°C of the first pressure-sensitive adhesive layer is within the above range, the resulting pressure-sensitive adhesive tape has superior adhesive strength and holding performance. In addition, the flexibility of the first pressure-sensitive adhesive layer is excellent, and the adhesive strength of the first pressure-sensitive adhesive layer to the fluororesin is improved, and the adhesion to the substrate is further improved. A more preferred lower limit of the shear storage modulus at 25°C of the first pressure-sensitive adhesive layer is 3.0 x 10 4 Pa, and a more preferable upper limit is 4.0 × 10 5 Pa, and a more preferable lower limit is 5.0 × 10 4 Pa, and a more preferable upper limit is 3.5×10 5 It is Pa.
[0114] The peak temperature of the loss tangent of the first pressure-sensitive adhesive layer measured at a frequency of 10 Hz and the shear storage modulus of the first pressure-sensitive adhesive layer at 25°C can be measured by dynamic viscoelasticity measurement. Specifically, a measurement sample consisting of only the pressure-sensitive adhesive layer is prepared by laminating a pressure-sensitive adhesive layer to a thickness of approximately 1 mm, and the dynamic viscoelasticity spectrum of the obtained measurement sample is measured from -50°C to 200°C using a dynamic viscoelasticity measurement device such as a viscoelasticity spectrometer (e.g., "DVA-200" manufactured by IT Measurement & Control Co., Ltd.) under conditions of shear mode, a heating rate of 5°C / min, and a measurement frequency of 10 Hz, thereby measuring the shear storage modulus of the first pressure-sensitive adhesive layer. Furthermore, the peak temperature of the loss tangent of the first pressure-sensitive adhesive layer can be obtained from the dynamic viscoelasticity spectrum obtained.
[0115] The peak temperature of the loss tangent (tan δ) of the first pressure-sensitive adhesive layer measured at a frequency of 10 Hz and the shear storage modulus at 25°C of the first pressure-sensitive adhesive layer can be adjusted by the types and content ratios of the monomers constituting the (meth)acrylic copolymer, the weight-average molecular weight of the (meth)acrylic copolymer, the presence or absence of the tackifier resin (T2), the types and contents of the tackifier resin (T1) and the tackifier resin (T2), the gel fraction of the first pressure-sensitive adhesive layer described below, and the like.
[0116] The preferred lower limit of the gel fraction of the first pressure-sensitive adhesive layer is 15% by mass, and the preferred upper limit is 70% by mass. A gel fraction of the first pressure-sensitive adhesive layer of 15% by mass or more increases the bulk strength of the first pressure-sensitive adhesive layer, further improving the holding performance of the resulting pressure-sensitive adhesive tape. A gel fraction of the first pressure-sensitive adhesive layer of 70% by mass or less appropriately reduces the shear storage modulus at 25°C of the first pressure-sensitive adhesive layer, thereby further improving the flexibility of the first pressure-sensitive adhesive layer, thereby improving the adhesive strength of the first pressure-sensitive adhesive layer to fluororesins and the adhesion to the substrate. A more preferred lower limit of the gel fraction of the first pressure-sensitive adhesive layer is 20% by mass, a more preferred upper limit is 65% by mass, an even more preferred lower limit is 25% by mass, and an even more preferred upper limit is 60% by mass. The gel fraction of the first pressure-sensitive adhesive layer can be measured by the following method, etc. A test piece is prepared by cutting the pressure-sensitive adhesive tape into a flat rectangular shape measuring 50 mm wide x 100 mm long. The test piece is immersed in an organic solvent at 23°C for 24 hours, then removed from the organic solvent and dried at 110°C for 1 hour. As the organic solvent, for example, ethyl acetate or the like can be used when the base polymer (P1) is a (meth)acrylic copolymer, and toluene or the like can be used when the base polymer (P1) is a styrene-based elastomer. The mass of the test piece after drying is measured, and the gel fraction is calculated using the following formula (1). Note that no release film for protecting the pressure-sensitive adhesive layer is laminated on the test piece. Gel fraction (mass%) = 100 × (W 2 -W 0 ) / (W 1 -W 0 ) (1) (W 0 : Mass of the substrate, W 1 : mass of test piece before immersion, W 2 : Mass of test piece after immersion and drying)
[0117] The gel fraction of the first pressure-sensitive adhesive layer can be adjusted to within the above range by, for example, adjusting the type and content ratio of the monomers constituting the (meth)acrylic copolymer, the weight average molecular weight of the (meth)acrylic copolymer, the type and content of the curing agent, etc.
[0118] The thickness of the first pressure-sensitive adhesive layer is preferably 20 μm at the lower limit and 500 μm at the upper limit. If the thickness of the first pressure-sensitive adhesive layer is within this range, the first pressure-sensitive adhesive layer can have sufficient adhesive strength. The thickness of the first pressure-sensitive adhesive layer is more preferably 25 μm at the lower limit, more preferably 300 μm at the upper limit, even more preferably 100 μm at the upper limit, and even more preferably 80 μm at the upper limit.
[0119] The pressure-sensitive adhesive tape of the present invention may have layers other than the first pressure-sensitive adhesive layer and the substrate, if necessary.
[0120] From the viewpoint of reworkability, the pressure-sensitive adhesive tape of the present invention preferably has an intermediate layer and a second pressure-sensitive adhesive layer in this order on the surface of the first pressure-sensitive adhesive layer opposite to the surface adjacent to the substrate. That is, the pressure-sensitive adhesive tape of the present invention preferably has the substrate, the first pressure-sensitive adhesive layer, an intermediate layer, and a second pressure-sensitive adhesive layer in this order.
[0121]
[0003] Generally, when a pressure-sensitive adhesive tape is adhered to an adherend made of metal or a highly polar resin (e.g., polyester, polyimide, etc.), the adhesive strength between the pressure-sensitive adhesive layer and the adherend tends to be higher than the adhesive strength between the pressure-sensitive adhesive layer and a substrate containing a fluororesin, such as the substrate described above, and the substrate. Therefore, when an attempt is made to re-peel the pressure-sensitive adhesive tape, the pressure-sensitive adhesive tape may break between the substrate containing a fluororesin and the pressure-sensitive adhesive layer. By having an intermediate layer in the pressure-sensitive adhesive tape of the present invention, it is possible to further suppress breakage between the substrate and the first pressure-sensitive adhesive layer, thereby facilitating re-peelability of the pressure-sensitive adhesive tape and improving reworkability. Furthermore, by having the second pressure-sensitive adhesive layer on the outermost surface of the pressure-sensitive adhesive tape, the pressure-sensitive adhesive tape can be made to adhere to a variety of adherends by reducing the adherend selectivity of the pressure-sensitive adhesive tape.
[0122] The second pressure-sensitive adhesive layer may have a single-layer structure or a multi-layer structure, but is preferably a single-layer structure from the viewpoint of preventing interlayer damage between the pressure-sensitive adhesive layers.
[0123] The second pressure-sensitive adhesive layer preferably contains a base polymer (P2). The base polymer (P2) preferably contains at least one selected from the group consisting of a (meth)acrylic copolymer and a styrene-based elastomer.
[0124] The styrene-based elastomer in the base polymer (P2) may be the same as the styrene-based elastomer in the base polymer (P1).
[0125] The (meth)acrylic copolymer in the base polymer (P2) may be the same as the (meth)acrylic copolymer in the base polymer (P1) described above.
[0126] From the viewpoint of further reducing contamination of the substrate of the pressure-sensitive adhesive tape, the second pressure-sensitive adhesive layer preferably does not contain an organosilicon compound, or the content of the organosilicon compound in the second pressure-sensitive adhesive layer is preferably 3.0 mass% or less. When the second pressure-sensitive adhesive layer contains an organosilicon compound, the upper limit of the content is more preferably 1.0 mass%. It is particularly preferred that the second pressure-sensitive adhesive layer does not contain an organosilicon compound.
[0127] From the viewpoint of further improving adhesive strength, the second pressure-sensitive adhesive layer preferably further contains a tackifier resin (T3). Examples of the tackifier resin (T3) include those similar to the tackifier resin (T2) described above.
[0128] When the base polymer (P2) contains the (meth)acrylic copolymer, the second pressure-sensitive adhesive layer preferably further contains a curing agent, which allows the (meth)acrylic copolymer to form a chemically crosslinked structure, thereby further improving the adhesive strength and holding performance of the resulting pressure-sensitive adhesive tape.
[0129] The curing agent contained in the second pressure-sensitive adhesive layer may be, for example, the same as the curing agent contained in the first pressure-sensitive adhesive layer.
[0130] The second pressure-sensitive adhesive layer preferably has a probe tack value of 20 N / 5 mmφ (hereinafter sometimes simply referred to as the "probe tack value of the second pressure-sensitive adhesive layer at 23°C") measured under conditions of 23°C, a pressure of 98 gf, a pressure-applying speed of 100 mm / sec, a pressure-applying time of 10 seconds, and a peeling speed of 5 mm / sec. Having a probe tack value of 20 N / 5 mmφ or less at 23°C for the second pressure-sensitive adhesive layer reduces stickiness of the second pressure-sensitive adhesive layer, resulting in superior lamination workability for the pressure-sensitive adhesive tape of the present invention. A more preferred upper limit for the probe tack value of the second pressure-sensitive adhesive layer at 23°C is 15 N / 5 mmφ, and an even more preferred upper limit is 10 N / 5 mmφ. A preferred lower limit for the probe tack value of the second pressure-sensitive adhesive layer at 23°C is 0.01 N / 5 mmφ. When the probe tack value of the second pressure-sensitive adhesive layer at 23°C is 0.01 N / 5 mmφ or more, the second pressure-sensitive adhesive layer has appropriate adhesive strength, and from the viewpoint of making it easier to adjust the attachment position of the pressure-sensitive adhesive tape of the present invention, the lamination workability is improved. A more preferred lower limit of the probe tack value of the second pressure-sensitive adhesive layer at 23°C is 0.1 N / 5 mmφ, and an even more preferred lower limit of the probe tack value of the second pressure-sensitive adhesive layer at 23°C is 1.0 N / 5 mmφ. The probe tack value of the second pressure-sensitive adhesive layer at 23°C can be measured by a probe tack test in accordance with JIS Z3284. Specifically, for example, the pressure-sensitive adhesive tape of the present invention is cut into a size of 30 mm wide x 30 mm long to prepare a test piece, and the second pressure-sensitive adhesive layer of the prepared test piece is subjected to a probe tack test using a probe tack tester (such as "TAC-2" manufactured by RHESCA) under conditions of 23°C, a pressure of 98 gf, a pressure rate of 100 mm / sec, a pressure time of 10 seconds, and a peel rate of 5 mm / sec, thereby enabling measurement.
[0131] Methods for adjusting the probe tack value at 23°C of the second pressure-sensitive adhesive layer include changing the composition, weight average molecular weight, or molecular weight distribution of the base polymer (P2), changing the type and content ratio of the tackifier resin (T3), changing the type and content of the fine particles and additives to be blended, changing the thickness of the second pressure-sensitive adhesive layer, changing the storage modulus or glass transition temperature, changing the crosslinking density, or changing the surface roughness.
[0132] The second pressure-sensitive adhesive layer preferably has an upper limit of 8.0 N / 25 mm in 180° peel strength from SUS at 23°C. When the second pressure-sensitive adhesive layer has a 180° peel strength from SUS at 23°C of 8.0 N / 25 mm or less, the reworkability of the resulting pressure-sensitive adhesive tape is further improved. The upper limit of the 180° peel strength from SUS at 23°C of the second pressure-sensitive adhesive layer is more preferably 7.0 N / 25 mm, and even more preferably 5.0 N / 25 mm. Furthermore, the lower limit of the 180° peel strength from SUS at 23°C of the second pressure-sensitive adhesive layer is preferably 2.0 N / 25 mm. When the second pressure-sensitive adhesive layer has a 180° peel strength from SUS at 23°C of 2.0 N / 25 mm or more, the adhesive strength of the resulting pressure-sensitive adhesive tape is further improved. A more preferred lower limit of the 180° peel strength of the second pressure-sensitive adhesive layer from SUS at 23° C. is 2.5 N / 25 mm, and an even more preferred lower limit is 3.0 N / 25 mm. The 180° peel strength of the second pressure-sensitive adhesive layer from SUS at 23° C. can be measured by the following method, etc. That is, the pressure-sensitive adhesive tape is cut to a size of 25 mm wide x 100 mm long, and then pressed against a SUS plate (a SUS304 plate that has been washed with ethanol and then wiped dry) using a 2 kg rubber roller, which is rolled back and forth once at a speed of 300 mm / min, and then left to stand for 20 minutes in an environment of 23° C. and 50% RH to cure, thereby preparing a test sample. The obtained test sample is subjected to a 180° peel test in accordance with JIS Z0237 using a tensile tester (such as "Tensilon" manufactured by ORIENTEC Co., Ltd.) under conditions of 23°C, 50% RH and a peel rate of 300 mm / min, and the 180° peel strength of the second pressure-sensitive adhesive layer against SUS at 23°C can be measured by peeling the pressure-sensitive adhesive tape from the SUS plate, etc.
[0133] The thickness of the second pressure-sensitive adhesive layer is preferably 20 μm at the lower limit and 500 μm at the upper limit. By having the thickness of the second pressure-sensitive adhesive layer within this range, the second pressure-sensitive adhesive layer can have sufficient adhesive strength. The thickness of the second pressure-sensitive adhesive layer is more preferably 25 μm at the lower limit, more preferably 300 μm at the upper limit, even more preferably 100 μm at the upper limit, and even more preferably 80 μm at the upper limit.
[0134] From the viewpoint of having high adhesiveness to the first and second pressure-sensitive adhesive layers, the intermediate layer preferably contains at least one selected from the group consisting of polyester resin, polyimide resin, polyolefin resin, polyurethane resin, glass fiber, carbon fiber, and metal, and more preferably contains at least one selected from the group consisting of polyester resin and polyolefin resin from the viewpoint of having higher adhesiveness.
[0135] Examples of the polyester resin include polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), polybutylene terephthalate (PBT), polyethylene furanoate (PEF), polylactic acid (PLA), and polybutylene succinate (PBS). Examples of the polyimide resin include Kapton (manufactured by DuPont) and Upilex (manufactured by UBE). Examples of the polyolefin resin include polyethylene (PE), polypropylene (PP), and ethylene-vinyl acetate copolymer (EVA). The polyurethane resin is a resin composition composed of a polyisocyanate and a polyol. Examples of the polyisocyanate include 4,4'-diphenylmethane diisocyanate (MDI), and examples of the polyol include polypropylene glycol (PPG). Examples of the metal include SUS, copper, and aluminum.
[0136] Examples of the shape of the intermediate layer include a film, a nonwoven fabric, and a woven fabric. Among these, at least one selected from the group consisting of a nonwoven fabric and a woven fabric is preferred, from the viewpoint of providing high adhesion between the intermediate layer and the first and second pressure-sensitive adhesive layers. An example of the nonwoven fabric substrate is G2260-1S (manufactured by Toray International Co., Ltd.). Examples of the woven fabric substrate are glass cloth and carbon cloth. Specific examples of the glass cloth include KS2770 (manufactured by Nitto Boseki Co., Ltd.), and specific examples of the carbon cloth include C-540 (manufactured by Hagiwara Kogyo Co., Ltd.).
[0137] The intermediate layer may have a foamed structure. When the intermediate layer has a foamed structure, the flexibility of the intermediate layer is further improved, and the holding performance and reworkability of the obtained pressure-sensitive adhesive tape are further improved. Examples of the intermediate layer having a foamed structure include a foam of the polyolefin resin and a foam of the polyurethane resin.
[0138] The thickness of the intermediate layer is preferably 4 μm at the lower limit and 500 μm at the upper limit. When the thickness of the intermediate layer is within the above range, the reworkability of the resulting pressure-sensitive adhesive tape is further improved. The thickness of the intermediate layer is more preferably 12 μm at the lower limit and 300 μm at the upper limit, even more preferably 23 μm at the lower limit and 200 μm at the upper limit.
[0139] From the viewpoint of ease of lamination, the pressure-sensitive adhesive tape of the present invention preferably comprises the substrate, the first pressure-sensitive adhesive layer, and a hot-melt pressure-sensitive adhesive layer in this order. In this specification, the term "hot-melt pressure-sensitive adhesive layer" refers to a pressure-sensitive adhesive layer that is melted by heating and adhered to an adherend.
[0140]
[0006] Conventionally, if an adhesive used to attach a fluororesin has too strong an adhesive strength to the adherend at room temperature, it can become sticky, resulting in poor workability, and it can be difficult to adjust the position where the fluororesin is attached to the adherend. Therefore, an adhesive that is less sticky and has excellent workability in attachment, making it easy to adjust the position where the fluororesin is attached to the adherend, is desirable. By having a hot-melt adhesive layer on the outermost surface of the adhesive tape of the present invention, the stickiness of the adhesive tape of the present invention at room temperature can be further suppressed, resulting in excellent workability in attachment.
[0141] The hot melt pressure-sensitive adhesive layer may have a single layer structure or a multilayer structure, but is preferably a single layer structure from the viewpoint of preventing interlayer damage between the pressure-sensitive adhesive layers.
[0142] The hot-melt pressure-sensitive adhesive layer has a 180° peel strength from SUS at 23°C when pressure-bonded at 0.1 MPa for 10 minutes in a 150°C environment (hereinafter sometimes simply referred to as "the 180° peel strength from SUS at 23°C after heating of the hot-melt pressure-sensitive adhesive layer") of preferably 5.0 N / 25 mm at its lower limit. When the hot-melt pressure-sensitive adhesive layer has a 180° peel strength from SUS at 23°C after heating of 5.0 N / 25 mm or more, excellent adhesive strength can be exerted upon heating, and the pressure-sensitive adhesive tape of the present invention can achieve both excellent lamination workability and excellent adhesive strength. The preferred lower limit of the 180° peel strength from SUS at 23°C after heating of the hot-melt pressure-sensitive adhesive layer is 7.0 N / 25 mm, and more preferably 10.0 N / 25 mm. There is no particular upper limit to the 180° peel strength of the hot-melt pressure-sensitive adhesive layer from SUS at 23° C. after heating, but a substantial upper limit is 500 N / 25 mm. The 180° peel strength of the hot-melt pressure-sensitive adhesive layer from SUS at 23° C. after heating can be measured by the following method, etc. That is, after cutting the pressure-sensitive adhesive tape to a size of 25 mm wide x 100 mm long, the first pressure-sensitive adhesive layer is backed with a 23 μm thick PET film (e.g., "FE2002" manufactured by Futamura Chemical Co., Ltd.), and the hot-melt pressure-sensitive adhesive layer is pressure-bonded to a SUS plate (a SUS304 plate washed with ethanol and then wiped dry) by applying pressure at 0.1 MPa for 10 minutes in an environment of 150° C., and then the hot-melt pressure-sensitive adhesive layer is air-cooled to prepare a test sample. The obtained test sample is subjected to a 180° peel test in accordance with JIS Z0237 using a tensile tester (such as "Tensilon" manufactured by ORIENTEC Co., Ltd.) under conditions of 23°C, 50% RH and a peel rate of 300 mm / min, and the adhesive tape is peeled from the SUS plate, whereby the 180° peel strength of the hot-melt adhesive layer against SUS at 23°C can be measured.
[0143] Examples of methods for adjusting the 180° peel strength from SUS at 23°C after heating of the hot-melt pressure-sensitive adhesive layer include a method of changing the composition of the base polymer (P3) described below and a method of changing the thickness of the hot-melt pressure-sensitive adhesive layer.
[0144] The hot-melt pressure-sensitive adhesive layer preferably has an upper limit of 15 N / 25 mm in 180° peel strength from SUS at 23°C. When the hot-melt pressure-sensitive adhesive layer has a 180° peel strength from SUS at 23°C of 15 N / 25 mm or less, the application workability of the resulting pressure-sensitive adhesive tape is further improved. The upper limit of the 180° peel strength from SUS at 23°C of the hot-melt pressure-sensitive adhesive layer is more preferably 12 N / 25 mm, and even more preferably 10 N / 25 mm. Specifically, the pressure-sensitive adhesive tape is cut to a size of 25 mm wide x 100 mm long, and then pressed against a SUS plate (a SUS304 plate that has been washed with ethanol and then wiped dry) using a 2 kg rubber roller, with one reciprocating motion at a speed of 300 mm / min. The cut tape is then left to stand for 20 minutes in an environment of 23°C and 50% RH to age, thereby preparing a test sample. The obtained test sample is subjected to a 180° peel test in accordance with JIS Z0237 using a tensile tester (such as "Tensilon" manufactured by ORIENTEC Co., Ltd.) under conditions of 23°C, 50% RH and a peel rate of 300 mm / min, and the adhesive tape is peeled from the SUS plate, etc., whereby the 180° peel strength of the hot-melt adhesive layer against SUS at 23°C can be measured.
[0145] Examples of methods for adjusting the 180° peel strength of the hot-melt pressure-sensitive adhesive layer from SUS at 23°C include changing the composition of the base polymer (P3) and changing the thickness of the hot-melt pressure-sensitive adhesive layer.
[0146] The hot melt pressure-sensitive adhesive layer preferably contains a base polymer (P3). The base polymer (P3) preferably contains at least one selected from the group consisting of a (meth)acrylic copolymer, a styrene-based elastomer, an ethylene-vinyl acetate copolymer, a chloroprene rubber, a nitrile rubber, a polyurethane resin, a polyamide resin, a polyolefin resin, a polyester resin, and an epoxy resin. Among these, from the viewpoints of tack control and heat resistance, a (meth)acrylic copolymer, a styrene-based elastomer, a chloroprene rubber, a nitrile rubber, a polyurethane resin, a polyamide resin, a polyolefin resin, and a polyester resin are preferred.
[0147] The (meth)acrylic copolymer and styrene-based elastomer in the base polymer (P3) may be the same as those in the base polymers (P1) and (P2). Specific examples of the (meth)acrylic copolymer in the base polymer (P3) include SK Dyne 1717DT (manufactured by Soken Chemical & Engineering Co., Ltd.).
[0148] Examples of the ethylene-vinyl acetate copolymer include HM200 (manufactured by Cemedine Co., Ltd.). Examples of the chloroprene rubber include 575F (manufactured by Cemedine Co., Ltd.) and G17 (manufactured by Konishi Co., Ltd.). Examples of the nitrile rubber include 501F (manufactured by Cemedine Co., Ltd.). Examples of the polyurethane resin include SHM107-PUR (manufactured by Seedum Co., Ltd.). Examples of the polyamide resin include SHM301-PAD (manufactured by Seedum Co., Ltd.). Examples of the polyolefin resin include PPET1401SG (manufactured by Toagosei Co., Ltd.). Examples of the epoxy resin include 1500 (manufactured by Cemedine Co., Ltd.). Examples of the polyester resin include PH-413 (manufactured by Nippon Matai Co., Ltd.).
[0149] From the viewpoint of minimizing contamination of the adhesive tape on the adherend, the hot-melt pressure-sensitive adhesive layer preferably does not contain an organosilicon compound, or the content of the organosilicon compound in the hot-melt pressure-sensitive adhesive layer is preferably 3.0 mass% or less. When the hot-melt pressure-sensitive adhesive layer contains an organosilicon compound, the upper limit of the content is more preferably 1.0 mass%. It is particularly preferred that the hot-melt pressure-sensitive adhesive layer does not contain an organosilicon compound.
[0150] From the viewpoint of further improving adhesive strength, the hot melt pressure-sensitive adhesive layer preferably further contains a tackifier resin (T4). Examples of the tackifier resin (T4) include those similar to the tackifier resin (T2) and tackifier resin (T3) described above.
[0151] When the base polymer (P3) contains the (meth)acrylic copolymer, the hot-melt pressure-sensitive adhesive layer preferably further contains a curing agent, which allows the (meth)acrylic copolymer to form a chemically crosslinked structure, thereby further improving the adhesive strength of the resulting pressure-sensitive adhesive tape.
[0152] The curing agent contained in the hot melt pressure-sensitive adhesive layer may be, for example, the same as the curing agent contained in the first pressure-sensitive adhesive layer or the second pressure-sensitive adhesive layer.
[0153] The hot melt pressure-sensitive adhesive layer may contain conventionally known fine particles and additives, such as inorganic fine particles, conductive fine particles, antioxidants, foaming agents, organic fillers, and inorganic fillers, as needed.
[0154] The probe tack value of the hot-melt pressure-sensitive adhesive layer measured under conditions of 23°C, a pressure of 98 gf, a pressure rate of 100 mm / sec, a pressure time of 10 seconds, and a peel rate of 5 mm / sec (hereinafter sometimes simply referred to as the "probe tack value of the hot-melt pressure-sensitive adhesive layer at 23°C") is preferably 20 N / 5 mmφ. When the probe tack value of the hot-melt pressure-sensitive adhesive layer at 23°C is 20 N / 5 mmφ or less, the stickiness of the hot-melt pressure-sensitive adhesive layer can be suppressed, thereby improving the adhesiveness of the pressure-sensitive adhesive tape of the present invention. The upper limit of the probe tack value of the hot-melt pressure-sensitive adhesive layer at 23°C is more preferably 15 N / 5 mmφ, and even more preferably 10 N / 5 mmφ. The lower limit of the probe tack value of the hot-melt pressure-sensitive adhesive layer at 23°C is preferably 0.01 N / 5 mmφ. When the hot-melt pressure-sensitive adhesive layer has a probe tack value of 0.01 N / 5 mmφ or more at 23°C, the hot-melt pressure-sensitive adhesive layer has appropriate adhesive strength, and from the viewpoint of easier adjustment of the application position of the pressure-sensitive adhesive tape of the present invention, application workability is improved. A more preferred lower limit of the probe tack value of the hot-melt pressure-sensitive adhesive layer at 23°C is 0.1 N / 5 mmφ, and an even more preferred lower limit of the probe tack value of the hot-melt pressure-sensitive adhesive layer at 23°C is 1.0 N / 5 mmφ. The probe tack value of the hot-melt pressure-sensitive adhesive layer at 23°C can be measured by the same method as for the probe tack value of the second pressure-sensitive adhesive layer described above.
[0155] Methods for adjusting the probe tack value at 23°C of the hot-melt pressure-sensitive adhesive layer include changing the composition, weight-average molecular weight, or molecular weight distribution of the base polymer (P3), changing the type and content ratio of the tackifier resin (T4), changing the type and content of the fine particles and additives to be blended, changing the thickness of the hot-melt pressure-sensitive adhesive layer, changing the storage modulus or glass transition temperature, changing the crosslinking density, or changing the surface roughness.
[0156] The thickness of the hot-melt pressure-sensitive adhesive layer is preferably 20 μm at its lower limit and 500 μm at its upper limit. By setting the thickness of the hot-melt pressure-sensitive adhesive layer within this range, the hot-melt pressure-sensitive adhesive layer can have sufficient adhesive strength. The thickness of the hot-melt pressure-sensitive adhesive layer is more preferably 25 μm at its lower limit, more preferably 300 μm at its upper limit, even more preferably 100 μm at its upper limit, and even more preferably 80 μm at its upper limit.
[0157] When the pressure-sensitive adhesive tape of the present invention has the substrate, the first pressure-sensitive adhesive layer, and the hot-melt pressure-sensitive adhesive layer in this order, it may have an intermediate layer between the first pressure-sensitive adhesive layer and the hot-melt pressure-sensitive adhesive layer. The presence of the intermediate layer improves the reworkability of the resulting pressure-sensitive adhesive tape. Examples of the intermediate layer include the same intermediate layer as the intermediate layer in the pressure-sensitive adhesive tape having the substrate, the first pressure-sensitive adhesive layer, the intermediate layer, and the second pressure-sensitive adhesive layer in this order.
[0158] The method for producing the pressure-sensitive adhesive tape of the present invention is not particularly limited, and for example, in the case of a pressure-sensitive adhesive tape having a substrate and a first pressure-sensitive adhesive layer adjacent to one surface of the substrate, the following method can be mentioned. First, a solvent is added to a (meth)acrylic copolymer, a tackifier resin (T1), a tackifier resin (T2), a curing agent, etc. to prepare a pressure-sensitive adhesive solution (a), and this pressure-sensitive adhesive solution is applied to one surface of the substrate, and the solvent in the solution is completely dried and removed to form a first pressure-sensitive adhesive layer. Next, a release film is superimposed on the formed pressure-sensitive adhesive layer with its release-treated surface facing the pressure-sensitive adhesive layer, thereby obtaining a pressure-sensitive adhesive tape having a substrate and a first pressure-sensitive adhesive layer adjacent to one surface of the substrate.
[0159] The step of applying the adhesive solution to one surface of the substrate may be completed in one step, or may be performed multiple times, with the adhesive solution being applied so as to overlap the applied adhesive solution. By adjusting the number of application steps, the thickness of the first adhesive layer can be easily adjusted. Furthermore, the thickness of the second adhesive layer and the hot-melt adhesive layer can also be easily adjusted by adjusting the number of adhesive application steps during the manufacturing process of the adhesive tape.
[0160] The pressure-sensitive adhesive tape of the present invention may be in the form of a roll. Since the pressure-sensitive adhesive tape of the present invention is in the form of a roll, it can be shipped in a long, wound form, and can be appropriately unwound from the pressure-sensitive adhesive tape roll and cut into an appropriate shape for use. When the pressure-sensitive adhesive tape of the present invention is in the form of a roll, examples of the manufacturing method include a method in which the pressure-sensitive adhesive tape is wound around a core after undergoing a step of applying an adhesive, a step of cutting with a slitter cutter, or a step of rewinding, etc.
[0161] The adhesive tape of the present invention is not particularly limited in its applications, but since it has a substrate including a film containing a fluororesin, it is suitable for bonding fluororesins to dissimilar materials for various purposes. More specifically, the various purposes include promoting the sliding of friction surfaces, preventing friction between sliding parts, insulating coating, and protecting adherends from high temperatures and chemical solutions. It is particularly suitable for protecting adherends, particularly from chemical solutions. The adherends to be protected from chemical solutions are not particularly limited, but examples include can bodies, trays, and walls. Specifically, it is suitable for use as a coating material for semiconductor chemical tanks, chemical tanks for the chemical industry, and pipes for transporting chemical solutions, as a coating material for electronic device components, and as a building material. Among these, the adhesive tape of the present invention is preferably used for lining the can bodies of semiconductor chemical tanks or chemical tanks for the chemical industry (surface treatment for covering the inner surface of the can body). Furthermore, when the pressure-sensitive adhesive tape of the present invention has a hot-melt pressure-sensitive adhesive layer on the outermost surface, the resulting pressure-sensitive adhesive tape also has excellent lamination workability, and is more preferably used for lining the can body of a chemical liquid tank for semiconductors or a chemical liquid tank for the chemical industry. A chemical liquid tank having the pressure-sensitive adhesive tape of the present invention attached to the inner surface of a can body also constitutes one aspect of the present invention.
[0162] The present invention also relates to a method for manufacturing a chemical tank for semiconductors or a chemical industry, which includes a step of attaching the adhesive tape of the present invention to the inner surface of a can body of the chemical tank. Because the adhesive tape has a substrate including a resin film containing a fluororesin, the method for manufacturing a chemical tank of the present invention includes a step of attaching the adhesive tape to the inner surface of a can body of the chemical tank. This eliminates the need for an adhesion-facilitating treatment on the fluororesin when joining the fluororesin to the can body of the chemical tank, making it easy to join the fluororesin. Furthermore, when the adhesive tape has a hot-melt adhesive layer on its outermost surface, the adhesive tape has excellent lamination workability. Therefore, the method for manufacturing a chemical tank of the present invention includes a step of attaching the adhesive tape to the inner surface of the can body of the chemical tank, making it easy to adjust the position where the fluororesin is joined to the can body of the chemical tank.
[0163] According to the present invention, it is possible to provide an adhesive tape that has excellent holding performance, is less likely to contaminate an adherend, and can easily bond a fluororesin. Also, according to the present invention, it is possible to provide a chemical liquid tank to which the adhesive tape is attached. Furthermore, according to the present invention, it is possible to provide a method for manufacturing a chemical liquid tank using the adhesive tape.
[0164] FIG. 1 is a schematic diagram showing a method for a retention test.
[0165] The following examples will explain the present invention in more detail, but the present invention is not limited to these examples.
[0166] (Preparation of Acrylic Copolymer) (Synthesis Example 1) 100 parts by mass of ethyl acetate was placed in a reactor equipped with a thermometer, a stirrer, and a condenser. The atmosphere was replaced with nitrogen, and the reactor was heated to initiate reflux. 30 minutes after the ethyl acetate boiled, 0.08 parts by mass of azobisisobutyronitrile was added as a polymerization initiator. A monomer mixture of the structural unit monomers shown in Table 1 was added dropwise evenly and gradually over 1 hour and 30 minutes to allow the reaction to proceed. 30 minutes after the dropwise addition was completed, 0.1 parts by mass of azobisisobutyronitrile was added, and the polymerization reaction was allowed to proceed for an additional 5 hours. Ethyl acetate was added to the reactor to dilute the mixture while cooling, yielding an acrylic copolymer solution with a solids content of 25% by mass. The resulting acrylic copolymer solution was filtered through a filter (material: polytetrafluoroethylene, pore diameter: 0.2 μm). The obtained filtrate was supplied to a gel permeation chromatograph (Waters, 2690 Separations Module), and GPC measurement was performed under conditions of a sample flow rate of 1 mL / min and a column temperature of 40°C. The polystyrene-equivalent molecular weight of the acrylic copolymer was measured, and the weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) were determined. A GPC KF-806L (Showa Denko KK) was used as the column, and a differential refractometer was used as the detector. The results are shown in Table 1.
[0167] (Synthesis Examples 2 to 10) Acrylic copolymers were obtained in the same manner as in Synthesis Example 1, except that the monomer mixture was changed as shown in Table 1. The results are shown in Table 1.
[0168] The structural unit monomers shown in Table 1 are as follows: BA: n-butyl acrylate, 2EHA: 2-ethylhexyl acrylate, LA: lauryl acrylate, nHA: n-heptyl acrylate, HEA: 2-hydroxyethyl acrylate, AAc: acrylic acid.
[0169]
[0170] (Preparation of Tackifier Resin (T1)) (Synthesis Example A) 50 parts by mass of toluene was placed in a reactor equipped with a thermometer, a stirrer, and a condenser, and the atmosphere was replaced with nitrogen. The reactor was then heated to initiate reflux. After 30 minutes, aluminum chloride (AlCl) was added to the toluene while maintaining the temperature at 75°C. 32 parts by mass of catechol (pyrocatechol) (n=2) and α-pinene (50 parts by mass in total, the molar ratio is as shown in Table 2) dissolved in 50 parts by mass of toluene was gradually added dropwise to the reactor over 1 hour and 30 minutes to allow the reaction to proceed. After the polymerization reaction had continued for 4 hours, the reactor was cooled while 0.1 parts by mass of pyridine was added to the reactor, and aluminum chloride (AlCl 3 The hydrochloric acid generated from the reaction mixture was neutralized. The precipitate formed by the neutralization was filtered, and the obtained filtrate was subjected to a liquid separation operation. Then, the toluene was evaporated to obtain a solid tackifier resin (T1). Regarding the obtained tackifier resin (T1), 1 H-NMR measurement was performed to confirm that the tackifier resin (T1) was a copolymer having a structural unit (A) derived from catechol (pyrocatechol) and a structural unit (B) derived from α-pinene (a copolymer having the structural unit (A) in the main chain skeleton or at the end of the main chain skeleton). A solution of the obtained tackifier resin (T1) dissolved in tetrahydrofuran was filtered through a filter (material: polytetrafluoroethylene, pore diameter: 0.2 μm). The obtained filtrate was supplied to a gel permeation chromatograph (Waters, 2690 Separations Module), and GPC measurement was performed under conditions of a sample flow rate of 1 mL / min and a column temperature of 40 °C. The polystyrene-equivalent molecular weight of the tackifier resin (T1) was measured, and the weight average molecular weight (Mw) was determined. A GPC KF-802.5L (Showa Denko KK) was used as the column, and a differential refractometer was used as the detector. The results are shown in Table 2.
[0171] (Measurement of Bio-derived Carbon Content of Tackifier Resin (T1)) The bio-derived carbon content of the obtained tackifier resin (T1) was measured in accordance with ASTM D6866-22. The results are shown in Table 2.
[0172] (Synthesis Examples B to C and E) Tackifier resin (T1) was synthesized and measured in the same manner as in Synthesis Example A above (Preparation of tackifier resin (T1)), except that the monomers were changed as shown in Table 2. The results are shown in Table 2.
[0173] Synthesis Example D Preparation of Tackifier Resin (T1) 50 parts by mass of toluene was placed in a reactor equipped with a thermometer, a stirrer, and a condenser, and the atmosphere was replaced with nitrogen. The reactor was then heated to initiate reflux. After 30 minutes, aluminum chloride (AlCl) was added to the toluene while maintaining the temperature at 75°C. 3 2 parts by mass of 4-vinylbenzoic acid (m=1) and α-pinene (70 parts by mass in total, the molar ratio is as shown in Table 2) dissolved in 50 parts by mass of toluene was gradually added dropwise to the reactor over 1 hour and 30 minutes to allow the reaction to proceed. After the polymerization reaction had been carried out for 4 hours, the reactor was cooled while 0.1 parts by mass of pyridine was added to the reactor, and aluminum chloride (AlCl 3 The hydrochloric acid generated from the reaction mixture was neutralized. The precipitate formed by the neutralization was filtered, and the obtained filtrate was subjected to a liquid separation operation. Then, the toluene was evaporated to obtain a solid tackifier resin (T1). Regarding the obtained tackifier resin (T1), 1 H-NMR measurement was performed to confirm that the tackifier resin (T1) was a copolymer having a structural unit (A) derived from 4-vinylbenzoic acid and a structural unit (B) derived from α-pinene (a copolymer having the structural unit (A) in its side chain). A solution of the obtained tackifier resin (T1) dissolved in tetrahydrofuran was filtered through a filter (material: polytetrafluoroethylene, pore diameter: 0.2 μm). The obtained filtrate was supplied to a gel permeation chromatograph (Waters, 2690 Separations Module), and GPC measurement was performed under conditions of a sample flow rate of 1 mL / min and a column temperature of 40°C. The polystyrene-equivalent molecular weight of the tackifier resin (T1) was measured, and the weight average molecular weight (Mw) was determined. A GPC KF-802.5L (Showa Denko KK) was used as the column, and a differential refractometer was used as the detector. The results are shown in Table 2.
[0174] (Measurement of Bio-derived Carbon Content of Tackifier Resin (T1)) The bio-derived carbon content of the obtained tackifier resin (T1) was measured in accordance with ASTM D6866-22. The results are shown in Table 2.
[0175]
[0176] Example 1 (1) Preparation of Adhesive Tape 20 parts by mass of tackifier resin (T2) (Arakawa Chemical Industries, Ltd., "Pine Crystal KE-359") was added to 100 parts by mass of the solids content of the acrylic copolymer (Synthesis Example 1). Furthermore, 30 parts by mass of ethyl acetate (Fuji Chemical Industries, Ltd.) and 1.0 part by mass of an isocyanate-based curing agent (Tosoh Corporation, "Coronate L45") were added and thoroughly stirred to obtain an adhesive solution. The resulting adhesive solution was applied to a 50 μm-thick PTFE sheet (Yodogawa Hutech Co., Ltd., "Yodoflon") and dried at 100°C for 5 minutes to form a 50 μm-thick first adhesive layer. Furthermore, a 150 μm-thick release PET film was prepared, and the film was placed on the first adhesive layer with a release-treated surface. The film was then heated at 40°C for 48 hours to cure. This produced an adhesive tape having a substrate and a first adhesive layer on one surface of the substrate, the surface of the first adhesive layer being covered with a release PET film.
[0177] (2) Measurement of 180° Peel Strength of First Pressure-Sensitive Adhesive Layer from Substrate at 23°C The obtained pressure-sensitive adhesive tape was cut into a size of 25 mm wide x 100 mm long. After peeling off the release PET film, a 2 kg rubber roller was used to press the cut pressure-sensitive adhesive tape onto a 50 μm thick PET film by rolling it back and forth once at a speed of 300 mm / min. The cut pressure-sensitive adhesive tape was then left to stand for 20 minutes in an environment of 23°C and 50% RH to age the tape, thereby preparing a test sample. The obtained test sample was subjected to a 180° peel test in accordance with JIS Z0237 using a tensile tester (manufactured by ORIENTEC, "Tensilon") under conditions of 23°C, 50% RH, and a peel speed of 300 mm / min. The first pressure-sensitive adhesive layer was peeled off from the substrate, and the 180° peel strength (N / 25 mm) of the first pressure-sensitive adhesive layer from the substrate at 23°C was measured. The results are shown in Table 3.
[0178] (3) Measurement of the Peak Temperature of the Loss Tangent (tan δ) of the First Pressure-Sensitive Adhesive Layer Measured at a Frequency of 10 Hz The pressure-sensitive adhesive solution prepared in the above-described "(1) Preparation of Pressure-Sensitive Adhesive Tape" was applied to a 50 μm-thick release PET film and dried at 100°C for 5 minutes to form a 50 μm-thick first pressure-sensitive adhesive layer. The formed first pressure-sensitive adhesive layer was then laminated to a thickness of 1 mm to prepare a measurement sample consisting of only the pressure-sensitive adhesive layer. The dynamic viscoelasticity spectrum of the obtained measurement sample was measured from -100°C to 200°C using a viscoelasticity spectrometer (manufactured by IT Measurement & Control Co., Ltd., "DVA-200") under shear mode, a heating rate of 5°C / min, and a measurement frequency of 10 Hz. The peak temperature (°C) of the loss tangent (tan δ) was obtained from the obtained dynamic viscoelasticity spectrum. The results are shown in Table 3.
[0179] (4) Measurement of shear storage modulus of first pressure-sensitive adhesive layer at 25°C The pressure-sensitive adhesive solution prepared in the above-mentioned "(1) Preparation of pressure-sensitive adhesive tape" was applied to a 50 μm-thick release PET film and dried at 100°C for 5 minutes to form a 50 μm-thick first pressure-sensitive adhesive layer, and the formed first pressure-sensitive adhesive layer was laminated to a thickness of 1 mm to prepare a measurement sample consisting of only the first pressure-sensitive adhesive layer. The dynamic viscoelasticity spectrum of the obtained measurement sample was measured from -100°C to 200°C using a viscoelasticity spectrometer (manufactured by IT Measurement & Control Co., Ltd., "DVA-200") under conditions of shear mode, heating rate of 5°C / min, and measurement frequency of 10 Hz, and the shear storage modulus (×10) at 25°C was calculated from the obtained dynamic viscoelasticity spectrum. 4 The results are shown in Table 3.
[0180] (5) Measurement of gel fraction of first pressure-sensitive adhesive layer A test piece was prepared by cutting the pressure-sensitive adhesive tape into a flat rectangular shape of 50 mm wide x 100 mm long. The test piece was immersed in ethyl acetate at 23°C for 24 hours, then removed from the ethyl acetate and dried at 110°C for 1 hour. The mass of the test piece after drying was measured, and the gel fraction (mass %) was calculated using the following formula (1). Note that no release film for protecting the first pressure-sensitive adhesive layer was laminated on the test piece. The results are shown in Table 3. Gel fraction (mass %) = 100 × (W2 -W 0 ) / (W 1 -W 0 ) (1) (W 0 : Mass of the substrate, W 1 : mass of test piece before immersion, W 2 : Mass of test piece after immersion and drying)
[0181] (Examples 2 to 46, Comparative Examples 1 to 4) Pressure-sensitive adhesive tapes were prepared and measurements were carried out in the same manner as in Example 1, except that in the above-mentioned "(1) Preparation of pressure-sensitive adhesive tapes", the composition of the first pressure-sensitive adhesive layer and the type and thickness of the substrate were changed as shown in Tables 3 to 5 and 9. The results are shown in Tables 3 to 5 and 9.
[0182] (Example 47) (1) Preparation of adhesive tape To 100 parts by mass of the solid content of the acrylic copolymer (Synthesis Example 1), 20 parts by mass of tackifier resin (T2) (Arakawa Chemical Industries, Ltd., "Pine Crystal KE-359") was added. Furthermore, 30 parts by mass of ethyl acetate (Fuji Chemical Industries, Ltd.) and 1.0 parts by mass of an isocyanate curing agent (Tosoh Corporation, "Coronate L45") were added and thoroughly stirred to obtain an adhesive solution (a). The obtained adhesive solution (a) was applied to a 50 μm thick PTFE sheet (Yodogawa Hutech Co., Ltd., "Yodoflon") and dried at 100 ° C. for 5 minutes to produce a laminate film (a) having a 50 μm thick first adhesive layer, and then a 50 μm thick PET film (Futamura Chemical Co., Ltd., FE2002) was laminated so that the first adhesive layer faced each other to obtain a laminate. Similarly, 10 parts by weight of tackifier resin (T3) (Yasuhara Chemical Co., Ltd., "YS Polystar G150") was added to 100 parts by weight of the solids of the acrylic copolymer (Synthesis Example 1), and 30 parts by weight of ethyl acetate (Fuji Chemical Co., Ltd.) and 1.0 part by weight of an isocyanate-based curing agent (Tosoh Corporation, "Coronate L45") were added. The mixture was thoroughly stirred to obtain a pressure-sensitive adhesive solution (b). The pressure-sensitive adhesive solution (b) was applied to the release-treated surface of a 50 μm-thick release PET film and dried at 100°C for 5 minutes to produce a laminate film (b) having a 20 μm-thick second pressure-sensitive adhesive layer. The laminate film (b) was then placed on the PET film side of the laminate, with the second pressure-sensitive adhesive layer facing the PET film, and the laminate was aged at 40°C for 48 hours to produce a pressure-sensitive adhesive tape having a substrate, a first pressure-sensitive adhesive layer, an intermediate layer, and a second pressure-sensitive adhesive layer, in that order.
[0183] (2) Measurement of 180° peel strength of first pressure-sensitive adhesive layer from substrate at 23° C. The 180° peel strength (N / 25 mm) of the first pressure-sensitive adhesive layer from a substrate at 23° C. was measured in the same manner as in Example 1, except that the laminate described above in "(1) Preparation of pressure-sensitive adhesive tape" was used as the test sample. The results are shown in Table 6.
[0184] (3) Measurement of Peak Temperature of Loss Tangent (tan δ) of First Pressure-Sensitive Adhesive Layer at a Frequency of 10 Hz The peak temperature (°C) of the loss tangent (tan δ) of the first pressure-sensitive adhesive layer at a frequency of 10 Hz was measured in the same manner as in Example 1. The results are shown in Table 6.
[0185] (4) Measurement of shear storage modulus of first pressure-sensitive adhesive layer at 25°C
[0112] The shear storage modulus of the first pressure-sensitive adhesive layer at 25°C (×10 4 The results are shown in Table 6.
[0186] (5) Measurement of gel fraction of first pressure-sensitive adhesive layer The gel fraction (% by mass) of the first pressure-sensitive adhesive layer was measured in the same manner as in Example 1, except that test pieces were prepared by cutting the laminate film (a) described above in "(1) Preparation of pressure-sensitive adhesive tape" instead of the pressure-sensitive adhesive tape. The results are shown in Table 6.
[0187] (6) Measurement of 180° Peel Strength of Second Pressure-Sensitive Adhesive Layer from SUS at 23°C The resulting pressure-sensitive adhesive tape was cut into a size of 25 mm wide x 100 mm long. A 2 kg rubber roller was used to press the tape against a SUS plate (a SUS304 plate washed with ethanol and then wiped dry) by rolling it back and forth once at a speed of 300 mm / min. The tape was then left to stand for 20 minutes at 23°C and 50% RH to prepare a test sample. The resulting test sample was subjected to a 180° peel test in accordance with JIS Z0237 using a tensile tester (Tensilon, manufactured by ORIENTEC Co., Ltd.) at 23°C, 50% RH, and a peel speed of 300 mm / min. The 180° peel strength (N / 25 mm) of the second pressure-sensitive adhesive layer from SUS at 23°C was measured by peeling the pressure-sensitive adhesive tape from the SUS plate. The results are shown in Table 6.
[0188] (7) Measurement of probe tack value of second pressure-sensitive adhesive layer at 23°C The obtained pressure-sensitive adhesive tape was cut to a size of 30 mm wide x 30 mm long to prepare a test piece. A probe tack test was performed on the second pressure-sensitive adhesive layer of the prepared test piece using a probe tack tester (manufactured by RHESCA, "TAC-2") under conditions of 23°C, pressure of 98 gf, pressure rate of 100 mm / sec, pressure time of 10 seconds, and peel rate of 5 mm / sec, and the probe tack value of the second adhesive layer at 23°C was measured. The results are shown in Table 6.
[0189] (Examples 48 to 80, Comparative Examples 5 to 7) Pressure-sensitive adhesive tapes were prepared and measurements were carried out in the same manner as in Example 47, except that in the above-mentioned "(1) Preparation of pressure-sensitive adhesive tapes", the composition and thickness of each layer were changed as shown in Tables 6 to 7 and 9. The results are shown in Tables 6 to 7 and 9.
[0190] (Example 81) An adhesive tape was produced and measured in the same manner as in Example 45, except that in the above-mentioned "(1) Production of adhesive tape", the intermediate layer was changed to a closed-cell PE foam (WL02, manufactured by Sekisui Chemical Co., Ltd.). The results are shown in Table 7.
[0191] An adhesive tape was prepared and measurements were carried out in the same manner as in Example 47, except that in the above-mentioned "(1) Preparation of adhesive tape", laminate film (a) and laminate film (b) were overlapped with each other so that the first adhesive layer and the second adhesive layer faced each other, and the resulting mixture was aged at 40°C for 48 hours to prepare an adhesive tape, and that in the above-mentioned "(2) Measurement of 180° peel strength of first adhesive layer from substrate at 23°C", laminate film (a) was used instead of the adhesive tape and the measurement was carried out in the same manner as in Example 1. The results are shown in Table 7.
[0192] (Example 83) (1) Preparation of adhesive tape To 100 parts by mass of the solid content of the acrylic copolymer (Synthesis Example 2), 10 parts by mass of tackifier resin (T1) (Synthesis Example B) was added. Furthermore, 30 parts by mass of ethyl acetate (manufactured by Fuji Chemical Co., Ltd.) and 0.5 parts by mass of an isocyanate-based curing agent (manufactured by Covestro, "Desmodur L-75") were added and thoroughly stirred to obtain an adhesive solution (a). The obtained adhesive solution (a) was applied to a 50 μm thick PTFE sheet (manufactured by Yodogawa Hutech Co., Ltd., "Yodoflon") and dried at 100 ° C. for 5 minutes to prepare a laminated film (a) having a first adhesive layer of 50 μm thickness, and then a 50 μm thick PET film (manufactured by Futamura Chemical Co., Ltd., "FE2002") was laminated so that the first adhesive layer faced each other to obtain a laminate. Similarly, 10 parts by weight of tackifier resin (T4) (Yasuhara Chemical Co., Ltd., "YS Polystar G150") was added to 100 parts by weight of the solids content of the acrylic copolymer (Synthesis Example 10), and 30 parts by weight of ethyl acetate (Fuji Chemical Co., Ltd.) and 1.0 part by weight of an isocyanate-based curing agent (Tosoh Corporation, "Coronate L45") were added. The mixture was thoroughly stirred to obtain a pressure-sensitive adhesive solution (c). The pressure-sensitive adhesive solution (c) was applied to the release-treated surface of a 50 μm-thick release PET film and dried at 100°C for 5 minutes to produce a laminate film (c) having a 20 μm-thick hot-melt pressure-sensitive adhesive layer. The laminate film (c) was then overlaid on the PET film side of the laminate with the hot-melt pressure-sensitive adhesive layer facing the PET film, and the mixture was aged at 40°C for 48 hours to produce a pressure-sensitive adhesive tape having a substrate, a first pressure-sensitive adhesive layer, an intermediate layer, and a hot-melt pressure-sensitive adhesive layer in this order.
[0193] (2) Measurement of 180° peel strength of first pressure-sensitive adhesive layer from substrate at 23° C. The 180° peel strength (N / 25 mm) of the first pressure-sensitive adhesive layer from a substrate at 23° C. was measured in the same manner as in Example 1, except that the laminate described above in "(1) Preparation of pressure-sensitive adhesive tape" was used as the test sample. The results are shown in Table 8.
[0194] (3) Measurement of Peak Temperature of Loss Tangent (tan δ) of First Pressure-Sensitive Adhesive Layer at a Frequency of 10 Hz The peak temperature (°C) of the loss tangent (tan δ) of the first pressure-sensitive adhesive layer at a frequency of 10 Hz was measured in the same manner as in Example 1. The results are shown in Table 8.
[0195] (4) Measurement of shear storage modulus of first pressure-sensitive adhesive layer at 25°C
[0112] The shear storage modulus of the first pressure-sensitive adhesive layer at 25°C (×10 4 The results are shown in Table 8.
[0196] (5) Measurement of gel fraction of first pressure-sensitive adhesive layer The gel fraction (% by mass) of the first pressure-sensitive adhesive layer was measured in the same manner as in Example 45. The results are shown in Table 8.
[0197] (6) Measurement of 180° peel strength of hot-melt pressure-sensitive adhesive layer against SUS at 23° C. The 180° peel strength (N / 25 mm) of the hot-melt pressure-sensitive adhesive layer against SUS at 23° C. was measured in the same manner as in Example 45, except that the measurement object was changed to a hot-melt pressure-sensitive adhesive layer. The results are shown in Table 8.
[0198] (7) Measurement of 180° peel force against SUS at 23°C after heating of hot-melt pressure-sensitive adhesive layer The obtained pressure-sensitive adhesive tape was cut to a size of 25 mm wide x 100 mm long, and then the first pressure-sensitive adhesive layer was backed with a 23 μm thick PET film (manufactured by Futamura Chemical Co., Ltd., "FE2002"), and the hot-melt pressure-sensitive adhesive layer was pressure-bonded to a SUS plate (a SUS304 plate that had been washed with ethanol and then wiped dry) by applying pressure at 0.1 MPa for 10 minutes in an environment of 150°C, followed by air-cooling to prepare a test sample. The obtained test samples were subjected to a 180° peel test in accordance with JIS Z0237 using a tensile tester ("Tensilon" manufactured by ORIENTEC Co., Ltd.) under conditions of 23°C, 50% RH, and a peel rate of 300 mm / min, and the 180° peel strength (N / 25 mm) from SUS at 23°C after heating of the hot-melt pressure-sensitive adhesive layer was measured by peeling the pressure-sensitive adhesive tape from the SUS plate. The results are shown in Table 8.
[0199] (Examples 84 to 85) Pressure-sensitive adhesive tapes were produced and measurements were carried out in the same manner as in Example 83, except that in the above-mentioned "(1) Production of Pressure-sensitive Adhesive Tape", the composition and thickness of each layer were changed as shown in Table 8. The results are shown in Table 8. In Example 85, a hot-melt pressure-sensitive adhesive layer was formed by directly applying 100 parts by mass of chloroprene rubber (manufactured by Cemedine Co., Ltd., "575F") directly to the release-treated surface of a 50 μm-thick release PET film, thereby producing a laminated film (c).
[0200] Examples 86 to 88 Pressure-sensitive adhesive tapes were prepared and measurements were carried out in the same manner as in Example 83, except that in the above-mentioned "(1) Preparation of Pressure-sensitive Adhesive Tape," the laminate film (a) and the laminate film (c) were overlapped with each other so that the first pressure-sensitive adhesive layer and the hot-melt pressure-sensitive adhesive layer faced each other, and the laminate film (c) was cured at 40°C for 48 hours to prepare a pressure-sensitive adhesive tape, and in the above-mentioned "(2) Measurement of the 180° peel strength of the first pressure-sensitive adhesive layer from the substrate at 23°C," the laminate film (a) was used instead of the pressure-sensitive adhesive tape, and measurements were carried out in the same manner as in Example 1. The results are shown in Table 8. The base polymer of the hot-melt pressure-sensitive adhesive layer shown in Table 8 was directly applied to the release-treated surface of a 50 μm-thick release PET film to form a hot-melt pressure-sensitive adhesive layer, and the laminate film (c) was prepared.
[0201]
[0202]
[0203]
[0204]
[0205]
[0206]
[0207]
[0208] <Evaluation> The pressure-sensitive adhesive tapes obtained in the examples and comparative examples were evaluated by the following methods. The results are shown in Tables 10 to 15.
[0209] (1) Retention Performance (1-1) Slippage The resulting adhesive tape was cut into 25 mm wide strips and then bonded to a SUS plate (SUS304 plate washed with ethanol and then wiped dry) by rolling a 2 kg rubber roller back and forth once at a speed of 300 mm / min. Next, an incision was made in the adhesive tape so that the adhesive area was 25 mm x 25 mm, and the tape was left to stand at 23 °C for 20 minutes to prepare a test sample. The prepared test sample was placed in an oven at 80 °C and heated for an additional 20 minutes. After heating at 80 °C and 50% RH, a 1 kg weight was hung from the tape and a load was applied in the shear direction as shown in Figure 1. The amount of slippage (movement) (mm) from the incision position one hour after the load was applied was measured using a scale magnifier. For Examples 83 to 88, which had a hot-melt pressure-sensitive adhesive layer on the outermost surface, test samples were prepared by making cuts in the pressure-sensitive adhesive tape and then heat-curing it for 10 minutes under conditions of 150°C and 0.1 MPa. Using the obtained slippage (mm), the holding performance of the pressure-sensitive adhesive tape was evaluated according to the following criteria: ◎: The slippage was 0.5 mm or less. ○: The slippage was more than 0.5 mm and 1.0 mm or less. △: The slippage was more than 1.0 mm and 2.0 mm or less. ×: The slippage was greater than 2.0 mm.
[0210] (1-2) Position where displacement occurred After the pressure-sensitive adhesive tape retention test in "(1-1) Amount of displacement" described above, the pressure-sensitive adhesive tape in the test sample was visually observed, and the position where displacement occurred was judged according to the following criteria. A: Displacement occurred between the SUS and the pressure-sensitive adhesive layer in contact with the SUS. B: Displacement occurred between the substrate and the first pressure-sensitive adhesive layer. C: Displacement occurred in the first pressure-sensitive adhesive layer or the second pressure-sensitive adhesive layer. In terms of adhesive reliability to the substrate and adherend at high temperatures, a rating of "C" is preferred, but even if the rating is "B," the pressure-sensitive adhesive tape of the present invention can be used without any problems.
[0211] (2) Contamination of Adherends After the adhesive tape retention test in "(1) Retention Performance" above, the surface from which the adhesive tape had been peeled was measured using a scanning X-ray photoelectron spectrometer ("PHI 5000 VersaProbe II" manufactured by ULVAC-PHI, Inc.) to measure the silicon atom concentration (at%) of the SUS plate surface from which the adhesive tape had been peeled. XPS measurements were performed under the following conditions. <Measurement Conditions> X-ray source: Monochromated AlKα (1486.6 eV) Spectrometer: Electrostatic concentric hemispherical analyzer Photoelectron take-off angle: 45 degrees Charge neutralization: Yes X-ray beam diameter: 200 μm Pass energy: 117 eV The obtained silicon atom concentration (at%) was used to evaluate the contamination of the adhesive tape on the adherend according to the following criteria: ○: The silicon atom concentration was 0.1 at% or less. △: The silicon atom concentration was greater than 0.1 at% and 1.0 at% or less. ×: The silicon atom concentration was greater than 1.0 at %.
[0212] (3) Reworkability The obtained pressure-sensitive adhesive tape was cut into a size of 25 mm wide x 100 mm long. A 2 kg rubber roller was used to press the second pressure-sensitive adhesive layer onto a SUS plate (a SUS304 plate that had been washed with ethanol and then wiped dry) by rolling it back and forth once at a speed of 300 mm / min. The test sample was then left to stand for 20 minutes at 23°C and 50% RH to cure, thereby preparing a test sample. The obtained test sample was subjected to a 180° peel test in accordance with JIS Z0237 using a tensile tester (manufactured by ORIENTEC, "Tensilon") under conditions of 23°C, 50% RH, and a peeling speed of 300 mm / min. The pressure-sensitive adhesive tape was peeled from the SUS plate, and the reworkability of the pressure-sensitive adhesive tape was evaluated according to the following criteria: ∘: The pressure-sensitive adhesive tape was peeled without breakage and no residue was left on the SUS. Δ: The pressure-sensitive adhesive tape was peeled without breakage, but residue was left on the SUS. ×: The adhesive tape broke during peeling. Note that even if the evaluation is "×", the adhesive tape of the present invention can be used without problems depending on the application. Furthermore, this evaluation was carried out only for Examples 47 to 85 and Comparative Examples 5 to 7.
[0213] (4) Lamination Workability The obtained adhesive tape was cut into a size of 25 mm wide x 100 mm long. The release PET film protecting the first adhesive layer of the cut adhesive tape was peeled off, and the first adhesive layer was pressed onto a 50 mm wide x 200 mm long x 2 mm thick polytetrafluoroethylene plate (manufactured by Yodogawa Hutec Co., Ltd., "Yodoflon") using a 2 kg rubber roller, with a speed of 300 mm / min. A laminate was thus produced. The release PET film protecting the hot-melt adhesive layer of the obtained laminate was then peeled off, and the hot-melt adhesive layer was then pressed onto the laminate using a 5 mmφ SUS probe at 23°C, a pressure of 98 gf, a pressure rate of 100 mm / sec, and a pressure time of 10 seconds. After leaving the tape for 10 minutes in an environment of 23°C and 50% RH, the hot-melt pressure-sensitive adhesive layer was peeled off from the SUS at a peeling speed of 5 mm / sec, and the surface of the hot-melt pressure-sensitive adhesive layer and the adhesive surface between the polytetrafluoroethylene plate and the first pressure-sensitive adhesive layer were observed visually and with an optical microscope. The adhesive tape was evaluated for its surface was not roughened and the adhesive tape did not peel off from the polytetrafluoroethylene plate, with an "O" rating; the adhesive tape was evaluated for its first pressure-sensitive adhesive layer peeling off from the polytetrafluoroethylene plate during the lamination process with an "X" rating. Note that this evaluation was performed only on the pressure-sensitive adhesive tapes having a hot-melt pressure-sensitive adhesive layer, i.e., Examples 83 to 88.
[0214]
[0215]
[0216]
[0217]
[0218]
[0219]
[0220] According to the present invention, it is possible to provide an adhesive tape that has excellent holding performance, is less likely to contaminate an adherend, and can easily bond a fluororesin. Also, according to the present invention, it is possible to provide a chemical liquid tank to which the adhesive tape is attached. Furthermore, according to the present invention, it is possible to provide a method for manufacturing a chemical liquid tank using the adhesive tape.
[0221] 1. Adhesive tape 2. SUS304 plate 3. 1 kg weight
Claims
1. An adhesive tape comprising a substrate and a first adhesive layer adjacent to one surface of the substrate, the substrate comprising a resin film containing a fluororesin, the first adhesive layer comprising a base polymer (P1) and a tackifier resin, the base polymer (P1) comprising at least one member selected from the group consisting of (meth)acrylic copolymers and styrene-based elastomers.
2. The adhesive tape according to claim 1, comprising, in this order, the substrate, the first adhesive layer, an intermediate layer, and a second adhesive layer, the second adhesive layer containing a base polymer (P2), and the base polymer (P2) containing at least one selected from the group consisting of (meth)acrylic copolymers and styrene-based elastomers.
3. An adhesive tape as described in claim 2, wherein the second adhesive layer has a probe tack value of 20 N / 5 mmφ or less measured under conditions of 23°C, pressure of 98 gf, pressure speed of 100 mm / sec, pressure time of 10 seconds, and peel speed of 5 mm / sec.
4. The adhesive tape according to claim 1, comprising the substrate, the first adhesive layer, and a hot melt adhesive layer in this order.
5. An adhesive tape as described in claim 1, 2, 3 or 4, wherein the (meth)acrylic copolymer in the base polymer (P1) has a structural unit derived from an alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms at the ester end, and at least one structural unit selected from the group consisting of a structural unit derived from a carboxyl group-containing (meth)acrylate and a structural unit derived from a hydroxyl group-containing (meth)acrylate.
6. The adhesive tape according to claim 5, wherein the alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms at the ester end comprises an alkyl (meth)acrylate having an alkyl group having 6 to 8 carbon atoms at the ester end.
7. The adhesive tape according to claim 5 or 6, wherein the alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms at the ester terminal includes n-heptyl (meth)acrylate.
8. An adhesive tape as described in claim 6 or 7, wherein the content of structural units derived from alkyl (meth)acrylate having an alkyl group having 6 to 8 carbon atoms at the ester end in the (meth)acrylic copolymer is 50% by mass or more and 99.5% by mass or less.
9. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7 or 8, wherein the tackifier resin comprises a tackifier resin (T1) having at least one structural unit (A) selected from the group consisting of structural unit (A-1), structural unit (A-1'), structural unit (A-2), structural unit (A-2'), structural unit (A-3), structural unit (A-3'), structural unit (A-4), and structural unit (A-4') represented by the following formula: In the formula, R 1 ~R 7 each represents a hydrogen atom, an aliphatic hydrocarbon group, an aromatic hydrocarbon group, a polar functional group, an aliphatic hydrocarbon group having a polar functional group, or an aromatic hydrocarbon group having a polar functional group. n and l each represent an integer of 2 or more and 4 or less, and n' and l' each represent an integer of 2 or more and 5 or less. m and k each represent an integer of 1 or more and 4 or less, and m' and k' each represent an integer of 1 or more and 5 or less. * represents a linking portion.
10. The adhesive tape according to claim 9, wherein the tackifier resin (T1) further comprises a structural unit (B) derived from at least one monomer (b) selected from the group consisting of terpene monomers and vinyl monomers.
11. The adhesive tape according to disclosure 9 or 10, wherein the content of the tackifier resin (T1) is 5 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the base polymer (P1).
12. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or 11, wherein the tackifier resin comprises at least one tackifier resin (T2) selected from the group consisting of rosin ester-based resins, terpene-based resins, terpene phenolic resins, and petroleum-based resins.
13. The adhesive tape according to claim 12, wherein the tackifier resin (T2) contains a rosin ester resin.
14. The adhesive tape according to claim 12 or 13, wherein the softening temperature of the tackifier resin (T2) is 50° C. or higher and 200° C. or lower.
15. An adhesive tape as described in claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13 or 14, wherein the first adhesive layer does not contain an organosilicon compound, or the content of the organosilicon compound in the first adhesive layer is 3.0 mass% or less.
16. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15, wherein the first adhesive layer has a 180° peel strength from the substrate at 23° C. of 2.5 N / 25 mm or more.
17. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 or 16, wherein the first adhesive layer has a peak loss tangent (tan δ) in a temperature range of -30°C or higher and 15°C or lower, measured at a frequency of 10 Hz in dynamic viscoelasticity measurement.
18. The first pressure-sensitive adhesive layer has a shear storage modulus of 1.0 x 10 at 25°C measured at a frequency of 10 Hz in a dynamic viscoelastic measurement. 4 Pa or more 5.0×10 5 18. The pressure-sensitive adhesive tape according to claim 17, wherein the loss tangent (tan δ) measured at a frequency of 10 Hz in dynamic viscoelasticity measurement has a peak in a temperature range of -30°C or more and 15°C or less.
19. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17 or 18, wherein the first adhesive layer has a gel fraction of 15% by mass or more and 70% by mass or less.
20. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18 or 19, wherein the first adhesive layer has a thickness of 20 μm or more and 500 μm or less.
21. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20, wherein the resin film containing a fluororesin includes at least one type selected from the group consisting of a fluororesin-impregnated glass cloth and a laminated film having a fluororesin layer and a glass cloth layer laminated together.
22. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 or 21, wherein the substrate has a thickness of 50 μm or more and 5,000 μm or less.
23. The adhesive tape according to claim 2 or 3, wherein the 180° peel strength of the second adhesive layer against SUS at 23° C. is 8.0 N / 25 mm or less.
24. The adhesive tape according to claim 2, 3 or 23, wherein the second adhesive layer has a thickness of 20 μm or more and 500 μm or less.
25. The adhesive tape according to claim 2, 3, 23 or 24, wherein the intermediate layer contains at least one material selected from the group consisting of polyester resin, polyimide resin, polyolefin resin, polyurethane resin, glass fiber, carbon fiber, and metal.
26. The adhesive tape according to claim 2, 3, 23, 24 or 25, wherein the intermediate layer has a foamed structure.
27. The adhesive tape according to claim 4, wherein the hot melt adhesive layer is bonded to SUS by applying a pressure of 0.1 MPa for 10 minutes in an environment of 150°C, and the 180° peel strength against SUS at 23°C is 5.0 N / 25 mm or more.
28. An adhesive tape as described in claim 4 or 27, wherein the hot melt adhesive layer contains a base polymer (P3), and the base polymer (P3) includes at least one selected from the group consisting of (meth)acrylic copolymers, styrene-based elastomers, ethylene-vinyl acetate copolymers, chloroprene rubber, nitrile rubber, polyurethane resins, polyamide resins, polyolefin resins, polyester resins, and epoxy resins.
29. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27 or 28, which is used for protecting an adherend.
30. The adhesive tape according to claim 29, which is used to protect an adherend from chemical solutions.
31. The adhesive tape according to claim 30, which is used for lining the can body of a chemical tank for semiconductors or a chemical tank for the chemical industry.
32. A chemical tank having the adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 or 31 attached to the inner surface of a can body.
33. A method for manufacturing a chemical tank for semiconductors or a chemical tank for the chemical industry, comprising a step of attaching the adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 or 31 to the inner surface of a can body of the chemical tank.
Citation Information
Patent Citations
Thermally conductive adhesive tape, article and image display device
JP2015021067A
Base material for heat-resistant adhesive tape and heat-resistant adhesive tape composed of the same
JP2015052050A
Double-sided adhesive sheet
JP2015120876A
Corrosion protective lining laminate
JP1984019151A
Resin coated metallic material
JP1986182939A